Polyurea resin composition, noncombustible powder, and method for forming polyurea resin layer

A polyurea resin composition with specific ratios of polyamine, polyisocyanate, and expandable graphite, sprayed at controlled temperatures and pressures, addresses the lack of flame retardancy in conventional polyurea resins, achieving semi-fire resistance while maintaining other properties and ensuring uniform application.

JP7566510B2Active Publication Date: 2024-10-15米川寿夫 +2
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020113173
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-30
Filing Date
2020-06-30
Publication Date
2024-10-15
Estimated Expiration
2040-06-30

AI Technical Summary

Technical Problem

Conventional polyurea resins lack effective flame retardancy without compromising their inherent properties such as corrosion resistance, abrasion resistance, waterproofness, impact resistance, and elasticity, and existing methods for adding flame retardants to polyurea resins are not suitable for forming a polyurea resin layer using conventional spraying methods.

Method used

A polyurea resin composition comprising 100 parts by mass of polyamine, 100 to 160 parts by mass of polyisocyanate, and 15 to 30 parts by mass of expandable graphite with a particle size of 100 mesh, sprayed at a temperature between 60 to 80 degrees Celsius and pressurized to a predetermined pressure using a polyurea spraying device with specific temperature and pressure controls, to form a polyurea resin layer.

Benefits of technology

The method allows for the formation of a polyurea resin layer with excellent flame retardancy (semi-fire resistance) without impairing the inherent properties, preventing clogging in the spraying device and ensuring uniform application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566510000008
    Figure 0007566510000008
  • Figure 0007566510000009
    Figure 0007566510000009
  • Figure 0007566510000010
    Figure 0007566510000010
Patent Text Reader

Abstract

To provide a polyurea resin composition which has flame resistance (semi fire resistance) without impairing characteristics inherent to a polyurea resin, and can be sprayed by a conventional method, and a method for forming a polyurea resin layer by spraying.SOLUTION: A polyurea resin composition contains 100 pts.mass of polyamine, 100-160 pts.mass of polyisocyanate, and 15-30 pts.mass of expanded graphite, and a particle diameter of the expanded graphite is equal to or smaller than 100 meshes. A polyurea spraying apparatus 100 adds the expanded graphite to at least one of polyamine and polyisocyanate. A polyurea resin produced by mixing and stirring of polyamine and polyisocyanate is heated at 60°C to 80°C, is pressurized at a pressurized pressure, and then is sprayed toward an object from a spray port 52A.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyurea resin composition, a noncombustible powder, and a method for forming a polyurea resin layer, and in particular to a polyurea resin composition, a noncombustible powder, and a method for forming a polyurea resin layer that are useful for forming a polyurea resin layer having excellent corrosion resistance, abrasion resistance, waterproofness, impact resistance, elasticity, and further noncombustibility. [Background technology]

[0002] Conventionally, polyurea resins have been proposed that are excellent in waterproofness, impact resistance, corrosion resistance, etc. Among these polyurea resins, in particular, high-purity polyurea resins (pure polyurea resins) formed using only polyisocyanate and polyamine as organic polymer compounds can improve corrosion resistance, abrasion resistance, waterproofness, impact resistance, UV protection, and elasticity by adding various fillers (intrinsic properties of polyurea resins).

[0003] Polyurea resin can be used, for example, to reinforce a concrete block wall by applying it to the surface of the wall to form a resin layer (approximately 1.5 mm to 3 mm), or to repair / reinforce the wall by injecting it into cracks in a concrete wall.

[0004] However, like other organic polymer compounds (eg, polyurethane resins), polyurea resins have the disadvantage that, in the event of a fire, they break down into smaller molecules due to an increase in temperature, generating flammable gases and therefore combust easily.

[0005] For this reason, when polyurethane resin is actually used to repair cracks in block walls or concrete walls installed outdoors, or even when it is attempted to be laid on the roof of a house because of its waterproofing properties, its flammability prevents the building from achieving flame retardancy (semi-fire resistance), and so it is unsuitable for use in these structures.

[0006] Conventionally, ammonium polyphosphate, borax, expandable graphite, etc. have been used as a filler for other common organic polymer compounds (e.g., polyurethane) other than polyurea resin to impart flame retardancy to these other organic polymer compounds. Regarding polyurea resins, it has been proposed in, for example, the following patent documents and non-patent documents that the addition of various fillers used in other organic polymer compounds to the resins can impart flame retardancy. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2017-082229 A [Patent Document 2] CN-A-102559022 [Non-patent literature]

[0008] [Non-Patent Document 1] "Further studies on the flame retardancy of polyurea: Effects of coatings and flame retardant additions" J-GLOBAL ID No.: 11A1320776 Summary of the Invention [Problem to be solved by the invention]

[0009] In particular, the above-mentioned Non-Patent Document 1 discloses that in order to impart flame retardancy to a polyurea resin, it is possible to include flame retardant additives (ammonium polyphosphate, expandable graphite, zinc borate, etc.) that have conventionally been used in other organic polymer compounds. However, there is no specific disclosure or suggestion as to what fillers should actually be added to the polyurea resin and in what ratio, and further, whether the polyurea resin to which these fillers have been added still retains its inherent properties (corrosion resistance, abrasion resistance, waterproofing, impact resistance, UV protection, elasticity), etc.

[0010] Incidentally, polyurea resin is generally sprayed onto an object (such as a block wall or a crack in concrete) to form a layer of a desired thickness on the surface of the object (spraying method). However, none of the above patent documents or non-patent documents discloses or suggests at all whether or not polyurea resin containing the above-mentioned flame retardant additive (filler) can actually be sprayed using the conventional spraying method.

[0011] The present invention has been made in view of the above circumstances, and has an object to provide a polyurea resin composition suitable for forming a polyurea resin layer having flame retardancy and noncombustibility (preferably semi-fire resistance) on an object by a conventional method (spraying method) without impairing the inherent properties of the polyurea resin (corrosion resistance, abrasion resistance, waterproofness, impact resistance, elasticity, etc.), a noncombustible powder, and a method for forming a polyurea resin layer using the polyurea resin composition. [Means for solving the problem]

[0012] The first invention is a method for producing a polyurea resin composition comprising: 100 parts by mass The composition contains 100 to 160 parts by mass of polyisocyanate and 15 to 30 parts by mass of expandable graphite, the particle size of the expandable graphite being 100 mesh or smaller.

[0013] The second invention is a polyamine 100 parts by massThe method for forming a polyurea resin layer of a desired thickness by spraying a polyurea resin composition containing 100 to 160 parts by mass of polyisocyanate and 15 to 30 parts by mass of expandable graphite (having a particle size of 100 mesh or smaller) onto an object includes the steps of adding the expandable graphite to at least one of polyamine and polyisocyanate, heating the polyamine and the polyisocyanate so that the temperature of the polyurea resin produced by mixing and stirring the polyamine and the polyisocyanate is between 60 degrees Celsius and 80 degrees Celsius, pressurizing the polyamine and the polyisocyanate so that the pressure of the polyurea resin produced by mixing and stirring the polyamine and the polyisocyanate is a predetermined pressure, and spraying the polyurea resin that has been heated to 60 degrees Celsius to 80 degrees Celsius and pressurized to the predetermined pressure onto the object.

[0014] A third invention is the method according to the second invention, further comprising, in the step of heating the polyamine and the polyisocyanate, heating the polyisocyanate to 70 to 80 degrees Celsius when the expanded graphite is added to the polyisocyanate, and heating the polyamine to 70 to 80 degrees Celsius when the expanded graphite is added to the polyamine.

[0015] A fourth invention is a method for producing a polyurea resin by mixing and stirring the polyisocyanate and the polyamine, comprising: a first tank for storing a polyisocyanate; a second tank for storing a polyamine; a first heating means for adjusting the temperature of the polyisocyanate supplied from the first tank; a second heating means for adjusting the temperature of the polyamine supplied from the second tank; a first pressurizing means for pressurizing the polyisocyanate supplied from the first tank; a second pressurizing means for pressurizing the polyamine supplied from the second tank; a compression means for compressing a gas; and a spraying means for spraying the produced polyurea resin from the spraying orifice, the polyurea resin composition of the first invention is sprayed onto an object to form a polyurea resin layer, the temperature of the polyurea resin in the spraying means is maintained at 60 to 80 degrees Celsius by the first heating means and the second heating means, the pressure of the polyurea resin in the spraying means is pressurized to a predetermined pressure by the first pressurizing means and the second pressurizing means, and the pressurized polyurea resin is sprayed onto the object from the spraying orifice to form a polyurea resin layer.

[0016] In addition, the fifth invention is the polyurea spraying device of the fourth invention, in which the diameter of the nozzle is 1.5 mm, and the specified pressure adjusted by the first pressure means and the second pressure means is 23.5 MPa to 24.0 MPa.

[0017] In addition, the sixth invention is the fourth or fifth invention, wherein when the expanded graphite is added to the polyisocyanate, the first heating means heats the polyisocyanate to 70 to 80 degrees Celsius, and when the expanded graphite is added to the polyamine, the second heating means heats the polyamine to 70 to 80 degrees Celsius. Effect of the Invention

[0026] According to the first invention, 15 to 30 parts by mass of expanded graphite having a particle size of 100 mesh or smaller is added to a polyurea resin produced by mixing and stirring 100 parts by mass of polyamine and 100 to 160 parts by mass of polyisocyanate, so that the polyurea resin can be sprayed onto an object using a conventionally used polyurea spraying device, and a polyurea resin layer of a desired thickness can be formed on the surface of the object. At this time, there is no clogging due to expanded graphite in the polyurea spraying device (especially inside the spray gun device). The polyurea resin layer formed at this time can be imparted with excellent flame retardancy (quasi-fire resistance) without impairing the inherent properties of the polyurea resin.

[0027] Furthermore, according to the second invention, even if the expanded graphite is added to at least one of the polyamine and the polyisocyanate in a spraying method using a conventional polyurea spraying device, by adjusting the temperature of the polyurea resin generated by mixing and stirring the polyamine and the polyisocyanate to between 60°C and 80°C and pressurizing the generated polyurea resin to a predetermined pressure, the generated polyurea resin can be sprayed onto a target object without causing clogging inside the polyurea spraying device, and a polyurea resin layer with a desired thickness can be formed.

[0028] Furthermore, according to the third invention, in the second invention, when the expanded graphite is added to the polyisocyanate, the polyisocyanate is heated to 70 to 80 degrees Celsius, and when the expanded graphite is added to the polyamine, the polyamine is heated to 70 to 80 degrees Celsius, whereby a polyurea resin can be sprayed from the nozzle of a polyurea spraying device.

[0029] Furthermore, according to the fourth invention, when the polyurea resin composition of the first invention is sprayed onto an object, the temperature of the polyurea resin in the spray section is maintained at 60 to 80 degrees Celsius by the first heating means and the second heating means, and the pressure of the polyurea resin in the spray section is pressurized to a predetermined pressure by the first pressurizing means and the second pressurizing means, so that the heated / pressurized polyurea resin can be sprayed onto the object from the spray nozzle to form a polyurea resin layer of the desired thickness.

[0030] Furthermore, according to the fifth invention, the polyurea resin composition of the first invention can be sprayed onto an object using a conventional polyurea spraying device having an injection port diameter of 1.5 mm and a pressurizing capacity of 23.5 MPa to 24.0 MPa.

[0031] In addition, according to the sixth invention, when the expanded graphite is added to the polyisocyanate, the polyisocyanate is heated to 70 to 80 degrees Celsius, and when the expanded graphite is added to the polyamine, the polyamine is heated to 70 to 80 degrees Celsius, whereby a polyurea resin composition can be sprayed onto an object to form a polyurea resin layer of a desired thickness.

[0032] In addition, when expanded graphite is added to both the polyisocyanate and the polyamine, the temperatures of both the polyisocyanate and the polyamine can be adjusted to 70 to 80 degrees Celsius, and the polyurea resin composition can be sprayed onto an object to form a polyurea resin layer of the desired thickness. [Brief description of the drawings]

[0044] [Figure 1] FIG. 1 is a diagram showing a schematic configuration of a polyurea spraying device (spraying device) 100. As shown in FIG. [Diagram 2] FIG. 2 is a photograph showing a combustion experiment in which the noncombustible powder of the second embodiment is not added to the polyurea resin. [Diagram 3]FIG. 3 is a photograph showing a combustion experiment in which 15 parts by mass of noncombustible powder was added to 100 parts by mass of a base material made of a polyurea resin. [Figure 4] FIG. 4 is a photograph showing a combustion experiment in which 20 parts by mass of noncombustible powder was added to 100 parts by mass of a base material made of a polyurea resin. [Diagram 5] FIG. 2 is a photograph showing a combustion experiment in which 25 parts by mass of noncombustible powder was added to 100 parts by mass of a base material made of a polyurea resin. [Figure 6] FIG. 2 is a photograph showing a combustion experiment in which 30 parts by mass of noncombustible powder was added to 100 parts by mass of a base material made of a polyurea resin. [Figure 7] FIG. 2 is a photograph showing a combustion experiment in which 40 parts by mass of noncombustible powder was added to 100 parts by mass of a base material made of a polyurea resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0045] (First embodiment) Hereinafter, a description will be given of a polyurea resin having excellent flame retardancy (preferably having semi-fire resistance) according to the first embodiment, and a method for forming a polyurea resin layer using the same. The base material of the polyurea resin used in the first embodiment uses only polyisocyanate and polyamine as organic polymer compounds (pure polyurea resin). Pure polyurea resin, which uses only polyisocyanate and polyamine as organic polymer compounds, can exhibit excellent corrosion resistance, abrasion resistance, waterproofing, impact resistance, and elasticity by adding various fillers.

[0046] First, the "intrinsic properties" of pure polyurea resin will be described. The following "Table 1" shows the properties of the polyurea resin "Qtech-406" provided by Qingdao Shamu New Materials Co., Ltd. This "Qtech-406" has particularly high "waterproofing" properties due to the ingenuity of the filler added. [Table 1]

[0047] The following "Table 2" shows the properties of the polyurea resin "Qtech-417" provided by Qingdao Shamu New Materials Co., Ltd. This "Qtech-417" has particularly high "elasticity" due to the ingenuity of the filler added. [Table 2]

[0048] The following "Table 3" shows the properties of the polyurea resin "Qtech-420" provided by Qingdao Shamu New Materials Co., Ltd. This "Qtech-420" has particularly high "impact resistance" due to the ingenuity of the filler added. [Table 3]

[0049] However, these polyurea resins, like other organic polymer compounds, undergo thermal decomposition with increasing temperature to lower molecular weight and generate combustible gaseous products, and therefore are easily combusted in the event of a fire, etc. Therefore, they are not suitable for use in places where there is fire, in particular.

[0050] In order to impart flame retardancy to a polyurea resin, it is conceivable to use as a filler a flame retardant (e.g., ammonium polyphosphate, borax, expandable graphite, etc.) that has conventionally been used in other organic polymer compounds (e.g., polyurethane) (e.g., Non-Patent Document 1), but it is necessary to specifically consider what type of filler should be added and how it should be added in order to achieve flame retardancy without impairing the inherent properties of the above-mentioned polyurea resin.

[0051] Furthermore, since it is planned that polyurea resin will be applied to cracks in block walls and concrete walls, and to waterproof sheets on the roofs of buildings, it is necessary to specifically consider whether a flame-retardant (semi-fire-resistant) polyurea resin layer of the desired thickness (1.5 to 3 mm) can be formed on these block walls and other objects using a simple method (spraying method) that uses conventionally used polyurea spraying equipment.

[0052] In this embodiment, the polyurea resin composition to which flame retardancy (preferably, semi-fire resistance) is added is a pure polyurea resin that uses only polyisocyanate (Part A) and polyamine (Part B) as organic polymer compounds, with 100 to 160 parts by mass of polyisocyanate per 100 parts by mass of polyamine. It will be obvious to those skilled in the art that the optimum ratio of polyurea resin is 110 parts by mass of polyisocyanate to 100 parts by mass of polyamine.

[0053] The present inventors have confirmed that the inherent properties expected of polyurea resin (determined by the presence or absence of elasticity, which is a representative property) can be exhibited when the polyisocyanate is in the range of 100 to 160 parts by mass per 100 parts by mass of polyamine. [Table 4] If the polyisocyanate is used in an amount of 90 parts by mass per 100 parts by mass of polyamine, the desired elasticity cannot be obtained, and the inherent properties of the polyurea resin cannot be expected. Furthermore, even when 170 parts by mass of polyisocyanate is used per 100 parts by mass of polyamine, the desired elasticity is not obtained, and the inherent properties of the polyurea resin cannot be expected.

[0054] The required elasticity of polyurea resin (e.g., breaking elongation in Tables 1 to 3 above) varies depending on the intended use. In other words, the allowable elasticity varies depending on the intended use (e.g., sprayed concrete block walls, cracks in poured concrete, building rooftops, etc.) and the specifications required by the customer.

[0055] For this reason, the present inventors considered that, in light of common general technical knowledge, sufficient elasticity, etc. would be obtained for the above-mentioned applications, etc., if the polyurea resin (base material) is 100 to 160 parts by mass of polyisocyanate per 100 parts by mass of polyamine, as described above. With regard to waterproofing, no problems occurred with any of No. 1 to No. 5 in "Table 4."

[0056] In order to study how to impart flame retardancy (quasi-fire resistance) to this polyurea resin, the present inventor prepared a conventional filler (ammonium polyphosphate, borax, expanded graphite (80 mesh: 175 to 177 microns)) that has been proposed in the past, and added it to a composition with an optimal mixture ratio of 100 parts by mass of polyamine and 110 parts by mass of polyisocyanate. (1) Whether or not a polyurea resin layer can be easily formed on the target object using conventional methods (2) Whether the formed polyurea resin layer exhibits flame retardancy (quasi-fire resistance) or not was considered.

[0057] The results are as shown in Table 5 below. [Table 5]

[0058] As is clear from the above "Table 5", the polyurea resin composition to which 20 parts by mass of ammonium polyphosphate is added as a filler can be made flame-retardant compared to the one without the addition, but since it dissolves immediately upon combustion, the flame-retardant (quasi-fireproof) effect is quickly lost. However, it is possible to form a polyurea resin layer by a spraying method using a conventional polyurea spraying device.

[0059] A polyurea resin composition containing 20 parts by mass of borax (powder) as a filler can be made more flame-retardant than one containing no borax, but it dissolves quickly when burned, so the flame-retardant (quasi-fireproof) effect quickly disappears. However, it is possible to form a polyurea resin layer by a spraying method using a conventional polyurea spraying device. A polyurea resin composition to which 15 parts by mass of conventionally widely used expanded graphite (equivalent to 175 to 177 microns in 80 mesh) was added as a filler was able to achieve extremely excellent flame retardancy (semi-flame retardancy) compared to a composition to which the graphite was not added (confirmed by hand application here).

[0060] However, when attempting to form a polyurea resin layer containing added expanded graphite (80 mesh) by spraying it onto an object using a conventional polyurea spraying device, the polyurea resin generated inside the polyurea spraying device becomes highly pressurized, causing a problem in that the expanded graphite, which has a large particle size, adheres to the inside of the spray gun and the nozzle (approximately 1.5 mm) of the polyurea spraying device, resulting in clogging. This is because the particle size of the expanded graphite itself is large (80 mesh) and the viscosity of the polyurea resin increases due to the addition of expanded graphite.

[0061] Taking the above results ("Table 5") into consideration, the present inventors have determined that expandable graphite is the most preferable filler for imparting flame retardancy (quasi-fire resistance) to polyurea resin. The inventors then investigated how to prevent the problem that occurs when using expanded graphite, namely, clogging that can occur inside the polyurea spraying equipment (particularly the spray gun part), and to develop a polyurea resin composition that enables spraying work to be performed using conventional polyurea spraying equipment as is.

[0062] Here, a polyurea spraying device that has been conventionally used for forming a polyurea resin layer will be described. A known example of a conventional polyurea spraying device is the "Polyurea Sprayer" manufactured by Sham. The following "Table 6" shows the performance of the polyurea spraying equipment listed in the specifications for the Siamese Polyurea Sprayer (PHX-3). [Table 6]

[0063] FIG. 1 is a schematic diagram showing the configuration of a general polyurea spraying device 100 that has been conventionally used. The polyurea spraying device 100 includes a first tank 10 for storing polyisocyanate (agent A), a second tank 20 for storing polyamine (agent B), a compressor 40, and a spray gun device 50 for spraying a polyurea resin (polyurea resin composition) produced by mixing and stirring the polyisocyanate and polyamine onto an object.

[0064] The first tank 10 is connected to the spray gun device 50 by a first pipe 11 , and the second tank 20 is connected to the inside of the spray gun device 50 by a second pipe 21 .

[0065] A first pump 12 is provided in the first piping 11 between the first tank 10 and the spray gun device 50. In addition, a second pump 22 is provided in the second piping 21 between the second tank 20 and the spray gun device 50. The first pump 12 adjusts the pressure of the polyisocyanate supplied from the first tank 10 to the spray gun device 50 according to a control signal from a compression adjusting mechanism 30. The second pump 22 adjusts the pressure of the polyamine supplied from the second tank 20 to the spray gun device 50 according to a control signal from the compression adjusting mechanism 30. The compression adjustment mechanism 30 receives a command from the control unit 60 and outputs the control signal to each of the first pump 12 and the second pump 22 . By using the first pump 12 and the second pump 22, the maximum pressure in the spray gun device 50 can be adjusted to about 24 MPa (see Table 6).

[0066] The polyisocyanate and polyamine pressurized by the first pump 12 and the second pump 22, respectively, are mixed and stirred inside the spray gun device 50, and a polyurea resin is produced. The compressor 40 is in communication with the inside of the spray gun device 50 through a third pipe 41. Air compressed by the compressor 40 is supplied to the inside of the spray gun device 50.

[0067] A first heater 13 is disposed in the first pipe 11, and the temperature of the polyisocyanate supplied from the first tank 10 to the inside of the spray gun device 50 can be adjusted to a desired temperature (at least 60 degrees Celsius to 80 degrees Celsius). The temperature of the polyisocyanate heated by the first heater 13 is maintained by a hose heater 14 (maximum heating value is 88 degrees Celsius: see Table 6).

[0068] Further, a second heater 23 is disposed in the second pipe 21, and the temperature of the polyamine supplied from the second tank 20 to the inside of the spray gun device 50 can be adjusted to a desired temperature (60 degrees Celsius to 80 degrees Celsius). The temperature of the polyamine heated by the second heater 23 is maintained by a hose heater 24 (maximum heating value is 88 degrees Celsius: see "Table 6").

[0069] Based on the switching state of switch SW, the control unit 60 recognizes whether or not expanded graphite has been added to the isocyanate (agent A), whether or not expanded graphite has been added to the polyamine (agent B), the amount of expanded graphite added, etc., and based on this information, appropriately controls the pressure of the polyurea resin by the first pump 12 and the second pump 22, and the temperature of the polyurea resin by the first heater 13 and the second heater 23.

[0070] In this embodiment, expanded graphite (filler) with a particle size of 100 mesh is added to the polyisocyanate (Part A). For this reason, the temperature of the polyisocyanate is adjusted to 70° C. to 80° C. by the first heater 13. The polyamine to which no expanded graphite is added is adjusted to a lower temperature than the polyisocyanate (60° C. to 70° C.) by the second heater 23.

[0071] The reason for adjusting the temperature of the polyisocyanate to which the expanded graphite is added to be higher than that of the polyamine to which the expanded graphite is not added is to suppress the increase in viscosity due to the addition of the expanded graphite by increasing the temperature. At this time, the polyurea resin generated inside the spray gun device 50 is generally at a temperature between 60°C and 80°C.

[0072] If expanded graphite with a particle size of 100 mesh is added only to polyamine, the temperature of the polyamine may be set to 70° C. to 80° C., and the temperature of the polyisocyanate may be set to 60° C. to 70° C. In this case, the polyurea resin generated inside the spray gun device 50 will be generally between 60° C. and 80° C. In this way, by increasing only the temperature of the solvent (here, agent A), whose viscosity increases due to the addition of expanded graphite with a particle size of 100 mesh, the power required for heating can be reduced.

[0073] Furthermore, if expanded graphite is added to both the polyisocyanate (agent A) and the polyamine (agent B), the viscosity of both can be kept low by setting the temperatures of both the polyisocyanate and the polyamine to 70° C. to 80° C. In this case, the polyurea resin generated inside the spray gun device 50 will be at a temperature of approximately 70° C. to 80° C.

[0074] The polyisocyanate (agent A) pressurized by the first pump 12 and heated by the first heater 13, and the polyamine (agent B) pressurized by the second pump 22 and heated by the second heater 23 are both fed into the spray gun device 50 and mixed and stirred (impingement mixing), and a polyurea resin is produced by a chemical reaction.

[0075] The polyurethane resin produced by mixing and stirring inside the spray gun device 50 is mixed with compressed air supplied from the compressor 40, and by pulling the trigger 52B of the gun part 52, it is released from the nozzle 52A and sprayed in the form of a mist.

[0076] At this time, the polyurethane resin produced by mixing and stirring inside the spray gun device 50 is kept at a predetermined temperature (60 to 80 degrees Celsius) and has low viscosity, so that when the nozzle 52A (diameter 1.5 mm) is opened, it is sprayed at a desired flow rate (10 L / min in the first embodiment) (the polyurethane resin is at 23.5 to 24.0 MPa inside the spray gun device 50). At this time, the expanded graphite added has a small particle size, and the viscosity of the polyurea resin is low, so that clogging does not occur inside the spray gun device 50 (particularly, the injection port 52A).

[0077] In this way, in the polyurea spraying device 100, the polyisocyanate (part A) and polyamine (part B) can be heated and adjusted to the desired temperature inside the spray gun device 50, making it possible to stabilize the reaction conditions (resin reaction) between the polyisocyanate (part A) and polyamine (part B). In addition, by adjusting the temperature of the polyisocyanate (part A) or polyamine (part B) to which expanded graphite has been added to a high temperature, it is possible to prevent the viscosity from increasing due to the addition of expanded graphite.

[0078] Incidentally, if the ratio of expanded graphite added to polyisocyanate is the same, it is believed that the flame retardancy decreases in proportion to the reduction in particle size (100 mesh or smaller). Therefore, in order to achieve the same flame retardancy (quasi-fire resistance) as when conventional expanded graphite with a relatively large particle size (particle size of 80 mesh or more) is added (15 parts by mass of expanded graphite for 100 parts by mass of polyamine and 100 to 160 parts by mass of polyisocyanate = "Table 5"), it is necessary to increase the amount of expanded graphite added to compensate for the smaller particle size (30 parts by mass of expanded graphite for 100 parts by mass of polyamine and 100 to 160 parts by mass of polyisocyanate).

[0079] Increasing the amount of expanded graphite added in this way increases the viscosity of the polyurethane resin produced by mixing and stirring; however, in this embodiment, the polyurethane resin produced by mixing and stirring is adjusted to a high temperature (60 degrees Celsius to 80 degrees Celsius), so that the viscosity can be kept low and spraying from the spray gun device 50 of the polyurethane spraying device 100 is possible.

[0080] In addition, if it is acceptable to weaken the flame retardant (semi-fireproof) effect of the expanded graphite somewhat, the amount of expanded graphite added can be the same as when conventional expanded graphite with a large particle size is used (15 parts by mass of expanded graphite for 100 parts by mass of polyamine and 100 to 160 parts by mass of polyisocyanate).

[0081] When 15 parts by mass of conventionally used 80 mesh particle size expanded graphite is added to 100 parts by mass of polyamine and 100 to 160 parts by mass of polyisocyanate, the time until the polyurea resin is carbonized without generating a flame is 60 seconds (see Table 5). However, when the same amount (15 parts by mass) of 100 mesh expanded graphite is used, the time until the polyurea resin is carbonized without generating a flame is slightly shorter at about 30 seconds (see Table 7 below).

[0082] As described above, in this first embodiment, in order to enable the use of conventional polyurea spraying equipment (nozzle diameter 1.5 mm, pressure capacity 23.5 to 24.0 MPa, temperature adjustment possible up to 88 degrees Celsius = "Table 6") as is, the particle size of the expanded graphite added to the polyurea resin is made small (particle size 100 mesh), and the amount added is 15 to 30 parts by mass per 100 parts by mass of polyamine and 100 to 160 parts by mass of polyisocyanate. Polyurea resin produced by mixing and stirring polyisocyanate and polyamine is heated and maintained at 60° C. to 80° C. inside the spray gun device, and the polyurea resin can be sprayed onto an object to form a polyurea resin layer of a desired thickness. At this time, clogging does not occur in the polyurea spray device 100 (particularly, inside the spray gun device 50).

[0083] The present inventors confirmed the flame retardancy (quasi-fire resistance) of a polyurea resin layer of a predetermined thickness (here, 2 mm) formed on an object using polyurea resin (polyurea resin composition) to which expanded graphite with a particle size of 100 mesh was added (combustion experiment). The experimental results are shown in Table 7 below.

[0084] As mentioned above, the ratio of polyamine to polyisocyanate at which the inherent properties (elasticity) of polyurea are fully exhibited is 100 parts by mass of polyamine to 100 to 160 parts by mass of polyisocyanate, so a polyurea resin composition with the following ratio was prepared. (1) 100 parts by mass of polyamine, 100 parts by mass of polyisocyanate, 15 parts by mass of expanded graphite = (Sample 1) (2) 100 parts by mass of polyamine, 100 parts by mass of polyisocyanate, 30 parts by mass of expanded graphite = (Sample 2) (3) 100 parts by mass of polyamine, 160 parts by mass of polyisocyanate, 15 parts by mass of expanded graphite = (Sample 3) (4) 100 parts by mass of polyamine, 160 parts by mass of polyisocyanate, 30 parts by mass of expanded graphite = (Sample 4)

[0085] Each of the above polyurea resin compositions (samples 1 to 4) was formed on a target object (a 20 cm x 20 cm concrete plate) to a film thickness of about 2 mm, and this was left at room temperature (about 20°C) for 6 hours to be thoroughly dried. In this combustion experiment, since it was sufficient to confirm the flame retardancy (semi-fire resistance) of the polyurea resin when expanded graphite with a particle size of 100 mesh was added at a certain ratio (15 to 30 parts by mass of expanded graphite for 100 parts by mass of polyamine and 10 to 160 parts by mass of polyisocyanate), for convenience, a polyurea resin layer was formed by so-called "hand painting" and its flame retardancy (semi-fire resistance) was confirmed.

[0086] Concrete plates 1 to 4, each having a polyurethane resin layer (thickness: 2 mm) with different composition ratios (samples 1 to 4), were placed vertically, and their surfaces were burned with a commercially available torch burner. The tip of the flame of the torch burner was placed so as to be in contact with the concrete plate. The combustion time and combustion results of each of the concrete panels 1 to 4 are as shown in Table 7 below.

[0087] In order to confirm the flame retardancy (quasi-fire resistance) obtained in the first embodiment, a 20 cm x 20 cm concrete plate 5 was prepared by forming a 2 mm-thick layer of polyurea resin (sample 5) containing 80 mesh expanded graphite on the surface thereof. [Table 7]

[0088] As is clear from the experimental results in "Table 7", in both cases where the polyurea resin layer was formed using Sample 1 and Sample 2, in which 15 parts by mass and 30 parts by mass of expanded graphite (100 mesh) were added to the base material of the polyurea resin consisting of 100 parts by mass of polyamine and 100 parts by mass of polyisocyanate, respectively, no fire occurred until 30 to 60 seconds had elapsed. This was almost the same result as the experimental result (60 seconds) of Sample 5, in which 30 parts by mass of expanded graphite (80 mesh) was used as a filler.

[0089] In addition, in both cases where the polyurea resin layer was formed using Sample 3 and Sample 4, in which 15 parts by mass and 30 parts by mass of expanded graphite (100 mesh) were added to the base material of the polyurea resin consisting of 100 parts by mass of polyamine and 160 parts by mass of polyisocyanate, respectively, no fire occurred until 30 to 60 seconds had elapsed. This was almost the same as the experimental result (60 seconds) of Sample 5, in which 30 parts by mass of expanded graphite (80 mesh) was used as the filler.

[0090] Furthermore, there was no visible difference in the state of the sample surface after a certain period of combustion among Samples 1 to 4 and Sample 5. From these findings, it was found that even if the particle size of the expanded graphite was changed from the conventional 80 mesh (175 to 177 microns) to 100 mesh (147 to 149 microns), a polyurea resin layer with a thickness of approximately 2 mm was able to adequately withstand combustion for 30 to 60 seconds.

[0091] As described above, even when 15 to 30 parts by mass of 100 mesh expanded graphite was added as a filler to a polyurea resin base material consisting of 100 to 160 parts by mass of polyisocyanate per 100 parts by mass of polyamine (polyurea resin composition) and this was sprayed to form a polyurea resin layer, excellent flame retardancy (quasi-fire resistance) equivalent to that obtained when expanded graphite with a large particle size (particle size of 80 mesh or more) was used as a filler was obtained.

[0092] A polyurea resin (base material) containing 100 parts by mass of polyamine and 100 to 160 parts by mass of polyisocyanate to which 15 to 30 parts by mass of expanded graphite has been added is produced by mixing and stirring in a conventionally used polyurea spraying device 100. The produced polyurea resin is heated and adjusted to 60 to 80 degrees Celsius within the spray gun device 50 of the polyurea spraying device 100, so that its viscosity is kept low and it can be sufficiently sprayed onto the target object from the nozzle (diameter 1.5 mm). At this time, by adjusting the pressure of the polyurea resin inside the spray gun device 50 to 23.5 to 24.0 MPa, the amount of the resin sprayed from the nozzle 52A can be set to 10 L / min.

[0093] In addition, the smaller the amount of expanded graphite added, the less the risk of impairing the inherent properties of the formed polyurea resin layer, and the less expanded graphite is required, the lower the production cost can be. Therefore, depending on the purpose of use, by using 15 parts by mass of expanded graphite for 100 parts by mass of polyamine and 100 to 160 parts by mass of polyisocyanate, the formed polyurea resin layer can be imparted with non-flammability (quasi-fire resistance) and the production cost can be reduced.

[0094] In the first embodiment, the particle size of the expanded graphite is described as 100 mesh, but even if the particle size is smaller than 100 mesh, it is fully possible to spray the polyurea resin using the conventional polyurea spraying device 100. This is because if the particle size becomes smaller, there will be no risk of clogging in the polyurea spraying device 100 (particularly inside the spray gun device 50). If the viscosity increases due to the addition of expanded graphite, the temperature of the solution to which the expanded graphite has been added (agent A or agent B) can be adjusted even higher (for example, to nearly 88 degrees Celsius in the case of the polyurea spraying device in "Table 6").

[0095] When the particle size of the expanded graphite is made smaller in this way, it is possible to increase the amount added in order to achieve sufficient flame retardancy (quasi-fire resistance); in that case, by further increasing the adjustment temperature of the polyurea resin produced by mixing and stirring, it is possible to enable spraying from the spray gun device 50 while keeping the viscosity low.

[0096] In the above embodiment, an example in which expanded graphite having a particle size of 100 mesh is added to isocyanate has been mainly described, but it goes without saying that expanded graphite may be added only to polyamine, or may be added to both polyisocyanate and polyamine.

[0097] (Second embodiment) Next, a second embodiment of the present invention will be described with reference to FIGS. In this second embodiment, the non-combustible powder added to the base material consisting of polyamine and polyisocyanate (the same high purity base material as in the first embodiment is used in this second embodiment) contains at least the following: (A) Expanded graphite (grain size 100 mesh) (B) Brominated flame retardants (C) Melamine polyphosphate (D) Silica powder

[0098] The particle size of the expanded graphite is set to be smaller than 100 mesh so that a polyurea resin layer can be formed using the polyurea spraying device 100 of the first embodiment. Incidentally, by appropriately modifying the design of the spraying pressure, temperature adjustment, and size of the opening of the polyurea spraying device 100, it is also possible to make the particle size of the expanded graphite about 80 mesh.

[0099] The optimum ratios of the components (A) to (D) in the noncombustible powder are as follows: (A) Expanded graphite: 40 parts by mass (B) Brominated flame retardant: 80 parts by mass (C) Melamine polyphosphate: 80 parts by mass (D) Silica powder: 100 parts by mass

[0100] The amount (percentage) of such a "non-flammable powder" to be added to a polyurea resin base material (base material composition) consisting of polyamine and polyisocyanate varies depending on the level of "non-flammability (semi-fire resistance)" to be achieved in the polyurea resin layer actually formed by the spraying method.

[0101] Therefore, the inventors changed the ratio of the "non-combustible powder" added to the polyurea resin base material (polyamine and polyisocyanate) as shown below in (2) to (6), and conducted combustion experiments to confirm the degree to which "non-combustible property (quasi-fire resistance)" could be achieved at each ratio. In conducting the following combustion experiments, (A) the expanded graphite was "9510045 (-100mesh)" from Ito Graphite Industries, (B) the brominated flame retardant was "Fireguard (FG8500)" from Teijin Limited ("Fireguard" is a registered trademark of Teijin Limited), and (C) the melamine polyphosphate was "EXOLIT AP462" from Clariant Chemicals Japan Co., Ltd. ("EXOLIT" is a registered trademark of Clariant Produkte (Deutschland) Gesellschaft mit Beschlenkter Haftung). As for (D) silica powder, a commercially available common silica powder (fine silica dioxide, low melting point glass powder) was used. (1) 0% (Figure 2) (2) 15% (Figure 3) (3) 20% (Figure 4) (4) 25% (Figure 5) (5) 30% (Figure 6) (6) 40% (Figure 7)

[0102] In carrying out this combustion experiment, samples were prepared by forming a polyurethane resin layer of about 3 mm thickness on the surface of a 300 mm x 300 mm, 9 mm thick plywood board using a polyurethane resin (1) without the addition of non-combustible powder, and polyurethane resins (2) to (6) with the addition of non-combustible powder (Figs. 2 to 7). Note that, in the combustion experiment, the samples were prepared by so-called "hand painting", but the polyurethane resin layer formed by the "spraying method" using the polyurethane spraying device 100 has better uniformity of film quality than the polyurethane resin layer formed by "hand painting" which may cause unevenness, and is superior in the main properties of the polyurethane resin layer and in the non-combustibility (quasi-fire resistance) according to the present invention.

[0103] The results of a combustion experiment conducted for 120 seconds (2 minutes) using each of the samples (1) to (6) prepared above are shown in Figs. 2 to 7. In the combustion experiment, each sample (1) to (6) was placed vertically and a flame from a torch burner was applied vertically from a position 150 mm away from the combustion surface for 2 minutes (the burner temperature was approximately 1200 degrees).

[0104] In the case of (1) where the "noncombustible powder" according to the second embodiment is not added (0%), as shown in FIG. 2, discoloration begins in the area where the burner flame hits after 15 seconds, and smoke and dripping begin after 30 seconds. Dripping becomes more noticeable and there is more smoke after 60 seconds. Dripping becomes more intense after 1 minute 30 seconds, and the base of the plywood becomes visible, and the fire begins to spread after 1 minute 50 seconds.

[0105] In the case of (2), in which 15% "non-combustible powder" was added, as shown in Figure 3, 10 seconds after the start of combustion, the area where the burner flame hit began to swell, and at 30 seconds, the swelling increased and carbonization progressed, and dripping began due to the melting of the resin (during this time, a flame appeared momentarily, but it quickly went out and did not spread). At 60 seconds, the dripping became more noticeable and the flame grew larger (again, the fire did not spread). At 1 minute 20 seconds, the dripping became even more intense, and the base of the plywood began to become visible, and at 1 minute 30 seconds, the resin where the burner flame hit melted off and part of the plywood burned, but the polyurethane resin layer itself did not spread to the fire.

[0106] In the case of (3), in which 20% of the "non-combustible powder" was added, as shown in Figure 4, 10 seconds after the start of combustion, carbonization began at the point where the burner flame hit, and at 20 seconds, carbonization had progressed around that point, causing it to swell more (a flame appeared momentarily at this point, but quickly went out). Dripping began at 30 seconds, and at 60 seconds, the dripping became noticeable. At 1 minute 30 seconds, the dripping became even more noticeable, and the occasional flames became more noticeable (even in this case, the flames did not spread to the polyurea resin). At 2 minutes, the dripping became more intense, and the expansion due to carbonization of the burning surface also became more intense (the flames still did not spread). Sufficient non-combustibility (semi-fire resistance) was achieved throughout.

[0107] In the case of (4), in which 25% "non-combustible powder" was added, as shown in Figure 5, 10 seconds after the start of combustion, the area where the burner flame hit changed color (carbonization had barely begun), and 30 seconds later, carbonization became noticeable (a flame appeared for a moment, but quickly disappeared, and there was no dripping). The condition remained almost unchanged from 30 to 60 seconds. Although dripping became noticeable at 1 minute 30 seconds, there was no significant change in the burning surface (the area where the burner flame hit). There was no significant change from 1 minute 30 seconds to 2 minutes, with the burning surface merely expanding. Although dripping of the resin occurred throughout the experiment, sufficient non-combustibility (semi-fire resistance) was obtained, even compared to the case of (3).

[0108] In the case of (5), in which 30% "noncombustible powder" was added, as shown in Figure 6, 10 seconds after the start of combustion, there was a slight discoloration, mainly in the area where the burner flame hit (carbonization had barely begun). Up until 30 seconds, there was almost no change, and carbonization only progressed slightly. At 60 seconds, carbonization became noticeable (a flame appeared for a moment, but quickly went out, and no dripping occurred). At 1 minute 30 seconds, a large flame appeared for a moment, but quickly went out and did not spread. After 1 minute 30 seconds, even after 2 minutes had passed, there was no dripping, and there was almost no change in the burning surface (the area where the burner flame hit).

[0109] In the case of (6), in which 40% of the “noncombustible powder” was added, the results were almost the same as when 30% was added as mentioned above, except that the discoloration of the burning surface and the spread of carbonization were slightly narrower than when 30% was added. In this way, in both cases where the non-combustible powder was used at 30% or 40% to the base material (base material composition) of the polyurea resin made of polyisocyanate and polyamine, no noticeable flames or smoke were generated during the combustion test lasting at least two minutes, and extremely excellent non-combustibility (quasi-fire resistance) was achieved. Moreover, the area discolored and carbonized by the burner flame did not spread much over time, and no resin dripping occurred.

[0110] In view of the above, if the objective is simply to prevent the polyurea resin itself from burning during combustion, the amount of "non-combustible powder" added may be approximately 15 parts by mass (15%) per 100 parts by mass of the polyurea resin base material. Furthermore, if one wishes to achieve non-combustibility (semi-fire resistance) sufficient to prevent the spread of flames in the polyurea resin layer for a certain period of time or longer, it is understood that the amount of "non-combustible powder" added should be approximately 20 parts by mass (20%) per 100 parts by mass of the polyurea resin base material. Furthermore, if you wish to achieve non-flammability (semi-fire resistance) that not only prevents the "spread of flames" but also suppresses carbonization and expansion of the burning surface and also suppresses dripping, the amount of "non-flammable powder" to be added should be approximately 25 parts by mass (25%) per 100 parts by mass of polyurea resin (base material).

[0111] Furthermore, if one wishes to prevent the "spread of flames," suppress the carbonization and expansion of the burning surface, and achieve a level of non-combustibility (quasi-fire resistance) that does not cause dripping, the amount of "non-combustible powder" added should be 30 parts by mass (30%) per 100 parts by mass of polyurea resin (base material). In this case, throughout a two-minute combustion experiment, the polyurea resin layer shows almost no deformation during combustion. In addition, when 40% non-combustible powder is added, there is no difference in non-combustibility (quasi-fire resistance) between the case where 40% is added and the case where 30% is added. Therefore, in order to maintain the inherent properties of the polyurea resin, impurities should be reduced as much as possible, and further, in consideration of reducing the cost of forming the polyurea resin layer, adding 30% non-combustible powder is sufficient.

[0112] When actually spraying the non-flammable (semi-fireproof) polyurethane resin described above onto an object, the polyurethane spraying device 100 of the first embodiment can be used (FIG. 1). This is because the "expanded graphite" added to the "noncombustible powder" in the second embodiment is 100 mesh.

[0113] The following method is used to spray a polyurea resin (polyurea resin composition) containing "noncombustible powder" onto an object using the polyurea spraying device (spraying device) 100. Note that the configuration and operation of the polyurea spraying device 100 are explained in the first embodiment, and therefore detailed explanations thereof will be omitted in this second embodiment. (1) First, a desired amount of nonflammable powder (15% to 40% in this embodiment) is added to at least one of polyamine and polyisocyanate. (2) The polyamine and polyisocyanate are mixed and stirred to produce a polyurea resin, which is then heated to a temperature between 60°C and 80°C. (3) The polyamine and polyisocyanate are mixed and stirred to produce a polyurea resin, which is then pressurized to a predetermined pressure. (4) The polyurethane resin, which has been heated to 60 to 80 degrees Celsius and pressurized to a predetermined pressure, is sprayed onto an object.

[0114] In this case, when the polyamine and polyisocyanate are heated, if a non-flammable powder is added to the polyisocyanate, the polyisocyanate is heated to 70 to 80 degrees Celsius. On the other hand, when noncombustible powder is added to the polyamine, the polyamine is heated to 70° C. to 80° C. The heating is performed by heaters 13 and 23 provided in the polyurea spraying device 100.

[0115] As described above, this polyurea spraying device 100 has a nozzle diameter of 1.5 mm and the specified pressure is 23.5 MPa to 24.0 MPa, so that even if a noncombustible powder containing expanded graphite with a particle size of 100 mesh (or smaller) is added to the polyurea resin base material (base material composition), the polyurea spraying device 100 can be used to form a uniform polyurea resin layer on the target object.

[0116] In addition, according to the polyurea spraying device 100, when a non-combustible powder is added to a polyisocyanate, the viscosity of the polyisocyanate can be kept low by heating the polyisocyanate to 70 to 80 degrees Celsius, and when a non-combustible powder is added to a polyamine, the viscosity of the polyamine can be kept low by heating the polyamine to 70 to 80 degrees Celsius. Therefore, the viscosity of the polyurea resin (polyurea resin composition) as a whole can be reduced, and even if a "non-combustible powder" containing expanded graphite with a particle size of 100 mesh (or a particle size smaller than this) is added to the base material of the polyurea resin, the polyurea resin (polyurea resin composition) can be uniformly sprayed onto the target object to form the polyurea resin. The polyurea resin layer formed by uniform spraying achieves excellent non-combustibility (quasi-fire resistance) without impairing the inherent properties of the polyurea resin.

[0117] Furthermore, the spraying method using this polyurethane spraying device 100 can efficiently form a polyurethane resin layer as needed at the work site where the target object is located, dramatically improving the efficiency of the formation / installation work of a non-flammable (semi-fireproof) polyurethane resin layer. [Explanation of symbols]

[0118] 10. First Tank 11 First Pipe 12 First pump (first pressurizing means) 13 First heating device (first heating means) 14,24 Hose heater 20 Second Tank 21 Second Pipe 22 Second pump (second pressurizing means) 23 Second heating device (second heating means) 30 Compression adjustment mechanism 40 Compressor (compression means) 41 Third Pipe 50 Spray gun device (generation means, injection means) 52 Gun Club 52A injection port 52B Trigger 60 Control section SW Switch

Claims

1. A polyurea resin composition comprising 100 parts by mass of polyamine, 100 to 160 parts by mass of polyisocyanate, and 15 to 30 parts by mass of expanded graphite, wherein the particle size of the expanded graphite is 100 mesh or smaller.

2. A method for forming a polyurea resin layer by spraying the polyurea resin composition according to claim 1 onto an object to form a polyurea resin layer having a desired thickness, comprising the steps of: adding the expanded graphite to at least one of a polyamine and a polyisocyanate; a step of heating the polyamine and the polyisocyanate so that the temperature of the polyurea resin produced by mixing and stirring the polyamine and the polyisocyanate is between 60 degrees Celsius and 80 degrees Celsius; a step of pressurizing the polyamine and the polyisocyanate so that a pressure of a polyurea resin produced by mixing and stirring the polyamine and the polyisocyanate becomes a predetermined pressure; A method for forming a polyurea resin layer, comprising the steps of: heating the polyurea resin to 60 degrees Celsius to 80 degrees Celsius and pressurizing it to the predetermined pressure, and spraying the polyurea resin onto an object.

3. 3. The method for forming a polyurea resin layer according to claim 2, characterized in that in the step of heating the polyamine and the polyisocyanate, when the expanded graphite is added to the polyisocyanate, the polyisocyanate is heated to 70 to 80 degrees Celsius, and when the expanded graphite is added to the polyamine, the polyamine is heated to 70 to 80 degrees Celsius.

4. 2. A method for forming a polyurea resin layer by spraying the polyurea resin composition according to claim 1 onto an object using a polyurea spraying device including: a first tank for storing a polyisocyanate; a second tank for storing a polyamine; a first heating means for adjusting the temperature of the polyisocyanate supplied from the first tank; a second heating means for adjusting the temperature of the polyamine supplied from the second tank; a first pressurizing means for pressurizing the polyisocyanate supplied from the first tank; a second pressurizing means for pressurizing the polyamine supplied from the second tank; a compression means for compressing a gas; a generating means for mixing and stirring the polyisocyanate and the polyamine to generate a polyurea resin; and a spraying means having a spray nozzle and spraying the generated polyurea resin from the spray nozzle, The temperature of the polyurethane resin in the injection means is maintained at 60° C. to 80° C. by the first heating means and the second heating means; The pressure of the polyurethane resin in the injection means is increased to a predetermined pressure by the first pressurizing means and the second pressurizing means; The method for forming a polyurea resin layer comprises spraying the pressurized polyurea resin from the nozzle onto an object to form a polyurea resin layer.

5. 5. The method for forming a polyurea resin layer according to claim 4, wherein the diameter of the injection port is 1.5 mm, and the predetermined pressure is 23.5 MPa to 24.0 MPa.

6. the first heating means heats the polyisocyanate to 70° C. to 80° C. when the expanded graphite is added to the polyisocyanate; The method for forming a polyurea resin layer according to claim 4 or claim 5, characterized in that the second heating means heats the polyamine to 70 to 80 degrees Celsius when the expanded graphite is added to the polyamine.

Citation Information

Patent Citations

  • Polyurea expanding type fireproof paint as well as preparation method and application thereof

    CN102559022A

  • Corrosion-proof execution method for concrete

    JP1996238453A

  • Flame-retardant auxiliary comprising polyamine- polyisocyanate cross-linked product, flame-retardant composition and flame-retardant resin composition compounded with the same

    JP2001106926A

  • Mixed polycycloaliphatic amine (MPCA) and mpca alkylate

    JP2010047757A

  • Fire resistant construction and method of manufacturing the same, and fire resistant composition