Method for producing cellulose nanofiber dry solid and redispersion of cellulose nanofiber
The method of dispersing, drying, and redispersing cellulose nanofibers with controlled shear rates and densities addresses aggregation issues, enhancing dispersibility and mechanical properties in composites while reducing storage and transportation costs.
Patent Information
- Application Number
- JP2020022573
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-02-13
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-02-13
AI Technical Summary
Cellulose nanofibers aggregate in a dry state, making it difficult to reproduce a good dispersion state after drying, leading to storage and transportation challenges and reduced mechanical properties in composites.
A method involving dispersing cellulose nanofibers in a first medium, drying to form a solid, and then redispersing in a second medium with controlled shear rates and densities to maintain good dispersibility, using aprotic polar solvents and shearing forces.
The method enables the reproduction of a good dispersion state for cellulose nanofibers, improving mechanical properties in composites and reducing storage and transportation costs by maintaining high apparent densities.
Smart Images

Figure 0007566472000003 
Figure 0007566472000004 
Figure 0007566472000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a dry solid of cellulose nanofibers and a redispersion of cellulose nanofibers. [Background technology]
[0002] Thermoplastic resins are light and have excellent processability, and therefore are widely used in many fields such as automobile parts, electrical and electronic parts, office equipment housings, and precision parts. However, resins alone often have insufficient mechanical properties and dimensional stability, and therefore composites of resins and various fillers are generally used. In recent years, the use of nanofibers such as cellulose nanofibers (CNF) as such fillers has been considered. Nanofibers such as CNF have the property of easily agglomerating in a dry state, so they are produced as a dispersion liquid that allows stable dispersion. When applying cellulose nanofibers to various applications, the above dispersion liquid may be dried and then redispersed in a dispersion medium to prepare a redispersion liquid.
[0003] Patent Document 1 describes a method for redispersing a cellulose nanofiber dispersion by drying a produced cellulose nanofiber dispersion and dispersing the cellulose nanofiber powder particles produced in an aqueous solvent again, which is characterized in that when the cellulose nanofiber powder particles are redispersed in the aqueous solvent, they are stirred and mechanical shear force is applied.
[0004] Patent document 2 describes a method for treating chemically modified fibril cellulose, which comprises introducing the chemically modified fibril cellulose material into a thermal drying device (20) comprising a belt (22) so that the fibril cellulose material forms at least one rod-shaped body on the belt (22), and dewatering the chemically modified fibril cellulose material on the belt (22) using a heated air flow having a temperature of at least 40°C, concentrating and / or drying the chemically modified fibril cellulose material such that the dry solids content of the fibril cellulose material after the thermal drying device (20) is at least 10%.
[0005] Patent Document 3 describes powdered nanofibers, which are characterized in that (A) powdered nanofibers are mixed with (B) a dispersant in an amount of 1 to 40% by weight, calculated as solid content, and have a bulk density of 90 to 200 g / L.
[0006] Patent Document 4 describes a method in which cellulose nanofibers are homogenized in the presence of an organic solvent, and then the organic solvent is removed to produce dry microfibers with a moisture content of 0 to 1% by mass. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2017 / 154568 [Patent Document 2] Special Publication No. 2015-512964 [Patent Document 3] JP 2017-210596 A [Patent Document 4] JP 2012-224960 A Summary of the Invention [Problem to be solved by the invention]
[0008] When cellulose nanofibers are stored or transported in the form of a dispersion liquid, problems arise in that the cellulose nanofibers are easily deteriorated (putrefaction, etc.) because they are placed in a humid environment, and in that the dispersion medium takes up extra volume and weight, which increases storage and transportation costs. If the cellulose nanofibers are stored or transported in a dry state, the volume and weight can be reduced, and there is also the advantage that they can be easily composited with other materials depending on the application. However, once the cellulose nanofibers are dried from the dispersion liquid state, it is difficult to reproduce the good dispersion state of the cellulose nanofibers before drying, even if they are subsequently redispersed in a dispersion medium.
[0009] The present invention aims to solve the above-mentioned problems and provide a cellulose nanofiber dry solid that exhibits good redispersibility, and a method for producing a redispersion liquid of cellulose nanofibers that can reproduce the good dispersion state of the cellulose nanofibers before drying when the cellulose nanofiber dry solid obtained by drying the dispersion liquid is redispersed in a dispersion medium. [Means for solving the problem]
[0010] As a result of intensive research to solve the above problems, the present inventors discovered that cellulose nanofibers that have been dried to a specific apparent density have excellent dispersibility in a dispersion medium, which led to the creation of the present invention. That is, the present invention encompasses the following aspects. [1] A method for producing a redispersion of cellulose nanofibers, comprising: A dispersing step of preparing a dispersion liquid by dispersing cellulose nanofibers in a first dispersion medium; A drying step of drying the dispersion to obtain a dry solid of cellulose nanofibers; A redispersion step of redispersing the cellulose nanofiber dry solid in a second dispersion medium to prepare a redispersion liquid; Including, The cellulose nanofibers in the redispersion were adjusted to a water dispersion with a solid content of 0.5% by mass, and the shear rate of the water dispersion was 100 seconds. -1The viscosity at shear rate of the aqueous dispersion of the cellulose nanofibers of the dispersion adjusted to a solid content of 0.5 mass% was 100 s -1 The viscosity of the solution is 30% or more of that in the solution. [2] The method according to aspect 1, wherein the apparent density of the dry solid cellulose nanofiber is 210 g / L to 1,500 g / L. [3] The method according to aspect 1 or 2, wherein the average degree of substitution DS of the cellulose nanofiber dry solid is 0.5 or less. [4] The method according to any one of aspects 1 to 3 above, wherein the content of the dispersant in the dry solid cellulose nanofiber is less than 1 mass%. [5] The second dispersion medium is an aprotic polar solvent; The method according to any one of the above-mentioned aspects 1 to 4, wherein the redispersion is carried out by applying a shear force through stirring. [6] The method according to any one of the above aspects 1 to 5, wherein the shear force is applied using one or more selected from the group consisting of ultrasonic waves, a bead mill, a ball mill, and a homomixer. [7] The method according to any one of the above aspects 1 to 6, wherein the aprotic polar solvent is one or more selected from the group consisting of dimethylsulfoxide, N-methylpyrrolidone, dimethylacetamide, and dimethylformamide. [8] The method according to any one of aspects 1 to 7 above, further comprising chemically modifying the cellulose nanofibers during and / or after the redispersion step. [9] A cellulose nanofiber dry solid having an apparent density of 210 g / L to 1,500 g / L.
[10] The cellulose nanofiber dry solid according to the above-mentioned embodiment 9, wherein the average degree of substitution DS is 0.5 or less.
[11] The cellulose nanofiber dry solid according to aspect 9 or 10, wherein the content of the dispersant is less than 1% by mass.
[12] A method for producing a cellulose nanofiber composite containing a cellulose nanofiber and an organic binder, comprising: A step of preparing a redispersion of cellulose nanofibers by a method according to any one of aspects 1 to 8 above; and mixing the redispersion liquid or a dried product thereof with an organic binder; A method comprising:
[13] A method for producing a resin composite containing cellulose nanofibers and a resin, comprising: A step of preparing a redispersion of cellulose nanofibers by a method according to any one of aspects 1 to 8 above; and a mixing step of mixing the redispersion liquid, an aqueous dispersion obtained by replacing the second dispersion medium of the redispersion liquid with water, or a dried product thereof with a resin; A method comprising:
[14] A method for producing a resin composition containing cellulose nanofibers and a thermoplastic resin, comprising: A cellulose nanofiber solid forming step for obtaining a cellulose nanofiber solid, which is a dry solid of defibrated cellulose nanofibers; A redispersion step of redispersing the cellulose nanofiber solid in a second dispersion medium to prepare a redispersion liquid; and a kneading step of kneading the redispersion liquid, an aqueous dispersion obtained by replacing the second dispersion medium of the redispersion liquid with water, or a dried product thereof with a thermoplastic resin; Including, The cellulose nanofibers in the redispersion were adjusted to a water dispersion with a solid content of 0.5% by mass, and the shear rate of the water dispersion was 100 seconds. -1 The viscosity at shear rate of the aqueous dispersion of the cellulose nanofibers of the dispersion adjusted to a solid content of 0.5 mass% was 100 s -1 The viscosity of the solution is 30% or more of that in the solution.
[15] The method described in claim 14, wherein in the cellulose nanofiber solid, the cellulose nanofibers are bonded to each other by hydrogen bonds of hydroxyl groups.
[16] The method according to aspect 14 or 15 above, wherein the rate of change (YX) / Y of the mass of the dry solid matter (X) when the cellulose nanofiber solid is allowed to stand in water at 20°C for 2 hours and then removed from the water relative to the mass (Y) of the cellulose nanofiber solid before standing is 30 mass% or less.
[17] The method according to any one of Aspects 14 to 16, wherein the second dispersion medium is selected from the group consisting of dimethylsulfoxide, N-methylpyrrolidone, dimethylacetamide, and dimethylformamide. Effect of the Invention
[0011] According to one aspect of the present invention, there can be provided a cellulose nanofiber dry solid that exhibits good redispersibility, and a method for producing a redispersion liquid of cellulose nanofibers that can reproduce the good dispersion state of the cellulose nanofibers before drying when the cellulose nanofiber dry solid obtained by drying the dispersion liquid is redispersed in a dispersion medium. [Brief description of the drawings]
[0012] [Figure 1] 13 is an explanatory diagram of a method for calculating the IR index 1730 and the IR index 1030. FIG. [Diagram 2] FIG. 2 is an explanatory diagram of a method for calculating the average substitution degree of hydroxyl groups in cellulose. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Exemplary embodiments of the present invention will be described in detail below, but the present invention is not limited to these embodiments.
[0014] <<Method for producing redispersed cellulose nanofiber liquid, and dried cellulose nanofiber solid>> One aspect of the present disclosure provides a method for producing a redispersion of cellulose nanofibers, the method including a dispersion step of preparing a dispersion by dispersing cellulose nanofibers in a first dispersion medium, a drying step of drying the dispersion to obtain a dry solid of cellulose nanofibers, and a redispersion step of redispersing the dry solid of cellulose nanofibers in a second dispersion medium to prepare a redispersion. Another aspect of the present invention provides a dry solid cellulose nanofiber with excellent redispersibility. In one aspect, the dry solid cellulose nanofiber has an apparent density of 210 g / L to 1500 g / L.
[0015] The cellulose nanofiber refers to fine cellulose obtained by treating pulp or the like with hot water of 100°C or higher, hydrolyzing and weakening hemicellulose, and then defibrating the cellulose by a pulverizing method such as a high-pressure homogenizer, a microfluidizer, a ball mill, a disk mill, or a mixer (e.g., a homomixer). The cellulose nanofiber may be chemically modified as described below. Since cellulose nanofibers are extremely prone to aggregation in a dry state, it was thought that in a typical cellulose nanofiber dry solid, the cellulose nanofibers are tightly aggregated with each other, and that even if the dry solid is redispersed in a dispersion medium, it is not easily redispersed. The present inventor unexpectedly discovered that a cellulose nanofiber dry solid having a high apparent density within a specific range can be well redispersed in a dispersion medium. A cellulose nanofiber dry solid having good redispersibility in a dispersion medium can be well dispersed in a resin, for example, when the cellulose nanofiber is composited with a resin, and therefore has an excellent effect of improving the physical properties of a composite containing a cellulose nanofiber and a resin (also referred to as a resin composite in the present disclosure). In addition, the cellulose nanofiber dry solid of the present disclosure has a high apparent density, and therefore has the advantage of reducing storage space and transportation costs. In one embodiment, the apparent density of the cellulose nanofiber dry solid is 210 g / L or more, or 300 g / L or more, or 400 g / L or more, or 500 g / L or more, and 1500 g / L or less, or 1400 g / L or less, or 1300 g / L or less, or 1200 g / L or less. The apparent density in the present disclosure is determined by Archimedes' method, and is a value obtained using an electronic balance (e.g., GR-202 electronic balance manufactured by A&D) and a specific gravity meter (e.g., AD-1653 manufactured by A&D).
[0016] As the cellulose raw material, natural cellulose and regenerated cellulose can be used. As the natural cellulose, wood pulp obtained from wood species (broadleaf or coniferous), non-wood pulp obtained from non-wood species (cotton, bamboo, hemp, bagasse, kenaf, cotton linters, sisal, straw, etc.), and cellulose fiber aggregates produced by animals (e.g., ascidians), algae, and microorganisms (e.g., acetic acid bacteria) can be used. As the regenerated cellulose, regenerated cellulose fibers (viscose, cupra, tencel, etc.), cellulose derivative fibers, and ultrafine threads of regenerated cellulose or cellulose derivatives obtained by electrospinning can be used.
[0017] Since the cellulose raw material contains alkali-soluble and sulfuric acid-insoluble components (lignin, etc.), the alkali-soluble and sulfuric acid-insoluble components may be reduced through a purification process such as delignification by cooking and a bleaching process. On the other hand, the purification process such as delignification by cooking and the bleaching process cut the molecular chains of cellulose, changing the weight-average molecular weight and number-average molecular weight, so that the purification process and bleaching process of the cellulose raw material are desirably controlled so that the weight-average molecular weight of cellulose and the ratio of the weight-average molecular weight to the number-average molecular weight do not deviate from appropriate ranges.
[0018] In addition, since the refining process such as delignification by cooking and the bleaching process reduce the molecular weight of cellulose molecules, there is a concern that these processes will result in a lower molecular weight of cellulose and an increase in the proportion of alkali-soluble matter present due to the alteration of the cellulose raw material. Since alkali-soluble matter has poor heat resistance, it is desirable to control the refining process and bleaching process of the cellulose raw material so that the amount of alkali-soluble matter contained in the cellulose raw material is within a certain range or less.
[0019] The cellulose raw material is obtained by a dry grinding process. Any type of grinder can be used in the dry grinding, but a high-speed rotary impact grinder is preferable because it can obtain a cellulose raw material with a good shape. A high-speed rotary impact grinder is a grinder that uses a pin rotating in a grinding chamber or a rotor with a special structure to impact or shear the cellulose raw material and grind it. In order to suppress fiber damage during dry grinding, the cellulose raw material may contain moisture to a certain extent based on its weight.
[0020] Examples of mills of this type include the Jiyuu mill, New Cosmomizer (manufactured by Nara Machinery Works, Ltd.), Victory Mill, Far in Victory Mill (manufactured by Hosokawa Micron, Ltd.), Turbo Mill (manufactured by Turbo Kogyo, Ltd.), Ultra Rotor (manufactured by WIR, Ltd.), Makino type mill, Ultraplex (manufactured by Makino Sangyo, Ltd.), Fine Mill (manufactured by Nippon Pneumatic Industry Co., Ltd.), Impeller Mill (manufactured by Seishin Enterprise Co., Ltd.), and Disc Refiner (manufactured by Aikawa Iron Works, Ltd.).
[0021] There is no particular limitation on the method for reducing the fiber diameter in order to convert the cellulose raw material into cellulose nanofibers, but it is preferable to make the defibration processing conditions (method of applying a shear field, shear field size, etc.) more efficient. In addition, in order to suppress the decrease in crystallinity due to shear, wet defibration using a solvent is preferable. There is no particular limitation on the defibration solvent, but examples include water and aprotic solvents. Water is preferable because it is an inexpensive solvent and does not require explosion-proofing of the production equipment. When the cellulose raw material is immersed in an aprotic solvent, cellulose swells in a short time, and the cellulose is finely pulverized by only applying slight stirring and shear energy. In addition, by adding a cellulose modifying agent before, during, or after fineness, chemically modified cellulose nanofibers (also called chemically modified cellulose nanofibers) can be obtained directly without solvent replacement. Therefore, aprotic solvents are preferable from the viewpoint of production efficiency.
[0022] Examples of the aprotic solvent include alkyl sulfoxides, alkyl amides, pyrrolidones, etc. These solvents may be used alone or in combination of two or more kinds.
[0023] Examples of the alkyl sulfoxides include di-C1-4 alkyl sulfoxides such as dimethyl sulfoxide (DMSO), methyl ethyl sulfoxide, and diethyl sulfoxide.
[0024] Examples of the alkylamides include N,N-diC1-4 alkylformamides such as N,N-dimethylformamide (DMF) and N,N-diethylformamide; and N,N-diC1-4 alkylacetamides such as N,N-dimethylacetamide (DMAc) and N,N-diethylacetamide.
[0025] Examples of pyrrolidones include pyrrolidones such as 2-pyrrolidone and 3-pyrrolidone; and N-C1-4 alkylpyrrolidones such as N-methyl-2-pyrrolidone (NMP).
[0026] These aprotic solvents can be used alone or in combination. Among these aprotic solvents, DMSO, DMF, DMAc, NMP, etc., especially DMSO, can be used to more efficiently produce chemically modified cellulose nanofibers. Although the mechanism of this action is not entirely clear, it is presumed to be due to the homogeneous micro-swelling of the cellulose raw material in the aprotic solvent.
[0027] The cellulose raw material can be pulverized using a device that effectively applies shear to the cellulose raw material, such as a disintegrator, beater, refiner, low-pressure homogenizer, high-pressure homogenizer, ultra-high-pressure homogenizer, emulsifier, homomixer, grinder, mass colloider, cutter mill, ball mill, bead mill, jet mill, single-screw extruder, twin-screw extruder, ultrasonic agitator, household juicer mixer, etc. Among these, pulverization using a homomixer using an aprotic solvent is preferred because it can defibrate with low energy and enables chemical modification of cellulose nanofibers in a non-aqueous system.
[0028] In one aspect, the number average fiber diameter of the cellulose nanofibers is preferably 1 to 1000 nm from the viewpoint of obtaining a good effect of improving physical properties by the cellulose nanofibers. The number average fiber diameter of the cellulose nanofibers is more preferably 4 nm or more, or 5 nm or more, or 10 nm or more, or 15 nm or more, or 20 nm or more, and more preferably 500 nm or less, or 450 nm or less, or 400 nm or less, or 350 nm or less, or 300 nm or less, or 250 nm or less.
[0029] From the viewpoint of satisfactorily improving the mechanical properties of a resin composite containing cellulose nanofibers with a small amount of cellulose nanofibers, the average L / D of the cellulose nanofibers is preferably 50 or more, or 80 or more, or 100 or more, or 120 or more, or 150 or more. There is no particular upper limit, but from the viewpoint of handleability, it is preferably 5,000 or less.
[0030] In the present disclosure, the length, diameter, and L / D ratio of each cellulose nanofiber are determined by diluting an aqueous dispersion of cellulose nanofibers with a water-soluble solvent (e.g., water, ethanol, tert-butanol, etc.) to 0.01 to 0.1% by mass, dispersing the cellulose nanofibers using a high-shear homogenizer (e.g., IKA, product name "Ultra Turrax T18") under processing conditions: rotation speed 25,000 rpm x 5 minutes, casting the homogenized material on mica, and air-drying the material to obtain a measurement sample, and measuring the length (L) and diameter (D) of 100 randomly selected fibrous substances in an observation field where the magnification is adjusted so that at least 100 fibrous substances are observed, and calculating the ratio (L / D). The number average value of the length (L), the number average value of the diameter (D), and the number average value of the ratio (L / D) of the cellulose nanofibers are calculated.
[0031] The length, diameter, and L / D ratio of the cellulose nanofibers in the resin composite can be confirmed by measuring the solid resin composite as a measurement sample using the above-mentioned measurement method. Alternatively, the length, diameter, and L / D ratio of the cellulose nanofibers in the resin composite can be confirmed by dissolving the resin component in the resin composite in an organic or inorganic solvent that can dissolve the resin component of the resin composite, separating the cellulose nanofibers, thoroughly washing with the solvent, and then replacing with a water-soluble solvent (e.g., water, ethanol, tert-butanol, etc.), preparing a 0.01 to 0.1 mass% dispersion, and redispersing with a high-shear homogenizer (e.g., IKA, product name "Ultra Turrax T18"). The redispersion can be confirmed by casting the redispersion on mica, air-drying it, and measuring it as a measurement sample using the above-mentioned measurement method. At this time, the measurement is performed on 100 or more randomly selected cellulose nanofibers.
[0032] The crystallinity of the cellulose nanofiber is preferably 55% or more. When the crystallinity is in this range, the mechanical properties (strength, dimensional stability) of the cellulose fiber itself are high, and therefore when the cellulose fiber is dispersed in a resin, the strength and dimensional stability of the resin composite tend to be high. A more preferable lower limit of the crystallinity is 60%, even more preferably 70%, and most preferably 80%. There is no particular upper limit for the crystallinity of the cellulose nanofiber, and the higher the better, but from the viewpoint of production, a preferable upper limit is 99%.
[0033] Alkali-soluble polysaccharides such as hemicellulose and acid-insoluble components such as lignin are present between the microfibrils of plant-derived cellulose and between the microfibril bundles. Hemicellulose is a polysaccharide composed of sugars such as mannan and xylan, and plays a role in binding the microfibrils together by hydrogen bonding with cellulose. Lignin is also a compound having an aromatic ring, and is known to be covalently bonded to hemicellulose in the cell walls of plants. If there is a large amount of impurities such as lignin remaining in the cellulose nanofiber, discoloration may occur due to heat during processing. Therefore, from the viewpoint of suppressing discoloration of the resin composite during extrusion processing and molding processing, it is desirable to set the crystallinity of the cellulose nanofiber within the above-mentioned range.
[0034] The degree of crystallinity here, when the cellulose nanofiber is cellulose type I crystal (derived from natural cellulose), is calculated from the diffraction pattern (2θ / deg. is 10 to 30) obtained by measuring the sample by wide-angle X-ray diffraction, using the Segal method and the following formula. Crystallinity (%) = ([diffraction intensity due to the (200) plane at 2θ / deg. = 22.5] - [diffraction intensity due to amorphous matter at 2θ / deg. = 18]) / [diffraction intensity due to the (200) plane at 2θ / deg. = 22.5] × 100
[0035] Furthermore, when the cellulose nanofiber is a cellulose II type crystal (derived from regenerated cellulose), the degree of crystallinity can be calculated from the absolute peak intensity h0 at 2θ=12.6° assigned to the (110) plane peak of the cellulose II type crystal in wide-angle X-ray diffraction and the peak intensity h1 from the baseline at this interplanar spacing, according to the following formula: Crystallinity (%) =h1 / h0 ×100
[0036] Known crystalline forms of cellulose include type I, type II, type III, and type IV, of which types I and II are particularly widely used, and types III and IV have been obtained on a laboratory scale but are not widely used on an industrial scale. The cellulose nanofibers of the present disclosure are preferably cellulose fibers containing cellulose type I crystals or cellulose type II crystals, since they have relatively high structural mobility and, by dispersing the cellulose nanofibers in a resin, a resin composite having a lower linear expansion coefficient and superior strength and elongation during tensile and bending deformation can be obtained, and more preferably cellulose nanofibers containing cellulose type I crystals and having a crystallinity of 55% or more.
[0037] In addition, the degree of polymerization of the cellulose nanofiber is preferably 400 or more, more preferably 420 or more, more preferably 430 or more, more preferably 440 or more, more preferably 450 or more, and preferably 3500 or less, more preferably 3300 or less, more preferably 3200 or less, more preferably 3100 or less, and more preferably 3000 or less.
[0038] From the viewpoint of processability and mechanical property expression, it is desirable that the degree of polymerization of the cellulose nanofiber is within the above-mentioned range. From the viewpoint of processability, it is preferable that the degree of polymerization is not too high, and from the viewpoint of mechanical property expression, it is desirable that the degree of polymerization is not too low.
[0039] The degree of polymerization of cellulose nanofibers refers to the average degree of polymerization measured according to the reduced specific viscosity method using a copper ethylenediamine solution described in the Verification Test (3) of the "15th Revised Japanese Pharmacopoeia Commentary (published by Hirokawa Shoten)."
[0040] In one embodiment, the weight average molecular weight (Mw) of the cellulose nanofiber is 100,000 or more, more preferably 200,000 or more. The ratio (Mw / Mn) of the weight average molecular weight to the number average molecular weight (Mn) is 6 or less, preferably 5.4 or less. The larger the weight average molecular weight, the fewer the number of terminal groups of the cellulose molecule. In addition, since the ratio (Mw / Mn) of the weight average molecular weight to the number average molecular weight represents the width of the molecular weight distribution, the smaller the Mw / Mn, the fewer the number of terminals of the cellulose molecule. Since the terminals of the cellulose molecules are the starting points of thermal decomposition, when the cellulose molecules of the cellulose nanofibers not only have a large weight average molecular weight but also have a narrow molecular weight distribution, a particularly heat-resistant cellulose nanofiber and a resin composite containing the cellulose nanofiber and a resin can be obtained. The weight average molecular weight (Mw) of the cellulose nanofiber may be, for example, 600,000 or less, or 500,000 or less, from the viewpoint of the availability of the cellulose raw material. From the viewpoint of ease of production of cellulose nanofibers, the ratio (Mw / Mn) of the weight average molecular weight to the number average molecular weight (Mn) may be, for example, 1.5 or more, or 2 or more. Mw can be controlled to the above range by selecting a cellulose raw material having an Mw appropriate for the purpose, performing physical and / or chemical treatment on the cellulose raw material appropriately within a moderate range, and the like. Mw / Mn can also be controlled to the above range by selecting a cellulose raw material having an Mw / Mn appropriate for the purpose, performing physical and / or chemical treatment on the cellulose raw material appropriately within a moderate range, and the like. In both the control of Mw and the control of Mw / Mn, examples of the physical treatment include dry or wet grinding using a microfluidizer, ball mill, disk mill, etc., physical treatment that applies mechanical forces such as impact, shear, shear, friction, etc. using a crusher, homomixer, high-pressure homogenizer, ultrasonic device, etc., and examples of the chemical treatment include digestion, bleaching, acid treatment, regenerated cellulose, etc.
[0041] The weight average molecular weight and number average molecular weight of cellulose referred to here are values determined by dissolving cellulose in N,N-dimethylacetamide containing added lithium chloride and then subjecting the cellulose to gel permeation chromatography using N,N-dimethylacetamide as a solvent.
[0042] Methods for controlling the degree of polymerization (i.e., average degree of polymerization) or molecular weight of cellulose nanofibers include hydrolysis. Hydrolysis promotes depolymerization of amorphous cellulose inside the cellulose nanofibers, decreasing the average degree of polymerization. At the same time, hydrolysis removes impurities such as hemicellulose and lignin in addition to the above-mentioned amorphous cellulose, making the inside of the fiber more porous.
[0043] The hydrolysis method is not particularly limited, and examples thereof include acid hydrolysis, alkali hydrolysis, hydrothermal decomposition, steam explosion, and microwave decomposition. These methods may be used alone or in combination of two or more. In the acid hydrolysis method, for example, α-cellulose obtained as pulp from a fibrous plant is used as a cellulose raw material, and this is dispersed in an aqueous medium, and an appropriate amount of a protonic acid, a carboxylic acid, a Lewis acid, a heteropoly acid, etc. is added, and the mixture is heated while stirring, so that the average degree of polymerization can be easily controlled. The reaction conditions at this time, such as temperature, pressure, and time, vary depending on the cellulose type, cellulose concentration, acid type, acid concentration, etc., and are appropriately adjusted so that the desired average degree of polymerization is achieved. For example, a condition in which cellulose is treated for 10 minutes or more at 100°C or higher under pressure using an aqueous mineral acid solution of 2% by mass or less can be exemplified. Under these conditions, the catalyst component such as acid penetrates into the inside of the cellulose nanofiber, promoting hydrolysis, reducing the amount of catalyst component used, and making subsequent purification easier. The dispersion of the cellulose raw material during hydrolysis may contain, in addition to water, a small amount of an organic solvent within a range that does not impair the effects of the present invention.
[0044] Alkali-soluble polysaccharides that may be contained in cellulose nanofibers include hemicellulose, β-cellulose, and γ-cellulose. Alkali-soluble polysaccharides are understood by those skilled in the art as components obtained as the alkali-soluble portion of holocellulose obtained by solvent extraction and chlorine treatment of plants (e.g., wood) (i.e., components obtained by removing α-cellulose from holocellulose). Alkali-soluble polysaccharides are polysaccharides containing hydroxyl groups and have poor heat resistance, and may cause inconveniences such as decomposition when exposed to heat, yellowing during heat aging, and a decrease in strength of cellulose fibers. Therefore, it is preferable that the content of alkali-soluble polysaccharides in cellulose nanofibers is low.
[0045] In one aspect, the average content of alkali-soluble polysaccharides in the cellulose nanofibers is preferably 20% by mass or less, 18% by mass or less, or 15% by mass or less, relative to 100% by mass of the cellulose nanofibers, from the viewpoint of obtaining good dispersibility of the cellulose nanofibers. From the viewpoint of ease of production of the cellulose nanofibers, the above content may be 1% by mass or more, 2% by mass or more, or 3% by mass or more.
[0046] The average alkali-soluble polysaccharide content can be determined by the method described in the non-patent literature (Wood Science Experiment Manual, edited by the Japan Wood Research Society, pages 92-97, 2000), by subtracting the α-cellulose content from the holocellulose content (Wise method). This method is understood in the industry as a method for measuring the amount of hemicellulose. The alkali-soluble polysaccharide content is calculated three times for each sample, and the number average of the calculated alkali-soluble polysaccharide contents is taken as the average alkali-soluble polysaccharide content.
[0047] In one aspect, the average content of acid-insoluble components in the cellulose nanofibers is preferably 10% by mass or less, 5% by mass or less, or 3% by mass or less, relative to 100% by mass of the cellulose nanofibers, from the viewpoint of avoiding a decrease in heat resistance of the cellulose nanofibers and the associated discoloration. From the viewpoint of ease of production of the cellulose nanofibers, the above content may be 0.1% by mass or more, 0.2% by mass or more, or 0.3% by mass or more.
[0048] The average acid-insoluble content is determined as a quantitative determination of the acid-insoluble content using the Clason method described in the non-patent literature (Wood Science Experiment Manual, edited by the Japan Wood Research Society, pages 92-97, 2000). This method is understood in the industry as a method for measuring the amount of lignin. The sample is stirred in a sulfuric acid solution to dissolve cellulose, hemicellulose, etc., and then filtered through a glass fiber filter paper, and the resulting residue corresponds to the acid-insoluble content. The acid-insoluble content is calculated from the weight of the acid-insoluble content, and the number average of the acid-insoluble content calculated for the three samples is taken as the average acid-insoluble content.
[0049] The cellulose nanofibers may be chemically treated (e.g., oxidized or chemically modified using a modifying agent). As an example, fine cellulose fibers obtained by oxidizing cellulose fibers with 2,2,6,6-tetramethylpiperidine-1-oxyl radical as shown in Cellulose (1998) 5, 153-164, followed by washing and mechanical fiberization, may be used.
[0050] The cellulose modification agent can be a compound that reacts with the hydroxyl group of cellulose, and includes an esterification agent, an etherification agent, and a silylating agent. In a preferred embodiment, the chemical modification is acylation using an esterification agent. The esterification agent is preferably an acid halide, an acid anhydride, a vinyl carboxylate, or a carboxylic acid.
[0051] The acid halide may be at least one selected from the group consisting of compounds represented by the following formula (1). R1 -C(=O)-X (1) (In the formula, R 1 represents an alkyl group having 1 to 24 carbon atoms, an alkenyl group having 2 to 24 carbon atoms, a cycloalkyl group having 3 to 24 carbon atoms, or an aryl group having 6 to 24 carbon atoms, and X is Cl, Br, or I. Specific examples of acid halides include, but are not limited to, acetyl chloride, acetyl bromide, acetyl iodide, propionyl chloride, propionyl bromide, propionyl iodide, butyryl chloride, butyryl bromide, butyryl iodide, benzoyl chloride, benzoyl bromide, and benzoyl iodide. Among them, acid chlorides can be preferably used in terms of reactivity and handling. In addition, in the reaction of acid halides, one or more alkaline compounds may be added to act as a catalyst and neutralize the by-product acidic substances. Specific examples of alkaline compounds include, but are not limited to, tertiary amine compounds such as triethylamine and trimethylamine; and nitrogen-containing aromatic compounds such as pyridine and dimethylaminopyridine.
[0052] As the acid anhydride, any suitable acid anhydride can be used. For example, Saturated aliphatic monocarboxylic acid anhydrides, such as acetic acid, propionic acid, (iso)butyric acid, and valeric acid; unsaturated aliphatic monocarboxylic acid anhydrides, such as (meth)acrylic acid and oleic acid; Alicyclic monocarboxylic acid anhydrides such as cyclohexanecarboxylic acid and tetrahydrobenzoic acid; Aromatic monocarboxylic acid anhydrides such as benzoic acid and 4-methylbenzoic acid; Examples of dibasic carboxylic acid anhydrides include saturated aliphatic dicarboxylic acid anhydrides such as succinic anhydride and adipic acid, unsaturated aliphatic dicarboxylic acid anhydrides such as maleic anhydride and itaconic anhydride, alicyclic dicarboxylic acid anhydrides such as 1-cyclohexene-1,2-dicarboxylic acid anhydride, hexahydrophthalic anhydride and methyltetrahydrophthalic anhydride, and aromatic dicarboxylic acid anhydrides such as phthalic anhydride and naphthalic anhydride; Examples of polybasic carboxylic acid anhydrides having three or more bases include polycarboxylic acids (anhydrides) such as trimellitic anhydride and pyromellitic anhydride. In addition, in the reaction of an acid anhydride, one or more types of acidic compounds such as sulfuric acid, hydrochloric acid, phosphoric acid, etc., or Lewis acids (for example, Lewis acid compounds represented by MYn, where M represents a semimetal element such as B, As, Ge, etc., or a base metal element such as Al, Bi, In, etc., or a transition metal element such as Ti, Zn, Cu, etc., or a lanthanoid element, n is an integer corresponding to the atomic valence of M and represents 2 or 3, and Y represents a halogen atom, OAc, OCOCF3, ClO4, SbF6, PF6, or OSO2CF3(OTf)), or alkaline compounds such as triethylamine, pyridine, etc. may be added as a catalyst.
[0053] The vinyl carboxylate may be represented by the following formula (1): R-COO-CH=CH2…Formula (1) Preferred is a vinyl carboxylate represented by the formula: {wherein R is any one of an alkyl group having 1 to 24 carbon atoms, an alkenyl group having 2 to 24 carbon atoms, a cycloalkyl group having 3 to 16 carbon atoms, and an aryl group having 6 to 24 carbon atoms.} The vinyl carboxylate is more preferably at least one selected from the group consisting of vinyl acetate, vinyl propionate, vinyl butyrate, vinyl caproate, vinyl cyclohexanecarboxylate, vinyl caprylate, vinyl caprate, vinyl laurate, vinyl myristate, vinyl palmitate, vinyl stearate, vinyl pivalate, vinyl octylate, divinyl adipate, vinyl methacrylate, vinyl crotonate, vinyl pivalate, vinyl octylate, vinyl benzoate, and vinyl cinnamate. In the esterification reaction with a vinyl carboxylate, one or more catalysts selected from the group consisting of alkali metal hydroxides, alkaline earth metal hydroxides, alkali metal carbonates, alkaline earth metal carbonates, alkali metal hydrogencarbonates, primary to tertiary amines, quaternary ammonium salts, imidazole and derivatives thereof, pyridine and derivatives thereof, and alkoxides may be added.
[0054] Examples of the alkali metal hydroxides and alkaline earth metal hydroxides include sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide, barium hydroxide, etc. Examples of the alkali metal carbonates, alkaline earth metal carbonates, and alkali metal hydrogen carbonates include lithium carbonate, sodium carbonate, potassium carbonate, cesium carbonate, magnesium carbonate, calcium carbonate, barium carbonate, lithium hydrogen carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, cesium hydrogen carbonate, etc.
[0055] The primary, secondary and tertiary amines refer to primary, secondary and tertiary amines, and specific examples thereof include ethylenediamine, diethylamine, proline, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethyl-1,3-propanediamine, N,N,N',N'-tetramethyl-1,6-hexanediamine, tris(3-dimethylaminopropyl)amine, N,N-dimethylcyclohexylamine and triethylamine.
[0056] Examples of imidazole and its derivatives include 1-methylimidazole, 3-aminopropylimidazole, and carbonyldiimidazole.
[0057] Examples of pyridine and its derivatives include N,N-dimethyl-4-aminopyridine and picoline.
[0058] Examples of the alkoxide include sodium methoxide, sodium ethoxide, and potassium t-butoxide.
[0059] The carboxylic acid may be at least one selected from the group consisting of compounds represented by the following formula (1). R-COOH …(1) (In the formula, R represents an alkyl group having 1 to 16 carbon atoms, an alkenyl group having 2 to 16 carbon atoms, a cycloalkyl group having 3 to 16 carbon atoms, or an aryl group having 6 to 16 carbon atoms.)
[0060] Specific examples of carboxylic acids include at least one selected from the group consisting of acetic acid, propionic acid, butyric acid, caproic acid, cyclohexane carboxylic acid, caprylic acid, capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, pivalic acid, methacrylic acid, crotonic acid, pivalic acid, octylic acid, benzoic acid, and cinnamic acid.
[0061] Among these carboxylic acids, at least one selected from the group consisting of acetic acid, propionic acid, and butyric acid, and particularly acetic acid, is preferred from the viewpoint of reaction efficiency. In addition, in the reaction of carboxylic acid, one or more types of acidic compounds such as sulfuric acid, hydrochloric acid, phosphoric acid, etc., or Lewis acids (for example, Lewis acid compounds represented by MYn, where M represents a semimetal element such as B, As, Ge, etc., or a base metal element such as Al, Bi, In, etc., or a transition metal element such as Ti, Zn, Cu, etc., or a lanthanoid element, n is an integer corresponding to the atomic valence of M and represents 2 or 3, and Y represents a halogen atom, OAc, OCOCF3, ClO4, SbF6, PF6, or OSO2CF3(OTf)), or alkaline compounds such as triethylamine, pyridine, etc. may be added as a catalyst.
[0062] Among these esterification reactants, at least one selected from the group consisting of acetic anhydride, propionic anhydride, butyric anhydride, vinyl acetate, vinyl propionate, vinyl butyrate, and acetic acid, and among these, acetic anhydride and vinyl acetate are preferred from the viewpoint of reaction efficiency.
[0063] When cellulose nanofibers are hydrophobized (for example, by chemical modification such as acylation), the redispersibility of the dry solid tends to be good, but the cellulose nanofiber dry solid of the present disclosure is advantageous in that it can exhibit good redispersibility even when it is unsubstituted or has a low degree of substitution. Thus, in one embodiment, the average degree of substitution (DS) of the cellulose nanofiber dry solid (average number of substituted hydroxyl groups per glucose, which is the basic building block of cellulose) can be 0.5 or less, or 0.3 or less, or 0.1 or less, or 0. In one embodiment, the average degree of substitution (DS) can be 0 or more, or 0.1 or more, or 0.2 or more, depending on the intended use of the cellulose nanofiber.
[0064] When the modification group of the chemically modified cellulose nanofiber is an acyl group, the degree of acyl substitution (DS) can be calculated from the reflection infrared absorption spectrum of the esterified cellulose nanofiber based on the peak intensity ratio between the peak derived from the acyl group and the peak derived from the cellulose skeleton. The peak of the absorption band of C=O based on the acyl group is at 1730 cm -1 The absorption band of CO based on the cellulose backbone appears at 1030 cm -1 The DS of the esterified cellulose nanofibers was calculated by plotting a correlation graph between the DS obtained from the solid-state NMR measurement of the esterified cellulose nanofibers described below and the modification ratio (IR index 1030), which is defined as the ratio of the peak intensity of the absorption band of C=O based on the acyl group to the peak intensity of the absorption band of CO in the cellulose backbone chain, and then calculating the calibration curve from the correlation graph. Degree of substitution DS = 4.13 × IR index (1030) It can be found by using
[0065] The method for calculating the DS of esterified cellulose nanofibers using solid-state NMR is as follows: 13C solid-state NMR measurement was performed, and the intensity can be calculated using the area intensity (Inf) of a signal assigned to one carbon atom derived from the modifying group relative to the total area intensity (Inp) of signals assigned to carbons C1-C6 derived from the pyranose ring of cellulose, which appear in the range from 50 ppm to 110 ppm, using the following formula. DS = (Inf) x 6 / (Inp) For example, when the modifying group is an acetyl group, the signal at 23 ppm assigned to -CH3 may be used. Use 13 The conditions for the C solid-state NMR measurement are, for example, as follows: Equipment:Bruker Biospin Avance500WB Frequency: 125.77MHz Measurement method: DD / MAS method Waiting time: 75sec NMR sample tube: 4mmφ Accumulation times: 640 times (approx. 14 hours) MAS: 14,500Hz Chemical shift standard: glycine (external standard: 176.03 ppm)
[0066] The DS heterogeneity ratio (DSs / DSt), defined as the ratio of the degree of modification (DSs) of the fiber surface to the degree of modification (DSt) of the entire fiber of the chemically modified cellulose nanofiber (which is synonymous with the above-mentioned degree of acyl substitution (DS)), is preferably 1.05 or more. The larger the value of the DS heterogeneity ratio, the more pronounced the sheath-core-like heterogeneous structure (i.e., a structure in which the fiber surface is highly chemically modified while the fiber center retains a cellulose structure close to the original unmodified structure), and while maintaining high tensile strength and dimensional stability derived from cellulose, it is possible to improve the affinity with the resin when composited with the resin and to improve the dimensional stability of the resin composition. The DS heterogeneity ratio is more preferably 1.1 or more, or 1.2 or more, or 1.3 or more, or 1.5 or more, or 2.0 or more, and from the viewpoint of ease of production of the chemically modified cellulose nanofiber, it is preferably 30 or less, or 20 or less, or 10 or less, or 6 or less, or 4 or less, or 3 or less. The value of DSs varies depending on the degree of modification of the esterified cellulose, but for example, it is preferably 0.1 or more, or 0.2 or more, or 0.3 or more, or 0.5 or more, and preferably 3.0 or less, or 2.5 or less, or 2.0 or less, or 1.5 or less, or 1.2 or less, or 1.0 or less. The preferred range of DSt is as described above for the acyl substituent (DS).
[0067] The smaller the coefficient of variation (CV) of the DS heterogeneity ratio of the chemically modified cellulose nanofiber, the smaller the variation in various physical properties of the resin composition, and therefore the more preferable. The coefficient of variation is preferably 50% or less, or 40% or less, or 30% or less, or 20% or less. The coefficient of variation can be further reduced, for example, by a method in which a cellulose raw material is defibrated and then chemically modified to obtain chemically modified cellulose nanofibers (i.e., a sequential method), whereas it can be increased by a method in which defibration and chemical modification of the cellulose raw material are performed simultaneously (i.e., a simultaneous method). Although the mechanism of this action is not clear, in the simultaneous method, chemical modification is more likely to proceed in the thin fibers generated in the early stage of defibration, and when hydrogen bonds between cellulose microfibrils are reduced by chemical modification, defibration proceeds further, which is thought to result in an increase in the coefficient of variation of the DS heterogeneity ratio.
[0068] The coefficient of variation (CV) of the DS heterogeneity ratio is calculated by taking 100 g of an aqueous dispersion of chemically modified cellulose nanofiber (solid content of 10 mass% or more) and freeze-pulverizing 10 g portions to use as measurement samples. The DS heterogeneity ratio is calculated from the DSt and DSs of the 10 samples, and then the standard deviation (σ) and arithmetic mean (μ) of the DS heterogeneity ratio among the obtained 10 samples are used to calculate the coefficient of variation (CV) of the DS heterogeneity ratio using the following formula. DS heterogeneity ratio = DSs / DSt Coefficient of variation (%) = standard deviation σ / arithmetic mean μ × 100
[0069] The DSs is calculated as follows. That is, the esterified cellulose powdered by freeze-pulverization is placed on a dish-shaped sample stage with a diameter of 2.5 mm, the surface is pressed down to make it flat, and then measurement is performed by X-ray photoelectron spectroscopy (XPS). The XPS spectrum reflects the constituent elements and chemical bond state of only the surface layer of the sample (typically about a few nm). Peak separation is performed on the obtained C1s spectrum, and DSs can be calculated by the following formula based on the area intensity (Ixf) of the peak assigned to one carbon atom derived from the modifying group relative to the area intensity (Ixp) of the peak (289 eV, CC bond) assigned to carbons C2-C6 derived from the pyranose ring of cellulose. DSs = (Ixf) x 5 / (Ixp) For example, if the modifying group is an acetyl group, after peak separation of the C1s spectrum at 285 eV, 286 eV, 288 eV, and 289 eV, the peak at 289 eV can be used for Ixp and the peak derived from the O-C=O bond of the acetyl group (286 eV) can be used for Ixf. The conditions for the XPS measurement are as follows, for example: Equipment used: ULVAC-Phi VersaProbe II Excitation source: mono.AlKα 15kV×3.33mA Analysis size: Approx. 200 μm φ Photoelectron extraction angle: 45° Capture Area Narrow scan: C 1s, O 1s Pass Energy: 23.5eV
[0070] The cellulose nanofiber dry solid of the present disclosure can have good redispersibility even in the absence of a dispersant. Thus, in one embodiment, the cellulose nanofiber dry solid is substantially composed of cellulose only (i.e., does not contain a dispersant). A cellulose nanofiber dry solid not containing a dispersant is advantageous in that it can avoid, for example, problems (such as a decrease in physical properties) caused by the dispersant in a resin complex. In one embodiment, the dry solid may contain a small amount of dispersant (e.g., less than 1% by mass, or 0.5% by mass or less, or 0.3% by mass or less, based on 100% by mass of the total dry solid). Examples of dispersants that the cellulose nanofiber dry solid may contain include compounds having hydrophilic groups (e.g., hydroxyl groups, amino groups, etc.). In one embodiment, the dispersant is a liquid at 23°C. In one embodiment, the dispersant is a monomer having a hydrophilic group (e.g., propylene glycol, N-vinylacetamide, etc.), and in one embodiment, a surfactant (i.e., a compound having a chemical structure in which a portion having a hydrophilic substituent and a portion having a hydrophobic substituent are covalently bonded).
[0071] As the surfactant, any of anionic surfactants, nonionic surfactants, amphoteric surfactants, and cationic surfactants can be used, but nonionic surfactants are preferred in terms of obtaining good dispersibility of the cellulose nanofibers.
[0072] As the hydrophilic group of the surfactant, from the viewpoint of affinity with cellulose nanofibers, polyoxyethylene chains, carboxyl groups, and hydroxyl groups are preferred, and polyoxyethylene chains are particularly preferred. Nonionic polyoxyethylene derivatives are particularly preferred. The polyoxyethylene chain length of the polyoxyethylene derivative may be 1 or more, or 4 or more, or 10 or more, or 15 or more. The longer the chain length, the higher the affinity for hydrophobic cellulose nanofibers, but from the viewpoint of balance with the properties of the resin composite (e.g., mechanical properties, etc.), the polyoxyethylene chain length may be 60 or less, or 50 or less, or 40 or less, or 30 or less, or 20 or less.
[0073] As the structure of the hydrophobic group of the surfactant, alkyl ether type, alkyl phenyl ether type, rosin ester type, bisphenol A type, β-naphthyl type, styrenated phenyl type, and hardened castor oil type are preferred in terms of high affinity with resin. The number of carbon atoms of the alkyl chain of the hydrophobic group (in the case of alkyl phenyl, the number of carbon atoms excluding the phenyl group) is preferably 5 or more, or 10 or more, or 12 or more, or 16 or more. For example, when the resin is a polyolefin resin, the more carbon atoms of the surfactant, the higher the affinity with the resin. The number of carbon atoms may be, for example, 30 or less, or 25 or less.
[0074] Preferred examples of each step of the method for producing a redispersion of cellulose nanofibers are described below.
[0075] <Dispersion process> In this step, a dispersion liquid is prepared by dispersing cellulose nanofibers in a first dispersion medium. As the first dispersion medium, a liquid medium such as water or an organic solvent can be used alone or in combination of two or more. As the organic solvent, a commonly used water-miscible organic solvent, for example, polyol (e.g., polyether polyol such as polypropylene glycol and polyethylene glycol), ethanol, methanol, dimethylformamide, dimethyl sulfoxide, N-methylpyrrolidone, dimethylacetamide, acetonitrile, acetone, acetic acid, t-butanol, etc. can be used. The dispersion step may be a fiberization step of the cellulose raw material in the cellulose nanofiber production process. The first dispersion medium may contain an additive (dispersant, etc.) in addition to the liquid medium, but in one embodiment does not contain an additive.
[0076] The concentration of cellulose nanofibers in the dispersion is preferably 0.5% by mass or more, or 1% by mass or more, or 1.5% by mass or more from the viewpoint of process efficiency in subsequent drying steps, etc., and is preferably 10% by mass or less, or 8% by mass or less, or 5% by mass or less from the viewpoint of avoiding an excessive increase in the viscosity of the dispersion and maintaining good handleability.
[0077] <Drying process> In this step, the dispersion obtained in the dispersion step is dried to obtain a dry solid of cellulose nanofibers. An example of a drying method is drying under reduced pressure in a stirrer, and drying can be performed, for example, at a temperature of 50 to 150°C for 60 to 180 minutes under normal pressure or reduced pressure conditions. Heat press drying or spray drying may also be used. In one aspect, a dry solid of cellulose nanofibers having the properties (particularly the apparent density) described above in the section "Dry Solid of Cellulose Nanofibers" can be obtained in this step.
[0078] <Redispersion process> In this step, the cellulose nanofiber dry solid obtained in the drying step is redispersed in a second dispersion medium to obtain a redispersion liquid. The second dispersion medium may be the same or different from the first dispersion medium, and liquid media such as water and organic solvents can be used alone or in combination of two or more. In a preferred embodiment, the second dispersion medium is an aprotic polar solvent. As the aprotic polar solvent, one or more selected from the group consisting of dimethyl sulfoxide (DMSO), N-methylpyrrolidone (NMP), dimethylacetamide (DMAc), and dimethylformamide (DMF) are preferred. The second dispersion medium may contain additives (dispersants, organic binders, etc.) in addition to the liquid medium, but in one embodiment does not contain additives. Redispersion can be performed by applying a shear force by stirring (for example, a shear force by one or more selected from the group consisting of ultrasonic waves, a bead mill, a ball mill, and a homomixer). During and / or after the redispersion step, the cellulose nanofibers may be chemically modified using the above-mentioned modifying agent.
[0079] In one embodiment, the shear rate of an aqueous dispersion of the redispersion (also referred to as a simulated redispersion in the present disclosure) obtained by adjusting the cellulose nanofibers in the redispersion to an aqueous dispersion with a solid content of 0.5% by mass was 100 s. -1 The viscosity at 100 s was measured using a shear rate of 100 s for an aqueous dispersion of the cellulose nanofibers from the above dispersion adjusted to a solid content of 0.5% by mass (also referred to as a simulated dispersion in the present disclosure). -1The viscosity is 30% or more of the viscosity at the time of redispersion. The viscosity is a value measured by a hysteresis loop measurement method using a double cylinder type rheometer. The ratio is an index showing the extent to which the dispersibility of the cellulose nanofiber before drying can be reproduced after redispersion (i.e., redispersibility). The ratio is preferably 40% or more, 50% or more, or 60% or more. The higher the ratio, the more preferable it is, and most preferably 100%, but from the viewpoint of ease of production of the cellulose nanofiber, it may be, for example, 90% or less, or 80% or less. The simulated redispersion liquid is an aqueous dispersion with a solid content of 0.5% by mass obtained by repeating five cycles of adding 5 times the mass of water to the redispersion liquid, stirring, centrifuging, and discarding the supernatant, and then adding water. The simulated dispersion liquid is also an aqueous dispersion with a solid content of 0.5% by mass obtained by repeating five cycles of adding 5 times the mass of water to the dispersion liquid, stirring, centrifuging, and discarding the supernatant, and then adding water.
[0080] Shear rate of simulated dispersion: 100 seconds -1 From the viewpoint of obtaining a dispersion in which the cellulose nanofibers are highly dispersed, the viscosity in an aqueous dispersion having a cellulose solids content of 0.5 mass% may be preferably 10 mPa·s or more, or 13 mPa·s or more, or 15 mPa·s or more, and from the viewpoint of handleability of the dispersion, the viscosity may be preferably 150 mPa·s or less, or 140 mPa·s or less, or 130 mPa·s or less.
[0081] Shear rate of simulated redispersion liquid: 100 seconds -1 From the viewpoint of obtaining a re-dispersion in which the cellulose nanofibers are highly dispersed, the viscosity at may be preferably 6 mPa·s or more, or 7.5 mPa·s or more, or 9 mPa·s or more, and from the viewpoint of handleability of the re-dispersion, the viscosity at may be preferably 150 mPa·s or less, or 140 mPa·s or less, or 130 mPa·s or less.
[0082] The concentration of cellulose nanofibers in the redispersion is preferably 1 mass% or more, or 3 mass% or more, or 5 mass% or more from the viewpoint of process efficiency when using the redispersion in a cellulose nanofiber composite or resin composite, and of satisfactorily combining the cellulose nanofibers with other components, and is preferably 10 mass% or less, or 8 mass% or less, or 5 mass% or less from the viewpoint of handleability of the redispersion.
[0083] <Cellulose nanofiber composite> The redispersion of cellulose nanofibers described above may be further combined with other materials in the state of the redispersion or in the state of its dried form. In one embodiment, a cellulose nanofiber composite can be produced by a method including a step of preparing a redispersion of cellulose nanofibers by the method of the present disclosure, and a mixing step of mixing the redispersion or its dried form with an organic binder. The dried form of the redispersion can be formed by a method of drying the redispersion under reduced pressure while stirring, or the like.
[0084] The organic binder includes polymers having hydrophilic groups (e.g., hydroxyl groups, amino groups, etc.) (e.g., polyacrylamides, polyalkylene oxides, polyacrylic acids and salts thereof, polysaccharides (e.g., cellulose derivatives, starches, alginic acids and salts thereof (e.g., sodium alginate), guar gum, gellan gum, gelatin, etc.), polyvinyl alcohol, etc.). In one embodiment, the organic binder is a solid at 23°C.
[0085] Examples of the alkylene oxide unit of the polyalkylene oxide include alkylene oxides having 2 to 4 carbon atoms, preferably ethylene oxide and propylene oxide. In a preferred embodiment, the polyalkylene oxide is composed of ethylene oxide units and / or propylene oxide units. A particularly preferred polyalkylene oxide is polyethylene oxide.
[0086] Examples of cellulose derivatives include cellulose ethers (for example, methyl cellulose, carboxymethyl cellulose, carboxyethyl cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxypropylmethyl cellulose, etc.).
[0087] The weight average molecular weight of the organic binder is preferably 1000 or more, more preferably 5000 or more, and even more preferably 10000 or more, and is preferably 5×10 8 Less than or equal to 10, more preferably 8 Less than 5×10, more preferably 7 The following is the result.
[0088] The amount of organic binder may be, relative to 100 parts by mass of cellulose nanofiber, preferably 1 part by mass or more, or 10 parts by mass or more, or 20 parts by mass or more, and may be preferably 50 parts by mass or less, or 40 parts by mass or less, or 30 parts by mass or less.
[0089] <Resin composite> According to one aspect of the present invention, a resin composite (resin composition) can be produced by a method including a step of preparing a redispersion of cellulose nanofibers by the method disclosed herein, and a mixing step of mixing the redispersion or a dried form thereof with a resin. The dried form of the redispersion can be formed by a method of drying the redispersion under reduced pressure while stirring, for example. Since the aforementioned organic binder has the effect of improving the affinity between cellulose nanofibers and resin, in one aspect, it is preferable to combine the redispersion of cellulose nanofibers or a dried form thereof with the organic binder and then further combine it with a resin.
[0090] In one embodiment, the cellulose nanofiber dry solid obtained by drying the cellulose nanofiber dispersion may be a cellulose nanofiber solid. The cellulose nanofiber solid means a solid in which cellulose nanofibers are firmly bonded to each other. In a typical embodiment, the cellulose nanofiber solid can have a size (in one embodiment, the smallest dimension in the solid) of 1 mm or more, and is distinguished from powders, fibrous materials, and the like. In one embodiment, in the cellulose nanofiber solid, the cellulose nanofibers are bonded to each other by hydrogen bonds of hydroxyl groups. On the other hand, the cellulose nanofiber solid also has the property of being able to be well redispersed by a second dispersion medium to form a redispersion, and thus the redispersion or its dried body can be kneaded with a resin to form a resin composition. It is particularly preferable that the second dispersion medium applied to the cellulose nanofiber solid is selected from the group consisting of dimethyl sulfoxide (DMSO), dimethyl sulfoxide (DMSO), N-methylpyrrolidone (NMP), dimethylacetamide (DMAc), and dimethylformamide (DMF). In a preferred embodiment, the amount of water in the second dispersion medium is 10% by mass or less, or 5% by mass or less, or 0% by mass.
[0091] In one embodiment, the rate of change (YX) / Y of the mass (X) of the dry solid content when the cellulose nanofiber solid is left to stand in water at 20°C for 2 hours and then removed from the water relative to the mass (Y) of the cellulose nanofiber solid before standing is preferably 30% by mass or less, or 20% by mass or less, or 10% by mass (i.e., little disintegration in water). The rate of change may be 0% by mass, but in one embodiment, it may be 0.01% by mass or more. The mass (X) is the mass of the dry solid content obtained by removing the solid from the water and then drying it under vacuum at 120°C for 2 hours.
[0092] In one embodiment, the rate of change (ZY) / Y of the mass (Z) of the cellulose nanofiber solid when it is left to stand in water at 20°C for 2 hours and then removed from the water relative to the mass (Y) of the cellulose nanofiber solid before standing is 10% by mass or less (i.e., it absorbs almost no water). The rate of change may be 0% by mass, but in one embodiment, it may be 0.01% by mass or more. The mass (Z) is a value measured within 5 minutes after removing the solid from the water (thus avoiding the effects of drying) after wiping off the surface moisture with filter paper.
[0093] <Resin> The resin may be a thermoplastic resin, a thermosetting resin, or a photocurable resin. The resin may be an elastomer. From the viewpoints of moldability and productivity, a thermoplastic resin is more preferable.
[0094] (thermoplastic resin) When the resin is a thermoplastic resin, the melting point of the thermoplastic resin may be appropriately selected depending on the application of the resin composite, etc. The melting point of the thermoplastic resin can be, for example, 150°C to 190°C or 160°C to 180°C for a resin with a relatively low melting point (e.g., polyolefin resin), and 220°C to 350°C or 230°C to 320°C for a resin with a relatively high melting point (e.g., polyamide resin).
[0095] The thermoplastic resin may preferably be at least one selected from the group consisting of polyolefin-based resins, polyacetate-based resins, polycarbonate-based resins, polyamide-based resins, polyester-based resins, polyphenylene ether-based resins, and acrylic-based resins.
[0096] The polyolefin resin preferred as the thermoplastic resin is a polymer obtained by polymerizing olefins (e.g., α-olefins) and / or alkenes as monomer units.Specific examples of the polyolefin resin include ethylene (co)polymers such as low-density polyethylene (e.g., linear low-density polyethylene), high-density polyethylene, ultra-low-density polyethylene, and ultra-high-molecular-weight polyethylene, polypropylene (co)polymers such as polypropylene, ethylene-propylene copolymer, and ethylene-propylene-diene copolymer, and copolymers of ethylene and α-olefins such as ethylene-acrylic acid copolymer, ethylene-methyl methacrylate copolymer, and ethylene-glycidyl methacrylate copolymer.
[0097] Here, the most preferred polyolefin resin is polypropylene. In particular, polypropylene having a melt mass flow rate (MFR) of 3 g / 10 min or more and 30 g / 10 min or less, measured at 230° C. and a load of 21.2 N according to ISO1133, is preferred. The lower limit of MFR is more preferably 5 g / 10 min, even more preferably 6 g / 10 min, and most preferably 8 g / 10 min. The upper limit is more preferably 25 g / 10 min, even more preferably 20 g / 10 min, and most preferably 18 g / 10 min. From the viewpoint of improving the toughness of the resin composite, it is desirable that the MFR does not exceed the above upper limit, and from the viewpoint of the fluidity of the resin composite, it is desirable that the MFR does not exceed the above lower limit.
[0098] In addition, in order to increase the affinity with cellulose nanofibers, an acid-modified polyolefin resin can also be suitably used. As the acid used for the acid modification, a mono- or polycarboxylic acid can be used, and examples thereof include maleic acid, fumaric acid, succinic acid, phthalic acid and their anhydrides, and citric acid. Maleic acid or its anhydride is particularly preferred because it is easy to increase the modification rate. There is no particular restriction on the modification method, but a method in which a polyolefin resin is heated to a melting point or higher in the presence or absence of a peroxide and melt-kneaded is common. As the polyolefin resin to be acid-modified, all of the above-mentioned polyolefin resins can be used, but polypropylene is particularly suitable. The acid-modified polypropylene resin may be used alone, but it is more preferable to use it in combination with an unmodified polypropylene resin in order to adjust the modification rate of the resin as a whole. In this case, the ratio of the acid-modified polypropylene resin to all polypropylene resins is preferably 0.5% by mass to 50% by mass. A more preferred lower limit is 1 mass%, or 2 mass%, or 3 mass%, or 4 mass%, or 5 mass%. A more preferred upper limit is 45 mass%, or 40 mass%, or 35 mass%, or 30 mass%, or 20 mass%. In order to maintain the interfacial strength between the resin and the cellulose nanofiber, a content equal to or greater than the lower limit is preferred, and in order to maintain the ductility of the resin, a content equal to or less than the upper limit is preferred.
[0099] The melt mass flow rate (MFR) of the acid-modified polypropylene resin measured in accordance with ISO 1133 at 230°C under a load of 21.2 N is preferably 50 g / 10 min or more, 100 g / 10 min or more, 150 g / 10 min or more, or 200 g / 10 min or more from the viewpoint of increasing the affinity at the interface between the resin and the cellulose nanofiber. There is no particular upper limit, but it is preferably 500 g / 10 min from the viewpoint of maintaining mechanical strength.
[0100] Examples of polyamide-based resins that are preferable as the thermoplastic resin include polyamides obtained by polycondensation reaction of lactams (e.g., polyamide 6, polyamide 11, polyamide 12, etc.); diamines (e.g., 1,6-hexanediamine, 2-methyl-1,5-pentanediamine, 1,7-heptanediamine, 2-methyl-1-6-hexanediamine, 1,8-octanediamine, 2-methyl-1,7-heptanediamine, 1,9-nonanediamine, 2-methyl-1,8-octanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, m-xylylenediamine, etc.) and dicarboxylic acids (e.g., butanedioic acid, pentanedioic acid, hexanedioic acid, , heptanedioic acid, octanedioic acid, nonanedioic acid, decanedioic acid, benzene-1,2-dicarboxylic acid, benzene-1,3-dicarboxylic acid, benzene-1,4-dicarboxylic acid, cyclohexane-1,3-dicarboxylic acid, cyclohexane-1,4-dicarboxylic acid, etc.) (for example, polyamide 6,6, polyamide 6,10, polyamide 6,11, polyamide 6,12, polyamide 6,T, polyamide 6,I, polyamide 9,T, polyamide 10,T, polyamide 2M5,T, polyamide MXD,6, polyamide 6,C, polyamide 2M5,C, etc.); and copolymers in which these are copolymerized (for example, polyamide 6,T / 6,I, etc.).
[0101] Among these polyamide resins, aliphatic polyamides such as polyamide 6, polyamide 11, polyamide 12, polyamide 6,6, polyamide 6,10, polyamide 6,11, and polyamide 6,12, and alicyclic polyamides such as polyamide 6,C and polyamide 2M5,C are more preferred.
[0102] From the viewpoint of improving the heat resistance of the resin composite, the melting point of the polyamide resin is preferably 220°C or more, or 230°C or more, or 240°C or more, or 245°C or more, or 250°C or more, and from the viewpoint of ease of production of the resin composite, the melting point is preferably 350°C or less, or 320°C or less, or 300°C or less.
[0103] The terminal carboxyl group concentration of the polyamide resin is not particularly limited, but is preferably 20 μmol / g or more, or 30 μmol / g or more, and preferably 150 μmol / g or less, or 100 μmol / g or less, or 80 μmol / g or less.
[0104] In the polyamide resin, the ratio of carboxyl end groups to all end groups ([COOH] / [total end groups]) is preferably 0.30 or more, or 0.35 or more, or 0.40 or more, or 0.45 or more from the viewpoint of dispersibility of cellulose nanofibers in the resin composite, and is preferably 0.95 or less, or 0.90 or less, or 0.85 or less, or 0.80 or less from the viewpoint of the color tone of the resin composite.
[0105] The terminal group concentration of the polyamide resin can be adjusted by a known method, such as adding a terminal regulator (e.g., a diamine compound, a monoamine compound, a dicarboxylic acid compound, a monocarboxylic acid compound, an acid anhydride, a monoisocyanate, a monoacid halide, a monoester, a monoalcohol, etc.) that reacts with the terminal group during polymerization of the polyamide to the polymerization liquid so as to obtain a predetermined terminal group concentration.
[0106] Examples of the terminal regulator that reacts with the terminal amino group include aliphatic monocarboxylic acids such as acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, pivalic acid, and isobutyric acid; alicyclic monocarboxylic acids such as cyclohexanecarboxylic acid; aromatic monocarboxylic acids such as benzoic acid, toluic acid, α-naphthalenecarboxylic acid, β-naphthalenecarboxylic acid, methylnaphthalenecarboxylic acid, and phenylacetic acid; and mixtures of a plurality of terminal regulators selected from the above. Among these, from the viewpoints of reactivity, stability of the blocked terminal, and cost, one or more terminal regulators selected from the group consisting of acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, and benzoic acid are preferred, and acetic acid is most preferred.
[0107] Examples of the terminal regulator that reacts with the terminal carboxyl group include aliphatic monoamines such as methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, decylamine, stearylamine, dimethylamine, diethylamine, dipropylamine, dibutylamine, etc., alicyclic monoamines such as cyclohexylamine, dicyclohexylamine, etc., aromatic monoamines such as aniline, toluidine, diphenylamine, naphthylamine, etc., and any mixtures thereof. Among these, one or more terminal regulators selected from the group consisting of butylamine, hexylamine, octylamine, decylamine, stearylamine, cyclohexylamine, and aniline are preferred in terms of reactivity, boiling point, stability of the blocked terminal, price, etc.
[0108] The concentration of amino end groups and carboxyl end groups of the polyamide resin is 1 It can be determined from the integral value of the characteristic signal corresponding to each terminal group by H-NMR. This method is preferable in terms of accuracy and simplicity. More specifically, it is recommended to use the method described in JP-A-7-228775, use deuterated trifluoroacetic acid as the measurement solvent, and set the number of integration scans to 300 or more.
[0109] The intrinsic viscosity [η] of the polyamide resin measured under the condition of 30°C in concentrated sulfuric acid is preferably 0.6 to 2.0 dL / g, or 0.7 to 1.4 dL / g, or 0.7 to 1.2 dL / g, or 0.7 to 1.0 dL / g, from the viewpoint that the fluidity in the mold is good and the appearance of the molded piece is good when the resin composite is, for example, injection molded. In the present disclosure, the "intrinsic viscosity" is synonymous with the viscosity generally called the limiting viscosity. The intrinsic viscosity is obtained by measuring the ηsp / c of several measurement solvents having different concentrations under the temperature condition of 30°C in 96% concentrated sulfuric acid, deriving the relational expression between each of the ηsp / c and the concentration (c), and extrapolating the concentration to zero. The value extrapolated to zero is the intrinsic viscosity. Details of the above method are described, for example, in Polymer Process Engineering (Prentice-Hall, Inc. 1994), pages 291 to 294, etc. From the viewpoint of accuracy, it is desirable to set the concentrations in the measurement solvents having different concentrations to at least four points (for example, 0.05 g / dL, 0.1 g / dL, 0.2 g / dL, and 0.4 g / dL).
[0110] As the polyester resin preferred as the thermoplastic resin, one or more selected from polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), polybutylene adipate terephthalate (PBAT), polyhydroxyalkanoic acid (PHA), polylactic acid (PLA), polyarylate (PAR), etc. can be used. Among them, PET, PBS, PBSA, PBT and PEN are more preferred, and PBS, PBSA and PBT are particularly preferred.
[0111] The terminal groups of the polyester resin can be changed as desired by the monomer ratio during polymerization, the presence or absence and amount of addition of a terminal stabilizer, etc. The ratio of carboxyl terminal groups to all terminal groups of the polyester resin ([COOH] / [total terminal groups]) is preferably 0.30 or more, or 0.35 or more, or 0.40 or more, or 0.45 or more from the viewpoint of dispersibility of cellulose nanofibers in the resin composite, and is preferably 0.95 or less, or 0.90 or less, or 0.85 or less, or 0.80 or less from the viewpoint of the color tone of the resin composite.
[0112] As the polyacetal resin preferred as the thermoplastic resin, homopolyacetal made from formaldehyde and copolyacetal containing trioxane as the main monomer and 1,3-dioxolane as the comonomer component are generally used, and although both can be used, copolyacetal is preferred from the viewpoint of thermal stability during processing. The amount of the structure derived from the comonomer component (e.g., 1,3-dioxolane) is preferably 0.01 mol% or more, or 0.05 mol% or more, or 0.1 mol% or more, or 0.2 mol% or more from the viewpoint of thermal stability during extrusion processing and molding processing, and is preferably 4 mol% or less, or 3.5 mol% or less, or 3.0 mol% or less, or 2.5 mol% or less, or 2.3 mol% or less from the viewpoint of mechanical strength.
[0113] (thermosetting resin) Examples of thermosetting resins include bisphenol type epoxy resins such as bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol E type epoxy resin, bisphenol M type epoxy resin, bisphenol P type epoxy resin, and bisphenol Z type epoxy resin; novolac type epoxy resins such as bisphenol A novolac type epoxy resin, phenol novolac type epoxy resin, and cresol novolac epoxy resin; biphenyl type epoxy resin, biphenyl aralkyl type epoxy resin, aryl alkylene type epoxy resin, tetraphenylol ethane type epoxy resin, naphthalene type epoxy resin, anthracene type epoxy resin, phenoxy type epoxy resin, dicyclopentadiene type epoxy resin, norbornene type epoxy resin, adamantane type epoxy resin, fluorene type epoxy resin, glycidyl methacrylate copolymer epoxy resin, cyclohexylmaleimide and glycidyl methacrylate copolymer epoxy resin, epoxy modified polybutadiene rubber derivative, CTBN modified epoxy resin, trimethylolpropane polyglycidyl ether, Phenyl-1,3-diglycidyl ether, biphenyl-4,4'-diglycidyl ether, 1,6-hexanediol diglycidyl ether, diglycidyl ether of ethylene glycol or propylene glycol, sorbitol polyglycidyl ether, tris(2,3-epoxypropyl)isocyanurate, triglycidyl tris(2-hydroxyethyl)isocyanurate, novolac-type phenolic resins such as phenol novolac resin, cresol novolac resin, and bisphenol A novolac resin, unmodified resol phenolic resin, paulownia wood Examples of the resin include phenolic resins such as resol-type phenolic resins, such as oil-modified resol phenolic resins modified with oil, linseed oil, walnut oil, etc.; triazine ring-containing resins, such as phenoxy resins, urea (urea) resins, and melamine resins; unsaturated polyester resins, bismaleimide resins, diallyl phthalate resins, silicone resins, resins having a benzoxazine ring, norbornene resins, cyanate resins, isocyanate resins, urethane resins, benzocyclobutene resins, maleimide resins, bismaleimide triazine resins, polyazomethine resins, and thermosetting polyimides.
[0114] (light curing resin) Examples of photocurable resins include (meth)acrylate resins, vinyl resins, and epoxy resins. These are generally classified into radical reaction types in which a monomer reacts with radicals generated by light, and cationic reaction types in which a monomer undergoes cationic polymerization, according to the reaction mechanism. Examples of radical reaction type monomers include (meth)acrylate compounds and vinyl compounds (e.g., certain vinyl ethers). Examples of cationic reaction types include epoxy compounds and certain vinyl ethers. For example, an epoxy compound that can be used as a cationic reaction type can be a monomer for both thermosetting resins and photocurable resins.
[0115] The (meth)acrylate compound is a compound having one or more (meth)acrylate groups in the molecule. Examples of the (meth)acrylate compound include monofunctional (meth)acrylates, polyfunctional (meth)acrylates, epoxy acrylates, polyester acrylates, and urethane acrylates.
[0116] Examples of vinyl compounds include vinyl ether, styrene, and styrene derivatives. Examples of vinyl ether include ethyl vinyl ether, propyl vinyl ether, hydroxyethyl vinyl ether, and ethylene glycol divinyl ether. Examples of styrene derivatives include methyl styrene and ethyl styrene. Other examples of vinyl compounds include triallyl isocyanurate and trimethallyl isocyanurate.
[0117] As a raw material for the photocurable resin, a so-called reactive oligomer may be used. Examples of the reactive oligomer include an oligomer having any combination selected from a (meth)acrylate group, an epoxy group, a urethane bond, and an ester bond in the same molecule, such as a urethane acrylate having a (meth)acrylate group and a urethane bond in the same molecule, a polyester acrylate having a (meth)acrylate group and an ester bond in the same molecule, and an epoxy acrylate derived from an epoxy resin having an epoxy group and a (meth)acrylate group in the same molecule.
[0118] (Elastomer) Examples of elastomers (i.e. rubber) include natural rubber (NR), butadiene rubber (BR), styrene-butadiene copolymer rubber (SBR), isoprene rubber (IR), butyl rubber (IIR), acrylonitrile-butadiene rubber (NBR), acrylonitrile-styrene-butadiene copolymer rubber, chloroprene rubber, styrene-isoprene copolymer rubber, styrene-isoprene-butadiene copolymer rubber, isoprene-butadiene copolymer rubber, chlorosulfonated polyethylene rubber, modified natural rubber (epoxidized natural rubber (ENR), hydrogenated natural rubber, deproteinized natural rubber, etc.), ethylene-propylene copolymer rubber, acrylic rubber, epichlorohydrin rubber, polysulfide rubber, silicone rubber, fluororubber, urethane rubber, and the like.
[0119] When the resin is a thermoplastic resin, a resin composite can be produced by kneading a redispersion of cellulose nanofibers or a dried product thereof (hereinafter also referred to as a cellulose nanofiber component) with a thermoplastic resin. - A method in which a resin monomer and a cellulose nanofiber component are mixed, a polymerization reaction is carried out, the resulting resin composite is extruded into a strand shape, and cooled and solidified in a water bath to obtain a pellet-shaped molded product; A method in which a mixture of a resin and a cellulose nanofiber component is melt-kneaded using a single-screw or twin-screw extruder, extruded into a strand shape, and cooled and solidified in a water bath to obtain a pellet-shaped molded product; - A method in which a mixture of a resin and a cellulose nanofiber component is melt-kneaded using a single-screw or twin-screw extruder, extruded into a rod or tube, and cooled to obtain an extrusion molded product; A method in which a mixture of a resin and a cellulose nanofiber component is melt-kneaded using a single-screw or twin-screw extruder, and extruded through a T-die to obtain a sheet or film-like molded product; In a preferred embodiment, a mixture of a resin and a cellulose nanofiber component is melt-kneaded using a single-screw or twin-screw extruder, extruded into a strand shape, and cooled and solidified in a water bath to obtain a pellet-shaped molded product. A specific example of a method for melt-kneading a resin and a cellulose nanofiber component includes a method in which a resin and a cellulose nanofiber component transported in a desired ratio are mixed together and then melt-kneaded. When the resin is a thermoplastic resin, the minimum processing temperatures recommended by thermoplastic resin suppliers are 255 to 270°C for nylon 66, 225 to 240°C for nylon 6, 170 to 190°C for polyacetal resin, and 160 to 180°C for polypropylene. The heating temperature setting is preferably in the range of 20°C higher than these recommended minimum processing temperatures. By setting the mixing temperature within this temperature range, the cellulose nanofibers and the resin can be mixed uniformly.
[0120] Resin composites containing a thermoplastic resin as a resin can be provided in various shapes. Specifically, resin pellets, sheets, fibers, plates, rods, etc. can be mentioned, but the resin pellet shape is more preferable from the viewpoint of ease of post-processing and ease of transportation. In this case, preferred pellet shapes include round, elliptical, and cylindrical shapes, which differ depending on the cutting method used during extrusion processing. Pellets cut by a cutting method called underwater cutting are often round, pellets cut by a cutting method called hot cutting are often round or elliptical, and pellets cut by a cutting method called strand cutting are often cylindrical. In the case of round pellets, the preferred size is a pellet diameter of 1 mm or more and 3 mm or less. In the case of cylindrical pellets, the preferred diameter is 1 mm or more and 3 mm or less, and the preferred length is 2 mm or more and 10 mm or less. It is desirable to set the above diameter and length to the lower limit or more from the viewpoint of operational stability during extrusion, and it is desirable to set them to the upper limit or less from the viewpoint of bite into the molding machine in post-processing.
[0121] A resin composite containing a thermoplastic resin as a resin can be used as various resin molded products. There is no particular limitation on the manufacturing method of the resin molded product, and any manufacturing method may be used, but injection molding, extrusion molding, blow molding, inflation molding, foam molding, etc. can be used. Among these, injection molding is most preferable from the viewpoint of design and cost.
[0122] When the resin is a thermosetting resin or a photocurable resin, the resin composite can be produced by, for example, a method of thoroughly dispersing the cellulose nanofiber component in a resin solution or resin powder dispersion and drying it, a method of thoroughly dispersing the cellulose nanofiber component in a resin monomer liquid and polymerizing it by heat, UV irradiation, a polymerization initiator, etc., a method of thoroughly impregnating a molded body (e.g., a sheet, a powder particle molded body, etc.) made of a dry solid of the cellulose nanofiber dispersion with a resin solution or resin powder dispersion and drying it, a method of thoroughly impregnating a molded body made of a dry solid of the cellulose nanofiber dispersion with a resin monomer liquid and polymerizing it by heat, UV irradiation, a polymerization initiator, etc. When curing, various polymerization initiators, curing agents, curing accelerators, polymerization inhibitors, etc. can be blended.
[0123] When the resin is a thermosetting resin or a photocurable resin, a method may be used in which an uncured or semi-cured sheet called a prepreg is prepared, the prepreg is made into a single layer or a laminate, and the resin is cured and molded by applying pressure and heat. Examples of the method of applying pressure and heat include a press molding method, an autoclave molding method, a bagging molding method, a wrapping tape method, and an internal pressure molding method.
[0124] When the resin is a photocurable resin, various curing methods using active energy rays can be used to produce a resin molded product.
[0125] When the resin is an elastomer, the resin composite can be produced by a method of kneading the dry solid of the cellulose nanofiber dispersion with the raw rubber in a dry state, or a method of dispersing or dissolving the cellulose nanofiber component and the raw rubber in a dispersion medium, and then drying and mixing them. As a mixing method, a mixing method using a homogenizer is preferable because it can apply high shear force and pressure to promote dispersion, but other methods such as a propeller type stirring device, a rotary stirring device, an electromagnetic stirring device, and manual stirring can also be used. The resin composite containing the elastomer can be molded using a desired molding method such as mold molding, injection molding, extrusion molding, hollow molding, and foam molding to obtain an unvulcanized molded body of a desired shape such as a sheet, pellet, or powder. The unvulcanized molded body can be vulcanized by heat treatment or the like as necessary to obtain a resin molded body.
[0126] The resin molded product containing a thermoplastic resin or an elastomer may be partially (e.g., several portions) melted by heat treatment and then bonded to, for example, a resin or metal substrate. The resin molded product may be a coating applied to a resin or metal substrate, or may form a laminate with the substrate. The sheet-, film-, or fiber-shaped resin molded product may be subjected to secondary processing such as annealing, etching, corona treatment, plasma treatment, grain transfer, cutting, and surface polishing.
[0127] In the resin composite, the amount of cellulose nanofibers per 100 parts by mass of resin may be, from the viewpoint of the balance between processability and mechanical properties, preferably 0.001 part by mass or more, or 0.01 part by mass or more, or 0.1 part by mass or more, or 1 part by mass or more, and may be preferably 100 parts by mass or less, or 80 parts by mass or less, or 70 parts by mass or less, or 50 parts by mass or less. EXAMPLES
[0128] The present invention will be further described with reference to examples, but the present invention is not limited to these examples.
[0129] <Production of cellulose nanofiber dispersion, dry solid, and redispersion thereof> [Production Example 1] Cotton linter pulp was mixed with water to prepare a dispersion with a solid content of 1.5% by mass, and the aqueous dispersion was beaten for 30 minutes using an SDR14 lab refiner (pressurized disk type) manufactured by Aikawa Iron Works Co., Ltd. as a disk refiner device with a clearance between disks of 1 mm. Subsequently, thorough beating was performed under conditions in which the clearance was reduced to a level close to zero, to obtain a beaten aqueous dispersion (solid content: 1.5% by mass). The obtained cellulose nanofiber slurry (as a dispersion) was diluted to obtain an aqueous dispersion with a solid content of 0.5% by mass, and the shear rate of the aqueous dispersion was 100 seconds. -1 The viscosity at was 40.1 mPa s.
[0130] The obtained cellulose nanofiber slurry was filtered and concentrated using a paper machine to a solid content of about 10 to 20% by mass, and the obtained sheet-like wet cake was dried in a steam oven until the moisture content was 7% by mass or less to obtain an aggregated dried product of cellulose nanofibers (as a cellulose nanofiber dry solid). The apparent density of the obtained dry solid was 685 g / L. The cellulose nanofibers had a degree of polymerization of 2900 and an average fiber diameter of 32 nm before drying.
[0131] [Production Example 2] Cotton linter pulp and water were mixed to prepare a dispersion with a solid content of 1.5% by mass. The aqueous dispersion was beaten for 30 minutes using a SDR14 lab refiner (pressurized disk type) manufactured by Aikawa Iron Works Co., Ltd. as a disk refiner device, with the clearance between the disks set to 1 mm. Subsequently, thorough beating was performed under conditions in which the clearance was reduced to a level close to zero, to obtain a beaten aqueous dispersion (solid content: 1.5% by mass). The obtained beaten aqueous dispersion was directly subjected to a high-pressure homogenizer (NSO15H manufactured by Niro Soavi Co., Ltd. (Italy)) for 10 rounds of refinement under an operating pressure of 100 MPa to obtain a cellulose nanofiber slurry (as a dispersion liquid) (solid content: 1.5% by mass). The obtained cellulose nanofiber slurry was diluted to obtain an aqueous dispersion with a solid content of 0.5% by mass, and the shear rate of the dispersion was 100 seconds. -1The viscosity at was 141.3 mPa s.
[0132] The obtained cellulose nanofiber slurry was filtered and concentrated to a solid content of about 10 to 20% by mass using a papermaking machine, and the obtained wet sheet was sandwiched between Asahi Kasei Silky Fine (nonwoven fabric), and 10 sheets of filter paper were placed on the outside. A metal plate was placed on the outermost side, and the sheet was pressed for 5 minutes at a pressure of 410 kPA. The swollen cardboard was replaced and the pressing operation was repeated to concentrate the sheet to a moisture content of 55% by mass. The obtained cellulose nanofiber wet sheet was vacuum-dried at a pressure of 410 kPa and 150°C until the moisture content was 5% by mass or less, and a cellulose nanofiber dry product (as a cellulose nanofiber dry solid) was obtained. The apparent density of the obtained dry solid was 1150 g / L. The cellulose nanofiber had a degree of polymerization of 2700 and an average fiber diameter of 18 nm before drying.
[0133] [Production Example 3] Shear rate of diluted water dispersion with solid content of 0.5% by mass: 100 seconds -1 Celish KY-100G (Daicel Chemical Industries) (cellulose nanofiber) with a viscosity of 14.9 mPa·s at 20°C was dried under reduced pressure at -0.1 MPa in a closed planetary mixer (Kodaira Seisakusho Co., Ltd., product name "ACM-5LVT", mixing blade is hook type) with a 60°C hot bath set and a rotation speed of 307 rpm until the moisture content was 5% by mass or less, to obtain an aggregated dried product of cellulose nanofiber (as cellulose nanofiber dry solid). The apparent density of the obtained dry solid was 291 g / L. The cellulose nanofiber before drying had a degree of polymerization of 1450 and an average fiber diameter of 125 nm.
[0134] [Redispersion examples 1-6] 0.5 parts by mass of the obtained cellulose nanofiber dry solid and 24.5 parts by mass of dimethyl sulfoxide were added to KAPPA VITA HM35 manufactured by NETZSCH VAKUMIX, and after stirring for 2 hours, the cellulose nanofiber was redispersed by treatment in a homomixer at a rotation speed of 6,500 rpm for the time shown in Table 1 to obtain a cellulose nanofiber / DMSO slurry (as redispersion liquid). Table 1 shows the redispersion conditions, and the shear rate 100 seconds of an aqueous dispersion with a solid content of 0.5% by mass prepared from the obtained redispersion liquid by the method described below. -1 and the ratio (%) of (viscosity of the aqueous dispersion obtained from the redispersion) / (viscosity of the aqueous dispersion obtained from the dispersion) as the viscosity recovery rate are shown.
[0135] [Redispersion examples 7-9] 0.5 parts by mass of each of the dry cellulose nanofiber solids obtained in Production Examples 1 to 3 and 24.5 parts by mass of pure water were added to a KAPPA VITA HM35 manufactured by NETZSCH VAKUMIX, and the mixture was allowed to stand for 2 hours. After that, the dry cellulose nanofiber solid was taken out. The mass (X) of the dry solid content obtained after drying for 2 hours at 120°C under vacuum conditions was measured. The rate of change (YX) / Y relative to the mass (Y) of the dry solid cellulose nanofiber before standing was 6 mass% for Production Example 1, 2 mass% for Production Example 2, and 10 mass% for Production Example 3. An attempt was made to redisperse the obtained cellulose / water dispersion at a homogenizer rotation speed of 6,500 rpm, but redispersion was not achieved and the device became clogged, resulting in a halt.
[0136] [Redispersion example 10] (Acetylation of cellulose nanofibers after redispersion) 0.321 parts by mass of sodium bicarbonate and 1 part by mass of vinyl acetate were added to 50 parts by mass of the cellulose nanofiber / DMSO slurry (redispersion liquid) obtained in Redispersion Example 5, and the mixture was allowed to react at 60°C for 1 hour to obtain acetylated cellulose nanofibers with their surfaces acetylated.
[0137] <Production of resin composite> [Examples 1 to 7 and Control Examples 1 to 3] The cellulose nanofiber slurry (dispersion) obtained in each manufacturing example and the cellulose nanofiber DMSO slurry (redispersion) obtained in each redispersion example were used as shown in Table 2, and resin composites were produced by the following procedure. For the cellulose nanofiber DMSO slurry (redispersion), 5 parts by mass of water was added to 1 part by mass of the slurry, and after stirring, centrifugal separation was performed and the supernatant was discarded. The above cycle of adding 5 parts by mass of water, stirring, centrifugal separation, and discarding the supernatant was repeated 5 times, and then 2 parts by mass of water was added to the residue to obtain an aqueous dispersion. To each of the above dispersions and the above aqueous dispersions obtained from the redispersions, 43 parts by mass of PEG-PPG (GL-3000, manufactured by Sanyo Chemical Industries, Ltd.) was added per 100 parts by mass of cellulose solids, and the mixture was stirred at 70 rpm for 80 minutes at 25°C and atmospheric pressure in an enclosed planetary mixer (manufactured by Kodaira Manufacturing Co., Ltd., trade name "ACM-5LVT", stirring blade is hook type) and then dried under reduced pressure at 307 rpm for 5 hours in a 60°C hot bath under reduced pressure conditions of -0.1 MPa to obtain a cellulose / PEG-PPG dried body. The obtained cellulose / PEG-PPG dried body and a thermoplastic resin (UBE nylon 1013B manufactured by Ube Industries, Ltd.) were used in the formulations shown in Table 2, and a resin composite was produced according to the following procedure.
[0138] The obtained resin composite was mixed in a small mixer (manufactured by Xplore instruments, product name "Xplore") at 260°C and 100 rpm (shear rate 1570 (1 / s)) for 5 minutes, and then passed through a die to obtain a resin composite strand with a diameter of 1 mm. Resin composite pellets obtained from the strand (cut into 1 cm lengths) were melted at 260°C in an attached injection molding machine to prepare dumbbell-shaped test pieces according to the JIS K7127 standard and used for evaluation. The resin composite 1 in the form of the obtained thin film, pellet, and dumbbell-shaped test piece were used for appropriate evaluation.
[0139] Evaluation <Preparation of measurement sample> The cellulose nanofiber slurry obtained in each manufacturing example was filtered to adjust the solid content concentration to 10% by mass, and 4 g of the cellulose slurry was dispersed in 96 g of tert-butanol, and further dispersed in a homogenizer (IKA, product name "Ultra Turrax T18") under the treatment conditions of 25,000 rpm for 5 minutes until no aggregates were present (solid content concentration 0.4% by mass). 100 g of the obtained tert-butanol dispersion was filtered on a filter paper (5C, Advantec, diameter 90 mm). The wet paper obtained by filtration was heated at 150 ° C for 5 minutes with the filter paper attached, sandwiched between two sheets of 150 mm diameter filter paper, and the periphery of the wet paper was pressed down with a cylindrical weight (inner diameter 110 mm) of about 300 g to obtain a porous sheet. This porous sheet was used as a measurement sample.
[0140] <Average degree of substitution (DS) (degree of acetylation) of cellulose nanofiber> The infrared spectrum of the porous sheet was measured by the ATR-IR method using a Fourier transform infrared spectrophotometer (FT / IR-6200 manufactured by JASCO Co., Ltd.) The infrared spectrum measurement was performed under the following conditions. Number of times accumulated: 64 times, Wavenumber resolution: 4cm -1 , Measurement wave number range: 4000~600cm -1 , ATR crystal: Diamond, Incident angle: 45° From the obtained IR spectrum, the IR index was calculated according to the following formula (1): IR index = H1730 / H1030(1) In the formula, H1730 and H1030 are at 1730 cm -1 , 1030cm -1 (absorption band of CO stretching vibration of cellulose backbone chain) -1 and 1500cm -1 The line connecting the -1 and 1500cm -1 The line connecting these points is taken as the baseline, and the absorbance is calculated when this baseline is taken as 0. Then, the average degree of substitution (DS) was calculated from the IR index according to the following formula (2). DS = 4.13 × IR index (2)
[0141] <Degree of polymerization of cellulose nanofiber> The viscosity was measured by the reduced specific viscosity method using a copper ethylenediamine solution as specified in the crystalline cellulose identification test (3) in the "Japanese Pharmacopoeia, 14th Edition" (published by Hirokawa Publishing).
[0142] <Crystallization degree of cellulose nanofiber> The porous sheet was subjected to X-ray diffraction measurement, and the crystallinity was calculated according to the following formula. Crystallinity (%)=[I (200) -I (amorphous) ] / I (200) ×100 I (200) : Diffraction peak intensity due to 200 plane (2θ=22.5°) in cellulose I crystal I (amorphous) : The halo peak intensity due to the amorphous phase in cellulose I crystals, which is the peak intensity at an angle 4.5° lower than the diffraction angle of the 200 plane (2θ=18.0°)
[0143] (X-ray diffraction measurement conditions) Equipment: MiniFlex (Rigaku Corporation) Operation axis 2θ / θ Source CuKα Measurement method: Continuous Voltage 40kV Current 15mA Starting angle 2θ=5° End angle 2θ=30° Sampling width 0.020° Scan speed: 2.0° / min Sample: A porous sheet is attached onto the sample holder.
[0144] <Average fiber diameter of cellulose nanofiber> The cellulose nanofiber slurry was dispersed using a high-shear homogenizer (manufactured by Nippon Seiki Co., Ltd., product name "Excel Auto Homogenizer ED-7", processing conditions: rotation speed 15,000 rpm x 5 minutes) to form an aqueous dispersion, which was diluted with pure water to 0.1 to 0.5 mass%, cast onto mica, air-dried, and measured with an atomic force microscope (AFM). The measurement was performed by adjusting the magnification so that at least 100 cellulose nanofibers were observed, and the fiber diameters of 100 randomly selected cellulose nanofibers were determined, and the arithmetic average of the 100 cellulose nanofibers was calculated.
[0145] <Apparent density of cellulose nanofiber dry solid> The apparent density of the dry solid cellulose nanofiber was determined according to the Archimedes method using an electronic balance GR-202 and a specific gravity meter AD-1653 manufactured by A&D Corporation.
[0146] <Viscosity of aqueous dispersions obtained from dispersions and redispersions of cellulose nanofibers> Water was added to the dispersion as described above to obtain an aqueous dispersion with a solid content of 0.5% by mass. The redispersion was subjected to a cycle of adding 5 times the amount of water by mass, stirring, centrifuging, and discarding the supernatant 5 times, and then water was added to obtain an aqueous dispersion with a solid content of 0.5% by mass. Viscosity measurements were performed on these aqueous dispersions. A Thermo Fisher Scientific rheometer HAAKE MARS was used for the measurements, and the viscosity was measured in a concentric cylinder configuration. Shear rate 100 seconds -1 In order to suppress the variation in the data, the viscosity was measured by applying a constant shear history and then measuring the shear rate for 100 seconds. -1 Specifically, a 0.5% by mass aqueous dispersion (obtained from a dispersion or redispersion) was placed in a concentric cylinder cup, and the viscosity was measured using a rheometer for 1 second. -1 100 seconds from -1 The shear rate was then increased over 100 seconds to 100°C. -1 1 second from -1 The shear rate was then reduced over 100 seconds to 100°C, and then reduced again for 1 second. -1 100 seconds from-1 Increase the shear rate over 100 seconds to 100 seconds. -1 The viscosity was read when it reached
[0147] <Tensile breaking strength of resin composite> Multipurpose test pieces conforming to ISO294-3 were molded using an injection molding machine with a maximum clamping pressure of 75 tons, and the tensile breaking strength was measured under conditions conforming to JIS K6920-2, n=10. Note that since polyamide resin changes due to moisture absorption, it was stored in an aluminum moisture-proof bag immediately after molding to suppress moisture absorption.
[0148] <Coefficient of linear thermal expansion (CTE) of resin composite> The steam multipurpose test piece was cut into a 3 mm width x 25 mm length to be used as a measurement sample. Using an SII TMA6100 device, the specimen was heated from room temperature to 120°C at 5°C / min. in a nitrogen atmosphere with a chuck distance of 10 mm and a load of 5 g in compression mode, then cooled to 25°C at 5°C / min., and then heated again from 25°C to 120°C at 5°C / min. In this case, the average linear thermal expansion coefficient between 30°C and 100°C during the second heating was measured.
[0149] [Table 1]
[0150] [Table 2] [Industrial Applicability]
[0151] According to the present invention, cellulose nanofibers can be provided that can be provided as a dry solid that exhibits good redispersibility, which is advantageous in terms of storage and transportation costs and is extremely useful as a property improver for resin composites.
Claims
1. A method for producing a redispersion of cellulose nanofibers, comprising the steps of: A dispersing step of preparing a dispersion liquid by dispersing cellulose nanofibers in a first dispersion medium; A drying step of drying the dispersion to obtain a dry solid of cellulose nanofibers; A redispersion step of redispersing the cellulose nanofiber dry solid in a second dispersion medium to prepare a redispersion liquid; Including, The apparent density of the cellulose nanofiber dry solid is 210 g / L to 1500 g / L; the second dispersion medium is an aprotic polar solvent; The redispersion liquid was adjusted to have a solid content of 0.5% by mass in the cellulose nanofibers, and the shear rate of the redispersion liquid was 100 seconds. -1 The viscosity at shear rate of the aqueous dispersion of the cellulose nanofibers of the dispersion was adjusted to 0.5% by mass in an aqueous dispersion having a solid content of 100 s -1 The viscosity of the solution is 30% or more of that in
2. The method according to claim 1, wherein the average degree of substitution (DS) of the cellulose nanofiber dry solid is 0.5 or less.
3. The method according to claim 1 or 2, wherein the content of the dispersant in the cellulose nanofiber dry solid is less than 1 mass%.
4. The method according to any one of claims 1 to 3, wherein the redispersion is carried out by applying a shear force through stirring.
5. The method according to claim 4, wherein the shear force is applied using one or more selected from the group consisting of ultrasonic waves, a bead mill, a ball mill, and a homomixer.
6. The method according to any one of claims 1 to 5, wherein the aprotic polar solvent is one or more selected from the group consisting of dimethylsulfoxide, N-methylpyrrolidone, dimethylacetamide, and dimethylformamide.
7. The method according to any one of claims 1 to 6, further comprising chemically modifying the cellulose nanofibers during and / or after the redispersion step.
8. A method for producing a cellulose nanofiber composite containing a cellulose nanofiber and an organic binder, comprising: A step of preparing a redispersion of cellulose nanofibers by the method according to any one of claims 1 to 7; and mixing the redispersion liquid or a dried product thereof with an organic binder; A method comprising:
9. A method for producing a resin composite containing cellulose nanofibers and a resin, comprising: A step of preparing a redispersion of cellulose nanofibers by the method according to any one of claims 1 to 7; and a mixing step of mixing the redispersion liquid, an aqueous dispersion liquid obtained by replacing the second dispersion medium of the redispersion liquid with water, or a dried product thereof with a resin; A method comprising:
10. A method for producing a resin composition containing cellulose nanofibers and a thermoplastic resin, comprising: A cellulose nanofiber solid forming step for obtaining a cellulose nanofiber solid, which is a dry solid of defibrated cellulose nanofibers; A redispersion step of redispersing the cellulose nanofiber solid body in a second dispersion medium to prepare a redispersion liquid; and a kneading step of kneading the redispersion, an aqueous dispersion obtained by replacing the second dispersion medium of the redispersion with water, or a dried product thereof with a thermoplastic resin; Including, The apparent density of the cellulose nanofiber solid body is 210 g / L to 1500 g / L, the second dispersion medium is an aprotic polar solvent; The redispersion liquid was adjusted to have a solid content of 0.5% by mass in the cellulose nanofibers, and the shear rate of the redispersion liquid was 100 seconds. -1 The viscosity at shear rate of the aqueous dispersion of the defibrated cellulose nanofibers adjusted to a solid content of 0.5% by mass is 100 s -1 The viscosity of the solution is 30% or more of that in
11. The method according to claim 10, wherein in the cellulose nanofiber solid, the cellulose nanofibers are bonded to each other by hydrogen bonds of hydroxyl groups.
12. The method according to claim 10 or 11, wherein the rate of change (Y-X) / Y of the mass of the dry solid content (X) when the cellulose nanofiber solid is allowed to stand in water at 20°C for 2 hours and then removed from the water relative to the mass (Y) of the cellulose nanofiber solid before standing is 30 mass% or less.
13. The method according to any one of claims 10 to 12, wherein the second dispersion medium is selected from the group consisting of dimethylsulfoxide, N-methylpyrrolidone, dimethylacetamide, and dimethylformamide.
Citation Information
Patent Citations
Microfiber and method for producing the same
JP2012224960A
Methods, systems, and apparatus for processing fibrilcellulose and fibrilcellulose materials.
JP2015512964A
Powdery cellulose nanofibers for the production of compositions, method for producing the same, and compositions
JP2017210596A
Method for producing chemically modified pulp dry solid
JP2018095761A
Block for producing cellulose nanofiber resin composite and method for producing the same
JP2019073661A