Resin composition for plating and plated molded product
A resin composition with polycarbonate, graft copolymer, and phosphate ester addresses the balance of heat resistance, fluidity, and adhesion strength in plating, enhancing performance in vehicle parts.
Patent Information
- Application Number
- JP2020119185
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-10
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-07-10
AI Technical Summary
Existing resin compositions for plating, particularly those based on PC alloy resin, face challenges in achieving a balance between heat resistance, fluidity, and plating adhesion strength, especially in large and thin vehicle parts, with previous solutions either compromising on heat resistance or failing to optimize fluidity and adhesion.
A resin composition comprising specific amounts of polycarbonate resin, graft copolymer, and phosphate ester, with a balanced content of 40-70% polycarbonate resin, 8-20% rubbery polymer, and 0.5-5% phosphate ester, along with optional additives, to enhance heat resistance, fluidity, and plating adhesion strength.
The composition achieves an excellent balance of heat resistance, fluidity, and plating adhesion strength, suitable for large and thin vehicle parts, by optimizing the resin components and their proportions.
Smart Images

Figure 0007566515000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition for plating that exhibits an excellent balance of heat resistance, fluidity and plating adhesion strength, and to a plated molded article. [Background technology]
[0002] Compositions consisting of polycarbonate resin and rubber-reinforced styrene resin (hereinafter referred to as PC alloy resin) are excellent in impact resistance, heat resistance, and moldability, and are therefore used in a variety of applications, including vehicle parts, home appliances, and office equipment parts. In particular, vehicle parts tend to become larger and have more complex designs. In addition, in order to reduce vehicle weight, there is a trend toward thinner molded product designs, so materials with excellent moldability, impact resistance, and heat resistance are required. PC alloy resin is often used as one of the options.
[0003] In addition, in these applications, decorative plating is often applied to PC alloy resin for parts that require a metallic appearance and lightweight design. Methods for plating PC alloy resin include the so-called catalyst-accelerator method, which consists of processes such as degreasing, chemical etching, neutralization, catalyst application, activation, electroless plating, acid activation, and electroplating, as well as a direct plating method that omits the electroless plating bath.
[0004] For example, Patent Document 1 discloses a flame-retardant resin composition for plating substrates, which has good impact resistance, moldability, and plating performance. However, although the moldability and thermal cycle properties are good, the heat resistance of the resin composition tends to decrease because a large amount of a phosphate ester-based flame retardant needs to be added.
[0005] Furthermore, Patent Document 2 proposes a thermoplastic resin composition having improved fluidity without impairing plating ability and impact resistance. However, the balance of heat resistance, fluidity, and plating adhesion strength required for large and thin-walled vehicle parts and the like is still not satisfactory. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2003-147154 A
[0007] [Patent Document 2] JP 2009-292921 A Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to provide a resin composition for plating and a plated molded article which are excellent in balance between heat resistance, fluidity and plating adhesion strength. [Means for solving the problem]
[0009] As a result of extensive investigations, the present inventors have found that the above problems can be solved by containing specific amounts of a polycarbonate resin, a graft copolymer, a copolymer, and a phosphate ester, and have thus completed the present invention.
[0010] That is, the present invention comprises the following [1] to [3]. [1] A resin composition for plating comprising: a polycarbonate resin (A); a graft copolymer (B) obtained by graft polymerization of a rubber polymer (b-1) and a monomer component (b-2) containing at least one selected from an aromatic vinyl monomer, a vinyl cyanide monomer, and a (meth)acrylic acid ester monomer; a copolymer (C) obtained by polymerization of a monomer component containing an aromatic vinyl monomer and a vinyl cyanide monomer; and a phosphoric acid ester (D), wherein the polycarbonate resin (A) is 40 to 70 mass%, the rubber polymer (b-1) is 8 to 20 mass%, and the phosphoric acid ester (D) is more than 0 mass% and less than 5 mass% (the total of (A) + (B) + (C) + (D) is 100 mass%). [2] A resin composition for plating use, characterized in that the phosphoric acid ester (D) according to [1] is present in an amount of 0.5% by mass or more and less than 4% by mass. [3] A plated molded product having a plating film on a molded product made of the resin composition for plating according to [1] or [2]. Effect of the Invention
[0011] The present invention can provide a resin composition for plating and a plated molded article that are excellent in balance between heat resistance, fluidity, and plating adhesion strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below.
[0013] The resin composition for plating use of the present invention contains a polycarbonate resin (A), a graft copolymer (B), a copolymer (C), and a phosphoric acid ester (D).
[0014] The polycarbonate resin (A) is a polymer obtained by the phosgene process in which various dihydroxydiaryl compounds are reacted with phosgene, or the ester exchange process in which a dihydroxydiaryl compound is reacted with a carbonate ester such as diphenyl carbonate. A representative example is a polycarbonate resin produced from 2,2-bis(4-hydroxyphenyl)propane, or "bisphenol A."
[0015] Examples of the dihydroxydiaryl compound include, in addition to bisphenol A, bis(hydroxyaryl)alkanes such as bis(4-hydroxydiphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)octane, bis(4-hydroxyphenyl)diphenylmethane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 1,1-bis(4-hydroxy-3-tert-butylphenyl)propane, 2,2-bis(4-hydroxy-3-bromophenyl)propane, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, and 2,2-bis(4-hydroxy-3,5-dichlorophenyl)propane; bis(hydroxyaryl)cycloalkanes such as 1,1-bis(4-hydroxyphenyl)cyclohexane, dihydroxydiaryl ethers such as 4,4'-dihydroxydiphenyl ether and 4,4'-dihydroxy-3,3'-dimethyldiphenyl ether, dihydroxydiaryl sulfides such as 4,4'-dihydroxydiphenyl sulfide and 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfide, dihydroxydiaryl sulfoxides such as 4,4'-dihydroxydiphenyl sulfone, and dihydroxydiaryl sulfones such as 4,4'-dihydroxydiphenyl sulfone.
[0016] These may be used alone or in combination of two or more. In addition to these, piperazine, dipiperidylhydroquinone, resorcin, 4,4'-dihydroxydiphenyls, etc. may also be mixed.
[0017] Furthermore, the above dihydroxydiaryl compound may be mixed with a trivalent or higher phenolic compound as shown below. Examples of trivalent or higher phenolic compounds include phloroglucinol, 4,6-dimethyl-2,4,6-tri-(4-hydroxyphenyl)-heptene, 4,6-dimethyl-2,4,6-tri-(4-hydroxyphenyl)-heptane, 1,3,5-tri-(4-hydroxyphenyl)benzene, 1,1,1-tri-(4-hydroxyphenyl)ethane, and 2,2-bis-[4,4-bis(4-hydroxyphenyl)cyclohexyl]propane. In addition, when producing these polycarbonate resins, the weight average molecular weight of the polycarbonate resin is usually 10,000 to 80,000, and preferably 15,000 to 60,000. A molecular weight regulator, a catalyst, and the like can be used as necessary. In addition, the weight average molecular weight can be measured by gel permeation chromatography (GPC) using polystyrene as a standard substance.
[0018] The graft copolymer (B) is obtained by graft polymerizing a rubber polymer (b-1) with a monomer component (b-2) containing at least one monomer selected from an aromatic vinyl monomer, a vinyl cyanide monomer, and a (meth)acrylic acid ester monomer.
[0019] The rubbery polymer (b-1) constituting the graft copolymer (B) is not particularly limited, and one or more of conjugated diene rubbers such as polybutadiene rubber, styrene-butadiene rubber (SBR), and acrylonitrile-butadiene rubber (NBR) obtained by a known polymerization method, ethylene-propylene rubbers such as ethylene-propylene-non-conjugated diene (ethylidene norbornene, dicyclopentadiene, etc.) rubbers, acrylic rubbers such as polybutyl acrylate rubber, and silicone rubbers can be used. The acrylic rubbers also include rubbers having a multilayer structure. Examples of rubbers having a multilayer structure include conjugated diene rubber / acrylic rubber, silicone rubber / acrylic rubber, and hard polymer (glass transition temperature of 20° C. or higher) / acrylic rubber. Examples of the hard polymer (having a glass transition temperature of 20° C. or higher) include a polymer obtained by polymerizing a monomer containing one or more selected from an aromatic vinyl monomer, a vinyl cyanide monomer, and a (meth)acrylic acid ester monomer. Among the above, polybutadiene rubber, styrene-butadiene rubber, ethylene-propylene-diene rubber, conjugated diene rubber / acrylic rubber, silicone rubber / acrylic rubber, and hard polymer (having a glass transition temperature of 20° C. or higher) / acrylic rubber are preferred, and polybutadiene rubber and styrene-butadiene rubber are more preferred. The glass transition temperature of the hard polymer can be calculated by the FOX formula.
[0020] The mass average particle size of the rubbery polymer (b-1) is not particularly limited, but is preferably 0.1 to 2.0 μm, more preferably 0.15 to 1.0 μm, from the viewpoints of impact resistance and plating adhesion strength. It can also be adjusted by agglomerating and enlarging a rubbery polymer having a mass average particle size of 0.05 to 0.3 μm.
[0021] Examples of the aromatic vinyl monomer of the monomer component (b-2) include styrene, α-methylstyrene, paramethylstyrene, bromostyrene, etc., and one or more of them can be used.
[0022] Examples of the vinyl cyanide monomer of the monomer component (b-2) include acrylonitrile, methacrylonitrile, ethacrylonitrile, fumaronitrile, etc., and one or more of them can be used.
[0023] Examples of the (meth)acrylic acid ester monomer of the monomer component (b-2) include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl acrylate, phenyl (meth)acrylate, 4-t-butylphenyl (meth)acrylate, (di)bromophenyl (meth)acrylate, and chlorophenyl (meth)acrylate, and one or more of these may be used.
[0024] The monomer component (b-2) may contain other monomers copolymerizable with the aromatic vinyl monomer, the vinyl cyanide monomer, and the (meth)acrylic acid ester monomer. Examples of such monomers include maleimide monomers, amide monomers, unsaturated carboxylic acid monomers, and polyfunctional monomers, and one or more of these may be used.
[0025] Examples of the maleimide monomer include N-phenylmaleimide and N-cyclohexylmaleimide.
[0026] Examples of the amide monomer include acrylamide and methacrylamide.
[0027] Examples of the unsaturated carboxylic acid monomer include (meth)acrylic acid, 2-ethylacrylic acid, maleic acid, fumaric acid, itaconic acid, and crotonic acid.
[0028] Examples of the polyfunctional monomer include divinylbenzene, allyl (meth)acrylate, ethylene glycol di(meth)acrylate, diallyl phthalate, dicyclopentadiene di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol hexa(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, triallyl cyanurate, and triallyl isocyanurate.
[0029] The composition ratio of the above monomers to be graft-polymerized to the rubber-like polymer (b-1) is not particularly limited, but is preferably 50-90 mass% aromatic vinyl monomer, 10-50 mass% cyanide vinyl monomer, and 0-40 mass% other copolymerizable monomers, 0-50 mass% aromatic vinyl monomer, 50-100 mass% (meth)acrylic acid ester monomer, and 0-50 mass% other copolymerizable vinyl monomer, or 20-70 mass% aromatic vinyl monomer, 20-70 mass% (meth)acrylic acid ester monomer, 10-60 mass% cyanide vinyl monomer, and 0-50 mass% other copolymerizable monomer (the total amount of monomers to be graft-polymerized to the rubber-like polymer is taken as 100 mass%).
[0030] The content of the rubber polymer (b-1) in the graft copolymer (B) is preferably from 20 to 80% by mass, more preferably from 40 to 70% by mass, in view of the balance of physical properties such as impact resistance and flowability.
[0031] The graft ratio of the graft copolymer (B) and the reduced viscosity of the acetone soluble portion are not particularly limited, but from the viewpoint of the balance of physical properties such as impact resistance and fluidity, the graft ratio is preferably 20 to 150%, more preferably 30 to 100%, and particularly preferably 36 to 75%. The reduced viscosity of the acetone soluble portion is preferably 0.2 to 1.5 dl / g, and more preferably 0.3 to 1.0 dl / g.
[0032] The graft ratio and the reduced viscosity of the acetone soluble matter can be determined as follows.
[0033] Separation method Approximately 2 g of graft copolymer (B) and 60 ml of acetone were placed in an Erlenmeyer flask and left to soak for 24 hours. The mixture was then centrifuged at 15,000 rpm for 30 minutes in a centrifuge to separate the soluble and insoluble portions. The insoluble portion was obtained by drying overnight at room temperature using a vacuum dryer. The soluble portion was obtained by precipitating the acetone-soluble portion in methanol and drying overnight at room temperature using a vacuum dryer. Grafting rate Graft rate (%) = (X-Y) / Y x 100 X: Amount of acetone insoluble matter after vacuum drying (g) Y: Amount of rubber polymer in the graft copolymer (g) Reduced viscosity of acetone soluble matter (dl / g) The acetone soluble portion is dissolved in N,N-dimethylformamide to give a solution with a concentration of 0.4 g / 100 ml, and the reduced viscosity is calculated from the flow time measured at 30°C using a Cannon-Fenske type viscometer.
[0034] The graft copolymer (B) obtained as described above usually mainly contains a grafted polymer (B1 component) in which a monomer component containing a monomer component (b-2) is grafted to a rubber polymer (b-1), and also contains a copolymer (referred to as B2 component) in which a monomer component containing a monomer component (b-2) that is not grafted to the rubber polymer (b-1) is copolymerized. Therefore, in the present invention, when the B2 component contained in the graft copolymer (B) satisfies the monomer component constituting the copolymer (C), it means that the copolymer (C) is contained.
[0035] The copolymer (C) is obtained by polymerizing a monomer component containing an aromatic vinyl monomer and a vinyl cyanide monomer.
[0036] Examples of the aromatic vinyl monomer constituting the copolymer (C) include styrene, α-methylstyrene, paramethylstyrene, bromostyrene, etc., and one or more of them can be used.
[0037] Examples of the vinyl cyanide monomer constituting the copolymer (C) include acrylonitrile, methacrylonitrile, ethacrylonitrile, fumaronitrile, etc., and one or more of them can be used.
[0038] Furthermore, the copolymer (C) may contain other monomers copolymerizable with the aromatic vinyl monomer and the vinyl cyanide monomer, such as (meth)acrylic acid ester monomers, maleimide monomers, amide monomers, unsaturated carboxylic acid monomers, polyfunctional monomers, etc., and one or more of these monomers may be used. As these monomers, the same ones as the above-mentioned monomer component (b-2) may be used.
[0039] The composition ratio of the monomers constituting the copolymer (C) is not particularly limited, but examples thereof include a composition ratio of 50-90 mass% aromatic vinyl monomer, 10-50 mass% cyanide vinyl monomer, and 0-40 mass% other copolymerizable monomers, and a composition ratio of 20-70 mass% aromatic vinyl monomer, 10-60 mass% cyanide vinyl monomer, 20-70 mass% (meth)acrylic acid ester monomer, and 0-50 mass% other copolymerizable monomers. Among these, it is preferable that the content of the cyanide vinyl monomer constituting the copolymer (C) is 25-40 mass% in terms of plating deposition properties.
[0040] The reduced viscosity of the copolymer (C) is not particularly limited, but from the viewpoint of the balance of physical properties such as impact resistance and fluidity, it is preferably 0.2 to 1.5 dl / g, and more preferably 0.3 to 1.0 dl / g.
[0041] The reduced viscosity can be calculated by the following formula.
[0042] Copolymer (C) is dissolved in N,N-dimethylformamide to give a solution with a concentration of 0.4 g / 100 ml, and the reduced viscosity is determined from the flow time measured at 30° C. using a Cannon-Fenske viscometer.
[0043] The polymerization method for the graft copolymer (B) and copolymer (C) constituting the above-mentioned resin composition for plating is not particularly limited, and they can be produced, for example, by emulsion polymerization, suspension polymerization, solution polymerization, bulk polymerization, or a combination of these.
[0044] The phosphoric acid ester (D) refers to an ester compound of phosphoric acid and an alcohol compound or a phenol compound.
[0045] Specific examples of phosphoric acid esters include trimethyl phosphate, triethyl phosphate, tributyl phosphate, tri(2-ethylhexyl)phosphate, tributoxyethyl phosphate, triphenyl phosphate, tricresyl phosphate, trixylenyl phosphate, tris(isopropylphenyl)phosphate, tris(phenylphenyl)phosphate, trinaphthyl phosphate, cresyl diphenyl phosphate, xylenyl diphenyl phosphate, diphenyl(2-ethylhexyl)phosphate, di(isopropylphenyl)phenyl phosphate, monoisodecyl phosphate, 2-acryloyloxyethyl acid phosphate, 2- Examples of the condensed phosphate esters include methacryloyloxyethyl acid phosphate, diphenyl-2-acryloyloxyethyl phosphate, diphenyl-2-methacryloyloxyethyl phosphate, melamine phosphate, dimelamine phosphate, melamine pyrophosphate, triphenylphosphine oxide, tricresylphosphine oxide, diphenyl methanephosphonate, diethyl phenylphosphonate, resorcinol polyphenyl phosphate, resorcinol poly(di-2,6-xylyl)phosphate, bisphenol A polycresyl phosphate, hydroquinone poly(2,6-xylyl)phosphate, and condensates thereof. Examples of the condensed phosphate esters include resorcinol bis(di-2,6-xylyl)phosphate, resorcinol bis(diphenyl phosphate), bisphenol A bis(diphenyl phosphate), etc. Commercially available products of resorcinol bis(di-2,6-xylyl)phosphate include PX-200 (manufactured by Daihachi Chemical Industry Co., Ltd.) and Adeka STAB FP-500 (manufactured by ADEKA Corporation). Commercially available products of resorcinol bis(diphenyl phosphate) include CR-733S (manufactured by Daihachi Chemical Industry Co., Ltd.) and Phylorflex RDP (manufactured by ICL JAPAN Co., Ltd.). Commercially available products of bisphenol A bis(diphenyl phosphate) include CR-741 (manufactured by Daihachi Chemical Industry Co., Ltd.), Leophos BAPP (manufactured by Ajinomoto Fine-Techno Co., Ltd.), and Adeka STAB FP-600 (manufactured by ADEKA Corporation).Among these, resorcinol bis(di-2,6-xylyl) phosphate and bisphenol A bis(diphenyl phosphate) are preferably used because of their excellent hydrolysis resistance, heat resistance, and low volatility.
[0046] The content of the polycarbonate resin (A) constituting the resin composition for plating of the present invention must be 40 to 70 mass%, preferably 42 to 68 mass%, and more preferably 45 to 65 mass% (the total of (A)+(B)+(C)+(D) being 100 mass%). By adjusting it within the above range, it is possible to improve the balance of impact resistance, fluidity, and plating adhesion strength.
[0047] The content of the rubbery polymer (b-1) constituting the resin composition for plating of the present invention must be 8 to 20 mass%, preferably 9 to 18 mass%, and more preferably 10 to 15 mass% (the total of (A)+(B)+(C)+(D) being 100 mass%). By adjusting it to the above range, plating adhesion strength can be improved.
[0048] The content of the phosphoric acid ester (D) constituting the resin composition for plating of the present invention must be more than 0% by mass and less than 5% by mass, preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 1.5% by mass or more. Also, it is preferably less than 4% by mass, more preferably 3.5% by mass or less, and even more preferably 3% by mass or less (the total of (A)+(B)+(C)+(D) being 100% by mass). By adjusting it to the above range, the balance of fluidity, heat resistance, and plating adhesion strength can be improved.
[0049] The resin composition for plating of the present invention may also contain other thermoplastic resins within the range that does not impair the effects of the present invention. Examples of such other thermoplastic resins include acrylic resins such as polymethyl methacrylate, polyolefin resins such as polyethylene and polypropylene, polyester resins such as polybutylene terephthalate resin, polyethylene terephthalate resin and polylactic acid resin, polyamide resins, and polyimide resins.
[0050] Furthermore, the plating resin composition of the present invention may contain, within the scope of not impairing the effects of the present invention, a hindered amine-based light stabilizer, an antioxidant such as a hindered phenol-based, sulfur-containing organic compound-based, or phosphorus-containing organic compound-based, a heat stabilizer such as a phenol-based or acrylate-based, an ultraviolet absorber such as a benzoate-based, benzotriazole-based, benzophenone-based, or salicylate-based, an organic nickel-based, or higher fatty acid amide-based lubricant, a flame retardant or flame retardant assistant such as polybromophenyl ether, tetrabromobisphenol-A, brominated epoxy oligomer, brominated or other halogen-containing compound, or antimony trioxide, an odor masking agent, a pigment such as carbon black or titanium oxide, or a dye, etc. Furthermore, a reinforcing agent or filler such as talc, calcium carbonate, aluminum hydroxide, glass fiber, glass flake, glass beads, glass wool, carbon fiber, or metal fiber may also be added.
[0051] The plating resin composition of the present invention can be obtained by melt-kneading the above-mentioned components. For melt-kneading, a known kneading machine such as a roll, a Banbury mixer, a single-screw extruder, a multi-screw extruder, or a kneader can be used.
[0052] The thus obtained resin composition for plating is molded by injection molding, extrusion molding, compression molding, injection compression molding, blow molding or the like, and the obtained molded product can be plated by a known plating method, for example, under the same plating conditions as those for ordinary ABS resin. EXAMPLES
[0053] The present invention will be described in detail below using examples, but the present invention is not limited to these examples. In the examples, parts and percentages are based on mass. In each of the examples and comparative examples, various physical properties were measured by the following methods.
[0054] Charpy impact strength (NC) Using the pellets obtained in each of the Examples and Comparative Examples, various test pieces were molded in accordance with ISO test method 294, and the notched Charpy impact values were measured at a thickness of 4 mm in accordance with ISO test method 179. Unit: kJ / m 2
[0055] Melt Volume Flow Rate (MVR) The pellets obtained in each of the Examples and Comparative Examples were used to measure the melt volume flow rate under conditions of 220°C and a load of 98.07 N in accordance with ISO test method 1133. Unit: cm 3 / 10 minutes
[0056] Heat deflection temperature (HDT) Using the pellets obtained in each of the Examples and Comparative Examples, various test pieces were molded in accordance with ISO test method 294, and the deflection temperature under load of 1.8 MPa was measured in accordance with ISO 75. Unit: °C
[0057] Plating adhesion strength The pellets obtained in each Example and Comparative Example were molded into flat plate molded products for plating (55 mm × 90 mm × 3 mm) using an injection molding machine, and plated using the following method. The adhesion strength of the deposited plating film was evaluated based on JIS H-8630 by making cuts at 1 cm intervals in the metal film of the plated molded product so as to reach the substrate, and peeling the metal film in the perpendicular direction, as measured by the stress (N / cm). <Plating process> The above plating plate was used and the following procedure was followed. Degreasing (surfactant solution, 55℃ x 3 minutes), etching (sulfuric acid-chromic anhydride mixed solution, 68℃ x 10 minutes), rinsing with water, neutralization (hydrochloric acid solution, room temperature x 2 minutes), rinsing with water, catalyst (palladium chloride-stannous chloride-hydrochloric acid solution, 35℃ x 5 minutes), rinsing with water, accelerator (sulfuric acid solution, 40℃ x 5 minutes), rinsing with water, electroless plating (nickel plating solution mainly composed of nickel sulfate-sodium hypophosphite-sodium citrate, 50℃ x 8 minutes), rinsing with water, copper electroplating (room temperature x 2 hours, current density 3A / dm2, film thickness 50μm), rinsing with water, drying.
[0058] Polycarbonate resin (A) A polycarbonate resin made from phosgene and bisphenol A with a viscosity average molecular weight of 20,500.
[0059] Preparation of graft copolymer (B) In a glass reactor, 60 parts by mass of coagulated and thickened styrene-butadiene rubber (b-1) latex (styrene 5% by mass, butadiene 95% by mass, mass average particle size 440 nm) was charged in terms of solid content, stirring was started, and nitrogen substitution was performed. After nitrogen substitution, the temperature in the tank was raised to 65°C, and an aqueous solution in which 0.06 parts by mass of glucose, 0.03 parts by mass of anhydrous sodium pyrophosphate, and 0.001 parts by mass of ferrous sulfate were dissolved in 10 parts by mass of deionized water was added, and then the temperature was raised to 70°C. Then, a mixture of 10 parts by mass of acrylonitrile, 30 parts by mass of styrene, 0.3 parts by mass of tertiary decyl mercaptan, and 0.1 parts by mass of t-butyl hydroperoxide and an emulsifier aqueous solution in which 1.0 parts by mass of potassium oleate (solid content equivalent) was dissolved in 20 parts by mass of deionized water were continuously dropped over 4 hours. After dropping, the mixture was held for 3 hours to obtain a graft copolymer latex. Thereafter, salting out, dehydration and drying were performed to obtain a powder of graft copolymer (B). The graft rate of the obtained graft copolymer (B) was 42%, and the reduced viscosity of the acetone soluble portion was 0.28 dl / g. The mass average particle size of the aggregated and thickened styrene-butadiene rubber latex was determined as follows. The samples were stained with osmium tetroxide (OsO4), dried, and photographed with a transmission electron microscope. The area of 800 rubber particles was measured using an image analysis processing device (device name: Asahi Kasei Corporation IP-1000PC), and their circle equivalent diameters (diameters) were calculated to calculate the mass average particle diameter.
[0060] Preparation of copolymer (C) A copolymer (C) consisting of 75 parts by mass of styrene and 25 parts by mass of acrylonitrile was obtained by a known bulk polymerization method. The reduced viscosity of the copolymer (C) obtained by the above method was 0.50 dl / g.
[0061] Phosphate ester (D) Aromatic condensed phosphate ester manufactured by Daihachi Chemical Industry Co., Ltd.: PX-200
[0062] Example 1 and Comparative Examples 1-2 Polycarbonate resin (A), graft copolymer (B), copolymer (C) and phosphate ester (D) were mixed in the proportions shown in Table 1, and then melt-kneaded and pelletized in a φ26mm twin-screw extruder set at a cylinder temperature of 250°C, with a main screw rotation speed of 400 rpm and a discharge rate of 20 kg / hr. These pellets were then molded in an injection molding machine (cylinder temperature 250°C, mold temperature 60°C) to produce test pieces for measuring physical properties and flat plates for plating. The test pieces and flat plates were then used to measure physical properties and plating adhesion strength. The results are shown in Table 1.
[0063] [Table 1]
[0064] As is clear from Table 1, Example 1, in which the resin composition for plating of the present invention was used, provided an excellent balance of heat resistance, fluidity, and plating adhesion strength. In Comparative Example 1, the content of the phosphate ester (D) was below the lower limit of the range specified in the present application, and therefore the fluidity and plating adhesion strength were poor. In Comparative Example 2, the content of the phosphate ester (D) exceeded the upper limit of the range specified in the present application, and therefore the heat resistance and plating adhesion strength were poor. [Industrial Applicability]
[0065] As described above, the resin composition for plating of the present invention has an excellent balance of heat resistance, fluidity, and plating adhesion strength, and can therefore be used in a wide variety of applications for plated parts, such as vehicle interior parts and vehicle exterior parts.
Claims
1. The resin composition for plating contains a polycarbonate resin (A), a graft copolymer (B) obtained by graft polymerization of a rubber polymer (b-1) and a monomer component (b-2) containing at least one selected from an aromatic vinyl monomer, a vinyl cyanide monomer, and a (meth)acrylic acid ester monomer, a copolymer (C) obtained by polymerization of a monomer component containing an aromatic vinyl monomer and a vinyl cyanide monomer, and a phosphoric acid ester (D), the polycarbonate resin (A) being 40 to 70 mass%, the rubber polymer (b-1) being 8 to 20 mass%, and the phosphoric acid ester (D) being more than 0 mass% but not more than 3.5 mass% (the total of (A) + (B) + (C) + (D) being 100 mass%).
2. A resin composition for plating use, comprising the phosphoric acid ester (D) according to claim 1 in an amount of 0.5% by mass or more and 3.5% by mass or less.
3. A plated molded product comprising a molded product made of the resin composition for plating according to claim 1 or 2 and a plating film.
Citation Information
Patent Citations
Flame-retardant thermoplastic resin composition
JP1996193157A
Resin composition for plating base, and molding and electric plating part using the same
JP2003147154A
Thermoplastic polymer composition for multicolor-developing laser marking and laser marking method
JP2006083242A
Thermoplastic resin composition, molded product and plated molded product
JP2009292921A
Flame Retardant Thermoplastic Resin CompositionShowing Good Chemical Resistance
KR1020030095537A