Method for evaluating adhesion state of release agent, method for evaluating adhesion state of lubricant, and system for evaluating adhesion state of release agent

A method and system for evaluating mold release agent and lubricant adhesion on molds using a visible film-forming agent allows direct imaging and analysis, addressing inaccuracies and cleanup issues of existing methods, enhancing productivity and quality.

JP7566219B2Active Publication Date: 2024-10-11MORESCO
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024542389
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-09-30
Filing Date
2023-08-09
Publication Date
2024-10-11
Estimated Expiration
2043-08-09

AI Technical Summary

Technical Problem

Existing methods for evaluating the adhesion state of mold release agents and lubricants on molds are inaccurate and cumbersome, particularly for complex mold shapes, as they often require additives that alter the adhesion behavior and complicate post-measurement cleanup.

Method used

A method and system that utilizes a mold release agent forming a visible white film upon evaporation, allowing direct image acquisition and analysis of adhesion state through color numerical conversion and three-dimensional imaging, without the need for additives, to derive the adhesion state accurately.

Benefits of technology

Enables precise and efficient evaluation of mold release agent and lubricant adhesion on molds, ensuring uniform application and reducing post-measurement cleanup, thereby improving productivity and product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566219000002
    Figure 0007566219000002
  • Figure 0007566219000003
    Figure 0007566219000003
  • Figure 0007566219000004
    Figure 0007566219000004
Patent Text Reader

Abstract

This mold release agent adhesion state evaluation method is a method for evaluating the adhesion state of a mold release agent used in die casting and attached to a mold, the method comprising: a step for heating the mold; a step for attaching a mold release agent to the surface of the heated mold; a step for acquiring image data on the appearance of the surface of the mold to which the mold release agent is attached; a step for deriving, from color digitization information corresponding to the acquired image data on the appearance, the adhesion state of the mold release agent on the surface of the mold on the basis of the correlation between the color digitization information acquired in advance and the adhesion state of the mold release agent; and a step for outputting data regarding the derived adhesion state of the mold release agent.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for evaluating the adhesion state of a release agent, a method for evaluating the adhesion state of a lubricant, and a system for evaluating the adhesion state of a release agent. This application claims priority based on Japanese Application No. 2022-158330 filed on September 30, 2022, and incorporates all of the contents of the above-mentioned Japanese application by reference. [Background technology]

[0002] Techniques for measuring the amount of release agent applied have been disclosed (see, for example, Patent Documents 1, 2 and 3). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] WO2016 / 021006 [Patent Document 2] JP 2013-244508 A [Patent Document 3] JP 2003-251448 A Summary of the Invention [Problem to be solved by the invention]

[0004] When performing processing using a mold, such as casting or plastic processing, it is important to apply the liquid (processing liquid) used in processing, such as a release agent or lubricant, uniformly and without unevenness. For example, in die casting, in order to ensure good productivity and improve the quality of cast products, it is required to be able to evaluate the adhesion state of the release agent attached to the mold as accurately and simply as possible. Therefore, one of the objects of the present invention is to provide an evaluation method and an evaluation system for the adhesion state of the processing liquid, which can accurately and simply evaluate the adhesion state of the processing liquid attached to the mold. [Means for solving the problem]

[0005] The method for evaluating the adhesion state of a release agent according to the present invention is used for die casting and is a method for evaluating the adhesion state of a release agent attached to a die, and includes the steps of heating the die, attaching the release agent to the surface of the heated die, acquiring image data of the appearance of the surface of the die to which the release agent is attached, deriving the adhesion state of the release agent on the surface of the die based on the correlation between the previously acquired color numerical value information and the adhesion state of the release agent from the color numerical value information corresponding to the acquired image data of the appearance, and outputting the derived data on the adhesion state of the release agent. The evaluation method and evaluation system of the present invention can also be used to evaluate the adhesion state of a lubricant for plastic processing to a die. Effect of the Invention

[0006] According to the above-mentioned method for evaluating the adhesion state of a release agent, the adhesion state of the release agent adhered to a mold can be evaluated accurately and simply. [Brief description of the drawings]

[0007] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a part of a die casting apparatus used in a method for evaluating an adhesion state of a release agent in accordance with a first embodiment of the present invention. [Diagram 2] FIG. 2 is a block diagram showing the configuration of a system for evaluating the adhesion state of a release agent according to the present invention. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing a state in which the release agent is applied. [Figure 4] FIG. 4 is a flowchart showing typical steps in the method for evaluating the adhesion state of a release agent according to the first embodiment. [Diagram 5] FIG. 5 is a schematic cross-sectional view showing a state in which the surface of the fixed mold and the surface of the movable mold are photographed. [Figure 6] FIG. 6 shows an example of a captured image in which appearance image data is superimposed on a three-dimensional image formed from a captured image. [Figure 7] FIG. 7 is a graph showing the correspondence between film thickness and color numerical value information. [Figure 8] FIG. 8 is a schematic diagram showing the film thickness distribution state of the release agent adhered to the surface of the movable mold. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] [Overview of the embodiment] The evaluation method according to the present invention can evaluate the adhesion state of a processing liquid such as a release agent or a lubricant that is used by adhering it to a die. The evaluation method of the adhesion state of a release agent according to the present invention is a method for evaluating the adhesion state of a release agent that is used in die casting and that is attached to a die, and includes the steps of heating the die, adhering a release agent to the surface of the heated die, acquiring image data of the appearance of the surface of the die to which the release agent is attached, deriving the adhesion state of the release agent on the surface of the die based on the correlation between the previously acquired color numerical value information and the adhesion state of the release agent from the color numerical value information corresponding to the acquired image data of the appearance, and outputting the derived data on the adhesion state of the release agent. Note that, when the adhesion state of a lubricant to be attached to a die for plastic processing was evaluated by the evaluation method according to the present invention, the adhesion state of the lubricant was evaluated in a similar manner, and the distribution of the adhesion state was able to be displayed. Here, the evaluated lubricant is a lubricant for plastic processing that forms a visible coating when applied to a die.

[0009] In die casting, molten metal is poured into a cavity formed by combining dies heated to a predetermined temperature, and after molding, the product is removed from the combined dies to produce a casting. The release agent is attached to the surface of the die by a method such as coating, spraying, or ejection in order to prevent the molten metal from seizing between the die and the molten metal, to produce a casting with high precision, and to smoothly remove the casting from the die. If the amount of release agent attached is too large, the surface of the casting may become discolored, or the release agent components may evaporate, resulting in deterioration of quality. In addition, if the amount of release agent attached is too small or if the amount of release agent attached to the surface of the die is uneven, the production of a high-precision casting may be hindered, or the casting may be difficult to remove from the die. Therefore, it is required that the release agent be attached to the surface of the die in an appropriate amount as uniformly as possible.

[0010] Here, it is important from the viewpoint of good productivity and improvement of the quality of the castings to know the adhesion state of the release agent, that is, whether or not an appropriate amount of the release agent is uniformly attached to the surface of the mold. It is difficult to measure the thickness of the release agent to be attached by visual inspection or the like, and to know the adhesion state, because the thickness of the release agent is very thin, and the color of the release agent used conventionally is generally transparent, coupled with the fact that the mold is basically black. In particular, when the shape of the mold is complex, it is not easy to check whether the release agent is attached to every corner. In addition, when the color of the coating film cannot be distinguished from the color of the mold, it is also difficult to know the adhesion state of the release agent.

[0011] Conventionally, the coating formed by applying a release agent to a die is transparent and cannot be visually confirmed. Therefore, in order to grasp the adhesion state of the release agent, a fluorescent agent is mixed into the release agent and the agent is irradiated with ultraviolet light to observe the excited fluorescence to grasp the adhesion state of the release agent, or a release agent containing powder is used to grasp the adhesion state by touch, or the emissivity is measured to grasp the adhesion state of the release agent.

[0012] However, these methods involve mixing substances other than the release agent components into the release agent, which may result in adhesion behavior different from that of the original release agent, making it difficult to accurately grasp the adhesion state of the release agent. In addition, if the substance used for film thickness measurement remains on the die after film thickness measurement, it can cause problems, so it is necessary to thoroughly clean the die.

[0013] The present inventors have developed a release agent for die-casting dies that is excellent in releasability and heat resistance. This release agent contains a solvent and an organic acid salt, and has the property of forming a white coating when applied to a die. The present inventors have focused on this property and have come to create the present invention. The method for evaluating the adhesion state of a release agent according to the present invention can be suitably used for a release agent that can be visually observed after application. Such a release agent does not require any foreign matter to be mixed in to measure the film thickness, and the adhesion state of the release agent itself can be evaluated. For example, when the release agent contains an organic acid salt, when the release agent is applied to a die, the solvent evaporates and a white coating is formed on the surface of the die. Such a white coating has good visibility, and it is easy to grasp the remaining parts of the release agent from the appearance of the die. In this way, when image data of the appearance of the surface of the mold is acquired, the adhesion state of the release agent can be easily derived by a process of deriving the adhesion state of the release agent from the color numerical value information corresponding to the acquired image data of the appearance based on the correlation between the color numerical value information acquired in advance and the adhesion state of the release agent. Then, the derived data on the adhesion state of the release agent can be outputted, and the adhesion state of the release agent attached to the surface of the mold can be accurately evaluated. Note that, in such a method, the release agent is used as it is without mixing any additives into the release agent, so that the handling of the release agent is simplified. Therefore, according to such an evaluation method of the adhesion state of the release agent, the adhesion state of the release agent attached to the mold can be accurately and simply evaluated. Note that, as an example, a release agent containing a solvent and an organic acid salt is given, but the present invention can be applied without any restrictions to any processing liquid such as a release agent or a lubricant that shows visibility of the coating formed after application.

[0014] In the above-mentioned method for evaluating the adhesion state of the release agent, the step of acquiring an image may include a step of acquiring a three-dimensional image of the die to which the release agent is attached. The die used in die casting often has a complex shape, specifically, for example, a large number of concave and convex shapes and a large amount of undulations. In such a die, by acquiring a three-dimensional image of the die, more desirable information on the adhesion state of the release agent can be obtained. Specifically, for example, it is possible to easily grasp whether the release agent is reliably attached to the innermost part of the complex die, and whether the release agent is accumulated in the fine parts during multiple die castings. Therefore, the adhesion state of the release agent can be evaluated more accurately.

[0015] In the above-mentioned method for evaluating the adhesion state of a release agent, the image data of the appearance may include a color image. In this way, the adhesion state of the release agent can be derived by taking into account the information of the color image. Therefore, the adhesion state of the release agent can be evaluated more accurately.

[0016] In the above-mentioned method for evaluating the adhesion state of the release agent, the data regarding the adhesion state of the release agent may be data corresponding to the film thickness of the release agent. By doing so, the adhesion amount of the release agent, i.e., the film thickness of the release agent, can be derived with high accuracy. Therefore, the adhesion state of the release agent can be evaluated more accurately.

[0017] In the above-mentioned method for evaluating the adhesion state of a release agent, the color numerical value information may be lightness, hue, chroma, chromaticity, or chromaticity. In this way, the adhesion state of the release agent can be derived using lightness or the like. Therefore, the adhesion state of the release agent can be evaluated more accurately.

[0018] In the above-mentioned method for evaluating the adhesion state of the release agent, the step of outputting data may include a step of displaying the three-dimensional image of the mold and the distribution of the adhesion state of the release agent in correspondence with each other. In this way, the distribution of the adhesion state of the release agent can be visually understood in comparison with the three-dimensional image of the mold. Therefore, the adhesion state of the release agent can be evaluated more easily.

[0019] In the above-mentioned method for evaluating the adhesion state of the release agent, the step of outputting the data may include a step of generating and outputting image data expressed in different colors according to the film thickness of the release agent derived as the adhesion state of the release agent. By doing so, it is possible to easily visually recognize from the generated image that the film thickness differs depending on the color. Therefore, it is possible to more efficiently evaluate the adhesion state of the release agent.

[0020] In the method for evaluating the adhesion state of the release agent, a release agent that is visually recognizable after application is preferably used. The release agent includes, for example, a solvent and an organic acid salt. The solvent may include water or a basic compound. The organic acid salt may include a carboxylic acid compound represented by the following formula (1). In formula (1), R1 represents an alkanediyl group having 2 to 4 carbon atoms, a vinylene group, or a benzene ring, and x represents 2 or 3. The carboxylic acid compound may include at least one compound selected from the group consisting of succinic acid, adipic acid, maleic acid, fumaric acid, phthalic acid, isophthalic acid, terephthalic acid, and trimellitic acid. Such a release agent is excellent in releasability and lubricity.

[0021] [ka]

[0022] Since such a release agent contains the above-mentioned organic acid salt, it can be reliably left on the surface of the mold as a white coating when the solvent evaporates, which makes it possible to more reliably grasp the area where the release agent is attached and more accurately evaluate the state of attachment of the release agent.

[0023] The method for evaluating the adhesion state of a lubricant according to the present invention is a method for evaluating the adhesion state of a lubricant adhered to a die used in plastic processing, and includes the steps of heating the die, adhering a lubricant to the surface of the heated die, acquiring image data of the appearance of the die surface to which the lubricant is adhered, deriving the adhesion state of the lubricant on the die surface from color numerical information corresponding to the acquired image data of the appearance based on a correlation between previously acquired color numerical information and the adhesion state of the lubricant, and outputting the derived data regarding the adhesion state of the lubricant.

[0024] According to the above-mentioned method for evaluating the adhesion state of a lubricant, the adhesion state of a lubricant adhered to a die can be evaluated accurately and simply.

[0025] The evaluation system according to the present invention can evaluate the adhesion state of a processing liquid such as a release agent or a lubricant that is used by adhering it to a die. The evaluation system for the adhesion state of a release agent according to the present invention is used in die casting and is an evaluation system for the adhesion state of a release agent that is attached to a die. The evaluation system for the adhesion state of a release agent includes an image data acquisition unit that acquires image data of the appearance of the die, color numerical value information corresponding to the image data of the appearance of the die acquired from the image data, a derivation unit that derives the adhesion state of the release agent on the surface of the die based on the correlation between the color numerical value information acquired in advance and the adhesion state of the release agent, and an output unit that outputs data on the adhesion state of the release agent derived by the derivation unit. When the adhesion state of a lubricant to be attached to a die for plastic processing was evaluated using the evaluation system according to the present invention, it was possible to evaluate the adhesion state of the lubricant and display the distribution of the adhesion state. Here, the evaluated lubricant is a lubricant for plastic processing that forms a visible coating when applied to the die.

[0026] According to such a system for evaluating the adhesion state of a release agent, the adhesion state of the release agent adhered to a mold can be evaluated accurately and simply.

[0027] In the above-mentioned evaluation system for the adhesion state of the release agent, the image data acquisition unit may include a 3D scanner. The image data acquisition unit may acquire three-dimensional image data of the appearance of the mold by photographing with a 3D scanner. The output unit may display the adhesion state of the release agent superimposed on the three-dimensional image of the mold. In this way, the three-dimensional adhesion state of the release agent can be visually and easily grasped. Therefore, the adhesion state of the release agent can be evaluated more easily.

[0028] [Specific Example of the Embodiment] Next, a die-casting release agent will be described as an embodiment of the method and system for evaluating the adhesion state of a processing liquid according to the present invention with reference to the drawings. In the following drawings, the same or corresponding parts are designated by the same reference numerals, and the description thereof will not be repeated.

[0029] (Embodiment 1) First, a brief description will be given of an overview of the die casting machine used in the method for evaluating the adhesion state of a release agent according to the first embodiment of the present invention and the evaluation system for the adhesion state of a release agent. FIG. 1 is a schematic cross-sectional view showing a part of the die casting machine used in the method for evaluating the adhesion state of a release agent according to the first embodiment of the present invention. FIG. 1 shows a state in which a die, which will be described later, is opened. FIG. 2 is a block diagram showing the configuration of the evaluation system for the adhesion state of a release agent according to the present invention. The above system may be integrated as one device, or may be configured by combining a plurality of devices. Moreover, the evaluation system 51 and the die casting machine 11 may be integrated.

[0030] The following description will be given with reference to Fig. 1 and Fig. 2. The evaluation system 51 for evaluating the adhesion state of a release agent according to the present invention is used together with the die casting device 11 shown in Fig. 1, and includes an image data acquisition unit 28, a derivation unit 53, and an output unit 54. The image data acquisition unit 28 acquires image data of the appearance of the die, which will be described later. The derivation unit 53 derives the adhesion state of the release agent on the surface of the die from color numerical value information corresponding to the image data of the appearance of the die acquired by the image data acquisition unit 28, based on the correlation between the color numerical value information acquired in advance and the adhesion state of the release agent. The output unit 54 outputs the data on the adhesion state of the release agent derived by the derivation unit 53. These configurations will be described later.

[0031] The die casting device 11 includes a fixed mold 13, a movable mold 14, an injection sleeve 15, and an injection piston 16. The fixed mold 13 is fixed. On the other hand, the movable mold 14 is configured to be movable relative to the fixed mold 13. The direction of movement of the movable mold 14 is the direction indicated by the arrow D or the opposite direction. When the fixed mold 13 and the movable mold 14 are brought into contact with each other, a cavity 17 is formed. The injection sleeve 15 is hollow and cylindrical and is disposed in the fixed mold 13, with one open end communicating with the cavity 17. The injection sleeve 15 is provided with an injection port 18 for injecting molten metal into the injection sleeve 15 so as to penetrate the injection sleeve 15 in the radial direction. The molten metal, i.e., a metal such as molten aluminum, is injected into the injection sleeve 15 through the injection port 18. In order to facilitate understanding, the surface 25 of the fixed mold 13 and the surface 26 of the movable mold 14 are illustrated in a simplified manner, but in particular, complex uneven shapes are formed on the surface 25 of the fixed mold 13 and the surface 26 of the movable mold 14.

[0032] The injection piston 16 injects molten metal into the injection sleeve 15 into the cavity 17 formed by contacting the die, specifically the fixed die 13 and the movable die 14. The direction in which the molten metal is injected is the direction indicated by the arrow D in FIG. 1. The injection piston 16 includes a plunger tip 21 and an injection rod 22. The plunger tip 21 is disposed in the injection sleeve 15 and contacts the molten metal to push the molten metal into the cavity 17. The injection rod 22 is connected to the plunger tip 21 and has a portion protruding to the outside of the injection sleeve 15. By applying a lubricant to the inner wall surface 19 of the injection sleeve 15, friction between the outer diameter surface 24 of the plunger tip 21 and the inner wall surface 19 of the injection sleeve 15 when the plunger tip 21 is pushed out is reduced, allowing the plunger tip 21 to move smoothly.

[0033] Next, a process for manufacturing a casting using the die casting device 11 will be briefly described. First, the fixed die 13 and the movable die 14 are heated to a predetermined temperature in advance, and then the movable die 14 is moved in the direction of the arrow D in FIG. 1 to open the fixed die 13 and the movable die 14 as shown in FIG. 1. Then, a release agent is applied to the surface 25 of the fixed die 13 and the surface 26 of the movable die 14. FIG. 3 is a schematic cross-sectional view showing the state in which the release agent is applied. When applying the release agent to the surface 25 and the surface 26 with reference to FIG. 3, a release agent discharge member 27 that discharges the release agent is used. The release agent discharge member 27 is of a spray type and is configured to be able to discharge the release agent from a discharge port onto the surface 25 and the surface 26. The release agent is discharged from the release agent discharge member 27 and adheres to the entire surface 25 and the surface 26.

[0034] Then, the movable mold 14 is moved in the direction opposite to the arrow D to close the mold. Then, the injection rod 22 is moved in the direction of the arrow D. Then, the molten metal in the injection sleeve 15 is pushed out from the injection sleeve 15 and filled into the cavity 17. Then, this state is maintained for a predetermined time to solidify the molten metal. Then, the movable mold 14 is moved in the direction of the arrow D to open the mold. Then, the casting attached to the fixed mold 13 side or the movable mold 14 side is removed. In this way, a product is obtained as a casting. In this case, the release agent is attached to the surfaces 25 and 26, so that they can be easily removed. Then, the release agent is attached to the surfaces 25 and 26 again to manufacture a similar casting.

[0035] Here, the release agent used will be described. As an example, the release agent contains a solvent and an organic acid salt. In this embodiment, the solvent is water. The release agent may contain a basic compound. In this embodiment, the release agent contains water, adipic acid, terephthalic acid, and sodium hydroxide.

[0036] Here, in regard to the production of a casting using such a die casting device 11, it is very important to accurately and simply grasp the adhesion state of the release agent on the die. Next, a method for evaluating the adhesion state of the release agent will be described. FIG. 4 is a flow chart showing typical steps in the evaluation method of the adhesion state of the release agent according to the first embodiment. With reference to FIG. 4, in the evaluation method of the adhesion state of the release agent according to the first embodiment, a die heating step is carried out as a step (S10). In this step (S10), a heater (not shown) provided at a predetermined position inside or near the die casting device 11 is controlled. Then, the fixed die 13 and the movable die 14 are heated to a temperature at which casting is possible. In this case, for example, both the fixed die 13 and the movable die 14 may be heated overall by continuously producing several castings as trial castings.

[0037] After the fixed mold 13 and the movable mold 14 are heated to a predetermined temperature, a release agent application step is carried out as step (S20). In this step (S20), the release agent is applied to the surface 25 of the fixed mold 13 and the surface 26 of the movable mold 14 using the release agent discharge member 27 described above. The release agent used is the one described above.

[0038] Next, a drying step is performed as step (S30). This step (S30) is performed by blowing air onto surface 25 of fixed mold 13 and surface 26 of movable mold 14. At this time, the solvent contained in the release agent evaporates. Then, the organic acid salt component remains on surface 25 of fixed mold 13 and surface 26 of movable mold 14. That is, of the attached release agent, the organic acid salt component remains on surface 25 of fixed mold 13 and surface 26 of movable mold 14 as a white coating.

[0039] Next, as step (S40), a photographing step is performed. In this step (S40), the surface 25 of the fixed mold 13 and the surface 26 of the movable mold 14 are photographed by the image data acquisition unit 28. In this embodiment, the image data acquisition unit 28 includes an external image photographing element (color module camera) and a 3D scanner. Here, as an example, the external image photographing element is built into a 3D scanner, and photographing of the external image and the three-dimensional image of the mold are performed simultaneously. A general 3D scanner can be used, but a handy type is suitable for photographing a mold having an uneven shape without modifying the die casting device 11. FIG. 5 is a schematic cross-sectional view showing a state in which the surface 25 of the fixed mold 13 and the surface 26 of the movable mold 14 are photographed. Referring to FIG. 5, in photographing, the image data acquisition unit 28 is placed, for example, between the surface 25 and the surface 26, and photographed by moving the location or tilting it at various angles. In this case, the surface 25 of the fixed mold 13 and the surface 26 of the movable mold 14 are photographed from various positions and angles. The image data acquisition unit 28 changes the shooting position and shoots the image by manually or automatically moving the table on which the image data acquisition unit 28 is fixed. In this way, a three-dimensional image of the mold to which the release agent is attached is acquired. As an example of the image data acquisition unit 28, an external image shooting element (color module camera) and a 3D scanner are mounted. That is, the external image shooting element is mounted with a color module camera and a light source (LED), and color images of the surface 25 of the fixed mold 13 and the surface 26 of the movable mold 14 are shot. The color module camera can be a CMOS, a CCD, or the like. The light source is emitted as a flash when the image is shot, so that it is less susceptible to the influence of external light and the color saturation of the image can be kept constant. The 3D scanner is a non-contact type equipped with two cameras and an infrared light source, and measures the distance to the subject by a passive method, and a three-dimensional image of the mold is shot. By using infrared light, the shape can be accurately measured without being affected by external light. In this way, a color image of the surface of the mold to which the release agent is attached and a three-dimensional image of the mold are acquired. The appearance image data and the three-dimensional image data are stored in a memory or the like with the shooting positions corresponding to each other.In the above, the image data acquisition unit 28 is moved to capture images of the entire surface of the mold, but a method in which the image capture position is fixed and a predetermined location is captured may also be used.

[0040] Thereafter, an image processing step is performed as step (S50). In this step (S50), an appearance image and / or a 3D image, that is, a three-dimensional image of the surface 25 of the fixed mold 13 and the surface 26 of the movable mold 14, is formed from the captured image. In this case, since the three-dimensional image is captured by a 3D scanner included in the image data acquisition unit 28, the three-dimensional image of the surface 25 of the fixed mold 13 and the surface 26 of the movable mold 14 can be formed with high accuracy. In the following description, the image of the surface 26 of the movable mold 14 will be described. Of course, the image of the surface 25 of the fixed mold 13 is similar to the image of the surface 26 of the movable mold 14, although the uneven shape and the like are different. FIG. 6 is an example of a captured image, which is an image in which appearance image data is superimposed on a three-dimensional image formed from a captured image. Referring to FIG. 6, the surface 26 of the movable mold 14 has a mating surface 31 and a cavity surface 32 arranged inside the mating surface 31. It can be seen that the region 34 located around the center 33 on the upper side of the cavity surface 32 and many regions 35 on the surface on the lower side of the cavity surface 32 are dark white. On the other hand, it can be seen that the region 36 further around the region 34 located on the upper side of the cavity surface 32 and the region 37 to the right of the center of the cavity surface 32 have almost no white parts. As a result, the three-dimensional shape and the appearance information are displayed simultaneously, so that the distribution of the adhesion state of the release agent can be easily understood. The three-dimensional image and the appearance image may be displayed separately.

[0041] Next, in step (S60), an adhesion state deriving step is performed. In this step (S60), in the obtained three-dimensional image, the areas where the release agent is attached appear as white. Color numerical value information is obtained from the appearance image data, and the adhesion state is derived using the color numerical value information. The color numerical value information is information in which colors are quantified using indices such as lightness, hue, saturation, chromaticity, and color saturation. The adhesion state is derived using the following correlation line. The correlation is obtained individually for each release agent. Here, as an example, the film thickness is derived as the adhesion state. Figure 7 is a graph showing the correspondence between film thickness and color numerical value information. In Figure 7, the horizontal axis indicates film thickness (μm), and the vertical axis indicates color numerical value information (lightness L * 7, the solid line 41 is a calibration curve. That is, the line 41 is a relationship between each film thickness measured when the release agent is applied in advance and the L * When a photographed image is measured with a colorimeter, the lightness (L * The color quantification information such as the thickness (L value) is obtained. The film thickness is measured, for example, by a non-contact film thickness sensor. By using this calibration curve 41, the L * The film thickness in each region can be calculated with high accuracy from the value. That is, the process of deriving the adhesion state of the release agent includes a process of deriving the film thickness of the release agent based on color numerical information acquired from the image data. The color numerical information used may be an index that has a correlation with the adhesion state of the release agent, for example, lightness (L * value), chromaticity a * value or b *values, etc. can be used. That is, the color quantification information to be used is selected according to the type of release agent. The step of deriving the adhesion state includes a step of deriving the adhesion state from the color quantification information corresponding to the image data acquired in the photographing step based on the correlation between the color quantification information of the image measured in advance and the adhesion state of the release agent. The data on the adhesion state is information on the adhesion of the release agent, for example, information corresponding to the film thickness, the adhesion amount, the magnitude of the adhesion amount, whether the adhesion amount exceeds a reference value, the variation in the adhesion amount, etc. The information corresponding to the film thickness may be a numerical value of the film thickness, or the film thickness displayed as a level, the magnitude of the film thickness, whether the film thickness exceeds a reference value, the variation in the film thickness, etc., as long as it is information corresponding to the film thickness, the display form is not limited. The data on the adhesion state may be derived as a distribution on the mold, or only the adhesion information at a predetermined position may be derived. For example, an external image of the mold at a position where the release agent is difficult to adhere may be photographed to obtain the adhesion information. The correlation between the color quantification information and the adhesion state may be expressed in a form other than a calibration curve. The adhesion state is derived using a derivation unit 53 included in the evaluation system 51 for evaluating the adhesion state of a release agent. As the derivation unit 53, for example, a control device that is included in the evaluation system 51 for evaluating the adhesion state of a release agent and that controls the operation of the entire evaluation system 51 for evaluating the adhesion state of a release agent is used.

[0042] FIG. 8 is a schematic diagram showing an image of the film thickness distribution state of the release agent attached to the surface 26 of the movable mold 14. Referring to FIG. 8, in the image 29, a three-dimensional image is displayed in a color-coded manner according to the film thickness of the release agent. In FIG. 8, colors are assigned according to the film thickness scale. For example, a film thickness of 0 μm is displayed in black, and as the film thickness value increases, colors are assigned stepwise or continuously from cool colors (blue) to warm colors (red). By visually checking the image 29 shown in FIG. 8, it is possible to easily evaluate whether the release agent is properly attached to the surface. This output is performed using an output unit 54 included in the evaluation system 51 for the adhesion state of the release agent. As the output unit 54, for example, a display or a printer included in the evaluation system 51 for the adhesion state of the release agent and which displays an image in response to a signal from a control device is used.

[0043] According to the method for evaluating the adhesion state of a release agent according to the present invention, a release agent containing a solvent and an organic acid salt is used as an example of a release agent that can be visually recognized after adhesion. The film thickness of such a release agent can be measured using the release agent itself, and no foreign matter is mixed in. The organic acid salt contained in the release agent can be left on the surface of the mold as a white film, for example, by removing the solvent. Such a white film has good visibility, and it is easy to grasp the remaining part of the release agent from the appearance. Then, when an image of the surface of the mold is acquired, the adhesion state of the release agent can be easily derived from the obtained image by the deriving step of the adhesion state of the release agent. Then, the derived data on the adhesion state of the release agent can be output, and the adhesion state of the release agent attached to the surface of the mold can be accurately evaluated. Note that, in such a method, the release agent is used as it is without mixing any additives into the release agent, and therefore the handling of the release agent is simplified. Therefore, according to such a method for evaluating the adhesion state of a release agent, the adhesion state of the release agent attached to the mold can be accurately and simply evaluated.

[0044] According to the method for evaluating the adhesion state of the release agent of the present invention, since no impurities used for evaluating the adhesion state are added to the release agent, it is not necessary to wash the mold after the film thickness measurement. Therefore, in the middle of manufacturing a product as a casting, the adhesion state of the release agent during the manufacturing of the product can be evaluated by taking pictures by the image data acquisition unit 28 described above. For example, this method is particularly effective when periodically evaluating the adhesion state of the release agent during mass production. That is, the optimal adhesion amount of the release agent in each region and the optimal adhesion method of the release agent to realize this are arbitrarily determined according to the shape of the mold, the casting conditions, the capacity of the peripheral equipment, and the like. Furthermore, by implementing the method for evaluating the application state of the release agent according to the present invention in the middle of manufacturing the casting, the adhesion method and conditions of the release agent can be efficiently examined.

[0045] According to this embodiment, the step of acquiring an image includes a step of acquiring a three-dimensional image of the mold to which the release agent is attached. The molds used in die casting often have complex shapes, specifically, for example, many with a large number of concave and convex shapes and large undulations. In such molds, a three-dimensional image of the mold is acquired, and information corresponding to the film thickness is associated with the film thickness and visualized, thereby obtaining more detailed information on the adhesion state of the release agent. That is, the distribution of information corresponding to the film thickness is visualized by superimposing and displaying information corresponding to the film thickness on the three-dimensional image. This makes it possible to grasp adhesion information of the release agent over a wide range of the mold. Specifically, for example, it is possible to easily grasp whether there are any parts of a complex mold to which the release agent is not attached, whether the release agent is reliably attached to the back of the recessed parts, and whether the release agent is accumulated in the details as die casting is repeated multiple times. Therefore, the adhesion state of the release agent can be evaluated more accurately.

[0046] According to the present embodiment, the image data of the appearance includes a color image. Therefore, the adhesion state of the release agent can be derived by taking into account the information of the color image. Therefore, the adhesion state of the release agent can be evaluated more accurately.

[0047] According to the present embodiment, the data on the adhesion state of the release agent corresponds to the film thickness of the release agent. Therefore, the adhesion amount of the release agent, i.e., the film thickness of the release agent, can be derived with high accuracy. Therefore, the adhesion state of the release agent can be evaluated more accurately.

[0048] According to the present embodiment, the color quantification information is lightness, hue, saturation, chromaticity, or chromaticity. Therefore, the adhesion state of the release agent can be derived using the hue, etc. Therefore, the adhesion state of the release agent can be evaluated more accurately.

[0049] According to this embodiment, the step of outputting data includes a step of displaying the three-dimensional image of the mold and the distribution of the adhesion state of the release agent in correspondence with each other. Therefore, the distribution of the adhesion state of the release agent can be visually understood by comparing it with the three-dimensional image of the mold. Therefore, the adhesion state of the release agent can be more easily evaluated.

[0050] According to this embodiment, the step of outputting the data includes a step of generating and outputting image data expressed in different colors according to the film thickness of the release agent derived as the adhesion state of the release agent. Therefore, it is easy to visually recognize from the generated image that the film thickness differs depending on the color. Therefore, the adhesion state of the release agent can be evaluated more efficiently.

[0051] The evaluation system for the adhesion state of a release agent according to the present invention is used in die casting and evaluates the adhesion state of a release agent adhered to a die. The evaluation system for the adhesion state of a release agent includes an image data acquisition unit that acquires image data of the appearance of the die, color numerical information corresponding to the image data of the appearance of the die, a derivation unit that derives the adhesion state of the release agent on the surface of the die based on the correlation between the previously acquired color numerical information and the adhesion state of the release agent, and an output unit that outputs the data on the adhesion state of the release agent derived by the derivation unit.

[0052] According to such a system for evaluating the adhesion state of a release agent, the adhesion state of the release agent adhered to a mold can be evaluated accurately and simply.

[0053] In the above-mentioned evaluation system for the adhesion state of the release agent, the image data acquisition unit may include a 3D scanner. The image data acquisition unit may acquire three-dimensional image data of the appearance of the mold by photographing with a 3D scanner. The output unit may display the adhesion state of the release agent superimposed on the three-dimensional image of the mold. In this way, the three-dimensional adhesion state of the release agent can be visually and easily grasped. Therefore, the adhesion state of the release agent can be evaluated more easily.

[0054] (Other embodiments) In the above embodiment, the imaging element for capturing the appearance image of the mold is built into the 3D scanner, but it may be disposed separately. If a 3D image is not captured, the 3D scanner is not necessary. Although a color image is acquired as the appearance image of the mold, the present invention is not limited to this, and a monochrome image at a wavelength suitable for showing the characteristics (hue, brightness, etc.) of the release agent coating after adhesion may be acquired. In addition, when a 3D image is acquired, an image including planar position information and thickness direction information of the mold is obtained, which is preferable because it allows a more detailed evaluation of the release agent adhesion state, but the present invention is not limited to this, and a 2D image may be acquired.

[0055] In the above embodiment, the step S30 shown in FIG. 4 includes a drying step. However, depending on the release agent used, the drying step may be omitted.

[0056] The evaluation method and evaluation system of the present invention can also be used to evaluate the adhesion state of processing liquids such as lubricants and release agents that form a visible film when applied to a die or the like, similar to the above-mentioned die-casting release agent. An example of the processing liquid is a non-graphite-based lubricant for plastic processing. For example, a non-graphite-based lubricant for plastic processing contains an organic acid salt such as a carboxylic acid compound, and forms a white film when applied to a die (lubricant application process). The image data acquisition unit acquires the appearance and color numerical information of the plastic processing die (image data acquisition process), and the adhesion state of the lubricant is derived (adhesion state derivation process) based on the correlation between the previously acquired color numerical information and the adhesion state of the lubricant, and the result can be output (data output process), so that the evaluation method and evaluation system of the present invention can be suitably used.

[0057] It should be understood that the embodiments disclosed herein are illustrative in all respects and are not restrictive in any respect. The scope of the present invention is defined by the scope of the claims, and is intended to include all modifications within the scope and meaning equivalent to the scope of the claims. [Explanation of symbols]

[0058] 11 die casting device, 13 fixed mold, 14 movable mold, 15 injection sleeve, 16 injection piston, 17 cavity, 18 injection port, 19 inner wall surface, 21 plunger tip, 22 injection rod, 24 outer diameter surface, 25, 26 surface, 27 release agent discharge member, 28 image data acquisition unit, 29 image, 31 mating surface, 32 cavity surface, 33 center, 34, 35, 36, 37 area, 41 line (calibration curve), 51 evaluation system for release agent adhesion state, 53 lead-out unit, 54 output unit.

Claims

1. A method for evaluating an adhesion state of a release agent attached to a die for use in die casting, comprising the steps of: heating the mold; applying a release agent directly to the heated surface of the mold; acquiring image data of the appearance of the surface of the mold to which the release agent has been applied; deriving an adhesion state of the release agent on the surface of the mold from color numerical information corresponding to the acquired image data of the appearance based on a correlation between previously acquired color numerical information and the adhesion state of the release agent; and outputting the derived data relating to the adhesion state of the release agent.

2. The method for evaluating an adhesion state of a release agent according to claim 1 , wherein the release agent contains a solvent and an organic acid salt.

3. The method for evaluating the adhesion state of a release agent according to claim 1 , wherein the step of acquiring an image includes a step of acquiring a three-dimensional image of the mold to which the release agent is adhered.

4. The method for evaluating an adhesion state of a release agent according to claim 1 or 2, wherein the image data of the appearance includes a color image.

5. 3. The method for evaluating the adhesion state of a release agent according to claim 1, wherein the data regarding the adhesion state of the release agent is data corresponding to a film thickness of the release agent.

6. The method for evaluating the adhesion state of a release agent according to claim 1 or 2, wherein the color numerical value information is lightness, hue, saturation, chromaticity, or color saturation.

7. 3. The method for evaluating the adhesion state of a release agent according to claim 1, wherein the step of outputting the data includes a step of displaying a three-dimensional image of the die and the distribution of the adhesion state of the release agent in correspondence with each other.

8. 3. The method for evaluating the adhesion state of a release agent according to claim 1 or 2, wherein the step of outputting the data includes a step of generating and outputting image data expressed in a color according to the film thickness of the release agent derived as the adhesion state of the release agent.

9. A method for evaluating the adhesion state of a lubricant attached to a die used in plastic working, comprising the steps of: heating the mold; applying a lubricant directly to the heated surface of the die; acquiring image data of the appearance of the surface of the mold to which the lubricant has been applied; deriving an adhesion state of the lubricant on the surface of the die from color numerical information corresponding to the acquired image data of the appearance based on a correlation between pre-acquired color numerical information and the adhesion state of the lubricant; and outputting the derived data relating to the adhesion state of the lubricant.

10. A system for evaluating the adhesion state of a release agent used in die casting, which evaluates the adhesion state of a release agent that is directly attached to a die, comprising: An image data acquisition unit that acquires image data of the appearance of the mold; a derivation unit that derives the adhesion state of the release agent on the surface of the mold based on color numerical value information corresponding to image data of the appearance of the mold obtained from the image data and a correlation between the previously obtained color numerical value information and the adhesion state of the release agent; and an output unit that outputs the data regarding the adhesion state of the release agent derived by the derivation unit.

11. The image data acquisition unit includes a 3D scanner, The image data acquisition unit acquires three-dimensional image data of the appearance of the mold by photographing it with the 3D scanner, The system for evaluating the adhesion state of a release agent according to claim 10 , wherein the output unit displays the adhesion state of the release agent superimposed on a three-dimensional image of the die.

Citation Information

Patent Citations

  • Apparatus and method for evaluating adhesion degree related to adherend on mold surface

    JP2003231131A

  • Applicator for die casting

    JP2003251448A

  • Measuring method for thickness of liniment on die, and the control method for coverage of liniment on die

    JP2005188994A

  • Method and apparatus for detecting spreading-state of releasing agent

    JP2007069217A

  • Film thickness measuring apparatus, surface temperature measuring apparatus, film thickness measuring method and surface temperature measuring method

    JP2008215957A