Manufacturing method for low carbon ferrochrome

The use of a gas bottom blowing device in the production of low carbon ferrochrome enhances thermal and silicon efficiencies, allowing for higher chromium ore ratios and reduced power consumption, addressing the limitations of conventional methods.

JP7566744B2Active Publication Date: 2024-10-15JFE MATERIAL
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021533033
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-12
Filing Date
2020-07-10
Publication Date
2024-10-15
Estimated Expiration
2040-07-10

AI Technical Summary

Technical Problem

Conventional methods for producing low carbon ferrochrome face limitations in increasing the mass ratio of additional chromium ore to primary slag and result in high electric power consumption.

Method used

A method involving the use of a reaction vessel equipped with a gas bottom blowing device, where chromium ore and quicklime are melted, and a reducing agent is added, followed by inert gas bubbling to enhance thermal efficiency, silicon efficiency, and reactivity, allowing for a higher mass ratio of reloaded chromium ore to primary slag.

Benefits of technology

This approach increases the mass ratio of reloaded chromium ore to primary slag beyond 10%, reduces electric power consumption, and maintains high reaction temperatures, facilitating easier operations in subsequent processes while minimizing harmful hexavalent chromium generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566744000010
    Figure 0007566744000010
  • Figure 0007566744000011
    Figure 0007566744000011
  • Figure 0007566744000012
    Figure 0007566744000012
Patent Text Reader

Abstract

The present invention provides a method for producing low carbon ferrochromium, said method being capable of reducing the electric power consumption rate by increasing the mass ratio of additionally charged chromium ore with respect to a primary slag. A method for producing low carbon ferrochromium according to the present invention is provided with: a first step (S1) wherein chromium ore and quick lime are melted in an electric furnace; and a second step (S2) wherein a molten staring material (hereinafter referred to as a primary slag) melted in the first step (S1) is discharged into a reaction container that has a gas bottom-blowing device, and a reducing agent and a cold charge that contains additional chromium ore at a mass ratio of from 10% to 100% relative to the primary slag are charged into the reaction container, so that low carbon ferrochromium and a secondary slag are produced by stirring the materials by bottom-blowing an inert gas from the gas bottom-blowing device.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing low carbon ferrochromium. [Background technology]

[0002] Low-carbon ferrochrome, an Fe-Cr alloy containing 60% by mass or more of Cr and 0.1% by mass or less of C, is generally produced by reducing chromium ore with silicon. The so-called Perrin process is adopted as a specific production method. As shown in FIG. 7, the basic process of the Perrin process includes a first process in which chromium ore and quicklime are melted in an electric furnace, and a second process in which the melted raw material (hereinafter referred to as primary slag) melted in the first process is poured into a ladle, in which silicochrome is charged as a reducing agent and stirred to cause a reduction reaction to produce low-carbon ferrochrome and secondary slag. The stirring in the second process is usually performed by relay rings in which two ladles are prepared and the molten primary slag containing silicochrome is repeatedly transferred from one to the other.

[0003] The reduction reaction of reducing chromium ore with silicon is an exothermic reaction. In the conventional method for producing low-carbon ferrochrome, in order to effectively utilize the heat of reaction, chromium ore, which is a cold material, is added to a ladle and melted in the ladle, thereby reducing the unit power consumption and improving productivity (see Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 1-225743 Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the conventional method for producing low-carbon ferrochrome, in which molten metal is transferred between two ladles, there is a problem in that the mass ratio of the additional chromium ore to the primary slag (mass of additional chromium ore / mass of primary slag) can only be increased to 7-9% at most.

[0006] The present invention has been made in consideration of the above problems, and has an object to provide a method for producing low-carbon ferrochrome that can increase the mass ratio of additional chromium ore to primary slag and reduce the power consumption rate. [Means for solving the problem]

[0007] In order to solve the above problems, one aspect of the present invention includes a first step of melting chromium ore and quicklime in an electric furnace, a second step of pouring the melted raw material (hereinafter referred to as primary slag) melted in the first step into a reaction vessel having a bottom gas blowing device, charging a reducing agent and a cold material containing additional chromium ore in a mass ratio of 10% to 100% relative to the primary slag, and stirring the mixture by bottom blowing inert gas from the bottom gas blowing device to produce low-carbon ferrochromium and secondary slag. A third step of charging a reducing agent into the electric furnace or reaction vessel containing the secondary slag to generate recovered silicochrome and tertiary slag; Equipped with In the second step, the reaction end temperature of the low carbon ferrochromium and the molten secondary slag in the reaction vessel is 1620°C or higher and 1900°C or lower. This is a method for producing low carbon ferrochrome. Effect of the Invention

[0008] The present invention is based on the new finding that gas bubbling in a reaction vessel having a bottom gas blowing device can improve thermal efficiency, silicon efficiency, and reactivity of the reduction reaction. According to the present invention, by using a reaction vessel having a bottom gas blowing device, the mass ratio of additional chromium ore to primary slag can be increased to 10% or more, and the power consumption can be reduced. In addition, since a reaction vessel equipped with a bottom gas blowing device is used, even if the mass ratio of additional chromium ore to the primary slag is increased to 10% or more, the reaction end temperature of the molten metal in the reaction vessel can be kept at a high temperature of 1620°C to 1900°C. This makes it easier to operate the subsequent processes. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a process diagram of a method for producing low-carbon ferrochromium according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a diagram showing an entire facility used in the method for producing low carbon ferrochromium according to the present embodiment. [Diagram 3] FIG. 2 is a vertical sectional view of a reaction vessel used in the method for producing low carbon ferrochromium according to the present embodiment. [Figure 4] FIG. 4(a) is a vertical sectional view of a reaction vessel used in the method for producing low carbon ferrochromium according to the present embodiment (FIG. 4(a) shows an example in which the plug is disposed in the center of the bottom of the reaction vessel, and FIG. 4(b) shows an example in which the plug is disposed in the periphery of the bottom of the reaction vessel). [Diagram 5] FIG. 5(a) is a plan view of a plug of a reaction vessel used in the method for producing low-carbon ferrochromium of the present embodiment, and FIG. 5(b) is a vertical sectional view of the plug. [Figure 6] 1 is a graph showing the relationship between the basicity (CaO / SiO2) of secondary slag and the chromium content (Cr) by mass of the secondary slag in the second step of the manufacturing method of low-carbon ferrochromium according to the present embodiment. [Figure 7] FIG. 1 is a process diagram of a conventional method for producing low carbon ferrochromium. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, a method for producing low carbon ferrochrome according to an embodiment of the present invention will be described in detail with reference to the accompanying drawings. However, the method for producing low carbon ferrochrome according to the present invention can be embodied in various forms and is not limited to the embodiments described in the present specification. The present embodiment is provided with the intention of enabling those skilled in the art to fully understand the invention by fully disclosing the specification.

[0011] Fig. 1 is a process diagram of a method for producing low-carbon ferrochromium according to one embodiment of the present invention, and Fig. 2 is a diagram showing equipment used in the method for producing low-carbon ferrochromium according to the present embodiment.

[0012] As shown in FIG. 1, the method for producing low-carbon ferrochrome according to the present embodiment includes a first step (S1) of melting a mixture of chromium ore and quicklime as a flux in an electric furnace to produce a molten raw material (hereinafter referred to as primary slag).

[0013] As shown in Figure 2, chromium ore and quicklime are stored in a hopper 4. A fixed type electric furnace with a tapping port 1a provided at a position higher than the bottom of the furnace to form a basin is used as the electric furnace 1. The tapping port 1a may also be provided at the bottom of the furnace. The basin is formed in order to maintain a stable amount of heat even after the primary slag is tapped. The primary slag is tapped into a reaction vessel 2 from the tapping port 1a. The tapping temperature of the primary slag is a high temperature between 1400°C and 2000°C.

[0014] Next, as shown in Figures 1 and 2, the reaction vessel 2 from which the primary slag was discharged is charged with the auxiliary raw material silicochrome as a reducing agent, a cold material containing additional chromium ore of 10% to 100% by mass, preferably 15% to 65% by mass, relative to the primary slag, and a recovered silicochrome in an amount necessary for chromium reduction. Then, as shown in Figure 2, an inert gas such as Ar gas is blown from the bottom of the reaction vessel 2 from the bottom gas blowing device 2a to stir the mixture, reducing the oxides of the chromium ore to produce low-carbon ferrochrome and secondary slag. This reduction process is the second process (S2).

[0015] From the viewpoint of effectively utilizing the reaction heat of the reduction reaction, it is preferable to charge the silicochrome and the additional chromium ore in a mixed state or in a layered state of the silicochrome and the additional chromium ore into the reaction vessel 2, or it is preferable to charge the additional chromium ore into the reaction vessel 2 after charging the silicochrome into the reaction vessel 2.

[0016] In addition to the additional chromium ore, the cold material may include at least one of dust generated in the electric furnace 1, blowback metal generated in the reaction vessel 2 or the electric furnace 3, GP (undersize metal) generated in the reaction vessel 2 or the electric furnace 3, high chromium-containing slag generated in the reaction vessel 2 or the electric furnace 3, or chromium-containing raw material.

[0017] The recovered silicochrome is the silicochrome recovered in the third step described below, but other silicochromes may be used. Although silicochrome is used as the reducing agent, a silicon-based reducing agent such as metal silicon may be used in addition to silicochrome. Furthermore, an aluminum-based reducing agent such as aluminum or an aluminum alloy, a magnesium-based reducing agent such as magnesium or a magnesium alloy, or a calcium-based reducing agent such as calcium or a calcium alloy may be used in addition to the silicon-based reducing agent. Furthermore, a mixture of these reducing agents may be used.

[0018] In the reaction vessel 2, the reduction reaction between the chromium oxide of the chromium ore and silicon proceeds as follows. Cr2O3+3 / 2Si→2Cr+3 / 2SiO2…(1) Here, the liberated SiO2 reacts with quicklime as shown in the following equations (2) and (3) to produce secondary slag. CaO+SiO2→CaO·SiO2…(2) 2CaO+SiO2→2CaO·SiO2…(3) When secondary slag is generated as shown in equations (2) and (3), the amount of free SiO2 in equation (1) decreases, and the reduction reaction in equation (1) proceeds from left to right.

[0019] By using gas bubbling in the reaction vessel 2 having the bottom gas blowing device 2a with high stirring capacity, (1) the thermal efficiency, (2) the silicon efficiency, and (3) the reactivity of the reduction reaction can be improved as described below. Therefore, the mass ratio of the additional chromium ore to the primary slag can be increased to 10% or more.

[0020] (1) Since the reduction reaction is promoted by gas bubbling in the reaction vessel 2 having the bottom gas blowing device 2a, the heat loss in the reaction vessel 2 can be reduced (in other words, the thermal efficiency can be improved).

[0021] (2) Silicon efficiency can be improved by gas bubbling in the reaction vessel 2 having the bottom gas blowing device 2a. Silicon efficiency is the ratio of effectively reduced silicon (excluding silicon lost due to oxidation loss, etc.) that effectively works as a reducing agent, and is expressed as (amount of silicon used to reduce Cr and Fe oxides / amount of silicon input). Compared to relay ring, gas bubbling reduces the oxidation loss of silicon caused by contact between air and metal, and improves silicon efficiency accordingly. While the silicon efficiency in relay ring is about 80-85%, the silicon efficiency in gas bubbling is about 87-94%. This allows for a reduction in expensive silicon.

[0022] (3) Reactivity can also be improved by gas bubbling in the reaction vessel 2 equipped with the bottom gas blowing device 2a. If the amount of quicklime is reduced and basicity is lowered, the activity coefficient of SiO2 increases, the reduction reaction of chromium in equation (1) becomes less likely to occur, and the (Cr) mass% of the secondary slag becomes higher. However, as shown in Figure 6, the reduction reaction progresses due to gas bubbling in the bottom gas blowing device 2a, so the (Cr) mass% of the secondary slag can be lowered. Reducing the (Cr) mass% of the secondary slag allows for more advantageous operation. For example, even if the basicity is lowered to less than 1.65, it is possible to prevent a decrease in chromium yield.

[0023] The chromium oxide content (Cr2O3 mass%) of the secondary slag in the second step (S2) is adjusted to 10.0 mass% or less. The upper limit of the basicity (CaO / SiO2) of the secondary slag is adjusted to less than 1.65, preferably less than 1.5, and more preferably less than 1.4. By lowering the basicity of the secondary slag to less than 1.65, the basicity of the tertiary slag described below is lowered to less than 1.3, thereby preventing harmful hexavalent chromium from being generated in the tertiary slag. The lower the lower limit of the basicity of the secondary slag, the better, but in order to ensure reactivity in the third step (S3), the lower limit of the basicity of the secondary slag is set to 1.0 or more.

[0024] The reaction end temperature (temperature after the reaction is completed) of the molten metal of the low carbon ferrochrome and the secondary slag in the reaction vessel 2 is a high temperature of 1350°C or higher and 1900°C or lower.

[0025] Fig. 3 is a vertical cross-sectional view of a reaction vessel 2 having a bottom gas blowing device 2a. As shown in Fig. 3, refractories 8, 9 are provided on the bottom 6a of the steel shell 6 of the reaction vessel 2. A plug 19 of the bottom gas blowing device 2a is placed in the center of the bottom of the reaction vessel 2. When inert gas is introduced into the pipe portion 17 of the plug 19, the inert gas is blown into the reaction vessel 2 from the plug 19, and the molten metal in the reaction vessel 2 is stirred, i.e., gas bubbling is performed.

[0026] In the operation of the second step (S2), the reaction of formula (1) proceeds from the primary slag as described above. In the early stage of the operation, the primary slag is the main component in the reaction vessel 2. As the reaction proceeds, molten ferrochrome (metal 21) is produced, and the secondary slag 22 exists on the molten ferrochrome (metal 21). Eventually, the volume ratio of the secondary slag 22 to the metal 21 becomes approximately 4:1. In order to increase the reactivity in the presence of a large amount of highly viscous secondary slag 22, it is necessary to increase the stirring capacity, and for this purpose, a bottom gas blowing device 2a is used to blow inert gas into the bottom of the reaction vessel 2.

[0027] In general, when the molten metal is the main component, it is known that in order to improve the stirring efficiency, it is good to arrange the plug 19 of the bottom gas blowing device 2a at a position offset from the center of the bottom of the reaction vessel 2 (eccentric position) as shown in FIG. 4(b) (see, for example, JP-A-1-177333). However, when a large amount of highly viscous secondary slag 22 exists as in this embodiment, if the plug 19 of the bottom gas blowing device 2a is arranged at an eccentric position of the bottom of the reaction vessel 2 as shown in FIG. 4(b), the opposite side to the side where the plug 19 is arranged will be in a weakly stirred state, and unmelted additional chromium ore 23 will remain on the opposite side. In contrast, as shown in FIG. 4(a), by arranging the plug 19 of the bottom gas blowing device 2a at the center of the bottom of the reaction vessel 2, a flow of molten metal is formed that rises from the center of the bottom in the reaction vessel 2 and then radially moves toward the periphery. Therefore, the inside of the reaction vessel 2 can be uniformly stirred, and the additional chromium ore can be entrained and melted. A plurality of plugs may be arranged on a circle centered on the center of the bottom of the reaction vessel 2. In this manner, the inside of the reaction vessel 2 can be stirred uniformly.

[0028] FIG. 5(a) is a plan view of the plug 19, and FIG. 5(b) is a vertical cross-sectional view of the plug 19. The plug 19 includes a truncated cone-shaped main body 11 and a disk-shaped gas reservoir forming portion 12 provided at the bottom of the main body 11. A disk-shaped gas reservoir portion 13 is formed between the main body 11 and the gas reservoir forming portion 12. A pipe portion 17 is connected to the gas reservoir forming portion 12. The main body 11 is made of a refractory material containing MgO and / or Al2O3 to withstand the high temperature (1350°C or higher and 1900°C or lower) of the molten metal in the reaction vessel 2. The material of the main body 11 is, for example, 92% by mass MgO-4% by mass Cr2O3 or 98% by mass Al2O3-2% by mass MgO. The gas reservoir forming portion 12 and the pipe portion 17 are made of iron.

[0029] As shown in Fig. 5(a), a plurality of slits 15 for blowing out an inert gas are formed in the body 11 made of a refractory material. The slits 15 include a plurality of inner circumferential slits 15a arranged in a ring shape and a plurality of outer circumferential slits 15b arranged in a ring shape. As shown in Fig. 5(b), the slits 15 extend downward from the upper surface 11a and communicate with the gas reservoir 13 at the bottom.

[0030] As shown in FIG. 3, when an inert gas is introduced into the pipe portion 17 of the plug 19, the inert gas is blown into the reaction vessel 2 from the plug 19, and the molten metal of the low-carbon ferrochrome 21 and the slag 22 in the reaction vessel 2 is gas-bubbled.

[0031] As described above, the plug 19 is a slit-type plug. Compared to a porous plug, a slit-type plug has the characteristics of being superior in resistance to melting damage and having small bubbles at the outlet of the slit, resulting in strong stirring power. However, since stirring is possible, a porous plug may also be used.

[0032] The amount of gas blown into the plug 19, i.e., the amount of stirring gas Q (l / min), is set to 5 l / min or more and 1000 l / min or less per ton of molten metal. 5 l / min ≦ Q ≦ 1000 l / min is required to prevent the molten metal from penetrating the slit 15 of the plug 19 and to prevent gas from blowing through (gas blowing through in a straight line without being stirred). 5 l / min ≦ Q is required to smoothly proceed with the reduction reaction. Even if Q > 1000 l / min, it is ineffective in further progressing the reduction reaction, and instead the molten metal of low carbon ferrochrome 21 and slag 22 will cool. The amount of stirring gas Q is set according to the amount of additional chromium ore, and the larger the amount of additional chromium ore, the larger the value is set.

[0033] As shown in Fig. 1 again, the molten low-carbon ferrochrome produced by the reduction reaction is poured into a mold to become a product. The low-carbon ferrochrome product contains 60 mass% or more of Cr, 1.0 mass% or less of Si, and 0.1 mass% or less of C. Meanwhile, the molten secondary slag produced by the reduction reaction is separated from the molten low-carbon ferrochrome and then charged into an electric furnace 3.

[0034] Next, as shown in FIG. 1, ferrosilicon as a reducing agent is charged into the electric furnace 3 in which the secondary slag is charged, and reacts with the chromium oxide remaining in the secondary slag to generate recovered silicochrome and tertiary slag. This step is the third step (S3). Silica (SiO2) may be added to the electric furnace 3 to adjust the basicity. In addition, solidified slag containing chromium oxide that has been buried in the factory or left in the factory and solidified may be added to the electric furnace 3. The solidified slag includes slag that has solidified secondary slag produced in a previous low-carbon ferrochrome operation (secondary slag produced by relay ring using two conventional ladles and / or secondary slag produced by gas bubbling using the reaction vessel 2 of this embodiment) and contains chromium oxide.

[0035] The electric furnace 3 may be provided with a bottom gas blowing device. Instead of the electric furnace 3, a reaction vessel into which an inert gas is blown may be used. The reaction vessel may be a reaction vessel having a bottom gas blowing device, or a top-blown reaction vessel into which an inert gas is blown from a lance. The bottom gas blowing device provided in the electric furnace 3 or reaction vessel is preferably disposed in the center of the bottom of the electric furnace 3 or reaction vessel, similar to the bottom gas blowing device 2a of the reaction vessel 2 in the second step described above. The volume ratio of the slag (secondary slag 22) to the metal (low carbon ferrochrome 21) in the second step (S2) is about 4:1, whereas the volume ratio of the slag (tertiary slag) to the metal (recovered silicochrome) in the third step (S3) is about 10:1. In order to increase the stirring force of the molten metal in the third step (S3), it is desirable to make the amount of stirring gas (l / min) per ton of molten metal in the third step (S3) greater than the amount of stirring gas (l / min) per ton of molten metal in the second step (S2).

[0036] In the third step (S3), a large amount of ferrosilicon as a reducing agent, i.e., at least one time, preferably at least two times, the reduction equivalent of chromium oxide is charged, and strong reduction is performed to reduce the chromium oxide content of the tertiary slag to 1.4 mass% or less, preferably to 1.0 mass% or less. This is to reduce the hexavalent chromium in the tertiary slag and to improve the chromium yield. The Si content of the recovered silicochromium is 20 mass% or more and 70 mass% or less. Although ferrosilicon is used as the reducing agent, a silicon-based reducing agent such as metal silicon may be used in addition to ferrosilicon. In addition to the silicon-based reducing agent, an aluminum-based reducing agent such as aluminum or an aluminum alloy, a magnesium-based reducing agent such as magnesium or a magnesium alloy, or a calcium-based reducing agent such as calcium or a calcium alloy may be used. Furthermore, a mixture of these reducing agents may be used.

[0037] The basicity of the tertiary slag is adjusted to be lower than 1.3, preferably lower than 1.2, and more preferably lower than 1.1. When the basicity is lowered, it is thought that the hexavalent chromium compound (CaO CrO3) that bonds with CaO is removed, and the hexavalent chromium compound is converted to a trivalent chromium compound (Cr2O3), as shown in the following equation (4). 2(CaO·CrO3)+2SiO2→2(CaO·SiO2)+Cr2O3+3 / 2O2…(4)

[0038] Here, the lower limit of the basicity of the tertiary slag is preferably as low as possible, but in order to reduce the chromium content of the tertiary slag, it is set to 0.7 or more, preferably 0.8 or more, and more preferably 0.9 or more.

[0039] Table 1 shows the relationship between the basicity (CaO / SiO2) of the secondary slag and the basicity (CaO / SiO2) of the tertiary slag. When no auxiliary material for adjusting the basicity (CaO / SiO2) is added in the third step (S3), there is a positive correlation between the basicity of the secondary slag and the basicity of the tertiary slag. As shown in Table 1, if the basicity of the secondary slag is less than 1.65, the basicity of the tertiary slag can be reduced to less than 1.3. On the other hand, if the basicity of the secondary slag is greater than 1.65, the basicity of the tertiary slag will exceed 1.3. [Table 1]

[0040] A method for quantifying the chromium oxide content of the slag and a method for quantifying the basicity of the slag will be described. The chromium oxide content of the slag is the Cr content of the slag converted into oxide. Specifically, the total amount of chromium oxide is Cr2O3, and the chromium oxide content = Cr content x 152 / 104. In this embodiment, the chromium oxide content of the tertiary slag is set to 1.4 mass% or less, which means that the chromium content of the tertiary slag is set to 1.4 x 104 / 152 = 0.96 ≒ 1 mass% or less. The chromium content of the slag is expressed as ((Cr) mass%). The chromium oxide content of the slag is expressed as (Cr2O3 mass%). The Cr content of the slag is quantified by ICP (Inductively Coupled Plasma) emission spectroscopy. In this analysis method, the decomposition of the sample is based on "JIS G1313-1 2012 Decomposition by Alkali Fusion".

[0041] The basicity of slag (CaO / SiO2) is expressed as the CaO content of slag / SiO2 content of slag. The CaO content of slag is the Ca content of slag converted into oxide, and is calculated as CaO content = Ca content x 56 / 40. The SiO2 content of slag is the Si content of slag converted into oxide, and is calculated as SiO2 content = Si content x 60 / 28. The method for quantifying Ca and Si in slag is ICP (Inductively Coupled Plasma) emission spectrometry. In this analysis method, the sample is decomposed according to "JIS G1313-1 2012 Decomposition by alkali fusion".

[0042] As shown in FIG. 1 again, the recovered silicochrome is charged into the reaction vessel 2 together with the auxiliary silicochrome. Since a part of the auxiliary silicochrome is replaced by the recovered silicochrome, the auxiliary silicochrome is reduced. The recovered silicochrome may be charged into the electric furnace 3 or reaction vessel in the third step (S3) and used as a partial replacement for ferrosilicon. The tertiary slag is used as roadbed material or fertilizer, or is buried in a factory. The amount (concentration) of hexavalent chromium eluted from the tertiary slag is 0.05 mg / l or less.

[0043] The method for producing low carbon ferrochromium according to the present embodiment has been described above. The method for producing low carbon ferrochromium according to the present embodiment has the following advantages.

[0044] Gas bubbling in the reaction vessel 2 having the bottom gas blowing device 2a can improve (1) heat efficiency, (2) silicon efficiency, and (3) reactivity of the reduction reaction. Therefore, the amount of additional chromium ore can be increased to 10% or more, and the power consumption can be reduced.

[0045] Since the amount of stirring gas Q of the bottom gas blowing device 2a is 5 L / min or more per ton of molten metal, it is possible to prevent the molten metal from penetrating the slit 15 of the plug 19, and the reduction reaction can proceed smoothly. Also, since the amount of stirring gas Q of the bottom gas blowing device 2a is 1000 L / min or less, it is possible to prevent the gas from blowing through (gas blowing through in a straight line without being stirred), and it is possible to prevent the molten low-carbon ferrochrome and secondary slag from cooling.

[0046] Since the reaction vessel 2 having the bottom gas blowing device 2a is used, even if the basicity in the second step is lowered to less than 1.65, the chromium yield is prevented from decreasing. If the basicity in the second step is less than 1.65, the basicity of the tertiary slag in the third step can be reduced to less than 1.3, and the generation of harmful hexavalent chromium in the tertiary slag can be suppressed.

[0047] Since a reaction vessel 2 having a bottom gas blowing device 2a is used, even if the mass ratio of the additional chromium ore to the primary slag is increased to 10% or more, the reaction end temperature of the molten metal in the reaction vessel 2 can be kept at a high temperature of 1350°C to 1900°C. This makes it easier to operate the subsequent processes.

[0048] One plug 19 of the bottom gas blowing device 2a is arranged in the center of the bottom of the reaction vessel 2, and / or multiple plugs 19 of the bottom gas blowing device 2a are arranged on a circle centered on the center of the bottom of the reaction vessel 2, so that the reaction vessel 2 can be uniformly stirred and the additional chromium ore can be easily entrained and dissolved.

[0049] It is desirable to use a slit-type plug for the plug 19, which has excellent resistance to melting damage and high stirring capacity.

[0050] The silicochrome and the additional chromium ore are charged into the reaction vessel 2 in a mixed state, or in a layered state, or after the silicochrome is charged into the reaction vessel 2, the additional chromium ore is charged into the reaction vessel 2, so that the reaction heat of the reduction reaction can be effectively used for dissolving the additional chromium ore. Example 1

[0051] Low carbon ferrochrome was produced according to the production process diagram in Figure 1. Table 2 shows the composition of the chromium ore, which was the raw material used in this example. [Table 2]

[0052] 1000kg of chromium ore and 830kg of quicklime were charged into a stationary electric furnace and melted to produce primary slag. The primary slag was tapped into a reaction vessel, into which 750kg of additional chromium ore, 310kg of auxiliary raw material silicochrome, and 260kg of recovered silicochrome were charged. Argon gas was then blown into the bottom of reaction vessel 2 to stir the mixture. The reaction end temperature of the molten metal in reaction vessel 2 was 1650°C. The secondary slag produced was then separated, and the resulting molten metal of 1000kg of low-carbon ferrochrome was cast into a mold to produce the product. Table 3 shows the composition of the product low-carbon ferrochrome. The method for quantifying each component of ferrochrome is standardized in "JIS G1301-1~5 2012".

[0053] [Table 3]

[0054] Meanwhile, the separated secondary slag was received in a reactor, 230 kg of ferrosilicon was charged, and argon gas was blown into the reactor from the bottom and stirred. The generated tertiary slag and the recovered silicochrome were then separated, yielding 1930 kg of tertiary slag and 260 kg of recovered silicochrome. This recovered silicochrome was charged into the primary slag together with the auxiliary raw material silicochrome. Table 4 shows the composition of the tertiary slag, and Table 5 shows the composition of the recovered silicochrome.

[0055] [Table 4]

[0056] [Table 5] The power consumption rate was a low value of 2200 kWh / t. The power consumption rate is the amount of electricity used per ton of product, specifically (amount of electricity used for the primary slag melting / amount of product produced). Example 2

[0057] Low carbon ferrochrome was produced according to the manufacturing process diagram in Figure 1. As shown in Table 6, the make-up rate was set to 13% in operation 1, 21% in operation 2, 40% in operation 3, and 65% in operation 4. As shown in Table 6, even when the make-up rate was increased from 13% to 65%, the basicity of the tertiary slag was 1.0, and the generation of harmful hexavalent chromium in the tertiary slag was suppressed. The power consumption rate was a low value of 2400Kwh / t or less, and the higher the make-up rate was, the more the power consumption rate could be reduced. [Table 6] (Conventional example)

[0058] Low carbon ferrochrome was produced according to the production process diagram in Figure 7. This low carbon ferrochrome production process differs from the present embodiment in that the reduction of the primary slag is performed by relay ring, additional chromium ore is not charged to the primary slag, and the operation of recovering silicochrome from the secondary slag and adding it to the primary slag is not performed. Table 7 shows the composition of the chromium ore, which is the raw material used in the conventional example.

[0059] [Table 7]

[0060] 1740kg of chromium ore and 1060kg of quicklime were charged into an electric furnace and melted to produce the primary slag. The primary slag was tapped into a ladle, and 600kg of the auxiliary raw material silicochrome was charged without adding any additional chromium ore. The mixture was then stirred with a relay ring. 2200kg of the secondary slag was separated, and the resulting molten low-carbon ferrochrome (1000kg) was cast into a mold to produce the product. Table 8 shows the composition of the product low-carbon ferrochrome, and Table 9 shows the composition of the secondary slag.

[0061] [Table 8]

[0062] [Table 9] The electricity consumption rate was high at 2,980 kWh / t.

[0063] This specification is based on Japanese Patent Application No. 2019-130322, filed on July 12, 2019, the entire contents of which are incorporated herein by reference. [Explanation of symbols]

[0064] S1…1st process S2…Second process 2. Reaction vessel 2a…Bottom gas blowing device 11...Plug body 15...Slit 19…Plug

Claims

1. A first step of melting chromium ore and quicklime in an electric furnace; A second step is to pour the melted raw material (hereinafter referred to as primary slag) melted in the first step into a reaction vessel having a bottom gas blowing device, charge a reducing agent and a cold material containing additional chromium ore in a mass ratio of 10% to 100% relative to the primary slag, and stir the mixture by bottom blowing an inert gas from the bottom gas blowing device to produce low carbon ferrochromium and secondary slag; and a third step of charging a reducing agent into the electric furnace or reaction vessel containing the secondary slag to generate recovered silicochrome and tertiary slag. The method for producing low-carbon ferrochromium, wherein a reaction end temperature of the low-carbon ferrochromium and the molten secondary slag in the reaction vessel in the second step is 1620° C. or higher and 1900° C. or lower.

2. 2. The method for producing low carbon ferrochromium according to claim 1, wherein the amount of the agitating gas in the bottom gas blowing device is 5 L / min or more and 1000 L / min or less per ton of molten metal.

3. The chromium oxide content of the secondary slag (Cr 2 O 3 mass%) is 10.0 mass% or less, and basicity (CaO / SiO 2 3. The method for producing low carbon ferrochromium according to claim 1, wherein the ratio of Cr to Cu is adjusted to less than 1.

65.

4. 4. The method for producing low carbon ferrochromium according to claim 1, wherein one plug of the bottom gas blowing device for blowing out the inert gas is disposed at a center of a bottom of the reaction vessel, and / or a plurality of plugs of the bottom gas blowing device for blowing out the inert gas are disposed on a circle centered at the center of a bottom of the reaction vessel.

5. 5. The method for producing low carbon ferrochromium according to claim 1, wherein the bottom gas blowing device is provided with a slit type plug having a plurality of slits for blowing out the inert gas.

6. The slit type plug is made of MgO and / or Al 2 O 3 The body is made of a refractory material including 6. The method for producing low carbon ferrochrome according to claim 5, wherein the plurality of slits are formed in the body made of the refractory material.

7. The method for producing low carbon ferrochrome according to any one of claims 1 to 6, characterized in that the reducing agent and the additional chromium ore are mixed together or the reducing agent and the additional chromium ore are layered and charged into the reaction vessel, or the reducing agent is charged into the reaction vessel, and then the additional chromium ore is charged into the reaction vessel.

Citation Information

Patent Citations

  • Manufacture of low-carbon ferrochrome

    JP1989225743A

  • Production of low-carbon ferrochromium

    JP1993051690A

  • Chromium-containing metal and production method therefor

    JP2003049235A

  • Decarbonizing method for silicochromium

    JP2011094210A

  • Gas blowing plug and production method thereof

    JP2012041618A