Trivalent Chromium Plating Method

The trivalent chromium plating method addresses adhesion and appearance issues by using high metal halide content solutions, ensuring excellent film adhesion and quality without complexing agents, thus improving productivity and reducing environmental impact.

JP7566251B2Active Publication Date: 2024-10-15OKUNO CHEM IND CO LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020118276
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-12
Filing Date
2020-07-09
Publication Date
2024-10-15
Estimated Expiration
2040-07-09

AI Technical Summary

Technical Problem

Conventional trivalent chromium plating solutions face issues with adhesion and appearance of the plating film, leading to peeling and poor quality, while hexavalent chromium plating poses environmental concerns.

Method used

A trivalent chromium plating method involving immersion as an anode in a solution with high metal halide content, followed by electrolytic plating as a cathode, using components like trivalent chromium ions and metal halides, without complexing agents, to enhance adhesion and film quality.

Benefits of technology

The method achieves excellent adhesion and appearance of the trivalent chromium plating film, reducing contamination and improving productivity by preventing side reactions and enhancing current efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566251000005
    Figure 0007566251000005
  • Figure 0007566251000006
    Figure 0007566251000006
  • Figure 0007566251000001
    Figure 0007566251000001
Patent Text Reader

Abstract

To provide a trivalent chromium plating method in which a trivalent chromium plating film having excellent adhesion to the object to be plated and having excellent appearance can be formed.SOLUTION: Provided is a trivalent chromium plating method characterized by having (1) a step 1 in which an object to be plated is immersed in a trivalent chromium plating solution containing (A) trivalent chromium ion and (B) at least one metal halide selected from the group consisting of alkali metal chloride and alkaline earth metal chloride and in which the contained amount of the metal halide is 2 mol / L or more as an anode and a voltage is applied, and (2) a step 2 in which the object to be plated after applying voltage in the step 1 is immersed in a trivalent chromium plating solution containing (A) trivalent chromium ion and (B) at least one metal halide selected from the group consisting of alkali metal chloride and alkaline earth metal chloride and in which the contained amount of the metal halide is 2 mol / L or more as a cathode and electrolytic plating is performed, in this order.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a trivalent chromium plating method. [Background technology]

[0002] Chrome plating, which has high hardness and excellent corrosion resistance, wear resistance, etc., is widely used for automobile parts, molding dies, rolling rolls, printing rolls, etc. In particular, chrome plating called hard chrome plating is used for applications such as molding dies and rolls. Chrome plating used for the above applications is required to have an excellent appearance of the plating film.

[0003] Conventionally, a hexavalent chromium plating solution containing hexavalent chromium has been used as a chromium plating solution for carrying out chromium plating.

[0004] However, in recent years, there have been concerns about the environmental impact of using harmful hexavalent chromium plating solutions, and alternative technologies to hexavalent chromium plating solutions are being considered.

[0005] For this reason, the use of a trivalent chromium plating bath containing trivalent chromium, which has a lower environmental impact than hexavalent chromium, has been considered (see, for example, Patent Document 1).

[0006] However, Patent Document 1 does not fully consider the adhesion of the plating film formed. A trivalent chromium plating film formed from a trivalent chromium plating solution is required to have excellent appearance, and poor adhesion causes plating peeling and results in poor appearance.

[0007] Therefore, there is a need for the development of a trivalent chromium plating method capable of forming a trivalent chromium plating film that has excellent adhesion to the plated object and excellent appearance. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] International Publication No. 2015 / 037391 Summary of the Invention [Problem to be solved by the invention]

[0009] An object of the present invention is to provide a trivalent chromium plating method capable of forming a trivalent chromium plating film that has excellent adhesion to an object to be plated and has excellent appearance. [Means for solving the problem]

[0010] As a result of extensive research, the present inventors have found that the above-mentioned object can be achieved by a trivalent chromium plating method comprising, in this order: (1) step 1 of immersing an object to be plated as an anode in a trivalent chromium plating solution containing the above-mentioned components (A) and (B), with the content of the metal halide as component (B) being 2 mol / L or more, and applying a voltage; and (2) step 2 of performing electrolytic plating on the object to be plated after the voltage application in step 1, using the object to be plated as a cathode, thereby completing the present invention.

[0011] That is, the present invention relates to the following trivalent chromium plating method. 1. (1) Step 1 of immersing an object to be plated as an anode in a trivalent chromium plating solution containing (A) trivalent chromium ions and (B) at least one metal halide selected from the group consisting of alkali metal chlorides and alkaline earth metal chlorides, the content of the metal halide being 2 mol / L or more, and applying a voltage; and (2) A step 2 of electrolytic plating by immersing the object to be plated after the voltage application in the step 1 as a cathode in a trivalent chromium plating solution containing (A) trivalent chromium ions and (B) at least one metal halide selected from the group consisting of alkali metal chlorides and alkaline earth metal chlorides, the content of the metal halide being 2 mol / L or more. A trivalent chromium plating method comprising the steps of: 2. The trivalent chromium plating method according to item 1, wherein the content of the metal halide in the trivalent chromium plating solution is 4 mol / L or more. 3. The trivalent chromium plating method according to item 1 or 2, wherein the metal halide is at least one selected from the group consisting of calcium chloride and lithium chloride. 4. The trivalent chromium plating method according to any one of items 1 to 3, wherein the trivalent chromium plating solution further contains (C) a boron compound. 5. The trivalent chromium plating method according to item 4, wherein the boron compound is at least one selected from the group consisting of boric acid, borates, and boron oxide. 6. The trivalent chromium plating method according to item 4 or 5, wherein the content of the boron compound in the trivalent chromium plating solution is 5 to 100 g / L. 7. The trivalent chromium plating method according to any one of items 1 to 6, wherein the trivalent chromium plating solution further contains (D) at least one dispersant selected from the group consisting of glycols, water-soluble polymers, anionic surfactants, amphoteric surfactants, and fluorosurfactants. 8. The trivalent chromium plating method according to item 7, wherein the dispersant is a water-soluble polymer. 9. The trivalent chromium plating method according to item 7 or 8, wherein the content of the dispersant is 0.01 to 100 g / L. Effect of the Invention

[0012] The trivalent chromium plating method of the present invention can form a trivalent chromium plating film that has excellent adhesion to the substrate and excellent appearance. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a schematic diagram showing an example of step 1 of the trivalent chromium plating method of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing an example of step 2 of the trivalent chromium plating method of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The trivalent chromium plating method of the present invention comprises, in this order: (1) step 1 of immersing an object to be plated as an anode in a trivalent chromium plating solution containing (A) trivalent chromium ions, and (B) at least one metal halide selected from the group consisting of alkali metal chlorides and alkaline earth metal chlorides, the content of which is 2 mol / L or more, and applying a voltage; and (2) step 2 of immersing the object to be plated after the voltage application in step 1 as a cathode in a trivalent chromium plating solution containing (A) trivalent chromium ions, and (B) at least one metal halide selected from the group consisting of alkali metal chlorides and alkaline earth metal chlorides, the content of which is 2 mol / L or more, to perform electrolytic plating.

[0015] In the trivalent chromium plating method of the present invention, the object to be plated is immersed as an anode in step 1 and a voltage is applied, so that the oxide film present on the surface of the object to be plated is dissolved. Then, in step 2, the object to be plated after the voltage application in step 1 is used as a cathode for electrolytic plating, so that the oxide film that causes a decrease in the adhesion of the trivalent chromium plating film is dissolved, and therefore the adhesion between the formed trivalent chromium plating film and the object to be plated is excellent and peeling is suppressed, so that the appearance of the trivalent chromium plating film is excellent.

[0016] In conventional plating solutions, complexing agents have been added to obtain sufficient solubility of metals in the plating solution, but the addition of complexing agents causes contamination with nitrogen, carbon, sulfur, etc., resulting in reduced productivity and reduced quality of plated products, and making it difficult to manage the plating solution.

[0017] In addition, when plating is performed using conventional plating solutions, side reactions such as hydrogen generation may occur. As a result, the amount of electricity (current efficiency) used in the main reaction of producing the plated product decreases, resulting in a decrease in productivity of the plated product. In particular, in chromium plating, the absorbed hydrogen is a direct cause of cracking, which affects the quality of the plating film of the plated product obtained.

[0018] In the trivalent chromium plating method of the present invention, the trivalent chromium plating solution used in steps 1 and 2 contains components (A) and (B), and contains at least one metal halide selected from the group consisting of alkali metal halides and alkaline earth metal halides, which is component (B), at a high concentration of 2 mol / L or more, so that it can be used as a plating solution without using a complexing agent. Since the trivalent chromium plating solution does not need to contain a complexing agent, the inclusion of impurities such as nitrogen, carbon, and sulfur is suppressed, and therefore the appearance of the plating film is excellent, and a trivalent chromium plating film excellent in hardness and wear resistance can be formed, and excellent current efficiency can be exhibited.

[0019] In the trivalent chromium plating method of the present invention, the trivalent chromium plating solution used in steps 1 and 2 contains at least one metal halide selected from the group consisting of alkali metal halides and alkaline earth metal halides, which is component (B), at a high concentration of 2 mol / L or more. This allows the solvent molecules to coordinate with and stabilize the metal ions, thereby suppressing side reactions such as hydrogen generation when forming a plating film, thereby improving the productivity of the plating film and reducing the impact on the quality of the plating film.

[0020] The trivalent chromium plating method of the present invention will be specifically described below.

[0021] (Process 1) Step 1 is a step of immersing an object to be plated as an anode in a trivalent chromium plating solution containing (A) trivalent chromium ions and (B) at least one metal halide selected from the group consisting of alkali metal chlorides and alkaline earth metal chlorides, the content of the metal halide being 2 mol / L or more, and applying a voltage.

[0022] Step 1 will be explained using Figure 1. Figure 1 is a schematic diagram showing an example of step 1. In Figure 1, an object to be plated 1 is used as an anode, and is immersed together with a cathode 2 in a trivalent chromium plating solution 3, and a voltage is applied.

[0023] In step 1, the object to be plated (anode) is not particularly limited, and examples thereof include metal materials such as iron, stainless steel, brass, and zinc die-casting used in the manufacture of dies, rolling rolls, and printing rolls; and other metal materials such as nickel, aluminum, titanium, zirconium, and molybdenum. For such objects to be plated, thick plating of about 50 μm or more may be performed to form a trivalent chromium plating film. The object to be plated (anode) in step 1 is used as a cathode in step 2 by immersing it in a trivalent chromium plating solution.

[0024] The cathode in step 1 is used as an anode in step 2 by immersing it in a trivalent chromium plating solution. The cathode in step 1 (anode in step 2) is not particularly limited, and various insoluble or soluble anodes can be used. Examples of insoluble anodes include carbon, Ti / Pt (Ti coated with platinum-based coating), Ti / Ir oxide (Ti coated with Ir oxide), Ti / Ru oxide (Ti coated with Ru oxide), Ti / Ir oxide-Ru oxide (Ti coated with a mixture of Ir oxide and Ru oxide), Ti / Ir oxide-Ta oxide (Ti coated with a mixture of Ir oxide and Ta oxide), Ti / Pt / Ir oxide-Ru oxide (Ti / Pt coated with Ir oxide and Ta oxide), Examples of the electrode include a metal electrode (a metal electrode coated with Ru oxide mixed therein), Ti / Pt / Ir oxide-Ta oxide (a metal electrode coated with Ti / Pt mixed with Ir oxide and Ta oxide), stainless steel, aluminum, lead alloys (Pb-Sn alloy, Pb-Ag alloy, Pb-Sb alloy), lead oxide (lead monoxide, lead dioxide, lead trioxide, trilead tetroxide), lead, tin oxide, carbon, diamond electrodes (a metal electrode coated with a substrate such as silicon or niobium containing diamond containing nitrogen or boron), and ITO electrodes (indium tin electrodes). Among these, it is preferable to use a carbon electrode because of its excellent durability. In addition, when a metal chromium electrode is used as the cathode in step 1 (anode in step 2), the generation of halogen gas such as chlorine gas can be suppressed as described later.

[0025] The voltage applied in step 1 may be appropriately set depending on the size of the object to be plated, and is preferably 0.5 to 20 V, more preferably 1 to 10 V. When the lower limit of the applied voltage is within the above range, the oxide film present on the surface of the object to be plated is further dissolved, and the adhesion between the trivalent chromium plating film and the object to be plated is further improved. Also, when the upper limit of the applied voltage is within the above range, the object to be plated is prevented from dissolving more than necessary, and the plating appearance is further improved.

[0026] The applied current in step 1 may be appropriately set depending on the size of the object to be plated, and is preferably 0.05 to 1000 A, more preferably 0.5 to 500 A. When the lower limit of the applied current is within the above range, the oxide film present on the surface of the object to be plated is further dissolved, and the adhesion between the trivalent chromium plating film and the object to be plated is further improved. Also, when the upper limit of the applied current is within the above range, the object to be plated is prevented from dissolving more than necessary, and the plating appearance is further improved.

[0027] The current density in step 1 is 0.01 to 10 A / dm 2 is preferable, and 0.1 to 5 A / dm 2 is more preferable. When the lower limit of the current density is within the above range, the oxide film present on the surface of the plated object is further dissolved, and the adhesion between the trivalent chromium plating film and the plated object is further improved. When the upper limit of the current density is within the above range, the plated object is prevented from being dissolved more than necessary, and the plating appearance is further improved.

[0028] In step 1, the voltage application time is preferably 0.1 to 5 minutes, more preferably 0.5 to 2 minutes. When the lower limit of the voltage application time is within the above range, the oxide film present on the surface of the plated object is further dissolved, and the adhesion between the trivalent chromium plating film and the plated object is further improved. When the upper limit of the voltage application time is within the above range, the plated object is prevented from being dissolved more than necessary, and the plating appearance is further improved.

[0029] In step 1, the temperature of the trivalent chromium plating solution is preferably 20 to 70°C, more preferably 30 to 60°C. When the lower limit of the temperature of the trivalent chromium plating solution is within the above range, the oxide film present on the surface of the plated object is further dissolved, and the adhesion between the trivalent chromium plating film and the plated object is further improved. Also, when the upper limit of the temperature of the trivalent chromium plating solution is within the above range, the plated object is prevented from being dissolved more than necessary, and the plating appearance is further improved.

[0030] (Trivalent chromium plating solution) The trivalent chromium plating solution used in the present invention is described below. The trivalent chromium plating solution used in the present invention is a trivalent chromium plating solution containing (A) trivalent chromium ions and (B) at least one metal halide selected from the group consisting of alkali metal chlorides and alkaline earth metal chlorides, and having a metal halide content of 2 mol / L or more.

[0031] Component (A) The trivalent chromium plating solution contains trivalent chromium ions as component (A). The trivalent chromium ions are present in the trivalent chromium plating solution by dissolving a trivalent chromium compound in a solvent contained in the trivalent chromium plating solution.

[0032] The trivalent chromium compound may be any trivalent chromium compound that is soluble in a solvent, such as chromium chloride, chromium sulfate, basic chromium sulfate, etc. Among these, chromium chloride is preferred because it is less likely to produce an insoluble salt. The trivalent chromium compound may be used alone or in combination of two or more.

[0033] The concentration of trivalent chromium ions is not particularly limited, but is preferably, for example, 2 to 100 g / L, and more preferably 5 to 70 g / L.

[0034] (B) Component The trivalent chromium plating solution contains, as component (B), at least one metal halide selected from the group consisting of alkali metal halides and alkaline earth metal halides.

[0035] The alkali metal halide is not particularly limited, and examples thereof include chlorides and bromides of alkali metals. As the alkali metal halide, lithium chloride and lithium bromide are preferred, and lithium chloride is more preferred.

[0036] The alkaline earth metal halide is not particularly limited, and examples thereof include chlorides and bromides of alkaline earth metals. Examples of alkaline earth metal halides include calcium chloride.、 Calcium bromide is preferred, and calcium chloride is more preferred.

[0037] As the metal halide, calcium chloride and lithium chloride can be preferably used, and calcium chloride can be more preferably used.

[0038] The above metal halides may be used alone or in combination of two or more.

[0039] The content of the metal halide in the trivalent chromium plating solution is 2 mol / L or more. If the content of the metal halide is less than 2 mol / L, the appearance of the plating film is poor, and the hardness and wear resistance are reduced. The content of the metal halide is preferably 4 mol / L or more, more preferably 4.2 mol / L or more. The content of the metal halide is preferably 18 mol / L or less, more preferably 15 mol / L or less, even more preferably 10 mol / L or less, and particularly preferably 7 mol / L or less. By setting the upper limit of the content of the metal halide within the above range, the generation of halogen gas such as chlorine gas during the formation of the trivalent chromium plating film can be further suppressed.

[0040] (C) Component The trivalent chromium plating solution preferably contains a boron compound as component (C). By containing a boron compound in the trivalent chromium plating solution, the appearance of the trivalent chromium plating film is further improved, and the hardness and abrasion resistance are further improved.

[0041] The boron compound is not particularly limited, and examples thereof include boric acid, borates such as sodium borate and potassium borate, and boron oxide. Among these, boric acid and boron oxide are preferred because they are less likely to form insoluble salts. The boron compound may be used alone or in combination of two or more.

[0042] The concentration of the boron compound is not particularly limited, but is preferably 5 to 100 g / L, more preferably 10 to 90 g / L, even more preferably 10 to 80 g / L, and particularly preferably 20 to 80 g / L. When the content of the boron compound is within the above range, the appearance of the trivalent chromium plating film formed using the trivalent chromium plating solution is further improved, and the hardness and abrasion resistance are further improved.

[0043] (D) Component The trivalent chromium plating solution preferably contains at least one dispersant selected from the group consisting of glycols, water-soluble polymers, anionic surfactants, amphoteric surfactants, and fluorosurfactants as component (D). When the trivalent chromium plating solution contains the dispersant, the appearance of the trivalent chromium plating film is further improved, and the hardness and abrasion resistance are further improved. The dispersants can be used alone or in combination of two or more.

[0044] The glycols are not particularly limited, and examples thereof include alkyl glycols and derivatives thereof, such as ethylene glycol, propylene glycol, and diethylene glycol.

[0045] The trivalent chromium plating solution preferably contains a water-soluble polymer as component (D). When the trivalent chromium plating solution contains a water-soluble polymer, the occurrence of pitting corrosion in the formed trivalent chromium plating film is suppressed, the appearance of the trivalent chromium plating film is further improved, and the hardness and wear resistance are further improved. Although no limiting interpretation is desired, one of the reasons why the water-soluble polymer exerts a pitting corrosion suppression effect is thought to be that it captures halide ions such as chloride ions that cause pitting corrosion.

[0046] The water-soluble polymer is not particularly limited as long as it can exhibit the above-mentioned functions. Examples of the water-soluble polymer include synthetic polymers such as polyalkylene glycol (e.g., polyethylene glycol, polypropylene glycol, polybutylene glycol), polyvinyl alcohol, polyethylene oxide, polyvinylpyrrolidone, polyamide, polyimide, polyoxyethylene alkyl ether, polyoxyethylene glycol-glyceryl ether, polyoxypropylene glycol-glyceryl ether, polyethylene glycol-polypropylene glycol block ether, polyoxyalkylene alkyl ether, polyoxyethylene alkyl glycol, polyoxypropylene alkyl glycol, polyoxyethylene oxypropylene glycol, polyoxyethylene nonylphenyl ether, polyacrylic acid, polymethacrylic acid, polyacrylamide, poly(2-hydroxy-2-oxo-1,3,2-dioxaphospholane) (PHP), and polymethacryloyloxyethyl phosphorylcholine; natural or semi-synthetic polymers such as proteins and polysaccharides (dextran, starch, cellulose, cellulose derivatives, etc.). Among these, synthetic polymers are preferable, polyalkylene glycol, polyoxyalkylene alkyl ether, polyvinyl alcohol, etc. are more preferable, polyalkylene glycol is further preferable, and polyethylene glycol and polypropylene glycol are further preferable.

[0047] The water-soluble polymer may be a copolymer formed of two or more types of constitutional units, such as a random copolymer, a block copolymer, or a graft copolymer.

[0048] The average molecular weight of the water-soluble polymer is preferably 200 to 20,000, more preferably 200 to 5,000, and even more preferably 200 to 2,000. The average molecular weight here may be either a number average molecular weight or a weight average molecular weight, and these average molecular weights can be measured by gel permeation chromatography (GPC) or the like.

[0049] The anionic surfactant is not particularly limited, and examples thereof include sodium alkyl sulfate, sodium polyoxyethylene alkyl ether sulfate, and dialkyl sulfosuccinic acid.

[0050] The amphoteric surfactant is not particularly limited, and examples thereof include alkyl dimethylamine oxide and alkyl carboxybetaine.

[0051] The fluorine-based surfactant is not particularly limited, and may be an anionic fluorine-based surfactant. As the fluorine-based surfactant, a commercially available product may be used. As a commercially available fluorine-based surfactant, for example, Futergent 110 (a fluorine-based anionic surfactant manufactured by Neos Co., Ltd.) may be used.

[0052] As the dispersant, glycols, polyethylene glycol, polypropylene glycol, polybutylene glycol, polyoxyethylene glycol-glyceryl ether, polyoxypropylene glycol-glyceryl ether, polyethylene glycol-polypropylene glycol block ether, polyoxyethylene alkyl ether, and polyoxyethylene alkyl ether sulfate sodium salt are preferred, and polyethylene glycol and polypropylene glycol are more preferred.

[0053] The concentration of the dispersant is not particularly limited, but is preferably 0.01 to 100 g / L, more preferably 0.1 to 50 g / L, even more preferably 0.1 to 30 g / L, and particularly preferably 0.1 to 20 g / L. When the content of the dispersant is within the above range, the appearance of the trivalent chromium plating film formed using the trivalent chromium plating solution is further improved, and the hardness and abrasion resistance are further improved.

[0054] (Other additives) The trivalent chromium plating solution may contain additives other than the above components (A) to (D), such as complexing agents, fluorides, conductive salts, chlorine generation inhibitors, precipitation accelerators, mist inhibitors, and pit inhibitors, which are used in ordinary trivalent chromium plating solutions.

[0055] The complexing agent is not particularly limited as long as it is a compound that has a complexing ability with trivalent chromium. As the complexing agent, a complexing agent that does not form an insoluble salt with calcium, such as a water-soluble carboxylic acid compound, is preferable. Examples of such complexing agents include formic acid, acetic acid, malonic acid, succinic acid, citric acid, glycine, and salts thereof.

[0056] As the fluoride, sodium fluoride, potassium fluoride, ammonium fluoride, boron fluoride, calcium fluoride, aluminum fluoride, etc. can be used.

[0057] As the conductive salt, a chloride salt such as sodium chloride, potassium chloride, ammonium chloride, aluminum chloride, magnesium chloride, barium chloride, etc. can be used.

[0058] As the chlorine generation inhibitor, bromides such as sodium bromide, potassium bromide, and ammonium bromide can be used.

[0059] As the deposition accelerator, sulfur compounds such as sodium saccharin, sodium dithionate, sodium thiosulfate, and sodium thiocyanate can be used.

[0060] Trivalent chromium plating solution The trivalent chromium plating solution is prepared by dissolving the above-mentioned components (A) and (B), and, if necessary, components (C) and (D), and other additives, in a solvent, and the order in which each component is dissolved is arbitrary.

[0061] The solvent used in the trivalent chromium plating solution is not particularly limited as long as it can dissolve the above-mentioned components, and for example, water can be used.

[0062] The pH of the trivalent chromium plating solution is not particularly limited, but is preferably -2 to 4, and more preferably -1 to 2.

[0063] In step 1 described above, the object to be plated is immersed as an anode in the trivalent chromium plating solution, and a voltage is applied.

[0064] (Process 2) Step 2 is a step of performing electrolytic plating by immersing the object to be plated after the voltage application in step 1 as a cathode in a trivalent chromium plating solution containing (A) trivalent chromium ions and (B) at least one metal halide selected from the group consisting of alkali metal chlorides and alkaline earth metal chlorides, the content of the metal halide being 2 mol / L or more.

[0065] In step 2, the trivalent chromium plating solution used in the electrolytic plating may be the trivalent chromium plating solution having the above composition described in step 1, and for example, only one tank of the trivalent chromium plating solution described in step 1 may be prepared, and the trivalent chromium plating solution used in step 1 may be used as is in step 2. In addition, in step 2, a trivalent chromium plating solution having the above composition may be prepared separately from the trivalent chromium plating solution used in step 1, and steps 1 and 2 may be performed in separate tanks, using two tanks, a trivalent chromium plating solution tank for performing step 1 and a trivalent chromium plating solution tank for performing step 2.

[0066] Step 2 will be described with reference to FIG. 2. FIG. 2 is a schematic diagram showing an example of step 2. In FIG. 2, the object to be plated 1 is used as a cathode, and is immersed in a trivalent chromium plating solution 3 together with an anode 2, and a voltage is applied. That is, in FIG. 2, in step 2, the direction of the applied voltage in step 1 is reversed in the device in step 1, so that the anode in step 1 becomes the cathode in step 2, and the cathode in step 1 becomes the anode in step 2, and the anode and cathode are reversed from those in step 1, and a voltage is applied. In step 2 of the trivalent chromium plating method of the present invention, as described above, it is preferable to reverse the direction of the applied voltage in the device in step 1 as it is, and use the anode in step 1 as the cathode in step 2, and use the cathode in step 1 as the anode in step 2. That is, step 2 is preferably a step in which the object to be plated after the voltage application in step 1 is immersed as a cathode in the trivalent chromium plating solution used in step 1 to perform electrolytic plating.

[0067] The applied voltage in step 2 may be appropriately set depending on the size of the object to be plated, and is preferably 1 to 50 V, more preferably 3 to 20 V. When the lower limit of the applied voltage is within the above range, the trivalent chromium plating film is more sufficiently formed on the surface of the object to be plated, and the adhesion between the trivalent chromium plating film and the object to be plated is further improved. Also, when the upper limit of the applied voltage is within the above range, the generation of halogen gas is further suppressed.

[0068] The applied current in step 2 may be appropriately set depending on the size of the object to be plated, and is preferably 0.1 to 5000 A, more preferably 1 to 1000 A. When the lower limit of the applied current is within the above range, a trivalent chromium plating film is more sufficiently formed on the surface of the object to be plated, and the adhesion between the trivalent chromium plating film and the object to be plated is further improved. Also, when the upper limit of the applied current is within the above range, the generation of halogen gas is further suppressed.

[0069] The current density in step 2 is not particularly limited and may be appropriately determined depending on the type of object to be plated. For example, it may be 1 to 20 A / dm 2 An appropriate current density range can be appropriately determined from the current density ranges.

[0070] In step 2, the voltage application time is preferably 1 to 600 minutes, more preferably 2 to 300 minutes. When the lower limit of the application time is within the above range, a trivalent chromium plating film is more sufficiently formed on the surface of the plated object, and the adhesion between the trivalent chromium plating film and the plated object is further improved. When the upper limit of the application time is within the above range, the plating appearance is further improved. The plating time in step 2 may be appropriately determined depending on the desired film thickness of the trivalent chromium plating film.

[0071] In step 2, the temperature of the trivalent chromium plating solution is preferably 20 to 70° C., more preferably 30 to 60° C. When the lower limit of the temperature of the trivalent chromium plating solution is within the above range, the appearance, hardness, and abrasion resistance of the trivalent chromium plating film are further improved. Also, when the upper limit of the temperature of the trivalent chromium plating solution is within the above range, the throwing power of the trivalent chromium plating film is further improved.

[0072] The anode / cathode area ratio in step 2 is not particularly limited and may be appropriately determined depending on the type of object to be plated. For example, an appropriate anode / cathode area ratio may be appropriately determined within the anode / cathode area ratio range of 0.5 to 3.

[0073] In step 2 described above, the object to be plated after the voltage application in step 1 is immersed as a cathode in the trivalent chromium plating solution to perform electrolytic plating, and a trivalent chromium plating film is formed on the object to be plated.

[0074] In the trivalent chromium plating method of the present invention, it is preferable to use a soluble anode containing metallic chromium as the anode in step 2. In the trivalent chromium plating method of the present invention, a trivalent chromium plating solution containing 2 mol / L or more of metal halide is used as the trivalent chromium plating solution, so that halogen gas such as chlorine gas may be easily generated at the anode in step 2. However, when a soluble anode containing metallic chromium is used in step 2, metallic chromium (Cr 0 ) is trivalent chromium ion (Cr 3+ ), which further suppresses the generation of chlorine gas.

[0075] Metallic chromium used as a soluble anode is usually used as a metallic chromium electrode, and metallic chromium (Cr 0 ) is dissolved and trivalent chromium ions (Cr 3+The soluble anode is not particularly limited as long as it can produce the reaction: (1) Cr+Cr+H ...

[0076] The trivalent chromium plating solution may be stirred in steps 1 and / or 2. The stirring method is not particularly limited, and examples thereof include bubbling stirring with air or nitrogen, circulating stirring with a pump, and stirring by rocking the object to be plated in the plating solution.

[0077] By the above-described step 2, the object to be plated is plated with trivalent chromium, and an article having a trivalent chromium plating film formed thereon can be obtained.

[0078] The trivalent chromium plating method of the present invention may further include a washing step of washing the article on which the trivalent chromium plating film is formed with an alkaline solution. In the article on which the trivalent chromium plating film is formed, cracks may occur in the trivalent chromium plating film, or trivalent chromium plating solution may remain at the interface between the plated object and the trivalent chromium plating film, which may promote corrosion of the trivalent chromium plating film or the plated object. By including the washing step in the trivalent chromium plating method of the present invention, the remaining trivalent chromium plating solution can be removed, and the above-mentioned corrosion can be suppressed.

[0079] The alkaline compound contained in the alkaline solution used in the washing step is not particularly limited, and examples thereof include sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide, magnesium hydroxide, sodium carbonate, potassium carbonate, ammonium carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, ammonium hydrogen carbonate, and ammonia.

[0080] The method for cleaning the article on which the trivalent chromium plating film is formed is not particularly limited, and it is sufficient that the alkaline solution is brought into contact with the article on which the trivalent chromium plating film is formed. For example, there are a cleaning method in which the article on which the trivalent chromium plating film is formed is immersed in an alkaline solution, a method in which the article on which the trivalent chromium plating film is formed is sprayed with an alkaline solution, and the like.

[0081] The content of the alkaline compound in the alkaline solution is not particularly limited, and is preferably 0.01 to 10 mol / L, more preferably 0.1 to 7 mol / L, even more preferably 0.1 to 5 mol / L, and particularly preferably 1 to 5 mol / L. When the lower limit of the content of the alkaline compound is within the above range, the remaining trivalent chromium plating solution can be more effectively removed, and the corrosion of the article on which the trivalent chromium film is formed can be more effectively suppressed. In addition, when the upper limit of the content of the alkaline compound is within the above range, the adhesion of the alkaline compound to the article on which the trivalent chromium film is formed is suppressed, and the appearance of the trivalent chromium plating film is further improved.

[0082] The temperature of the alkaline solution is not particularly limited, and is preferably 20°C or higher, and more preferably 40°C or higher. When the lower limit of the alkaline solution temperature is within the above range, the remaining trivalent chromium plating solution can be more effectively removed, and the corrosion of the article on which the trivalent chromium film is formed can be more effectively suppressed. The upper limit of the alkaline solution temperature is not particularly limited as long as the evaporation of the alkaline solution can be suppressed, and is preferably 100°C or lower, more preferably 90°C or lower, and even more preferably 70°C or lower.

[0083] The cleaning time in the cleaning step is not particularly limited, and is preferably 1 minute or more, and more preferably 3 minutes or more. When the lower limit of the cleaning time is within the above range, the remaining trivalent chromium plating solution can be more effectively removed, and the corrosion of the article on which the trivalent chromium film is formed can be more effectively suppressed. The upper limit of the cleaning time is not particularly limited, and is preferably 30 minutes or less, and more preferably 15 minutes or less. When the upper limit of the cleaning time is within the above range, the adhesion of alkaline compounds to the article on which the trivalent chromium film is formed is suppressed, and the appearance of the trivalent chromium plating film is further improved.

[0084] (Articles on which a trivalent chromium plating film is formed by a trivalent chromium plating method) By the above-described trivalent chromium plating method, an article having a trivalent chromium plating film formed thereon can be obtained. The article is not particularly limited, and an article that requires hardness, corrosion resistance, and abrasion resistance is preferable. Such articles include automobile parts, molding dies, various mechanical parts that are easily worn, tools, rolls used in printing, papermaking, rolling, film processing, and steelmaking, etc. EXAMPLES

[0085] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the examples.

[0086] 1. Evaluation of trivalent chromium plating film The objects to be plated were treated and chrome plated according to the process shown in Table 1 below. Note that in Table 1, the degreasing process was performed with chemical solution (1) when the objects to be plated were Fe, stainless steel, Ni, Ti, Zr, or Mo, and with chemical solution (2) when the objects to be plated were Al.

[0087] [Table 1]

[0088] The chrome plating process of each of the examples and comparative examples will be described in detail below.

[0089] (Preparation of trivalent chromium plating solution) The raw materials shown in Table 2 were mixed in the proportions shown in the table to prepare 1 L of trivalent chromium plating solution.

[0090] [Table 2]

[0091] Examples 1 to 8 (Process 1) The object to be plated shown in Table 3 was immersed in the trivalent chromium plating solution prepared as described above, using the object as the anode and a carbon electrode as the cathode, at a current density of 2 A / dm 2 A voltage was applied for 1 minute at a liquid temperature of 40°C.

[0092] (Process 2) Next, in the device of step 1, the direction of the applied voltage in step 1 is reversed, and the object to be plated after the voltage application in step 1 is used as the cathode as shown in Table 3, and the carbon electrode is used as the anode, and electrolytic plating is performed under the conditions shown in Table 3. Test pieces of Examples 1 to 8 were prepared by applying marking.

[0093] [Table 3]

[0094] Comparative Examples 1 to 8 Test pieces of Comparative Examples 1 to 8 were prepared in the same manner as in Examples 1 to 8, except that, as the chrome plating process, step 1 was not carried out on the object to be plated, and only step 2 was carried out.

[0095] The test pieces prepared in the above Examples and Comparative Examples were used to carry out the following evaluations.

[0096] (Appearance of plating film (adhesion evaluation)) The surface of the trivalent chromium plating film of the test piece was visually observed and evaluated according to the following evaluation criteria. ○: No peeling of plating observed △: Some plating peeling is observed. ×: Peeling of plating is observed frequently

[0097] The results are shown in Table 4.

[0098] [Table 4]

[0099] The results in Table 4 show that in Examples 1 to 8, which include, in that order, step 1 of immersing the object to be plated as an anode in a trivalent chromium plating solution containing the components (A) and (B) and applying a voltage, and step 2 of performing electrolytic plating on the object to be plated after the voltage has been applied in step 1 as a cathode, the same object to be plated was used, and when compared with Comparative Examples 1 to 8 which do not include step 1 for each of the same objects to be plated, Examples 1 to 8 which include step 1 showed no plating peeling and had superior adhesion of the trivalent chromium plating film. [Explanation of symbols]

[0100] 1. Object to be plated (anode in step 1, cathode in step 2) 2. Cathode in step 1, anode in step 2 3. Trivalent chromium plating solution

Claims

1. (1) A step 1 of immersing an object to be plated as an anode in a trivalent chromium plating solution containing (A) trivalent chromium ions and (B) at least one metal halide selected from the group consisting of alkali metal chlorides and alkaline earth metal chlorides, the content of the metal halide being 2 mol / L or more, and applying a voltage; and (2) A step of immersing the plated object after the voltage application in the step 1 as a cathode in a trivalent chromium plating solution containing (A) trivalent chromium ions and (B) at least one metal halide selected from the group consisting of alkali metal chlorides and alkaline earth metal chlorides, the content of the metal halide being 2 mol / L or more, to perform electrolytic plating. in that order, The metal halide includes calcium chloride. A method for trivalent chromium plating comprising the steps of:

2. 2. The trivalent chromium plating method according to claim 1, wherein the content of the metal halide in the trivalent chromium plating solution is 4 mol / L or more.

3. The trivalent chromium plating method according to claim 1 or 2, wherein the trivalent chromium plating solution further contains (C) a boron compound.

4. The trivalent chromium plating method according to claim 3, wherein the boron compound is at least one selected from the group consisting of boric acid, a borate salt, and boron oxide.

5. The trivalent chromium plating method according to claim 3 or 4, wherein the content of the boron compound in the trivalent chromium plating solution is 5 to 100 g / L.

6. The trivalent chromium plating solution further contains (D) at least one dispersant selected from the group consisting of glycols, water-soluble polymers, anionic surfactants, amphoteric surfactants, and fluorine-based surfactants. The trivalent chromium plating method according to any one of claims 1 to 5.

7. The trivalent chromium plating method according to claim 6, wherein the dispersant is a water-soluble polymer.

8. The trivalent chromium plating method according to claim 6 or 7, wherein the content of the dispersant is 0.01 to 100 g / L.

Citation Information

Patent Citations

  • Electroplating solution and anode device thereof

    JP1979134038A

  • A photoresist layer on a substrate of the thermal imaging method

    JP1988501744A

  • Trivalent chromium plating bath

    JP2002285375A

  • Crystalline chromium alloy deposits

    JP2010540781A

  • Method for producing metal coatings

    JP2015518925A