Transparent resin composition
A transparent resin composition with improved tensile modulus and surface hardness is achieved by blending PMMA and PLA with silica in a specific ratio, maintaining transparency through reduced refractive index and silica reinforcement.
Patent Information
- Application Number
- JP2020179581
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-27
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-10-27
AI Technical Summary
Existing resin compositions of polymethyl methacrylate (PMMA) and polylactic acid (PLA) suffer from insufficient tensile modulus and surface hardness while maintaining transparency.
A transparent resin composition is formulated by blending PMMA and PLA in a specific ratio with silica having a silicon dioxide purity of 90% or more, with a mass ratio of PMMA:PLA ranging from 5:95 to 25:75, and a silica content of 1 to 100 parts by volume, to enhance tensile modulus and surface hardness while maintaining transparency.
The composition achieves excellent tensile modulus and surface hardness while retaining transparency, attributed to the reinforcing effect of silica and the reduction in refractive index difference between PMMA and PLA.
Smart Images

Figure 0007566240000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a transparent resin composition, and more particularly to a transparent resin composition containing polymethyl methacrylate and polylactic acid. [Background technology]
[0002] Polylactic acid has been attracting attention as an environmentally friendly material, but it has a problem in that it has a low glass transition temperature and therefore insufficient heat resistance in a temperature range above the glass transition temperature.
[0003] Therefore, Japanese Patent Application Laid-Open No. 2005-171204 (Patent Document 1) describes that by blending polymethyl methacrylate (PMMA) with polylactic acid (PLA) and improving their compatibility, a polylactic acid-containing resin composition with excellent heat resistance, transparency, moldability, and durability can be obtained, and discloses a resin composition containing 20 to 98 mass % of PMMA having a weight-average molecular weight of 20,000 to 300,000 and 80 to 2 mass parts of PLA. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2005-171204 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the resin composition described in Patent Document 1 still does not have sufficient tensile modulus and surface hardness.
[0006] The present invention has been made in consideration of the problems associated with the above-mentioned conventional techniques, and aims to provide a transparent resin composition that has excellent tensile modulus and surface hardness, while maintaining the transparency of a resin mixture of polymethyl methacrylate (PMMA) and polylactic acid (PLA). [Means for solving the problem]
[0007] As a result of extensive research to achieve the above-mentioned object, the inventors discovered that by blending silica with a resin mixture containing polymethylmethacrylate (PMMA) and polylactic acid (PLA) in a specific ratio, the tensile modulus and surface hardness are improved while the transparency of the resin mixture of PMMA and PLA is maintained, thereby completing the present invention.
[0008] That is, the transparent resin composition of the present invention contains polymethylmethacrylate (PMMA), polylactic acid (PLA), and silica having a silicon dioxide purity of 90% or more, the mass ratio of the PMMA to the PLA is PMMA:PLA=5:95 to 25:75, and the content of the silica is 1 to 100 parts by volume of the total of the PMMA and the PLA. 8.7 It is characterized in that it is a capacitive part.
[0009] In the transparent resin composition of the present invention, the mass ratio of the PMMA to the PLA is preferably PMMA:PLA=10:90 to 20:80, and the silica preferably has a silicon dioxide purity of 99.5% or more.
[0010] The reason why the transparent resin composition of the present invention has excellent tensile modulus and surface hardness and maintains the transparency of the resin mixture of PMMA and PLA is not necessarily clear, but the present inventors speculate as follows. That is, the transparent resin composition of the present invention is a resin mixture containing PMMA and PLA in a specific ratio and silica in a specific ratio. Since silica is contained in such a transparent resin composition, it is considered that the tensile modulus and surface hardness of the resin mixture are improved due to the reinforcing effect of silica. In addition, by blending PMMA and PLA in a specific ratio, the difference in refractive index between the resin mixture and silica is reduced, and therefore the transparency of the resin mixture is considered to be maintained. Effect of the Invention
[0011] According to the present invention, it is possible to obtain a transparent resin composition which has excellent tensile modulus and surface hardness, and which maintains the transparency of a resin mixture of polymethyl methacrylate (PMMA) and polylactic acid (PLA). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below based on preferred embodiments thereof.
[0013] The transparent resin composition of the present invention contains polymethyl methacrylate (PMMA), polylactic acid (PLA), and silica having a silicon dioxide purity of 90% or more.
[0014] There are no particular limitations on the PLA used in the present invention, but from the viewpoint of improving compatibility with PMMA and mechanical strength, it is preferable for the PLA to contain 50 mol % or more of lactic acid units, more preferably 60 mol % or more, even more preferably 70 mol % or more, and particularly preferably 100 mol % (i.e., a homopolymer of lactic acid).
[0015] When the lactic acid unit is less than 100 mol %, other monomers copolymerizable with lactic acid include polycarboxylic acids, polyols, hydroxycarboxylic acids, lactones, and the like.
[0016] The weight average molecular weight of the PLA is preferably from 10,000 to 600,000, more preferably from 40,000 to 600,000, and even more preferably from 100,000 to 500,000. If the weight average molecular weight of the PLA is less than the lower limit, the impact resistance of the resin composition tends to decrease, while if it exceeds the upper limit, the compatibility with PMMA tends to decrease.
[0017] There are no particular limitations on the PMMA used in the present invention, but from the viewpoint of improving compatibility with PLA and mechanical strength, it is preferable that the PMMA contains 90 mol % or more of methyl methacrylate units, more preferably 93 mol % or more, even more preferably 95 mol % or more, and particularly preferably 100 mol % (i.e., a homopolymer of methyl methacrylate).
[0018] When the methyl methacrylate unit is less than 100 mol %, other monomers copolymerizable with methyl methacrylate include vinyl monomers other than methyl methacrylate, such as olefins, (meth)acrylic acid alkyl esters (excluding methyl methacrylate), and styrene.
[0019] The weight average molecular weight of the PMMA is preferably from 10,000 to 400,000, more preferably from 40,000 to 350,000, and even more preferably from 50,000 to 260,000. If the weight average molecular weight of the PMMA is less than the lower limit, the transparency and heat resistance of the resin composition tend to decrease, while if it exceeds the upper limit, the compatibility with PLA decreases, the transparency of the resin composition tends to decrease, and the moldability of the resin composition tends to decrease.
[0020] The silica used in the present invention is not particularly limited as long as it has a silicon dioxide purity of 90% or more. From the viewpoint of improving the transparency of the resin composition, however, silica having a silicon dioxide purity of 95% or more is preferable, more preferably 97% or more, and particularly preferably 99.5% or more.
[0021] The shape of the silica is not particularly limited, and may be either particulate or fibrous.
[0022] When the silica is in the form of particles, the average particle size is preferably 0.1 to 50 μm, more preferably 0.5 to 30 μm, and even more preferably 1 to 20 μm. If the average particle size is less than the lower limit, the handleability of the silica particles tends to deteriorate, while if it exceeds the upper limit, the processability of the resin composition tends to deteriorate.
[0023] In addition, when the silica is in the form of fiber, the average fiber length is preferably 0.01 to 10 mm, more preferably 0.1 to 7 mm, and even more preferably 0.3 to 5 mm. If the average fiber length is less than the lower limit, the effect of improving the mechanical strength by the silica fiber tends to be small, while if it exceeds the upper limit, the processability of the resin composition tends to decrease and the appearance of the molded product tends to deteriorate. In addition, the average fiber diameter is preferably 1 to 50 μm, more preferably 3 to 30 μm, and even more preferably 5 to 25 μm. If the average fiber diameter is less than the lower limit, the handleability of the silica fiber tends to decrease, while if it exceeds the upper limit, the processability of the resin composition tends to decrease.
[0024] In the transparent resin composition of the present invention, the mass ratio of the PMMA to the PLA is in the range of PMMA:PLA=5:95 to 25:75. When the proportion of the PMMA is less than the lower limit, the heat resistance of the resin composition decreases. On the other hand, when the proportion of the PMMA exceeds the upper limit, the transparency of the resin composition decreases. From the viewpoint of improving the heat resistance and transparency of the resin composition, the mass ratio of the PMMA to the PLA is preferably 10:90 to 20:80, more preferably 10:90 to 15:85.
[0025] In addition, in the transparent resin composition of the present invention, the content of the silica is within the range of 1 to 100 parts by volume relative to 100 parts by volume of the total of the PMMA and the PLA. When the content of the silica is less than the lower limit, the tensile modulus and surface hardness of the resin composition are reduced. On the other hand, when the content of the silica is more than the upper limit, the moldability and transparency of the resin composition are reduced. In addition, from the viewpoint of improving the transparency, mechanical strength, and processability of the resin composition, the content of the silica is preferably 1 to 80 parts by volume, more preferably 1 to 50 parts by volume, relative to 100 parts by volume of the total of the PMMA and the PLA.
[0026] The transparent resin composition of the present invention may contain various known additives, such as a crystal nucleating agent, a hydrolysis inhibitor, an antioxidant, a heat stabilizer, a plasticizer, a lubricant, a light stabilizer, an ultraviolet absorber, an antistatic agent, a flame retardant, a release agent, and an antibacterial agent, within the range that does not impair the effects of the present invention (particularly, transparency).
[0027] The method for producing the transparent resin composition of the present invention is not particularly limited as long as it can uniformly mix (knead) the PMMA, PLA, and silica at a predetermined ratio, and for example, the PMMA and PLA are dry-blended so that the mass ratio is within the above range, and the resulting resin mixture (blend resin) and the silica are kneaded (preferably melt-kneaded) so that the volume ratio is within the above range. The kneading temperature is not particularly limited, but is usually within the range of 200 to 300°C. The kneading time is not particularly limited, but is usually within the range of 3 to 15 minutes.
[0028] The transparent resin composition of the present invention can be molded into transparent resin composite materials of various shapes by known molding methods such as injection molding, extrusion molding, blow molding, inflation molding, profile extrusion molding, injection blow molding, vacuum / pressure molding, spinning, etc. Examples of such transparent resin composite materials include injection molded products, extrusion molded products, compression molded products, blow molded products, sheets, films, threads, fabrics, etc. EXAMPLES
[0029] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited to the following examples.
[0030] Example 1 Polymethylmethacrylate (Kuraray Co., Ltd. "Parapet G Grade", weight average molecular weight: 86,000) and polylactic acid (Unitika Ltd. "Terramac TE-2000", weight average molecular weight: 120,000) were dry-blended in a mass ratio of PMMA:PLA = 10:90, and the resulting resin mixture and silica beads (Admatechs Co., Ltd. "SO-C6", silicon dioxide purity: 99.8%, average particle size: 1.8-2.3 μm) were added to a small benchtop kneader (Thermo Fisher Scientific KK microcompounder "Haake minilab") so that the volume ratio was resin mixture:silica = 92 vol%:8 vol% (8.7 vol parts of silica to 100 vol parts of resin mixture), and kneaded at 230 °C for 5 minutes. The obtained resin composition was pressure molded for 30 seconds using a small test press machine ("TW-08" manufactured by Takachiho Seiki Co., Ltd.) at a temperature of 200°C and a pressure of 10 MPa. The obtained molded body was then solidified using a water-cooled press machine (manufactured by Ueshima Seisakusho Co., Ltd.) to obtain a flat plate (composite material) of 50 mm x 50 mm x 0.5 mm.
[0031] Example 2 A 50 mm×50 mm×0.5 mm flat plate (composite material) was produced in the same manner as in Example 1, except that the mass ratio of the polymethyl methacrylate and the polylactic acid was changed to PMMA:PLA=20:80.
[0032] Comparative Example 1 Pelletized polylactic acid (Terramac TE-2000, manufactured by Unitika Ltd., weight-average molecular weight: 120,000) was subjected to pressure molding for 30 seconds at a temperature of 200°C and a pressure of 10 MPa using a small test press (TW-08, manufactured by Takachiho Seiki Co., Ltd.). The resulting molded body was then solidified using a water-cooled press (manufactured by Ueshima Seisakusho Co., Ltd.) to obtain a 50 mm x 50 mm x 0.5 mm flat plate (resin material).
[0033] Comparative Example 2 A 50 mm×50 mm×0.5 mm flat plate (resin material) was produced in the same manner as in Example 1, except that no silica beads were added.
[0034] Comparative Example 3 A 50 mm×50 mm×0.5 mm flat plate (resin material) was produced in the same manner as in Example 2, except that no silica beads were added.
[0035] Comparative Example 4 A 50 mm x 50 mm x 0.5 mm flat plate (resin material) was produced in the same manner as in Example 1, except that the mass ratio of the polymethyl methacrylate and the polylactic acid was changed to PMMA:PLA=30:70 and no silica beads were added.
[0036] Comparative Example 5 Polylactic acid (Terramac TE-2000, manufactured by Unitika Co., Ltd., weight average molecular weight: 120,000) and silica beads (SO-C6, manufactured by Admatechs Co., Ltd., silicon dioxide purity: 99.8%, average particle size: 1.8-2.3 μm) were put into a small tabletop kneader (Micro Compounder Haake minilab, manufactured by Thermo Fisher Scientific) so that the volume ratio was PLA:silica = 92 volume %: 8 volume % (8.7 volume parts of silica to 100 volume parts of PLA), and kneaded at 230 ° C for 5 minutes. The obtained resin composition was pressure molded for 30 seconds using a small test press machine (TW-08, manufactured by Takachiho Seiki Co., Ltd.) at a temperature of 200 ° C and a pressure of 10 MPa, and the obtained molded body was solidified using a water-cooled press machine (manufactured by Ueshima Seisakusho Co., Ltd.) to obtain a flat plate (composite material) of 50 mm × 50 mm × 0.5 mm.
[0037] Comparative Example 6 A 50 mm×50 mm×0.5 mm flat plate (composite material) was produced in the same manner as in Example 1, except that the mass ratio of the polymethyl methacrylate and the polylactic acid was changed to PMMA:PLA=30:70.
[0038] Comparative Example 7 A 50 mm × 50 mm × 0.5 mm flat plate (composite material) was prepared in the same manner as in Example 1, except that glass fibers ("Chopped Strand CS3J-256LS" manufactured by Nitto Boseki Co., Ltd., silicon dioxide purity: 53%, average fiber length: 3 mm, average fiber diameter: 11 μm) were used instead of the silica beads, in a volume ratio of resin mixture:glass fiber=92 volume %:8 volume % (8.7 volume parts of glass fiber per 100 volume parts of resin mixture).
[0039] Comparative Example 8 A 50 mm × 50 mm × 0.5 mm flat plate (composite material) was prepared in the same manner as in Example 2, except that glass fibers ("Chopped Strand CS3J-256LS" manufactured by Nitto Boseki Co., Ltd., silicon dioxide purity: 53%, average fiber length: 3 mm, average fiber diameter: 11 μm) were used instead of the silica beads, in a volume ratio of resin mixture:glass fiber=92 volume %:8 volume % (8.7 volume parts of glass fiber per 100 volume parts of resin mixture).
[0040] <Tensile modulus> A rectangular test piece of 10 mm x 50 mm x 0.5 mm was cut out from each flat plate (50 mm x 50 mm x 0.5 mm) obtained in the examples and comparative examples, and a tensile test was performed using a universal testing machine (Instron "5566") at a displacement rate of 2 mm / min, and the tensile modulus was calculated from the obtained stress-strain curve. The results are shown in Table 1.
[0041] <Transparency> The haze value of each of the flat plates (50 mm×50 mm×0.5 mm) obtained in the examples and comparative examples was measured using a haze meter ("HGM-3DP" manufactured by Suga Test Instruments Co., Ltd.). The results are shown in Table 1.
[0042] <Surface hardness> The surface hardness of each flat plate (50 mm × 50 mm × 0.5 mm) obtained in the examples and comparative examples was measured using a pencil hardness tester (Allgood Co., Ltd. "054", test pencil: Mitsubishi uni pencil for pencil hardness test). The results are shown in Table 1.
[0043] [Table 1]
[0044] As shown in Table 1, it was confirmed that the composite materials (Examples 1 and 2) made of a resin composition in which silica beads were blended with a resin mixture containing polymethylmethacrylate and polylactic acid in a specified ratio exhibited excellent tensile modulus and surface hardness due to the reinforcing effect of the silica beads. It was also confirmed that the composite materials obtained in Examples 1 and 2 had excellent transparency. This is believed to be because the refractive index difference between the resin mixture and the silica beads was reduced by blending polymethylmethacrylate and polylactic acid in a specified ratio.
[0045] On the other hand, the resin materials obtained in Comparative Examples 1 to 3 were found to have excellent transparency but poor tensile modulus and surface hardness because they did not contain silica beads, and the resin material obtained in Comparative Example 4 was found to have excellent transparency and surface hardness but poor tensile modulus because they did not contain silica beads.
[0046] Furthermore, it was found that the composite material (Comparative Example 5) made of a resin composition in which silica beads were blended with polylactic acid exhibited excellent tensile modulus and surface hardness due to the reinforcing effect of the silica beads, but was inferior in transparency. This is believed to be because the composite material obtained in Comparative Example 5 contains only polylactic acid as a resin, and the refractive index difference between polylactic acid and silica beads is large. In addition, it was found that the composite material (Comparative Example 6) made of a resin composition in which silica beads were blended with a resin mixture containing polymethylmethacrylate and polylactic acid and in which the polymethylmethacrylate content is greater than a specified ratio, exhibited excellent tensile modulus and surface hardness due to the reinforcing effect of the silica beads, but was inferior in transparency. This is believed to be because the composite material obtained in Comparative Example 6 contains polymethylmethacrylate in a greater amount than a specified ratio, and the refractive index difference between the resin mixture and silica beads is large.
[0047] In addition, it was found that the composite materials (Comparative Examples 7-8) made of a resin composition in which glass fibers were blended with a resin mixture containing polymethylmethacrylate and polylactic acid in a specified ratio exhibited excellent tensile modulus and surface hardness due to the reinforcing effect of the glass fibers, but were inferior in transparency. This is thought to be because the composite materials obtained in Comparative Examples 7-8 contain glass fibers as a filler, and the difference in refractive index between the resin mixture and the glass fibers is large. [Industrial Applicability]
[0048] As described above, according to the present invention, it is possible to obtain a transparent resin composition having excellent tensile modulus and surface hardness, and maintaining the transparency of a resin mixture of polymethyl methacrylate (PMMA) and polylactic acid (PLA). Therefore, the transparent resin composite material made of the transparent resin composition of the present invention is useful as a composite material used for automobile parts such as exterior panel parts such as bumpers, fenders, door panels, mudguards, pillar carnishes, spoilers, side moldings, and interior parts such as instrument panels, meter panels, door trims, console boxes, and cup holders. In addition, when the transparent resin composite material made of the transparent resin composition of the present invention is used as a sheet, it may be laminated with paper or other polymer sheets to be used as a laminate with a multilayer structure.
Claims
1. Contains polymethylmethacrylate (PMMA), polylactic acid (PLA), and silica with a silicon dioxide purity of 90% or more; a mass ratio of the PMMA to the PLA is PMMA:PLA=5:95 to 25:75; The content of the silica is 1 to 8.7 parts by volume per 100 parts by volume of the total of the PMMA and the PLA. A transparent resin composition comprising:
2. 2. The transparent resin composition according to claim 1, wherein a mass ratio of the PMMA to the PLA is PMMA:PLA=10:90 to 20:
80.
3. 3. The transparent resin composition according to claim 1, wherein the silica has a silicon dioxide purity of 99.5% or more.
Citation Information
Patent Citations
Resin composition and molded article obtained from the same
JP2005171204A
Heat-shrinkable film and molded article and container using the same film
JP2006316137A