Fluorine resin and its manufacturing method
A fluororesin with a specific residue unit and low metal content, produced via precipitation polymerization, addresses coloration issues during heating, ensuring high transparency and heat resistance for optical applications.
Patent Information
- Application Number
- JP2023106017
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-06-28
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2039-01-30
AI Technical Summary
Fluororesins containing an oxolane ring suffer from coloration during heating due to residual metal components and polymerization aids, which degrade transparency and heat resistance, making them unsuitable for optical applications.
A fluororesin with a residue unit represented by general formula (1) and a total metal content of chromium, iron, and nickel of 500 mass ppb or less, produced through precipitation polymerization with specific organic solvents and without emulsifiers or dispersants, ensuring high transparency and heat resistance.
The fluororesin exhibits reduced coloring during heating, maintaining excellent optical properties and moldability, with improved fluidity and fillability, suitable for optical applications.
Smart Images

Figure 0007566085000001 
Figure 0007566085000002 
Figure 0007566085000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a fluororesin having few impurities and excellent optical properties, and a method for producing the same. [Background technology]
[0002] Fluorine-based resins have traditionally been used in protective films for semiconductors and other electronic components, water-repellent films for inkjet printing, waterproof and oil-repellent coatings for filters, and optical components due to their excellent electrical and optical properties, chemical resistance, waterproofness, and liquid and oil repellency.
[0003] Among them, fluororesins containing oxolane rings have a bulky ring structure, making them amorphous and highly transparent and heat resistant. In addition, because they are composed only of carbon, fluorine, and oxygen, they have excellent optical properties, electrical properties, chemical resistance, waterproofness, and liquid and oil repellency. Furthermore, because they are amorphous, they can be melt-molded.
[0004] Non-Patent Document 1 describes a fluororesin containing an oxolane ring, and describes that the transparency of the resin decreases when stored in air for more than two weeks, and that the resin turns yellow when heated at 260 to 290°C. It describes that the transparency does not decrease even when the resin is stored in air by reprecipitation purification, removing impurities having carboxylic acid groups generated in a side reaction during polymerization, but does not describe coloring upon heating. According to the present inventors, when the fluororesin is reprecipitated, the metal components contained in the resin cannot be sufficiently removed, and there is a problem that coloring occurs upon heating.
[0005] Patent Document 1 also describes that it is possible to obtain fluororesin particles by means of suspension polymerization, emulsion polymerization, or the like. However, dispersants and emulsifiers used as polymerization aids remain inside the resin particles and cause coloring when heated, impairing the transparency and heat resistance, which are the characteristics of this resin. According to the present inventors, there was also a problem that coloring occurs when heated when the fluororesin contains a specific metal.
[0006] Since the above-mentioned fluororesin processed products need to be heated during molding, there is a possibility that they may become discolored. Therefore, from the viewpoint of using them for optical purposes, there has been a demand for fluororesins that are less discolored when heated. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Public Relations No. WO2014 / 156996 [Non-Patent Document 1] Macromolecules, 2005, 38, 4237-4245 Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made in view of the above problems, and aims to provide a fluororesin that is reduced in coloration when heated, and a method for producing the same. [Means for solving the problem]
[0009] The present inventors have discovered that a fluororesin containing a residue unit represented by the following general formula (1) and having a total content of chromium, iron, and nickel of 500 ppb or less by mass is less discolored when heated, and have completed the present invention.
[0010] [ka]
[0011] (In formula (1), Rf1, Rf2, Rf3, and Rf4 each independently represent a group selected from the group consisting of a linear, branched, or cyclic perfluoroalkyl group which may have a fluorine atom or an etheric oxygen atom having 1 to 7 carbon atoms. Rf1, Rf2, Rf3, and Rf4 may be bonded to each other to form a ring having 4 to 8 carbon atoms.)
[0012] The invention will be described in detail below.
[0013] The present invention is a resin that contains a residue unit represented by general formula (1) and has a total content of chromium, iron, and nickel metals of 500 ppb by mass or less.
[0014] The fluororesin of the present invention is amorphous and has high transparency and high heat resistance because it has a bulky ring structure contained in the general formula (1). In addition, because it is composed only of carbon, fluorine, and oxygen, it has excellent electrical properties, chemical resistance, waterproofness, and liquid and oil repellency.
[0015] In the present invention, Rf1, Rf2, Rf3, and Rf4 groups in the residue unit represented by general formula (1) each independently represent one type of a group consisting of a linear, branched, or cyclic perfluoroalkyl group which may have a fluorine atom or an etheric oxygen atom having 1 to 7 carbon atoms. Rf1, Rf2, Rf3, and Rf4 may be bonded to each other to form a ring having 4 to 8 carbon atoms. Examples of linear perfluoroalkyl groups having 1 to 7 carbon atoms include a trifluoromethyl group, a pentafluoroethyl group, a heptafluoropropyl group, a nonafluorobutyl group, an undecafluoropentyl group, a tridecafluorohexyl group, and a pentadecafluoroheptyl group. Examples of branched perfluoroalkyl groups having 3 to 7 carbon atoms include a heptafluoroisopropyl group, a nonafluoroisobutyl group, a nonafluorosec-butyl group, and a nonafluorotert-butyl group. Examples of cyclic perfluoroalkyl groups having 3 to 7 carbon atoms include a heptafluorocyclopropyl group, a nonafluorocyclobutyl group, and a tridecafluorocyclohexyl group. Examples of linear perfluoroalkyl groups having 1 to 7 carbon atoms which may have an etheric oxygen atom include, for example, a -CF2OCF3 group, a -(CF2)2OCF3 group, and a -(CF2)2OCF2CF3 group. Examples of cyclic perfluoroalkyl groups having 3 to 7 carbon atoms which may have an etheric oxygen atom include a 2-(2,3,3,4,4,5,5,6,6-decafluoro)-pyrinyl group, a 4-(2,3,3,4,4,5,5,6,6-decafluoro)-pyrinyl group, and a 2-(2,3,3,4,4,5,5-heptafluoro)-furanyl group.
[0016] In order to provide excellent heat resistance, it is preferable that at least one of Rf1, Rf2, Rf3, and Rf4 is a group selected from the group consisting of linear, branched, or cyclic perfluoroalkyl groups having 1 to 7 carbon atoms.
[0017] Specific examples of the residue unit represented by general formula (1) include the following residue units.
[0018] [ka]
[0019] Among these, resins containing the following residue units are preferred because they have excellent heat resistance and moldability, and resins containing perfluoro(4-methyl-2-methylene-1,3-dioxolane) residue units represented by general formula (3) are more preferred.
[0020] [ka]
[0021] The resin of the present invention has a total content of chromium, iron, and nickel metals of 500 mass ppb or less. This allows for a fluororesin with reduced coloration during heating to be obtained. The content is preferably 300 mass ppb or less, more preferably 120 mass ppb or less. This further reduces coloration during heating. Usually, the content is expressed as 5 mass ppb or more, but this is due to the lower limit of analysis, and may be less than 5 mass ppb if measurable.
[0022] Here, the contents of the metals chromium, iron, and nickel can be measured by general composition analysis, such as IPC-MS.
[0023] Furthermore, in order to obtain a fluororesin with further reduced coloration, the metal contents of chromium and nickel are each more preferably 100 ppb by mass or less.
[0024] The resin of the present invention preferably has a sodium content of 1000 ppb by mass or less.
[0025] Since the resin of the present invention has excellent fluidity and moldability, it is preferably in a particulate form, and more preferably has a volume average particle diameter of 5 μm or more and 500 μm or less. This is preferable because it allows continuous supply to a molding machine or the like when processing the resin. When the volume average particle diameter is 5 μm or more, the resin is less likely to be scattered by air currents, improving handleability. When the volume average particle diameter is 500 μm or less, the resin has high fluidity, allowing continuous supply to a molding machine or the like, improving handleability.
[0026] When the resin of the present invention has a particulate shape, the volume average particle size can be evaluated by particle size distribution measurement (volume distribution) by laser diffraction scattering method. The particle size distribution by laser diffraction scattering method can be quantified with good reproducibility by dispersing the resin particles in water and measuring after performing a process to homogenize the dispersion state of the crystal particles with an ultrasonic homogenizer. An example of a laser scattering meter is MT3000 manufactured by Microtrac.
[0027] When the resin of the present invention has a particulate form, it is preferably a precipitation polymer since it does not contain an emulsifier or dispersant and has excellent transparency and heat resistance.
[0028] When the resin of the present invention has a particulate shape, the bulk density is set to 0.2 g / cm from the viewpoint of packing property. 3 More than 1.5g / cm 3 It is preferable that:
[0029] The resin of the present invention may contain other monomer residue units, and examples of the other monomer residue units include tetrafluoroethylene (TFE), hexafluoropropylene (HFP), chlorotrifluoroethylene (CTFE), trifluoroethylene, hexafluoroisobutylene, perfluoroalkylethylene, fluorovinyl ether, vinyl fluoride (VF), vinylidene fluoride (VDF), perfluoro-2,2-dimethyl-1,3-dioxole (PDD), perfluoro(allyl vinyl ether), and perfluoro(butenyl vinyl ether).
[0030] In the present invention, there is no limitation on the molecular weight of the resin, and examples of the molecular weight include a weight average molecular weight of 2,500 to 2,000,000 in terms of PMMA measured by gel permeation chromatography (GPC). From the viewpoints of the melt viscosity and mechanical strength of the resin, it is preferably 10,000 to 1,000,000 (g / mol).
[0031] The yellowness index of the fluororesin of the present invention is preferably 3.0 or less, and more preferably 1.0 or less. This allows the molded product to be more suitably used for optical applications. The yellowness index can be measured, for example, by press-molding the fluororesin into a desired shape.
[0032] The yellowness can be measured by a general spectrophotometer.
[0033] Next, the method for producing the resin of the present invention will be described.
[0034] A first aspect of the method for producing a resin of the present invention is as follows: An example of the method for producing a fluororesin includes a precipitation polymerization step in which precipitation polymerization is carried out in the presence of a monomer represented by the following general formula (4), a radical polymerization initiator, and an organic solvent, with the water content in the reaction system being 1000 mass ppm or less.
[0035] In addition, since a particulate resin having excellent flowability and moldability can be obtained, the organic solvent is preferably an organic solvent that dissolves a monomer represented by the following general formula (4) and precipitates a resin containing a residue unit represented by the following general formula (5).
[0036] [ka]
[0037] (In formula (4), Rf5, Rf6, Rf7, and Rf8 each independently represent a group selected from the group consisting of linear, branched, or cyclic perfluoroalkyl groups which may have a fluorine atom or an etheric oxygen atom having 1 to 7 carbon atoms. Rf5, Rf6, Rf7, and Rf8 may be bonded to each other to form a ring having 4 to 8 carbon atoms.)
[0038] [ka]
[0039] (In formula (5), Rf5, Rf6, Rf7, and Rf8 each independently represent a group selected from the group consisting of linear, branched, or cyclic perfluoroalkyl groups which may have a fluorine atom or an etheric oxygen atom having 1 to 7 carbon atoms. Rf5, Rf6, Rf7, and Rf8 may be bonded to each other to form a ring having 4 to 8 carbon atoms.)
[0040] In the resin production method of the present invention, by using an organic solvent (hereinafter referred to as "precipitation polymerization solvent") that dissolves the monomer represented by general formula (4) and precipitates a resin containing a residue unit represented by general formula (5) as a polymerization solvent, the resin generated by the polymerization reaction can be precipitated as particles having a specific volume average particle size, and as a result, a resin having a particle shape with excellent moldability and packing properties can be produced. In addition, since no polymerization aids such as emulsifiers and dispersants are used, resin particles that do not contain emulsifiers and dispersants that cause a loss of transparency and heat resistance can be produced.
[0041] Whether or not a certain organic solvent is capable of precipitating a certain resin can be determined by whether or not the polarity of the organic solvent is within a certain range. In the present invention, it is preferable to select an organic solvent having a polarity within a certain range as the precipitation polymerization solvent based on the Hansen solubility parameters.
[0042] Hansen solubility parameters are solubility parameters introduced by Hildebrand, which Hansen divided into three components, dispersion term δD, polar term δP, and hydrogen bond term δH, and displayed in three-dimensional space. The dispersion term δD indicates the effect of dispersion forces, the polar term δP indicates the effect of dipole-dipole forces, and the hydrogen bond term δH indicates the effect of hydrogen bonding forces. In three-dimensional space, the greater the distance between the coordinates of a resin and the coordinates of an organic solvent, the more likely the resin is to precipitate in that organic solvent.
[0043] The definition and calculation method of Hansen solubility parameters are described in the following literature: Charles M. Hansen, "Hansen Solubility Parameters: A Users Handbook," CRC Press, 2007. In addition, for organic solvents for which literature values are not known, the Hansen solubility parameters can be easily estimated from the chemical structure by using computer software (Hansen Solubility Parameters in Practice (HSPiP)).
[0044] In the present invention, HSPiP 5th Edition is used, and for organic solvents registered in the database, the values are used, and for organic solvents not registered, estimated values are used.
[0045] The Hansen solubility parameter of a resin is usually determined by conducting a solubility test in which the resin is dissolved in many different organic solvents with established Hansen solubility parameters and the solubility is measured. Specifically, when the coordinates of the Hansen solubility parameters of all the organic solvents used in the solubility test are shown in a three-dimensional space, a sphere (solubility sphere) is found in which the coordinates of the organic solvents that dissolved resin A are all contained inside the sphere and the coordinates of the organic solvent to be precipitated are on the outside of the sphere, and the central coordinates of the solubility sphere are taken as the Hansen solubility parameter of the resin.
[0046] If the coordinates of the Hansen solubility parameters of an organic solvent not used in the solubility test are (δD, δP, δH), and the coordinates are included inside the solubility sphere, the organic solvent is considered to dissolve the resin. On the other hand, if the coordinates are outside the solubility sphere, the organic solvent is considered to precipitate the resin.
[0047] In the present invention, the Hansen solubility parameter of the resin is the value of the Hansen solubility parameter of the compound represented by the following general formula (6) (pentamer of the compound represented by the general formula (5)) estimated by HSPiP. By this method, for example, the Hansen solubility parameters δD, δP, and δH of the resin particles containing perfluoro(4-methyl-2-methylene-1,3-dioxolane) residue units represented by the general formula (3) are 11.6, 3.5, and 1.4 (MPa 1 / 2 ).
[0048] [ka]
[0049] (In formula (6), Rf9, Rf 10 , Rf 11 , Rf 12 Rf9 and Rf10 each independently represent a group selected from the group consisting of a fluorine atom or a linear, branched or cyclic perfluoroalkyl group having 1 to 7 carbon atoms which may have an etheric oxygen atom. 10 , Rf 11 , Rf12 may be linked together to form a ring having 4 to 8 carbon atoms.
[0050] As the precipitation polymerization solvent in the present invention, it is preferable to select an organic solvent having a resin solubility index R of 4 or more, calculated from the Hansen solubility parameter according to formula (7). R = 4 × {(δD1-δD2) 2 +(δP1-δP2) 2 +(δH1-δH2) 2} 0.5 (7) Here, δD1, δP1, and δH1 are the dispersion term, polar term, and hydrogen term of the Hansen solubility parameter of the resin particles, respectively, and δD2, δP2, and δH2 are the dispersion term, polar term, and hydrogen term of the Hansen solubility parameter of the organic solvent, respectively.
[0051] For example, examples of organic solvents having an affinity Ra of 4 or more with a resin containing a perfluoro(4-methyl-2-methylene-1,3-dioxolane) residue unit include the organic solvents listed in Table 1 below.
[0052] [Table 1]
[0053] Furthermore, as the precipitation polymerization solvent, an organic solvent containing fluorine atoms and hydrogen atoms in the molecule is preferable because it is difficult for chain transfer reaction to occur in radical polymerization, has excellent polymerization yield, and is easy to obtain a high molecular weight substance.Specific examples of the precipitation polymerization solvent containing fluorine atoms and hydrogen atoms in the molecule include 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, 2,2,2-trifluoroethanol, 1,1,1,3,3,3-hexafluoroisopropanol, and 1,2,2,3,3,4,4-heptafluorocyclopentane.
[0054] Examples of radical polymerization initiators for carrying out radical polymerization include organic peroxides such as benzoyl peroxide, lauryl peroxide, octanoyl peroxide, acetyl peroxide, di-tetr-butyl peroxide, tetr-butylcumyl peroxide, dicumyl peroxide, tetr-butyl peroxyacetate, perfluoro(di-tetr-butyl peroxide), bis(2,3,4,5,6-pentafluorobenzoyl)peroxide, tetr-butyl peroxybenzoate, and tetr-butyl perpivalate; and azo initiators such as 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-butyronitrile), 2,2'-azobisisobutyronitrile, dimethyl-2,2'-azobisisobutyrate, and 1,1'-azobis(cyclohexane-1-carbonitrile).
[0055] In the production method of the present invention, it is preferable that the monomer represented by the general formula (4) is perfluoro(4-methyl-2-methylene-1,3-dioxolane) represented by the following general formula (8), and the residue unit represented by the general formula (5) is a perfluoro(4-methyl-2-methylene-1,3-dioxolane) residue unit represented by the following general formula (9).
[0056] [ka]
[0057] [ka]
[0058] As a second aspect of the method for producing a resin of the present invention, The fluororesin can be produced by a method for producing the fluororesin, which comprises a solution polymerization step of carrying out solution polymerization in the presence of a monomer represented by the following general formula (4), a radical polymerization initiator, and an organic solvent with a water content in the reaction system of 1000 mass ppm or less, and a precipitation step of contacting a solution containing the fluororesin obtained by the solution polymerization with a poor solvent to precipitate the fluororesin while maintaining the water content in the system at 100 ppm or less.
[0059] The poor solvent here is preferably the same solvent as the organic solvent in the first embodiment of the method for producing a resin of the present invention.
[0060] The organic solvent in the second embodiment may be either a good solvent or a poor solvent for the fluororesin of the present invention, but is preferably a good solvent.
[0061] In the production method of the present invention, common to the first and second aspects, it is preferable to carry out polymerization after purifying at least one of the monomer represented by the general formula (4), the initiator, and the organic solvent with at least one of a filtration filter, an ion exchange resin, a metal ion removal filter, and a metal ion remover. Effect of the Invention
[0062] According to the present invention, it is possible to provide a fluororesin with reduced coloration and a method for producing the fluororesin. EXAMPLES
[0063] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0064] <Volume average particle size> The volume average particle size (unit: μm) was measured using MT3000 manufactured by Microtrac and methanol as a dispersion medium. <Metal component content> The fluororesin was dissolved in hexafluorobenzene and then extracted with a dilute acid solution, and the metal components (unit: ppb) were measured using Perkin Elmer's ELAN DRC II. <Yellowness (YI)> The fluororesin was hot-pressed at 230° C. for 50 minutes in a nitrogen atmosphere to prepare a pressed sheet having a thickness of 200 nm, and the yellowness index (YI) was measured using SD5000 manufactured by Nippon Denshoku Industries Co., Ltd.
[0065] Example 1: Preparation of perfluoro(4-methyl-2-methylene-1,3-dioxolane) resin particles The inside of a 1L SUS316 autoclave equipped with a SUS316 paddle-type stirring blade, a nitrogen inlet tube, and a thermometer was replaced with nitrogen. 1.215g (0.00288 mol) of bis(2,3,4,5,6-pentafluorobenzoyl) peroxide was added as an initiator, 140.0g (0.574 mol) of perfluoro(4-methyl-2-methylene-1,3-dioxolane) as a monomer, and 1250g of Asahiklin AE-3000 (manufactured by Asahi Glass, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether) as a precipitation polymerization solvent, and the mixture was stirred at 55°C for 24 hours to perform precipitation polymerization. The mixture was cooled to room temperature, and the liquid containing the purified resin particles was filtered and washed with acetone to obtain perfluoro(4-methyl-2-methylene-1,3-dioxolane) resin particles (resin A) (yield: 63%). The volume average particle size, metal content and yellowness of the obtained resin particles are shown in Table 2. The obtained resin particles had excellent flowability and filling property, low metal content, low yellowness and good transparency.
[0066] [Table 2]
[0067] Comparative Example 1: Production of perfluoro(4-methyl-2-methylene-1,3-dioxolane) resin The fluororesin was produced in accordance with Non-Patent Document 1 below. The inside of a 1L SUS316 autoclave equipped with a SUS316 paddle-type stirring blade, a nitrogen inlet tube, and a thermometer was replaced with nitrogen. 0.476 g (0.00113 mol) of bis(2,3,4,5,6-pentafluorobenzoyl) peroxide as an initiator, 140.0 g (0.574 mol) of perfluoro(4-methyl-2-methylene-1,3-dioxolane) as a monomer, and 230 g of hexafluorobenzene as a polymerization solvent were added, and radical solution polymerization was performed by maintaining the mixture at 55°C for 24 hours under stirring, resulting in a viscous liquid in which the resin was dissolved. The mixture was cooled to room temperature, and the resin solution was diluted with 1000 g of hexafluorobenzene to adjust the viscosity, to prepare a diluted resin solution. 3 L of hexane was added to the vat, and the diluted resin solution was extruded into the hexane with a syringe to precipitate the resin, thereby obtaining perfluoro(4-methyl-2-methylene-1,3-dioxolane) resin (yield: 68%).
[0068] The volume average particle size could not be measured because the resin obtained was amorphous. The metal content and yellowness of the resin obtained are shown in Table 2. The resin particles obtained were poor in fluidity and filling properties, and had a problem with transparency due to the high metal content and high yellowness. In addition, water droplets that had aggregated due to the heat of vaporization of the poor solvent were confirmed in the poor solvent used in the precipitation process, and the moisture content in the system was 100 ppm or more.
[0069] Comparative Example 2: Production of perfluoro(4-methyl-2-methylene-1,3-dioxolane) resin particles The inside of a 1L SUS316 autoclave equipped with a SUS316 paddle-type stirring blade, a nitrogen inlet tube, and a thermometer was replaced with nitrogen. 0.775g (0.00184 mol) of bis(2,3,4,5,6-pentafluorobenzoyl) peroxide was added as an initiator, 5.289g of Newcol 714SN (manufactured by Nippon Nyukazai Co., Ltd., polyoxyethylene polycyclic phenyl ether sulfate ester salt) as a dispersion stabilizer, 16.300g of methanol as a chain transfer agent, 140.0g (0.574 mol) of perfluoro(4-methyl-2-methylene-1,3-dioxolane) as a monomer, and 190.0g of ion-exchanged water as a suspension polymerization solvent were added, and the mixture was kept at 55°C for 24 hours under stirring to perform suspension polymerization. After cooling to room temperature, the liquid containing the purified resin particles was filtered and washed with acetone to obtain perfluoro(4-methyl-2-methylene-1,3-dioxolane) resin particles (yield: 85%). The volume average particle size, metal content, and yellowness of the obtained resin particles are shown in Table 2. The obtained resin particles have excellent fluidity and packing properties, but the large amount of metal content and high yellowness pose a problem in transparency.
[0070] (Example 2) Preparation of perfluoro(4-methyl-2-methylene-1,3-dioxolane) resin particles The inside of a 1L glass autoclave equipped with a SUS316 paddle-type stirring blade, a nitrogen inlet tube, and a thermometer was replaced with nitrogen. 1.190g (0.00282 mol) of bis(2,3,4,5,6-pentafluorobenzoyl) peroxide was added as an initiator, 140.0g (0.574 mol) of perfluoro(4-methyl-2-methylene-1,3-dioxolane) as a monomer, and 1250g of Asahiklin AE-3000 (manufactured by Asahi Glass, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether) as a precipitation polymerization solvent, and the mixture was stirred at 55°C for 24 hours to perform precipitation polymerization. The mixture was cooled to room temperature, and the liquid containing the purified resin particles was filtered and washed with acetone to obtain perfluoro(4-methyl-2-methylene-1,3-dioxolane) resin particles (resin A) (yield: 66%). The volume average particle size, metal content and yellowness of the obtained resin particles are shown in Table 2. The obtained resin particles had a small amount of metal content and were excellent in yellowness, fluidity and filling property.
[0071] Comparative Example 3: Production of perfluoro(4-methyl-2-methylene-1,3-dioxolane) resin particles The inside of a 1L glass autoclave equipped with a SUS316 paddle-type stirring blade, a nitrogen inlet tube and a thermometer was replaced with nitrogen. 0.726g (0.00172 mol) of bis(2,3,4,5,6-pentafluorobenzoyl) peroxide was added as an initiator, 5.314g of Newcol 714SN (manufactured by Nippon Nyukazai Co., Ltd., polyoxyethylene polycyclic phenyl ether sulfate ester salt) as a dispersion stabilizer, 16.280g of methanol as a chain transfer agent, 140.0g (0.573 mol) of perfluoro(4-methyl-2-methylene-1,3-dioxolane) as a monomer, and 186.7g of ion-exchanged water as a suspension polymerization solvent were added, and suspension polymerization was performed by maintaining at 55°C for 24 hours under stirring. The mixture was cooled to room temperature, and the liquid containing the purified resin particles was filtered and washed with acetone to obtain perfluoro(4-methyl-2-methylene-1,3-dioxolane) resin particles (yield: 85%). The volume average particle size, metal content, and yellowness of the obtained resin particles are shown in Table 2. The obtained resin particles have excellent fluidity and filling properties, but have a problem with transparency due to a large amount of metal content and high yellowness. [Industrial Applicability]
[0072] The present invention can provide a fluororesin that is less discolored when heated and a method for producing the fluororesin.
Claims
1. Fluororesin particles comprising a residue unit represented by the following general formula (1), a total content of chromium, iron and nickel being 120 mass ppb or less, a volume average particle diameter of 5 μm or more and 500 μm or less, and a yellowness index of a hot press molded product (thickness 200 nm) at 230° C. for 50 minutes being 1.0 or less: 【Chemistry 1】 (In formula (1), Rf 1 , Rf 2 , Rf 3 , Rf 4 Rf each independently represents a group selected from the group consisting of a fluorine atom or a linear, branched or cyclic perfluoroalkyl group having 1 to 7 carbon atoms which may have an etheric oxygen atom, and at least one of them is a group selected from the group consisting of a linear, branched or cyclic perfluoroalkyl group having 1 to 7 carbon atoms. 1 , Rf 2 , Rf 3 , Rf 4 may be linked to each other to form a perfluoroaliphatic ring having 4 to 8 carbon atoms which may have an etheric oxygen atom.
2. 2. The fluororesin particles according to claim 1, wherein the total content of chromium, iron and nickel is 5 ppb to 120 ppb by mass.
3. 3. The fluororesin particles according to claim 1, having a sodium content of 1000 ppb by mass or less.
4. 4. The fluororesin particles according to claim 1, having a volume average particle size of 5 μm or more and 64 μm or less and a particulate shape.
Citation Information
Patent Citations
JP1968029154B1
Copolymers of perhalo-2,2-di-lower alkyl-1,3-dioxole and perfluoro-2-methylene-4-methyl-1,3-dioxolane
JP1997512854A
Fluorocopolymer molding material
JP2000001518A
Fluororesin particle and method for producing the same
JP2020128520A
Fluorine-containing compound and fluorine-containing polymer
WO2008075545A1