A titanium alloy with medium strength and high ductility.

A titanium alloy with optimized vanadium, aluminum, iron, and silicon content, combined with specific manufacturing processes, addresses the cost and performance limitations of Ti-6Al-4V, offering enhanced strength, ductility, and machinability for impact-resistant applications.

JP7566729B2Active Publication Date: 2024-10-15TITANIUM METALS CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021516555
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-09-25
Filing Date
2019-09-25
Publication Date
2024-10-15
Estimated Expiration
2039-09-25

AI Technical Summary

Technical Problem

Existing high-strength titanium alloys, such as Ti-6Al-4V, are costly due to high alloying element content and do not effectively balance strength and ductility, leading to high manufacturing costs and performance limitations.

Method used

A titanium alloy composition with specific ranges of vanadium, aluminum, iron, oxygen, and silicon, along with controlled levels of carbon and nitrogen, is developed, combined with manufacturing processes like beta forging, rolling, and stress relaxation, to achieve a balance of strength and ductility.

Benefits of technology

The alloy exhibits improved strength and ductility, reducing manufacturing costs while enhancing energy absorption and machinability, making it suitable for applications requiring impact resistance and containment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566729000008
    Figure 0007566729000008
  • Figure 0007566729000001
    Figure 0007566729000001
  • Figure 0007566729000002
    Figure 0007566729000002
Patent Text Reader

Abstract

The present invention provides a titanium alloy composition. The alloy contains, in weight percent (wt%), 5.7-8.0% vanadium, 0.5-1.75% aluminum, 0.25-1.5% iron, 0.1-0.2% oxygen, 0.15% or less silicon, 0.1% or less carbon, and less than 0.03% nitrogen. In one form, the titanium alloy has a 0.2% yield strength of 600-850 MPa, an ultimate tensile strength of 700-950 MPa, an elongation to failure of 20-30%, a reduction in area of ​​40-80%, a Charpy U-notch impact energy of 30-70 J, and / or a Charpy V-notch impact energy of 40-150 J. [Selected Figure] Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

CROSS REFERENCE TO RELATED APPLICATIONS

[0001]

[0001] This application claims priority to and the benefit of Provisional Application No. 62 / 736,229, filed September 25, 2018, the disclosure of which is incorporated herein by reference. [Technical field]

[0002]

[0002] The present disclosure relates to titanium alloys, and more specifically, to titanium alloys having enhanced strength and ductility comparable to commercially available alloys. [Background technology]

[0003]

[0003] The statements in this section are merely intended to provide background information related to the present disclosure and may not constitute prior art.

[0004] Titanium-based alloys (simply referred to herein as "titanium alloys"), most commonly described as Ti-6Al-4V (containing 6% aluminum and 4% vanadium by weight), are commonly used in aircraft construction and other products that require a higher strength-to-weight ratio than that offered by steel and other engineering alloys. According to U.S. Patent No. 3,802,877 ("the '877 patent"), titanium alloys containing vanadium, aluminum, and iron, and optionally other elements, can be used to produce high-strength titanium alloys (compared to the industry standard Ti-6Al-4V). However, the '877 patent discloses relatively high alloying element contents to produce metastable beta titanium alloys with yield strengths (YS) of over 1038 MPa, which results in higher costs. Summary of the Invention [Problem to be solved by the invention]

[0004]

[0005] The present disclosure addresses these higher costs, among other issues associated with high strength titanium alloys. [Means for solving the problem]

[0005]

[0006] In one embodiment of the present disclosure, a titanium alloy is provided that contains (by weight) 5.7-8.0% vanadium, 0.5-1.75% aluminum, 0.25-1.5% iron, 0.1-0.2% oxygen, 0.15% or less silicon, 0.1% carbon, and less than 0.03% nitrogen. In some variations of the present disclosure, the vanadium is between 5.9-8%, for example, between 6.1-8%. In other embodiments, the vanadium is 6.8-7.8%, the aluminum is 0.9-1.5%, the iron is 0.5-1.1%, the oxygen is 0.12-0.19%, and the silicon is 0.12% or less. In one variation, the vanadium is 7.3%, the aluminum is 1.2%, the iron is 0.8%, the silicon is 0.05%, and the oxygen is 0.16%. In yet another variation, the titanium alloy contains 7.2% vanadium, 1.2% aluminum, 0.8% iron, 0.15% oxygen, 0.05% silicon, with carbon and nitrogen reduced to impurity levels.

[0007] In one embodiment, the titanium alloy has a yield strength (YS) at 0.2% plastic deformation (i.e., 0.2% YS) of 600-850 MPa, an ultimate tensile strength of 700-950 MPa, an elongation to break (percent elongation to break) of 20-30%, a reduction in area of ​​40-80%, a Charpy U-notch impact energy of 30-70 J, and / or a Charpy V-notch impact energy of 40-150 J. For example, the titanium alloy has a 0.2% yield strength of 650-850 MPa, an ultimate tensile strength of 750-950 MPa, an elongation to break (percent elongation to break) of 22-30%, a reduction in area of ​​55-75%, a Charpy U-notch impact energy of 40-60 J, and / or a Charpy V-notch impact energy of 60-100 J.

[0008] In another aspect of the present disclosure, a method for producing a titanium alloy is provided. The method includes melting and forming an ingot of a chemical composition within the disclosed ranges containing (by weight): 5.7-8% vanadium, 0.5-1.75% aluminum, 0.25-1.5% iron, 0.1-0.2% oxygen, 0.15% or less silicon, 0.1% or less carbon, and less than 0.03% nitrogen. A variation of this method includes beta forging and rolling the ingot to form an intermediate product (e.g., a plate or slab), alpha beta rolling the plate or slab to form a product, alpha beta solution heat treating (SHT) the product, and stress relieving the SHT treated product. In some embodiments of the present disclosure, the stress-softened product may have a 0.2% yield strength of 600-850 MPa, an ultimate tensile strength of 700-950 MPa, an elongation at break of 20-30%, a reduction in area of ​​40-80%, a Charpy U-notch impact energy of 30-70 J, and / or a Charpy V-notch impact energy of 40-150 J. For example, the stress-softened product may have a 0.2% yield strength of 650-850 MPa, an ultimate tensile strength of 750-950 MPa, an elongation at break of 22-30%, a reduction in area of ​​55-75%, a Charpy U-notch impact energy of 40-60 J, and / or a Charpy V-notch impact energy of 60-100 J.

[0009] In one embodiment of the present disclosure, a titanium alloy manufacturing method includes reheating the plate for sizing, straightening or flattening, and stress-relieving the product at a temperature in the range of 500°C to 650°C. The Charpy impact energy of the product is increased by alpha-beta rolling the plate or slab to reduce the cross-sectional area by at least 50%, followed by reheating the product at a temperature in the range of 500°C to 600°C to size, straightening, flattening, and stress-relieving. Alternatively or additionally, the tensile ductility of the product is increased by alpha-beta rolling the plate or slab to reduce the cross-sectional area by at least 50%, reheating the plate to a temperature 50°C to 150°C below the beta transus to size, solution heat treating the product to a temperature 30°C to 100°C below the beta transus to straighten or flatten, cooling at a desired rate to obtain improved strength, and stress-relieving at a temperature in the range of 500°C to 650°C.

[0010] The vanadium content in one embodiment of the titanium alloy is in the range of 5.7-8.0%, for example 5.9-8.0%, by weight. In one embodiment of the titanium alloy, the vanadium content is 6.8-7.8%, the aluminum content is 0.9-1.5%, the iron content is 0.5-1.1%, the oxygen content is 0.12-0.19%, and the silicon content is 0.12% or less by weight. In one variation of the present disclosure, the vanadium content is 7.3%, the aluminum content is 1.2%, the iron content is 0.8%, the silicon content is 0.05%, and the oxygen content is 0.16% by weight. In another embodiment of the present disclosure, the titanium alloy contains 7.2% vanadium, 1.2% aluminum, 0.8% iron, 0.15% oxygen, and 0.05% silicon by weight, with carbon and nitrogen reduced to the level of impurities.

[0011] Further areas of applicability of the present invention will become apparent from the written description provided herein. It will be understood that the description and specific examples herein are for purposes of illustration only and are not intended to limit the scope of the present disclosure. [Brief description of the drawings]

[0006]

[0012] In order that the disclosure may be fully understood, reference will now be made to the accompanying drawings which illustrate, by way of example, various embodiments thereof.

[0013] [Figure 1] FIG. 1 illustrates a backscattered electron image of an alpha-beta titanium alloy in accordance with the teachings of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007]

[0014] The following description is merely exemplary in nature and is not intended to limit the disclosure, application, or uses. It is understood that throughout the drawings, corresponding reference numerals indicate similar or corresponding parts and features. Examples are provided to fully convey the scope of the disclosure to those skilled in the art. Numerous specific details are shown, such as specific components, device, and method types, to provide a thorough understanding of the variations of the present disclosure. It will be apparent to those skilled in the art that the use of specific details is not necessary and that the examples provided herein may include alternative embodiments and are not intended to limit the scope of the present disclosure. In some examples, well-known and well-known processes, well-known device structures, well-known technologies are not described in detail.

[0015] The present disclosure generally relates to titanium (Ti) alloys for use in applications where the desired performance is related to the energy absorbed during deformation of a component, including impact, explosive blast, or other forms of shock loads. Titanium alloys manufactured and used in accordance with the teachings contained herein provide performance improvements and / or cost savings when used in such demanding applications. Titanium alloys are described throughout this disclosure in conjunction with their use in aircraft engine sealing casings to more fully explain the teachings of the present disclosure. When used in aircraft (such as jet) engine sealing casings, titanium alloys typically take the shape of a ring that surrounds the fan blades and maintains containment of the blades in the event of failure of the application of that component. Incorporation and use of titanium alloys in combination with other types of applications where the alloy may be exposed to impact, explosive blast, or other forms of shock loads is within the scope of the present disclosure.

[0016] Titanium alloys prepared according to the teachings of the present disclosure have several properties or a balance of properties that provide an overall improvement over conventional titanium alloys commonly used in engine containment. All properties are obtained from samples prepared under various heat treatment conditions using manufacturing simulation processing techniques. Properties and associated ranges exhibited by the titanium alloys of the present disclosure include (a) yield strength (YS) of 600-850 MPa, (b) ultimate tensile strength (UTS) of 700-900 MPa, (c) elongation to fracture of 20-30%, and (d) reduction in area at fracture of 40-80%. The titanium alloys of the present disclosure exhibit properties within the above ranges, as many of these properties are mutually influenced. For example, the mechanical and textural properties exhibited by the titanium alloys of the present disclosure affect the ballistic impact resistance of the alloy.

[0017] Compared to conventional titanium alloys, such as Ti-6Al-4V alloy, used in applications where the alloy is exposed to impact, explosive blast, or other forms of shock loading, the disclosed titanium alloys offer both improved performance and manufacturing cost savings. The disclosed titanium alloy formulations not only exhibit excellent workability and machinability in machining, but also exhibit excellent energy absorption under high strain rate conditions. This combination of performance and manufacturability allows for the design of sealing systems and functional components formed from these titanium alloys where containment of high velocity or ballistic impacts is critical at the lowest practical cost. Additionally, many titanium alloys, such as Ti-6Al-4V alloy, have a high aluminum equivalent and exhibit a high degree of aluminium as the primary deformation mechanism. In comparison, the aluminum equivalent of the present disclosure is much lower than that of the conventional product, which promotes twinning and<c+a> Promoting alternative deformation mechanisms such as slip, improving machinability and facilitating rapid energy absorption (e.g., The Effect of Aluminum on Binary Alpha-Titanium Twinning, Pfitzner et al., Journal of Biomaterials 103:341-351, January 2016, and The Effect of Aluminum on Twinning Deformation of Alpha-Titanium, Pfitzner et al.).

[0018] Titanium alloys according to the present disclosure may also be selected for use on economic grounds because of their advantages in manufacturing parts suitable for applications where strength and / or corrosion resistance are not the primary design criteria, even when subjected to blast, shock loading, or ballistic impact.

[0019] The present disclosure describes titanium alloys with improved ductility compared to Ti-6Al-4V alloy and improved strength compared to other commercially available titanium alloys. In particular, the present disclosure describes titanium alloys with lower levels of aluminum and higher levels of V compared to Ti-6Al-4V alloy and other commercially available titanium alloys. The titanium alloys described herein exhibit higher ductility and lower strength, e.g., 22%-30% ductility and 700 MPa-830 MPa yield strength, in the annealed and air-cooled (AC) condition, generally higher ductility and lower strength than Ti-6Al-4V alloy. The titanium alloys described herein also exhibit approximately the same ductility and greater strength as other commercially available titanium alloys. The alloys described in the present disclosure have advantages in "single load to failure" applications where the desired components are determined by high strain rate events such as blast and impact damage, and specific strength is balanced with material parameters such as ductility and Charpy impact energy.

[0020] With respect to commercially available titanium alloys, U.S. Patent No. 10,000,838, commonly assigned to this disclosure and incorporated herein by reference, discloses a titanium alloy commercially known as Ti-407 alloy and sold under the trademark TIMETAL 407 alloy® having a nominal composition (by weight percent) of Ti, 0.85Al, 3.9V, 0.25Si, 0.25Fe, 0.15O, which allows components for "single load to failure" applications to be manufactured to achieve improved performance at lower cost. The present disclosure includes titanium alloys having a yield strength intermediate between Ti-407 and Ti-6Al-4V alloys, generally comparable to Ti-407 alloy, and greater ductility than Ti-6Al-4V alloy.

[0021] In one embodiment of the present disclosure, the titanium alloy has a composition (by weight) of 5.7-8.0% V, 0.5-1.75% Al, 0.25-1.5% Fe, 0.1-0.2% O, and 0.15% or less Si, with the balance being titanium and unavoidable impurities. For example, the titanium alloy disclosed in the present disclosure may have a composition (by weight) of 6.8-7.8% V, 0.9-1.5% Al, 0.5-1.1% Fe, 0.12-0.19% O, and 0.12% or less Si, with the balance being titanium and unavoidable impurities. In one embodiment of the present disclosure, the titanium alloy may have a nominal composition (by weight) of Ti, 7.3% V, 1.2% Al, 0.8% Fe, 0.05% Si, 0.16% O, and unavoidable impurities.

[0022] In another aspect of the present disclosure, the titanium alloy has a composition including (by weight%) 5.7-8.0% V, 0.5-1.75% Al, 0.25-1.5% Fe, 0.1-0.2% O, up to 0.15% Si, up to 0.5% Sn, up to 0.25% Mo, and up to 0.25% Cr, with the balance being titanium and unavoidable impurities.

[0023] The titanium alloys disclosed herein can be formulated as alpha-beta titanium alloys. That is, the titanium alloys disclosed herein are melted by any of the conventional industrially established melting methods for titanium alloys, then beta forged and / or rolled, followed by forging and / or rolling in the alpha + beta phase temperature range, and heat treatment in the alpha-beta phase temperature range. The ductility of the alloy is improved by forging and / or rolling, reducing the cross-sectional area by at least 50% in the alpha + beta phase temperature range, followed by a stress relief heat treatment and, optionally, a solution heat treatment. The resulting microstructure includes a fine bimodal microstructure of primary alpha phase in a matrix of transformed beta phase (secondary alpha phase), with some residual beta phase as shown in FIG. 1.

[0024] In one aspect of the present disclosure, the titanium alloy provides enhanced strength (e.g., 0.2% yield strength of 600 MPa or more) compared to Ti-407 alloy (0.2% yield strength of 550 MPa or more) while maintaining approximately equivalent ductility and Charpy impact energy to Ti-407 alloy. It is understood that such an increase in strength without a decrease in ductility is a surprising result since, in titanium alloys, an increase in strength is generally accompanied by a decrease in ductility and Charpy impact energy.

[0025] The strength of the titanium alloys disclosed herein, as well as many other titanium alloys, may depend substantially on the last thermal operation in the alpha-beta phase temperature range and the cooling rate from that operation. In particular, rapid cooling from the last thermal operation in the alpha-beta phase temperature range may produce fine martensite secondary alpha that can provide higher strength. In one example, a 28 millimeter (mm) square block was solution treated, oil quenched, and then stress relieved, and the block exhibited a 0.2% yield strength of 940 MPa. Also, sufficiently slow cooling from the last thermal operation in the alpha-beta phase temperature range may result in a bimodal microstructure of primary alpha and retained beta phase, resulting in higher ductility and Charpy impact energy at lower strength, and lower modulus of elasticity. Non-limiting examples of cooling rates for sufficiently slow cooling from the last thermal operation in the alpha-beta phase temperature range include cooling rates of 200°C / min or less, which may include air cooling.

[0026] It is understood that vanadium (V) and iron (Fe) act as beta phase stabilizers when added to titanium alloys. In particular, V is an isomorphous beta stabilizer that dissolves to some extent in alpha phase titanium, while Fe is a eutectic forming beta stabilizer that exhibits high diffusion rates and low solubility in alpha phase titanium. Thus, when the titanium alloys disclosed herein are heat treated in the alpha plus beta phase temperature range, Fe will substantially partition to the beta phase. Although V and Fe both contribute (independently or in combination) to the strength of the titanium alloys disclosed herein via solid solution strengthening, V and Fe may help refine the transformation products when cooling from the beta phase field to the alpha phase field at a given cooling rate, and lower amounts of V and Fe in the titanium alloys disclosed herein can bring out the desired lower strength levels of the alloy. V and Fe also enhance the ductility of the titanium alloys disclosed herein by promoting retained beta phase in the microstructure, since the beta body-centered cubic phase accommodates larger strains even at high strain rates compared to the alpha hexagonal phase. Thus, the lower levels of V content in the titanium alloys disclosed herein are (by weight) 5.5%, 5.7%, 6.0%, 6.4% or 6.8%, and the lower levels (by weight) of Fe in the titanium alloys disclosed herein are 0.25%, 0.3%, 0.4%, or 0.5%.

[0027] Alternatively, if the V and Fe contents of the titanium alloy are too high, the ductility and Charpy impact energy of the alloy may be reduced, and under certain conditions, slow cooling from heat treatment may result in a high percentage of the alloy retaining the beta phase and an undesirably low modulus of elasticity. Subsequent aging heat treatments also present a virtual risk of embrittlement due to omega phase formation, especially when the aluminum content is at the lower end of the range. Furthermore, high Fe contents in titanium alloys present manufacturing challenges, particularly chemical segregation during ingot solidification, and tearing at the ingot surface during drawdown from ingot casting by cold hearth melting. Due to these considerations, the titanium alloys disclosed herein have maximum V and Fe contents to attempt to avoid such problems. Thus, the maximum V contents (wt%) in the titanium alloys disclosed herein are 8.0%, 7.8%, 7.5% or 7.3%. Additionally, the maximum content of Fe in the titanium alloys disclosed herein is (by weight) 1.5%, 1.25%, 1.1%, or 0.8%.

[0028] It should also be understood that aluminum (Al) and oxygen (O) are known in the art as alpha phase stabilizers for titanium alloys. Additionally, Al is a substitutional alloying element, and O is an interstitial alloying element. In the titanium alloys disclosed herein, Al and O are strengthening elements, particularly in strengthening the alpha phase, and the minimum content of these elements can be derived from the desired minimum strength level of the alloy. Thus, the minimum content (wt%) of Al in the titanium alloys disclosed herein is 0.5%, 0.7%, 0.9%, 1.1%, or 1.2%. Additionally, the minimum content (wt%) of O in the titanium alloys disclosed herein is 0.1%, 0.12%, 0.14%, or 0.16%.

[0029] Alternatively, if the Al and O content of the titanium alloy is too high, the ductility and Charpy impact energy of the alloy may decrease. The Charpy impact energy is particularly sensitive to oxygen content, and some experimental compositions disclosed in the present disclosure show good ductility in room temperature tensile tests at standard strain rates, but low Charpy impact energy. Such results are understood to be the result of strain rate dependent interactions between interstitial alloying elements and dislocations in the titanium alloy, and the maximum Al and O contents may be set based on these considerations. Thus, the maximum content (wt%) of Al in the titanium alloy disclosed herein is 1.75%, 1.6%, 1.5%, 1.4% or 1.2%. Also, the maximum content (wt%) of O in the titanium alloy disclosed herein is 0.2%, 0.19%, 0.18%, or 0.16%.

[0030] Silicon (Si) is known to add strength to titanium alloys through a combination of solution strengthening and the formation of titanium silicide precipitates. However, Si can have a significant detrimental effect on Charpy impact energy. Thus, the maximum Si content (wt%) in the titanium alloys disclosed herein is a nominal Si content of 0.25 wt%, which is reduced compared to the Si content of Ti-407 alloy, and is 0.12%, 0.10%, 0.075%, or 0.05%. In one aspect of the present disclosure, the nominal Si content is included in recognition of the occurrence of Si in some raw materials and the desire to control for this impurity.

[0031] Carbon (C) and nitrogen (N) are also interstitial impurities that, like oxygen and silicon, have a sensitive effect on the Charpy impact energy of titanium alloys. Even at levels where C and N do not significantly affect the ductility of titanium alloys, as measured in room temperature tensile tests at standard strain rates, C and N may result in a reduction in the Charpy impact energy. Thus, the maximum content (wt%) of C in the titanium alloys disclosed herein is 0.1%, 0.08%, 0.06%, 0.04%, or 0.02%. Also, the maximum content (wt%) of N in the titanium alloys disclosed herein is 0.03% (300 wt%), 0.02%, or 0.01%. Also, the total content C+O+Si affects the Charpy impact energy of the titanium alloy. For example, in some variations of the present disclosure, titanium alloys having a total content of C+O+Si of 0.4% or less have a U-notch Charpy impact energy of at least 25 J.

[0032] It should be understood that small amounts of other elements (e.g., less than 1%, less than 0.5%, or 0.25% or less) may be present in the titanium alloy and do not fall outside the scope of the titanium alloy disclosed herein. For example, beta stabilizers such as molybdenum (Mo) and chromium (Cr) may be present in the alloy up to 0.5Mo and 0.5%Cr. In at least one variation, the titanium alloy includes up to 0.25% Mo and / or up to 0.25% Cr. Tin (Sn) may also be present in the titanium alloys disclosed herein up to 1.0%. In other variations, the titanium alloy includes up to 0.5% Sn.

[0033] The following specific examples are provided to illustrate the composition, properties, and use of titanium alloys prepared according to the teachings of the present disclosure, and should not be construed as limiting the scope of the present disclosure. In light of the present disclosure, those skilled in the art will appreciate that many changes can be made in the specific examples disclosed herein and still obtain the same or similar results without departing from or exceeding the spirit or scope of the disclosure. EXAMPLES

[0008]

[0034] Example 1

[0035] A series of 0.4 pound (lbs.) (0.18 kg) "button" ingots of the comparative titanium alloy were produced by non-consumable argon arc melting and then converted into 0.5 inch (12.7 mm) square bars by a combination of beta forging and rolling, followed by alpha beta rolling, followed by alpha beta solution treatment at 25°C below the beta transus temperature for 1 hour (hr.), and stress relief at 800°C for 8 hours. The chemistry of the ingots (i.e., the target chemistry) and the mechanical test results for the 0.5 inch (12.7 mm) square bars are shown in Table 1 below. Here, "Elong'n5.65√A" refers to the percentage elongation of a sample or specimen where the gauge length is 5.65 times the square root of the gauge area, and "Elong'n4D" refers to the percentage elongation of a sample or specimen where the gauge length is 4 times the gauge area.

[0009] [Table 1]

[0010]

[0036] Analysis of the mechanical test results in Table 1 shows the alloying elements with the strongest negative impact on Charpy impact energy tested for 5mm U-notch samples in all Charpy impact energy tests performed according to BS EN ISO 148-1:2016 standard. For example, 0.5 inch (12.7 mm) square bars (MT6850, MT6852) with high Si, C, and / or O contents exhibited Charpy impact energies of less than 10 J. These results allowed for the formulation of additional samples aimed at imparting the desired strength and ductility in combination with improved Charpy impact energy.

[0037] Example 2

[0038] A series of 0.4 pound (0.18 kg) button ingots of titanium alloys according to the present disclosure were produced and converted into 0.5 inch (12.7 mm) square bars by the method used in Example 1, except for aging at 500° C. for 8 hours. The chemical compositions of the ingots and the mechanical testing results of the 0.5 inch (12.7 mm) square bars are shown in Table 2.

[0011] [Table 2]

[0012]

[0039] As shown in Table 2, the alloys of the present disclosure exhibit a superior combination of strength, ductility, and Charpy impact energy compared to the comparative alloys of Example 1 (Table 1). For example, the alloys of Table 2 had an average Charpy impact energy of 42.7 J compared to 19.1 J for the alloys of Table 1. Furthermore, the Ti-407 alloys A-1 to A-8, A-10 to A-17, and A-24 shown in Table 3, which were subjected to air-cooling +500°C x 8 hours aging treatment of U.S. Patent No. 10,000,838, have an average 0.2% yield strength (0.2% YS) of 622.5 MPa, an average ultimate tensile strength (UTS) of 703 MPa, and an average 4D elongation to fracture of 25.3%, while the alloys of the present invention (i.e., samples 3181, 3183 to 3186) which were subjected to the same air-cooling +500°C x 8 hours aging treatment (i.e., samples 3181, 3183 to 3186) have an average 0.2% yield strength (0.2% YS) of 789.7 MPa, an average ultimate tensile strength (UTS) of 895.3 MPa, and an average 4D elongation to fracture of 26.4%.

[0013] [Table 3]

[0014]

[0040] The data from Example 2 also shows that samples with the same composition but exposed to different cooling rates have significantly different mechanical properties. In particular, samples 3181 and 3182 have the same alloy composition (wt%) of Ti, 1.25Al, 0.8Fe, 7.0V, 0.03C, 0.8Si, and 0.16O. Sample 3181 was solution heat treated (SHT), air cooled (AC) at a cooling rate of 80°C / min, and aged / stress relieved at 500°C and exhibited an average 0.2% yield strength (0.2%YS) of 790.5 MPa, an average ultimate tensile strength (UTS) of 897 MPa, an average 4D elongation to failure of 25.0%, an average reduction in area of ​​66.5%, and an average Charpy U-notch impact energy of 42.0 J, respectively. Specimen 3182VC was solution heat treated (SHT), vermiculite cooled (VC) at a cooling rate of 30°C / min, and aged / stress relieved at 500°C, and exhibited an average 0.2% yield strength of 707 MPa, an average ultimate tensile strength of 817.5 MPa, an average 4D elongation of 27.5%, and an average reduction in area of ​​67.2%. Specimen 3182OQ was solution heat treated (SHT), oil quenched (QC) at a cooling rate of 500°C / min, and aged / stress relieved at 500°C, and exhibited a 0.2% yield strength of 932 MPa, an ultimate tensile strength of 1039 MPa, a 4D elongation to failure of 21.5%, and an average reduction in area of ​​63.5%. Thus, a faster cooling rate for the air-cooled sample (3181) compared to the vermiculite-cooled sample (3182VC) results in higher strength and lower ductility for the air-cooled sample. Similarly, a faster cooling rate for the oil-quenched sample (3182OQ) compared to the air-cooled sample (3181) results in higher strength and lower ductility for the oil-quenched sample.

[0041] Example 3

[0042] A number of titanium alloy 0.4 pound (0.18 kg) button ingots according to the present disclosure having a composition (wt%) of Ti, 0.95Al, 7.0V, 0.8Fe, 0.08Si, 0.03C, 0.16O were produced by the method used in Example 1 and converted into 0.5 inch (12.7 mm) square bars. The 0.5 inch (12.7 mm) square bars were solution heat treated (SHT), vermiculite cooled (VC), and cooled in air (AC) or oil quenched (OQ) before mechanical testing. Table 4 below shows the mechanical test results for the VC, AC, and OQ cooled samples. As shown, these samples show a superior combination of strength, ductility, and Charpy impact energy compared to the alloy of Example 1, and the effect of cooling rate from solution heat treatment (SHT) on the mechanical properties of the alloy is recognized.

[0015] [Table 4]

[0016]

[0043] In particular, the VC-cooled samples (MT7380, MT7381) had an average 0.2% YS of 678 MPa, an average UTS of 790 MPa, an average 4D elongation to failure of 28.8%, and an average reduction in area of ​​68.3%. The air-cooled (AC)-cooled samples (MT7382, MT7283) had an average 0.2% YS of 751.5 MPa, an average UTS of 862.5 MPa, an average 4D elongation to failure of 26.5%, and an average reduction in area of ​​71%. The OQ-cooled samples (MT7284, MT7285) had an average 0.2% YS of 902 MPa, an average UTS of 1010.5 MPa, an average 4D elongation of 22%, and an average reduction in area of ​​67.5%. Thus, with increasing cooling rate, the 0.2% yield strength and ultimate tensile strength increase, and the 4D elongation to failure decreases. Surprisingly, air cooling (AC) of this alloy resulted in both increased strength and increased ductility, as measured by reduction in area.

[0044] Example 4

[0045] A series of 0.4 pound (0.18 kg) button ingots of a series of titanium alloys of the present disclosure having compositions (i.e., Ti, 1.0Al, 7.5V, 0.7Fe, 0.02Si, 0.02C, 0.15O) (wt%) within the range of the present disclosure were produced and converted into 0.5 inch (12.7 mm) square bars by the method used in Example 1, which were subjected to various processing conditions and then mechanically tested. In particular, as shown in Table 5 below, the as-rolled 0.5 inch (12.7 mm) square bars, the 0.5 inch (12.7 mm) square bars stress-relieved at various temperatures, the solution heat treated and cooled in air (AC) and vermiculite (VC) and aged at 500°C for 8 hours, and the 0.5 inch (12.7 mm) square bars were mechanically tested.

[0017] [Table 5]

[0018]

[0046] As shown in Table 5, it was found that the 0.5 inch (12.7 mm) square bars stress-relieved at 525°C, 575°C and 625°C for 2 hours had improved mechanical properties, especially improved Charpy impact energy, compared to the specimens SHT, AC or VC cooled and aged at 500°C for 8 hours. Thus, the 0.5 inch (12.7 mm) square bars stress-relieved at temperatures ranging from 500°C to 650°C showed a 77% improvement in the Charpy impact energy of the alloy compared to the 0.5 inch (12.7 mm) square bars solution heat treated (SHC), air cooled (AC) and aged at 500°C for 8 hours.

[0047] Example 5

[0048] A series of 8 inch (203.2 mm) diameter, nominal 56 pound (25.4 kg) vacuum arc remelted (VAR) ingots of the disclosed alloys and comparative titanium alloys (comparative alloys) were fabricated and converted into 0.5 inch (12.7 mm) thick plates by combined beta forging and alpha beta forging and rolling followed by alpha beta solution heat treatment at 25°C below the beta transus temperature for 1 hour (hr.). The 0.5 inch (12.7 mm) plates were solution heat treated (SHC), vermiculite cooled (VC), and stress relieved at 550°C for 4 hours. The slow cooling through vermiculite cooled (VC) was chosen to be representative of material processed on an industrial scale, with thicker sections experiencing slower cooling rates than those experienced with air cooled (AC) laboratory samples. Table 6 lists the ranges of alloy compositions within and outside the disclosed ranges, along with mechanical testing results from the plates, respectively.

[0019] [Table 6]

[0020]

[0049] As shown, titanium alloys having compositions within the disclosed ranges exhibited 0.2% yield strengths of 622-787 MPa, ultimate tensile strengths of 721-885 MPa, 4D elongations to failure of 23.5-28.0%, reductions in area of ​​49.3-69.6%, U-notch Charpy impact energies of 36-65 J, and V-notch Charpy impact energies of 42-130 J. In contrast, comparative titanium alloys outside the disclosed ranges exhibited Charpy U-notch impact energies of less than 36 J. Thus, alloys such as V8778, V8782, and V8787 exhibit 0.2% yield strengths of at least 700 MPa, ultimate tensile strengths of at least 800 MPa, elastic moduli (Young's moduli) of at least 100 GPa, 4D elongations to failure of at least 20%, U-notch Charpy impact energies of at least 40 J, and V-notch Charpy impact energies of at least 70 J, respectively.

[0050] Example 6

[0051] Lathe machinability tests were performed on the titanium alloy compositions shown in Table 7 below. In particular, machinability V15 tests were performed, which is a guide to the speed at which a cutting tool will wear out within 15 minutes. Variable speed external turning was performed using a CNMG 12 04 08-23 H13A progressive tool insert with a C5-DCLNL-35060-12 holder at a feed rate of 0.1 mm / rev and a radial depth of cut of 2 mm. The role of aluminum content in the deformation mechanism and its effect on machinability is shown in the table below, with titanium alloys prepared according to the present disclosure exhibiting a machinability V15 turning benchmark of over 115 m / min, which is at least a 150% improvement over the machinability V15 of conventional Ti-6Al-4V alloy. Thus, the titanium alloys of the present disclosure exhibit improved machining performance over conventional titanium alloys.

[0021] [Table 7]

[0022]

[0052] The present disclosure provides titanium alloys with improved ductility compared to Ti-6V-4Al alloy and improved strength compared to Ti-407 alloy. In some forms of the present disclosure, the titanium alloys have a 0.2% yield strength of 600-850 MPa, an ultimate tensile strength of 700-950 MPa, an elongation to failure of 20-30%, a reduction in area of ​​40-80%, a Charpy U-notch impact energy of 30-70 J, and / or a Charpy V-notch impact energy of 40-150 J, respectively. Thus, such titanium alloys of the present disclosure can be used in applications requiring the absorption of high energy during deformation of components, including impact, explosive blast, or other forms of shock loading, such as for use in aircraft engine containment casings.

[0053] As used herein, the phrase at least one of A, B, and C should be interpreted as meaning the logical disjunction (A or B or C), using non-exclusive logical disjunction, and not as meaning "at least one of A, at least one of B, and at least one of C."

[0054] Unless otherwise indicated, all numerical values ​​or other characteristics indicating mechanical / thermal properties, percentages of composition, dimensions and / or tolerances should be understood as being modified by the word "about" or "approximately" in describing the scope of this disclosure. This variation is desirable for various reasons, including industrial practices, manufacturing techniques, testing capabilities, etc.

[0055] The terms used herein are for the purpose of describing specific exemplary embodiments only and are not intended to be limiting. The singular forms "a," "an," and "the" may be intended to include the plural unless the context clearly indicates otherwise. The terms "comprise" and "have" are inclusive and thus specify the presence of stated features, integers, steps, operations, elements, and / or components, but do not preclude the presence or addition of one or more other features, integers, steps, operations, elements, components, and / or groups thereof. The steps, processes, and operations of the methods described herein should not be construed as necessarily requiring their performance in the particular order described or illustrated, unless specifically identified as an order of performance. It should also be understood that additional or alternative steps may be used.

[0056] The description of the present disclosure is merely exemplary in nature, and therefore examples that do not depart from the substance of the present disclosure are intended to be within the scope of the present disclosure. Such examples should not be considered as departures from the spirit and scope of the disclosure. The broad teachings of the present disclosure can be implemented in various forms. Thus, although the present disclosure includes specific examples, other modifications will become apparent upon review of the drawings, specification, and claims below, and therefore the true scope of the disclosure should not be so limited. The invention as originally claimed in the present application is set forth below. [1] A titanium alloy containing, by weight, 5.7-8% vanadium, 0.5-1.75% aluminum, 0.25-1.5% iron, 0.1-0.2% oxygen, 0.15% or less silicon, 0.1% or less carbon, and less than 0.03% nitrogen. [2] The titanium alloy according to [1], wherein the vanadium content is 5.9 to 8%. [3] The titanium alloy according to [1], wherein the vanadium content is 6.1 to 8%. [4] The titanium alloy according to [1], having 6.8-7.8% vanadium, 0.9-1.5% aluminum, 0.5-1.1% iron, 0.12-0.19% oxygen, and 0.12% or less silicon. [5] The titanium alloy of [1], having 7.3% vanadium, 1.2% aluminum, 0.8% iron, 0.05% silicon, and 0.16% oxygen. [6] The titanium alloy of [1] containing 7.2% vanadium, 1.2% aluminum, 0.8% iron, 0.15% oxygen, and 0.05% silicon, with carbon and nitrogen reduced to impurities. [7] The titanium alloy according to [1], further having a 0.2% yield strength of 600 to 850 MPa, an ultimate tensile strength of 700 to 950 MPa, an elongation at break of 20 to 30%, a reduction in area of ​​40 to 80%, and at least one of a Charpy U-notch impact energy of 30 to 70 J and a Charpy V-notch impact energy of 40 to 150 J. [8] The titanium alloy according to [1], further having a 0.2% yield strength of 650 to 850 MPa, an ultimate tensile strength of 750 to 950 MPa, an elongation at break of 22 to 30%, a reduction in area of ​​55 to 75%, and at least one of a Charpy U-notch impact energy of 40 to 60 J and a Charpy V-notch impact energy of 60 to 100 J. [9] A method for producing a titanium alloy, comprising melting and forming an ingot having a chemical composition including 5.7-8% vanadium, 0.5-1.75% aluminum, 0.25-1.5% iron, 0.1-0.2% oxygen, 0.15% or less silicon, 0.1% or less carbon, and less than 0.03% nitrogen.

[10] beta-forging and rolling the ingot to form a plate or slab; rolling the plate or slab to form a product; subjecting said product to alpha-beta solution heat treatment (SHT); The method according to claim 9, wherein the SHT treated product is stress relaxed.

[11] The stress-relieved product has a 0.2% yield strength of 600-850 MPa, an ultimate tensile strength of 700-950 MPa, an elongation at break of 20-30%, and a reduction in area of ​​40-80%; and at least one of a Charpy U-notch impact energy of 30-70J and a Charpy V-notch impact energy of 40-150J.

[12] The stress-relieved product has a 0.2% yield strength of 650-850 MPa, an ultimate tensile strength of 750-950 MPa, an elongation at break of 22-30%, and a reduction in area of ​​55-75%, and at least one of a Charpy U-notch impact energy of 40-60J and a Charpy V-notch impact energy of 60-100J.

[13] The method according to

[10] , further comprising alpha-beta rolling to reduce the cross-sectional area of ​​the plate or slab by at least 50%.

[14] The method of

[13] , further comprising reheating the plate to size, straighten, or flatten, and stress relieving the product at a temperature in the range of 500°C to 600°C.

[15] The method of [9], wherein the Charpy impact energy of the product is increased by alpha-beta rolling the plate or slab to a cross-sectional reduction of at least 50%, followed by reheating the product for sizing, straightening, flattening, and relieving stress in the product at a temperature in the range of 500°C to 650°C.

[16] The method of [9], wherein the tensile ductility of the product is increased by alpha-beta processing the plate or slab for a minimum of 50% reduction in area, reheating the plate to a temperature 50°C to 150°C below the beta transus for sizing, straightening or flattening the product, solution heat treating the product at a temperature 30°C to 100°C below the beta transus, cooling at a desired rate to obtain a desired strength, and stress relieving at a temperature in the range of 500°C to 650°C.

[17] The method according to [9], wherein the vanadium content is 5.9 to 8.0%.

[18] The method according to [9], wherein the vanadium content is 6.1 to 8.0%.

[19] The method according to [9], wherein the vanadium content is 6.8-7.8%, the aluminum content is 0.9-1.5%, the iron content is 0.5-1.1%, the oxygen content is 0.12-0.19%, and the silicon content is 0.12% or less.

[20] The method according to [9], wherein the vanadium content is 7.3%, the aluminum content is 1.2%, the iron content is 0.8%, the silicon content is 0.05%, and the oxygen content is 0.16%.

Claims

1. Containing, by weight, 5.7-8% vanadium, 0.5-1.75% aluminum, 0.25-1.5% iron, 0.1-0.2% oxygen, 0.15% or less silicon, 0.1% or less carbon, and less than 0.03% nitrogen, the balance being titanium and unavoidable impurities; A titanium alloy having a 0.2% yield strength of 600-850 MPa and a fracture elongation of 20-30%.

2. 2. The titanium alloy of claim 1, wherein the vanadium is 5.9-8%.

3. 2. The titanium alloy of claim 1, wherein the vanadium is 6.1-8%.

4. 2. The titanium alloy of claim 1, comprising 6.8-7.8% vanadium, 0.9-1.5% aluminum, 0.5-1.1% iron, 0.12-0.19% oxygen, and up to 0.12% silicon.

5. 2. The titanium alloy of claim 1 having 7.3% vanadium, 1.2% aluminum, 0.8% iron, 0.05% silicon, and 0.16% oxygen.

6. 10. The titanium alloy of claim 1 comprising 7.2% vanadium, 1.2% aluminum, 0.8% iron, 0.15% oxygen, and 0.05% silicon, with carbon and nitrogen reduced to impurities.

7. 2. The titanium alloy of claim 1, having an ultimate tensile strength of 700-950 MPa and a reduction in area of ​​40-80%, and further having a Charpy U-notch impact energy of 30-70 J and / or a Charpy V-notch impact energy of 40-150 J.

8. 2. The titanium alloy of claim 1 having a 0.2% yield strength of 650-850 MPa, an ultimate tensile strength of 750-950 MPa, an elongation to break of 22-30%, a reduction in area of ​​55-75%, and further having a Charpy U-notch impact energy of 40-60 J and / or a Charpy V-notch impact energy of 60-100 J.

9. melting and forming an ingot containing 5.7-8% vanadium, 0.5-1.75% aluminum, 0.25-1.5% iron, 0.1-0.2% oxygen, up to 0.15% silicon, up to 0.1% carbon, and less than 0.03% nitrogen, the balance being titanium and unavoidable impurities; beta forging and rolling the ingot to form a plate or slab; rolling said plate or slab to form a product; subjecting said article to alpha-beta solution heat treatment (SHT); Stress-relaxing the SHT treated article; This results in a titanium alloy product having a 0.2% yield strength of 600 to 850 MPa, an ultimate tensile strength of 700 to 950 MPa, a fracture elongation of 20 to 30%, and a reduction in area of ​​40 to 80%, and further having a Charpy U-notch impact energy of 30 to 70 J and / or a Charpy V-notch impact energy of 40 to 150 J.

10. 10. The method of claim 9, wherein the stress softened product comprises a 0.2% yield strength of 650-850 MPa, an ultimate tensile strength of 750-950 MPa, an elongation at break of 22-30%, and a reduction in area of ​​55-75%, and further comprises a Charpy U-notch impact energy of 40-60 J and / or a Charpy V-notch impact energy of 60-100 J.

11. 10. The method of claim 9, wherein the cross-sectional area of ​​the plate or slab is reduced by a minimum of 50% by alpha-beta rolling.

12. 12. The method of claim 11, further comprising reheating the plate for sizing, straightening or flattening, and stress relieving the SHT treated product at a temperature in the range of 500°C to 600°C.

13. 10. The method of claim 9, wherein the Charpy impact energy of the product is increased by alpha-beta rolling the plate or slab to at least 50% reduction in area, followed by reheating the product for sizing, straightening, flattening, and stress relieving the product at a temperature in the range of 500°C to 650°C.

14. 10. The method of claim 9, wherein the tensile ductility of the product is increased by alpha-beta rolling the plate or slab to a minimum of 50% reduction in area, reheating the plate to 50°C to 150°C below the beta transus for sizing, straightening or flattening the product, solution heat treating the product at 30°C to 100°C below the beta transus, cooling at a desired rate to obtain a desired strength, and stress relieving at a temperature in the range of 500°C to 650°C.

15. 10. The method of claim 9, wherein the vanadium is 5.9 to 8.0%.

16. 10. The method of claim 9, wherein the vanadium is 6.1 to 8.0%.

17. 10. The method of claim 9, wherein vanadium is 6.8-7.8%, aluminum is 0.9-1.5%, iron is 0.5-1.1%, oxygen is 0.12-0.19%, and silicon is 0.12% or less.

18. 10. The method of claim 9, wherein the vanadium is 7.3%, the aluminum is 1.2%, the iron is 0.8%, the silicon is 0.05%, and the oxygen is 0.16%.

Citation Information

Patent Citations

  • High strength and high toughness near-Beta type titanium alloy material and preparation and bar processing method thereof

    CN104711452A

  • JP1973040165A

  • Iv b group transition metal base metal sponge

    JP1990070034A

  • High strength beta-series titanium alloy having excellent corrosion resistance and stress corrosion cracking resistance

    JP1990138429A

  • Titanium alloys exhibiting resistance to impact or impact loads and methods of manufacturing parts therefrom

    JP2017508882A