An amorphous polymer (P) comprising segments (S1), (S2), and (S3).
An amorphous polymer with specific segment ratios and production method enhances solvent resistance and solubility, overcoming the limitations of existing polyarylene ether sulfone polymers in chemical and process applications.
Patent Information
- Application Number
- JP2021558900
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-01
- Filing Date
- 2020-03-10
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-03-10
AI Technical Summary
Existing polyarylene ether sulfone polymers exhibit poor resistance to organic solvents such as FAM B and Skydrol, limited solubility in common solvents like N-methylpyrrolidone (NMP) or dimethylacetamide (DMAc), and are not transparent, posing challenges in membrane production and application.
An amorphous polymer containing 80-90 mol% segments with sulfone groups and 10-20 mol% segments with ketone groups, produced through a polycondensation reaction using specific aromatic dihalogen and dihydroxy compounds in the presence of potassium carbonate and an aprotic polar solvent, ensuring good chemical resistance and solubility in common solvents.
The resulting amorphous polymer demonstrates excellent chemical resistance to organic solvents, good solubility in common solvents, and transparency, addressing the limitations of prior polymers in terms of solvent resistance and processability.
Smart Images

Figure 0007566772000001 
Figure 0007566772000002 
Figure 0007566772000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an amorphous polymer (P) comprising a segment (S1) containing a sulfone group, a segment (S2) containing a ketone group, and a segment (S3) containing a polyarylene group. The present invention further relates to a method for producing said amorphous polymer (P), a composition comprising said amorphous polymer (P), and an article comprising said amorphous polymer (P). [Background technology]
[0002] Polyarylene ether sulfone polymers are high-performance thermoplastics in that they are characterized by high heat resistance, good mechanical properties, and inherent flame retardancy (EM Koch, H.-M. Walter, Kunststoffe 80 (1990) 1146; E. Doering, Kunststoffe 80, (1990) 1149; N. Inchaurondo-Nehm, Kunststoffe 98, (2008) 190). Polyarylene ethers are highly biocompatible and are therefore also used as materials for forming dialysis membranes (NA Hoenich, KP Katapodis, Biomaterials 23 (2002) 3853).
[0003] The polyarylene ether sulfone polymers can be formed, inter alia, by either the hydroxide method, in which a salt is first formed from a dihydroxy component and a hydroxide, or by the carbonate method.
[0004] General information regarding the formation of polyarylene ether sulfone polymers by the hydroxide method can be found, inter alia, in RN Johnson et al., J. Polym. Sci. A-1 5 (1967) 2375, while the carbonate method is described in JE McGrath et al., Polymer 25 (1984) 1827.
[0005] Methods for forming polyarylene ether sulfone polymers from aromatic bishalogen compounds and aromatic bisphenols or their salts in the presence of one or more alkali metal or ammonium carbonates or bicarbonates in aprotic solvents are known to those skilled in the art and are described, for example, in EP-A 297 363.
[0006] High performance thermoplastics, such as polyarylene ether sulfone polymers, are formed by polycondensation reactions, typically carried out at high reaction temperatures in dipolar aprotic solvents such as dimethylformamide (DMF), dimethylacetamide (DMAc), sulfolane, dimethylsulfoxide (DMSO), and N-methyl-2-pyrrolidone (NMP).
[0007] The application of polyarylene ether sulfone polymers in polymer membranes is becoming increasingly important.
[0008] The polyarylene ether sulfone polymers are amorphous and have poorer resistance to organic fluids such as FAM B (a toluene-containing test fluid) or Skydrol (a mixture of phosphate esters) than semi-crystalline polymers such as polyphenylene sulfide.
[0009] To improve the resistance to organic solvents, EP2225328 describes semicrystalline polymers containing sulfonyl, ketone and polyarylene groups. According to EP2225328, 4,4'-dichlorodiphenylsulfone, 4,4'-dichlorobenzophenone and 4,4'-dihydroxybiphenyl are preferably reacted in diphenylsulfone to obtain semicrystalline polymers. The melting point of the semicrystalline polymer according to EP2225328 is above 300°C. However, the polymers described in EP2225328 show poor solubility in common solvents such as N-methylpyrrolidone (NMP) or dimethylacetamide (DMAc), which therefore creates problems when using these polymers to produce membranes by phase inversion.
[0010] Furthermore, the polymers described in EP 2225328 are not transparent.
[0011] JP2008-37897 discloses a sulfonic acid group-containing photocrosslinkable polymer which may contain sulfone groups, ketone groups, and polyarylene groups.
[0012] The article "Synthesis and characterization of novel poly(aryl ether sulfone ketone)s containing phthalazinone and biphenyl moieties" by LH Xiao et al., Chin. Chem. Lett. 19 (2008) 227, discloses the preparation of amorphous poly(phthalazinone ether sulfone ketone)s by reacting, inter alia, 4,4'-biphenol (BP), 4,4'-dichlorobenzosulfone (DCS), and 4,4'-difluorobenzophenone (DFK).
[0013] CN103613763 and CN104497300 describe the synthesis of semi-crystalline, high flow polyphenylene ether sulfone ketones that contain sulfone groups, ketone groups, and polyarylene groups.
[0014] GB 2241245 discloses amorphous polysulfone ether ketone polymers containing sulfone groups, ketone groups, and polyarylene groups, in which the molar ratio of sulfone groups to ketone groups is 1:1. [Prior art documents] [Patent documents]
[0015] [Patent Document 1] EP-A297363 [Patent Document 2] EP2225328 [Patent Document 3] JP2008-37897 [Patent Document 4] CN103613763 [Patent Document 5] CN104497300 [Patent Document 6] GB2241245 [Non-patent literature]
[0016] [Non-Patent Document 1] E.M.Koch, H.-M.Walter, Kunststoffe 80(1990)1146 [Non-Patent Document 2] E.Doering, Kunststoffe 80, (1990)1149 [Non-Patent Document 3] N.Inchaurondo-Nehm, Kunststoffe 98, (2008)190 [Non-Patent Document 4] NAHoenich, KPKatapodis, Biomaterials 23(2002)3853 [Non-Patent Document 5] RN Johnson et al., J. Polym. Sci. A-1 5 (1967) 2375 [Non-Patent Document 6] JE McGrath et al., Polymer 25 (1984) 1827 [Non-Patent Document 7] LHXiao et al., Chin.Chem.Lett.19 (2008) 227 “Synthesis and characterization of novel poly(aryl ether sulfone ketone)scontaining phthalazinone and biphenyl moieties” Summary of the Invention [Problem to be solved by the invention]
[0017] It is therefore an object of the present invention to provide an amorphous polymer (P) which does not have the disadvantages of the prior art or which has the disadvantages of the prior art reduced. The amorphous polymer (P) should exhibit good chemical resistance to organic solvents such as FAM B or Skydrol. Another object of the present invention is to provide a process for preparing said amorphous polymer (P). This process should preferably be carried out within a short reaction time. [Means for solving the problem]
[0018] The purpose of this is to formula [ka] segment (S1) and; formula [ka] segment (S2) and; formula [ka] Segment (S3) and This is realized by an amorphous polymer (P) containing
[0019] The purpose of this is to formula [ka] Segment (S1), formula [ka] Segment (S2) of formula [ka] Segment (S3) and An amorphous polymer (P) comprising Based on the total number of moles of the segments (S1) and (S2) contained in the amorphous polymer (P), 80 to 90 mol % of segment (S1), and 10 to 20 mol% of segment (S2) This is further realized by the amorphous polymer (P), which comprises
[0020] Surprisingly, it has been found that the amorphous polymer (P) exhibits good chemical resistance to organic solvents such as FAM B or Skydrol, and that the amorphous polymer exhibits good solubility in common solvents such as N-methylpyrrolidone (NMP) or dimethylacetamide (DMAc). Furthermore, articles made with the amorphous polymer (P) are transparent. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The invention is described in more detail below.
[0022] The amorphous polymer (P) according to the invention generally comprises segments (S1), (S2) and (S3) as defined above. The segments (S1), (S2) and (S3) may be present in the amorphous polymer (P) according to the invention in its backbone, in its chain ends and / or in its repeating units. Preferably, the segments (S1), (S2) and (S3) are included in the repeating units of the amorphous polymer (P). The amorphous polymer (P) according to the invention is preferably obtained from two or more repeating units. More preferably, it is obtained from two different repeating units.
[0023] In a preferred embodiment, the amorphous polymer (P) comprises 80 to 90 mol%, more preferably 80.1 to 89 mol%, even more preferably 80.2 to 88 mol%, particularly preferably 80.3 to 87 mol%, and most preferably 80.4 to 86.5 mol% of the segment (S1), and 10 to 20 mol%, more preferably 11 to 19.9 mol%, even more preferably 12 to 19.8 mol%, particularly preferably 13 to 19.7 mol%, and most preferably 13.5 to 19.6 mol% of the segment (S2), based on the total number of moles of the segment (S1) and the segment (S2) contained in the amorphous polymer (P) in each case.
[0024] Therefore, another object of the present invention is to Based on the total number of moles of the segment (S1) and the segment (S2) contained in the amorphous polymer (P), 80 to 90 mol % of segment (S1), and 10 to 20 mol% of segment (S2) The amorphous polymer (P) comprises:
[0025] In another preferred embodiment, the ratio of the number of moles of segment (S1) to the number of moles of segment (S2) contained in the amorphous polymer (P) is 4 to 9, more preferably 4.02 to 8.09, even more preferably 4.05 to 7.33, particularly preferably 4.08 to 6.69, and most preferably 4.10 to 6.41.
[0026] The term "amorphous" in the context of the amorphous polymer (P) according to the invention in a preferred embodiment is defined as follows: In a preferred embodiment, the term "amorphous" means that the amorphous polymer (P) has a melting enthalpy ΔH in the range of 0 to 5 W / g, preferably in the range of 0 to 4 W / g, even more preferably in the range of 0 to 3 W / g, particularly preferably in the range of 0 to 2.5 W / g, most preferably in the range of 0 to 2 W / g. m In another most preferred embodiment, the amorphous polymer (P) does not exhibit a melting point. In this case, the enthalpy of fusion ΔHm is 0. The abbreviation W / g stands for watts per gram.
[0027] The term "amorphous" in the context of the amorphous polymer (P) according to the invention in a preferred embodiment is further defined as follows: In a preferred embodiment, the term "amorphous" further means that the amorphous polymer (P) has a crystallization enthalpy ΔH in the range of 0 to 5 W / g, preferably in the range of 0 to 4 W / g, even more preferably in the range of 0 to 3 W / g, particularly preferably in the range of 0 to 2.5 W / g, most preferably in the range of 0 to 2 W / g. c In another most preferred embodiment, the amorphous polymer (P) does not exhibit a crystallization point. In this case, the crystallization enthalpy ΔH m is 0. The abbreviation W / g stands for watts per gram.
[0028] Enthalpy of fusion ΔH m (if present) and crystallization enthalpy ΔH c The enthalpy of fusion ΔH (if present) is measured by DSC (differential scanning calorimetry) starting at 20° C. by heating a sample of the amorphous polymer (P) at a rate of 20 K / min to a temperature of 360° C., followed by cooling at a rate of >100 K / min to 20° C., followed by a second heating at a rate of 20 K / min to 360° C., followed by a second cooling at a rate of >100 K / min to 20° C. m and crystallization enthalpy ΔH c is measured during the second heating and second cooling.
[0029] Annealing of an amorphous polymer (P) at 250 °C for 0.5 h resulted in an enthalpy of fusion ΔH in the range of 0.1 to <4 W / g in some cases. m Small phase transitions (melting points) indicating the presence of a crystalline enthalpy ΔH in the range of 0.1 to <4 W / g may be detected by DSC. Annealing of amorphous polymers (P) at 250 °C for 0.5 h may also result in small phase transitions (melting points) indicating the presence of a crystalline enthalpy ΔH in the range of 0.1 to <4 W / g. c It may be possible to detect small phase transitions (crystallization points) that indicate
[0030] If the amorphous polymer (P) is not annealed, in a preferred embodiment, the melting point cannot be detected by DSC (using the method described above). If the amorphous polymer (P) is not annealed, in a preferred embodiment, the crystallization point cannot be detected by DSC (using the method described above).
[0031] Repeating unit (RU1) The amorphous polymer (P) as described above may comprise a repeating unit (RU1) obtainable by reaction of at least one aromatic dihalogen compound (D1,1) comprising at least one segment (S1) with at least one aromatic dihydroxy compound (aDHy1). The aromatic dihalogen compound (D1,1) is also called "aromatic dihalogen sulfone compound (D1,1)". These terms are used synonymously and have the same meaning. The repeating unit (RU1) comprises a segment (S1). The repeating unit (RU1) may comprise two or more segments (S1). In a preferred embodiment, the repeating unit (RU1) comprises one segment (S1). The repeating unit (RU1) may also comprise a segment (S2) and / or a segment (S3). It may also comprise no segment (S2) and no segment (S3). In a preferred embodiment, the repeating unit (RU1) comprises a segment (S1) and a segment (S2) or a segment (S3). In a more preferred embodiment, the repeating unit (RU1) comprises a segment (S1) and a segment (S3).
[0032] In a particularly preferred embodiment, the repeating unit (RU1) consists of the segment (S1) and the segment (S2) or the segment (S3). In a most preferred embodiment, the repeating unit (RU1) consists of the segment (S1) and the segment (S3).
[0033] The aromatic dihalogen compound (D1,1) from which the repeating unit (RU1) can be obtained is preferably 4,4'-dihalodiphenylsulfone or 4,4'-bis[(4-chlorophenyl)sulfonyl]-1,1'-biphenyl. More preferably, it is 4,4'-dihalodiphenylsulfone. Even more preferably, the 4,4'-dihalodiphenylsulfone is selected from the group consisting of 4,4'-dichlorodiphenylsulfone, 4,4'-difluorodiphenylsulfone, and mixtures thereof, with 4,4'-dichlorodiphenylsulfone being particularly preferred.
[0034] The aromatic dihydroxy compound (aDHy1) from which the repeating unit (RU1) can be obtained is preferably 4,4'-biphenol, 4,4'-dihydroxybenzophenone, or a mixture thereof, with 4,4'-biphenol being particularly preferred.
[0035] In a particularly preferred embodiment, the repeating unit (RU1) is obtained by reaction of the monomers 4,4'-dichlorodiphenylsulfone and 4,4'-biphenol.
[0036] Repeating unit (RU2) The amorphous polymer (P) as described above may comprise a repeating unit (RU2) obtainable by reaction of at least one aromatic dihalogen compound (D2,1) comprising at least one segment (S2) with at least one aromatic dihydroxy compound (aDHy2). The aromatic dihalogen compound (D2,1) is also called "aromatic dihalogen ketone (D2,1)". These terms are used synonymously and have the same meaning. The repeating unit (RU2) comprises a segment (S2). The repeating unit (R2) may comprise two or more segments (S2). In a preferred embodiment, the repeating unit (RU2) comprises one segment (S2). The repeating unit (RU2) may also comprise a segment (S1) and / or a segment (S3). It may also be free of segments (S1) and (S3). In a preferred embodiment, the repeating unit (RU2) comprises a segment (S2) and a segment (S1) or a segment (S3). In a more preferred embodiment, the repeating unit (RU2) comprises a segment (S2) and a segment (S3).
[0037] In a particularly preferred embodiment, the repeating unit (RU2) consists of the segment (S2) and the segment (S1) or the segment (S3). In a most preferred embodiment, the repeating unit (RU2) consists of the segment (S2) and the segment (S3).
[0038] The aromatic dihalogen compound (D2,1) from which the repeating unit (RU2) can be obtained is preferably 4,4'-dihalobenzophenone. More preferably, the 4,4'-dihalobenzophenone is selected from the group consisting of 4,4'-dichlorobenzophenone, 4,4'-difluorobenzophenone, and mixtures thereof, with 4,4'-dichlorobenzophenone being particularly preferred.
[0039] The aromatic dihydroxy compound (aDHy2) from which the repeating unit (RU2) can be obtained is preferably 4,4'-biphenol, 4,4'-dihydroxybenzophenone, or a mixture thereof, with 4,4'-biphenol being particularly preferred.
[0040] In a particularly preferred embodiment, the repeating unit (RU2) is obtained by reaction of the monomers 4,4'-dichlorobenzophenone and 4,4'-biphenol.
[0041] Repeating unit (RU3) The amorphous polymer (P) as described above may comprise a repeating unit (RU3) obtainable by reaction of at least one aromatic dihydroxy compound (D2,2) containing at least one segment (S2) with at least one aromatic dihalogen compound (aDHa1). The repeating unit (RU3) comprises a segment (S2). The repeating unit (R3) may comprise two or more segments (S2). In a preferred embodiment, the repeating unit (RU3) comprises one segment (S2). The repeating unit (RU3) may also comprise a segment (S1) and / or a segment (S3). It may also not comprise a segment (S1) and a segment (S3). In a preferred embodiment, the repeating unit (RU3) comprises a segment (S2) and a segment (S1) or a segment (S3). In a more preferred embodiment, the repeating unit (RU3) comprises a segment (S2) and a segment (S1).
[0042] In a particularly preferred embodiment, the repeating unit (RU3) consists of the segment (S2) and the segment (S1) or the segment (S3). In a most preferred embodiment, the repeating unit (RU3) consists of the segment (S2) and the segment (S1).
[0043] The aromatic dihydroxy compound (D2,2) from which the repeating unit (RU3) can be obtained is preferably 4,4'-dihydroxybenzophenone.
[0044] The aromatic dihalogen compound (aDHa1) is preferably 4,4'-dihalodiphenylsulfone or 4,4'-bis[(4-chlorophenyl)sulfonyl]-1,1'-biphenyl. More preferably, it is 4,4'-dihalodiphenylsulfone. Even more preferably, the 4,4'-dihalodiphenylsulfone is selected from the group consisting of 4,4'-dichlorodiphenylsulfone, 4,4'-difluorodiphenylsulfone, and mixtures thereof, with 4,4'-dichlorodiphenylsulfone being particularly preferred.
[0045] In a particularly preferred embodiment, the repeating unit (RU3) is obtained by reaction of the monomers 4,4'-dihydroxybenzophenone and 4,4'-dichlorodiphenylsulfone.
[0046] Repeating unit (RU4) The amorphous polymer (P) as described above may comprise a repeating unit (RU4) obtainable by reaction of at least one aromatic dihydroxy compound (D3,1) containing at least one segment (S3) with at least one aromatic dihalogen compound (aDHa2). The repeating unit (RU4) comprises a segment (S3). The repeating unit (R4) may comprise two or more segments (S3). In a preferred embodiment, the repeating unit (RU4) comprises one segment (S3). The repeating unit (RU4) may also comprise a segment (S1) and / or a segment (S2). It may also not comprise a segment (S1) and a segment (S2). In a preferred embodiment, the repeating unit (RU4) comprises a segment (S3) and a segment (S1) or a segment (S2). In a more preferred embodiment, the repeating unit (RU4) comprises a segment (S3) and a segment (S1).
[0047] In a particularly preferred embodiment, the repeating unit (RU4) consists of the segment (S3) and the segment (S1) or the segment (S2). In a most preferred embodiment, the repeating unit (RU4) consists of the segment (S3) and the segment (S1). In this case, the repeating unit (R4) is equal to the repeating unit (RU1).
[0048] The aromatic dihydroxy compound (D3,1) from which the repeating unit (RU4) can be obtained is preferably 4,4'-biphenol.
[0049] The aromatic dihalogen compound (aDHa2) is preferably 4,4'-dihalodiphenylsulfone or 4,4'-bis[(4-chlorophenyl)sulfonyl]-1,1'-biphenyl. More preferably, it is 4,4'-dihalodiphenylsulfone. Even more preferably, the 4,4'-dihalodiphenylsulfone is selected from the group consisting of 4,4'-dichlorodiphenylsulfone, 4,4'-difluorodiphenylsulfone, and mixtures thereof, with 4,4'-dichlorodiphenylsulfone being particularly preferred.
[0050] In a particularly preferred embodiment, the repeating unit (RU4) is obtained by reaction of the monomers 4,4'-biphenol and 4,4'-dichlorodiphenylsulfone, in which case the repeating unit (R4) is equal to the repeating unit (RU1).
[0051] The amorphous polymer (P) generally has a polydispersity (Q) of ≦5, preferably ≦4.5.
[0052] Polydispersity (Q) is the ratio M w :M n (M w / M n In a preferred embodiment, the polydispersity (Q) of the amorphous polymer (P) is in the range of from 2.0 to ≦5, preferably in the range of from 2.1 to ≦4.5.
[0053] Mass average molecular weight (M W ) and number average molecular weight (M n ) is measured using gel permeation chromatography.
[0054] The polydispersity (Q) and average molecular weight of the amorphous polymer (P) were measured using gel permeation chromatography (GPC). Dimethylacetamide (DMAc) was used as the solvent and narrow dispersity polymethylmethacrylate was used as the standard in the measurements.
[0055] The weight average molecular weight (M W The mass average molecular weight (M) is generally in the range of 30,000 to 120,000 g / mol, preferably in the range of 40,000 to 100,000 g / mol, and more preferably in the range of 45,000 to 80,000 g / mol. W ) is measured using gel permeation chromatography (GPC), which is carried out as described above.
[0056] The end groups of the amorphous polymer (P) are generally either halogen groups, in particular chlorine groups, or etherified groups, in particular alkyl ether groups. Etherified end groups can be obtained by reacting the terminal OH / phenoxide groups with a suitable etherifying agent.
[0057] Examples of suitable etherifying agents are monofunctional alkyl or aryl halides, such as C1-C6 alkyl chlorides, bromides or iodides, preferably methyl chloride or benzyl chloride, bromide or iodide, or mixtures thereof. The end groups of the polyarylene ether sulfone polymers according to the invention are preferably halogen groups, in particular chlorine, and also alkoxy groups, in particular methoxy, aryloxy groups, in particular phenoxy, or benzyloxy.
[0058] The ratio of the total mass of the repeating units (RU1), (RU2), (RU3) and (RU4) contained in the amorphous polymer (P) to the total mass of the amorphous polymer (P) is advantageously greater than 0.7. This ratio is preferably greater than 0.8, more preferably greater than 0.9 and even more preferably greater than 0.95. Most preferably, the polymer according to the invention does not contain repeating units other than the repeating units (RU1), (RU2), (RU3) and (RU4).
[0059] In a preferred embodiment, the ratio of the total mass of repeating units (RU1), (RU2) and / or (RU3) contained in the amorphous polymer (P) to the total mass of the amorphous polymer (P) is advantageously greater than 0.7. This ratio is preferably greater than 0.8, more preferably greater than 0.9 and even more preferably greater than 0.95. Most preferably, the polymer according to the invention does not contain repeating units other than repeating units (RU1), (RU2) and / or (RU3).
[0060] In another more preferred embodiment, the ratio of the total mass of the repeating units (RU1) and (RU2) contained in the amorphous polymer (P) to the total mass of the amorphous polymer (P) is advantageously greater than 0.7. This ratio is preferably greater than 0.8, more preferably greater than 0.9, even more preferably greater than 0.95. Most preferably, the polymer according to the invention does not contain repeating units other than the repeating units (RU1) and (RU2).
[0061] In a preferred embodiment, the repeating unit (RU1) can be obtained by reaction of the monomers 4,4'-dichlorodiphenylsulfone and 4,4'-biphenol, the repeating unit (RU2) can be obtained by reaction of the monomers 4,4'-dichlorobenzophenone and 4,4'-biphenol, and / or the repeating unit (RU3) can be obtained by reaction of the monomers 4,4'-dihydroxybenzophenone and 4,4'-dichlorodiphenylsulfone.
[0062] In a preferred embodiment, the amorphous polymer (P) is obtainable by reaction of compounds as defined above to prepare repeating units (RU1), (RU2) and / or (RU3), and therefore the above explanations and preferences apply.
[0063] In a preferred embodiment, the amorphous polymer (P) is Reaction of an aromatic dihalogen compound (D1,1) with an aromatic dihydroxy compound (aDHy1), and Reaction of aromatic dihalogen compounds (D2,1) with aromatic dihydroxy compounds (aDHy2) can be obtained by wherein the aromatic dihydroxy compounds (aDHy1) and (aDHy2) are both 4,4'-biphenol, the aromatic dihalogen compound (D1,1) is 4,4'-dichlorodiphenylsulfone, and the molar amount of the aromatic dihalogen compound (D1,1) used in the reaction is within a range of 80 to 90 mol%, more preferably 80.1 to 89 mol%, even more preferably 80.2 to 88 mol%, particularly preferably 80.3 to 87 mol%, and most preferably 80.4 to 86.5 mol%, The molar amount of the aromatic dihalogen compound (D2,1) used in the reaction is within the range of 10 to 20 mol%, more preferably 11 to 19.9 mol%, even more preferably 12 to 19.8 mol%, particularly preferably 13 to 19.7 mol%, and most preferably 13.5 to 19.6 mol%, In each case, it is based on the total molar amount of the aromatic dihalogen compound (D1,1) and the aromatic dihalogen compound (D2,1) used in the reaction.
[0064] In another preferred embodiment, the number of moles of the aromatic dihalogen compound (D1,1) relative to the number of moles of the dihalogen compound (D2,1) used in the reaction to obtain the amorphous polymer (P) is 4 to 9, more preferably 4.02 to 8.09, even more preferably 4.05 to 7.33, particularly preferably 4.08 to 6.69, and most preferably 4.10 to 6.41.
[0065] A further aspect of the invention is a composition comprising an amorphous polymer (P). In a preferred embodiment, the composition may comprise at least one further component. The further component may preferably be selected from the group consisting of further polymers, solvents, fillers, additives, colorants, reinforcing agents, smoothing agents, heat stabilizers, processing aids, antistatic agents, antioxidants, and flame retardants. Suitable further polymers are, for example, polysulfones, polyethersulfones, polyphenylenesulfones, polyetherimides, polyamideimides, which preferably have a thermal stability to withstand processing temperatures above 350°C. Suitable fillers are, for example, glass beads, glass fibers, carbon fibers, talc, calcium carbonate, wollastonite, and polyamide fibers.
[0066] Suitable colorants are, for example, pigments or dyes, such as titanium dioxide, zinc oxide, carbon black, and the like.
[0067] The composition according to the invention preferably comprises more than 50% by weight, more preferably more than 75% by weight, particularly preferably more than 90% by weight of the amorphous polymer (P) relative to the total weight of the composition. The weight of at least one component is generally within the range of 0-50%, preferably 0-25%, particularly preferably 0-10% by weight, relative to the total weight of the composition. In another embodiment, the composition may be substantially free of the above-mentioned components.
[0068] Another aspect of the invention is an article comprising an amorphous polymer (P). In a preferred embodiment, the article is selected from the group consisting of fittings, pipes, valves, manifolds, aircraft interior panels or components, cookware, medical devices or parts of devices, medical cases or trays, laboratory animal cages, laboratory equipment, coatings, composites, fibers, and fabrics.
[0069] Method for producing an amorphous polymer (P) Another aspect of the invention is a method for producing an amorphous polymer (P). The explanations and preferences given above in terms of the amorphous polymer (P) therefore apply to the method for producing the amorphous polymer (P). Furthermore, the explanations and preferences given below in terms of the method for producing the amorphous polymer (P) therefore apply to the amorphous polymer (P).
[0070] Another object of the present invention is to (A1) at least one aromatic dihalogen sulfone compound (D1,1); (A2) at least one aromatic dihalogen ketone compound (D2,1); (B1) 4,4'-biphenol, (C) Reaction mixture (R G At least one carbonate component comprising at least 80% by weight of potassium carbonate based on the total weight of component (C) in (D) at least one aprotic polar solvent; A reaction mixture (R G ) to produce an amorphous polymer (P).
[0071] In a preferred embodiment, the process of the present invention for producing an amorphous polymer (P) comprises the steps of: forming a reaction mixture (R G The method includes step I) of converting
[0072] Components (A1), (A2), and (B1) participate in a polycondensation reaction.
[0073] Component (D) acts as a solvent and component (C) acts as a base that deprotonates component (B1) prior to or during the condensation reaction.
[0074] The reaction mixture (R G ) is understood to mean the mixture used in the process according to the invention for producing the amorphous polymer (P). In the present case, the reaction mixture (R GAny details given with respect to the reaction mixture (R G During the process according to the invention, the components (A1), (A2) and (B1) react by polycondensation to give the desired product amorphous polymer (P). The mixture obtained after polycondensation, which contains the desired product amorphous polymer (P), is called product mixture (P G ) is also called the product mixture (P G ) typically further comprises at least one aprotic polar solvent (component (D)) and a halide compound. The halide compound is added to the reaction mixture (R G During the conversion, component (C) first reacts with component (B1) to deprotonate component (B1). The deprotonated component (B1) then reacts with component (A1), where a halide compound is formed. This process is known to those skilled in the art.
[0075] In one embodiment of the present invention, in step I) a first amorphous polymer (P1) is obtained. This embodiment is described in more detail below. In this embodiment, the product mixture (P G ) contains the first amorphous polymer (P1). G ) usually further comprises at least one aprotic polar solvent (component (D)) and a halide compound. The details above for the halide compound apply.
[0076] The reaction mixture (R G The components of are generally reacted simultaneously. The individual components may be mixed in an upstream process and then reacted. It is also possible to feed the individual components into a reactor where they are mixed and then reacted.
[0077] In the process according to the invention, the reaction mixture (R GThe individual components of (A1), (A2) and (B1) are generally reacted simultaneously in step I). The reaction is preferably carried out in one step. This means that the deprotonation of component (B1) and also the condensation reaction between components (A1), (A2) and (B1) are carried out in one reaction step without isolating intermediate products, such as the deprotonated species of component (B1).
[0078] The process according to step I) of the invention is carried out according to the so-called "carbonate process". The process according to the invention is not carried out according to the so-called "hydroxide process". This means that the process according to the invention is not carried out in two steps including isolation of the phenolate anion.
[0079] The reaction mixture (R G It is further preferred that the reaction mixture (R) does not contain toluene or chlorobenzene. G It is particularly preferred that the solvent does not contain any substances that form azeotropes with water.
[0080] Therefore, another object of the present invention is also to provide a method for producing a reaction mixture (R G ) does not include any substance that forms an azeotrope with water.
[0081] The molar ratio of the sum of components (A1) and (A2) to component (B1) (ratio (A1+A2) / (B1)) is derived in principle from the stoichiometry of the polycondensation reaction proceeding with the theoretical removal of hydrogen chloride and can be verified by the skilled person in the known manner.
[0082] Preferably, the molar ratio of component (B1) to the sum of components (A1) and (A2) is from 0.95 to 1.08, in particular from 0.96 to 1.06, most preferably from 0.97 to 1.05.
[0083] Therefore, another object of the present invention is also to provide a method for producing a reaction mixture (R G In the process, the molar ratio of the component (B1) to the total of the components (A1) and (A2) is within the range of 0.97 to 1.08.
[0084] In a preferred embodiment, the reaction mixture (RG ) comprises, in addition to components (A1), (A2), (B1), (C), and (D), a reaction mixture (R G ), more preferably at most 15% by weight, more preferably at most 7.5% by weight, particularly preferably at most 2.5% by weight, most preferably at most 1% by weight of further components different from components (A1), (A2), (B1), (C) and (D), based on the total weight of the composition.
[0085] In another most preferred embodiment, the reaction mixture (R G ) consists of components (A1), (A2), (B1), (C), and (D).
[0086] Preferably, the conversion in the polycondensation reaction is at least 0.9.
[0087] Step I) of the process for the preparation of the amorphous polymer (P) is typically carried out under the conditions of the so-called "carbonate process". G ) under the conditions of the so-called "carbonate process". The reaction (polycondensation reaction) is generally carried out at a temperature in the range of 80 to 250°C, preferably in the range of 100 to 220°C. The upper limit of the temperature is determined by the boiling point of at least one aprotic polar solvent (component (D)) at standard pressure (1013.25 mbar). The reaction is generally carried out at standard pressure. The reaction is preferably carried out for a time in the range of 2 to 12 hours, in particular 3 to 10 hours.
[0088] Product mixture (P G The isolation of the amorphous polymer (P) obtained by the process according to the invention in water or in a mixture of water and other solvents (P G The precipitated amorphous polymer (P) may then be extracted with water and then dried. In one embodiment of the present invention, the precipitate may also be taken up in an acidic medium. Suitable acids are, for example, organic or inorganic acids, for example carboxylic acids such as acetic acid, propionic acid, succinic acid or citric acid, and mineral acids such as hydrochloric acid, sulfuric acid or phosphoric acid.
[0089] In one embodiment of the present invention, in step I) a first amorphous polymer (P1) is obtained. The method of the present invention then preferably further comprises II) reacting the first amorphous polymer (P1) obtained in step I) with an alkyl halide; Includes.
[0090] Another object of the present invention is therefore also to provide a process for producing a polymerizable composition comprising the steps of: II) reacting the first amorphous polymer (P1) obtained in step I) with an alkyl halide; The method further comprises:
[0091] It is clear to the skilled person that if step II) is not carried out, the first amorphous polymer (P1) corresponds to the amorphous polymer (P).
[0092] The first amorphous polymer (P1) is typically G The first amorphous polymer (P1) is the product of a polycondensation reaction of components (A1), (A2) and (B1) contained in the reaction mixture (R G The above product mixture (P G As described above, this product mixture (P G ) comprises a first amorphous polymer (P1), component (D), and a halide compound. The first amorphous polymer (P1) is reacted with an alkyl halide to produce the product mixture (P G ) may be included.
[0093] The separation of the halide compounds from the first product mixture (P1) can be carried out by any method known to the person skilled in the art, for example by filtration or centrifugation.
[0094] The first amorphous polymer (P1) usually contains terminal hydroxy groups. In step II), these terminal hydroxy groups are further reacted with alkyl halides to obtain the polyarylene ether sulfone polymer (P). Preferred alkyl halides are alkyl chlorides, especially primary alkyl chlorides, especially with linear or branched alkyl groups having 1 to 10 carbon atoms, particularly preferably methyl halides, especially methyl chloride.
[0095] The reaction according to step II) is preferably carried out at a temperature in the range of from 90° C. to 160° C., in particular in the range of from 100° C. to 150° C. The time required may vary over a wide range and is usually at least 5 minutes, in particular at least 15 minutes. The time required for the reaction according to step II) is preferably from 15 minutes to 8 hours, in particular from 30 minutes to 4 hours.
[0096] Various methods can be used for the addition of the alkyl halide. It is further possible to add the alkyl halide in a stoichiometric amount or in an excess, which may be, for example, up to 5 times. In a preferred embodiment, the alkyl halide is added continuously, in particular by continuous introduction in the form of a gas stream.
[0097] In step II), a polymer solution (PL) is obtained, which usually contains an amorphous polymer (P) and component (D). In step II), the product mixture (P) from step I) is G When step II) is used, the polymer solution (PL) typically further contains halide compounds. The polymer solution (PL) can be filtered after step II), thereby removing the halide compounds.
[0098] The present invention therefore provides a method for producing a polymer solution (PL) in step II), III) Step of filtering the polymer solution (PL) obtained in step II) Also provided is a method, further comprising:
[0099] The isolation of the amorphous polymer (P) obtained in step II) according to the invention in the polymer solution (PL) is carried out by the reaction of the product mixture (P G ) of the amorphous polymer (P). For example, the isolation may be carried out by precipitation of the polymer solution (PL) in water or in a mixture of water and another solvent. The precipitated amorphous polymer (P) can then be extracted with water and then dried. In one embodiment of the present invention, the precipitate can also be taken up in an acidic medium. Suitable acids are, for example, organic or inorganic acids, for example carboxylic acids such as acetic acid, propionic acid, succinic acid or citric acid, and mineral acids such as hydrochloric acid, sulfuric acid or phosphoric acid.
[0100] Ingredient (A1) The reaction mixture (R G ) comprises at least one aromatic dihalogen sulfone compound (D1,1). The term "at least one aromatic dihalogen sulfone compound (D1,1)" is understood in the present invention to mean exactly one aromatic dihalogen sulfone compound (D1,1) and also mixtures of two or more aromatic dihalogen sulfone compounds (D1,1).
[0101] For component (A1) the explanations and preferences given above in terms of the aromatic dihalogen sulfone compound (D1,1) therefore apply.
[0102] Ingredients (A2) The reaction mixture (R G ) comprises at least one aromatic dihalogen ketone compound (D2,1). The term "at least one aromatic dihalogen ketone compound (D2,1)" is understood in the present invention to mean exactly one aromatic dihalogen ketone compound (D2,1) and also mixtures of two or more aromatic dihalogen ketone compounds (D2,1). For component (A2), the above explanations and preferences in terms of aromatic dihalogen ketone compound (D2,1) therefore apply.
[0103] Ingredients (B1) For component (B1), the above explanations and preferences in terms of at least one aromatic dihydroxy compound (aDHy1) and (aDHy2) therefore apply. Component (B1) in the present case is understood to mean exactly one aromatic dihydroxy compound (aDHy1; aDHy2) as well as mixtures of two or more aromatic dihydroxy compounds (aDHy1; aDHy2). In a preferred embodiment, component (B1) is 4,4'-biphenol.
[0104] Ingredients (C) The reaction mixture (R G ) comprises at least one carbonate component as component (C). The term "at least one carbonate component" is understood in the present case to mean exactly one carbonate component and also a mixture of two or more carbonate components. The at least one carbonate component is preferably at least one metal carbonate. The metal carbonate is preferably anhydrous.
[0105] Preference is given to alkali metal carbonates and / or alkaline earth metal carbonates as metal carbonates. At least one metal carbonate selected from the group consisting of sodium carbonate, potassium carbonate and calcium carbonate is particularly preferred as metal carbonate. Potassium carbonate is most preferred.
[0106] For example, component (C) may be added to the reaction mixture (R G ), more preferably at least 50% by weight, most preferably at least 70% by weight, and most preferably at least 90% by weight of potassium carbonate, based on the total weight of the at least one carbonate component in the composition.
[0107] Another object of the present invention is therefore also the process, wherein component (C) comprises at least 50% by weight of potassium carbonate relative to the total weight of component (C).
[0108] In a preferred embodiment, component (C) consists essentially of potassium carbonate.
[0109] "Consisting essentially of" in the present invention means that component (C) is in each case present in the reaction mixture (R G %, preferably more than 99.5% by weight and particularly preferably more than 99.9% by weight of potassium carbonate, based on the total weight of component (C) in the composition (C).
[0110] In a particularly preferred embodiment, component (C) consists of potassium carbonate.
[0111] Particularly preferred as potassium carbonate is potassium carbonate having a volume weighted mean particle size of less than 200 μm. The volume weighted mean particle size of potassium carbonate is measured in a suspension of potassium carbonate in chlorobenzene / sulfolane (60 / 40) using a Malvern Mastersizer 2000 Instrument particle size analyzer.
[0112] In a preferred embodiment, the reaction mixture (R G ) does not include any alkali metal hydroxides or alkaline earth metal hydroxides.
[0113] Ingredients (D) The reaction mixture (R G ) comprises at least one aprotic polar solvent as component (D). "At least one aprotic polar solvent" is understood according to the invention to mean exactly one aprotic polar solvent and also mixtures of two or more aprotic polar solvents.
[0114] Suitable aprotic polar solvents are, for example, selected from the group consisting of anisole, dimethylformamide, dimethylsulfoxide, N-methylpyrrolidone, N-ethylpyrrolidone, sulfolane, and N,N-dimethylacetamide.
[0115] Preferably, component (D) is selected from the group consisting of N-methylpyrrolidone, N,N-dimethylacetamide, dimethylsulfoxide, and dimethylformamide. N-methylpyrrolidone is particularly preferred as component (D).
[0116] Another object of the present invention is therefore also the process, wherein component (D) is selected from the group consisting of N-methylpyrrolidone, N,N-dimethylacetamide, dimethylsulfoxide, and dimethylformamide.
[0117] It is preferred that component (D) does not contain sulfolane. G It is even more preferred that the phenyl sulfone-free copolymer does not contain diphenyl sulfone.
[0118] Component (D) is added to the reaction mixture (R G It is preferred that the composition contains at least one solvent selected from the group consisting of N-methylpyrrolidone, N,N-dimethylacetamide, dimethylsulfoxide, and dimethylformamide in an amount of at least 50% by weight based on the total weight of component (D) in the composition. N-methylpyrrolidone is particularly preferred as component (D).
[0119] In a more preferred embodiment, component (D) consists essentially of N-methylpyrrolidone.
[0120] "Consists essentially of" is understood in the present invention to mean that component (D) comprises more than 98% by weight, particularly preferably more than 99% by weight and more preferably more than 99.5% by weight of at least one aprotic polar solvent selected from the group consisting of N-methylpyrrolidone, N,N-dimethylacetamide, dimethylsulfoxide and dimethylformamide, with preference being given to N-methylpyrrolidone.
[0121] In a preferred embodiment, component (D) consists of N-methylpyrrolidone, also called NMP or N-methyl-2-pyrrolidone. EXAMPLES
[0122] Ingredients Used DCDPS: 4,4'-dichlorodiphenyl sulfone; DCBPO: 4,4' dichlorobenzophenone, BP: 4,4'-biphenol; Potassium carbonate: K2CO3; anhydrous; volume average particle size of 34.5 μm; NMP: N-methylpyrrolidone, PPSU: Polyphenylene sulfone (ULTRASON® P3010)
[0123] General Procedure The viscosity numbers of the polymers are determined in accordance with DIN EN ISO 1628-1 in 1% solutions in NMP at 25°C.
[0124] The isolation of the polymer is carried out by dropping the polymer in NMP solution into demineralized water at room temperature (25° C.). The drop height is 0.5 m and the flow rate is about 2.5 l / h. The resulting beads are then extracted with water (water flow rate 160 l / h) at 85° C. for 20 h. The beads are dried at 150° C. under reduced pressure (<100 mbar) for 24 h until the residual moisture is less than 0.1% by weight.
[0125] The resulting amorphous polymer (P) was granulated in a ZSK 18 extruder with a throughput of 2.5 kg / h at a rotation speed of 300 rpm and a melt temperature of less than 385° C., measured by an insert thermometer in the molten cake.
[0126] The resulting granules were injection molded at a mass temperature of 370°C and a mould temperature of 140°C to obtain ISO bars (80*10*4mm*mm*mm) and S2 tensile specimens.
[0127] The melt stability of the samples was measured over a period of 60 min using a capillary rheometer at a mass temperature of 400 °C. Therefore, the melt stability was measured every 5 min for 55 s. -1 The apparent viscosity of the melt was measured at an apparent shear rate of 1000 μm. The melt stability is the apparent viscosity after 60 minutes divided by the apparent viscosity after 5 minutes. The results are shown in Table 1.
[0128] The glass transition temperature (T g) and the melting point are measured by differential scanning calorimetry DSC in the second heating cycle as above with a heating ramp of 20 K / min.
[0129] CDCl3 is used as the solvent 1 The content of benzophenone groups is measured by H-NMR.
[0130] The resistance of the polymers to hydraulic fluids, gasoline, and / or fuel was measured as resistance to Skydrol® LD4 (58 wt% tributyl phosphate, 20-30 wt% dibutylphenyl phosphate, 5-10 wt% butylphenyl phosphate, 1-5 wt% 2,6-di-tert-butyl-p-cresol, less than 10 wt% carboxylates). The S2-release rods were stored in Skydrol® LD4 for 24 hours. In each case, two of the S2-release rods were bent using a stencil to a bending radius of 132 mm before storage. A camera was used to take pictures every minute to measure the time to break point.
[0131] Polymer V1 In a 4 liter glass reactor equipped with a thermometer, a gas inlet tube, and a Dean-Stark trap, 522.63 g (1.82 mol) of DCDPS, 372.41 g (2.00 mol) of 4,4'-dihydroxybiphenyl, 50.22 g (0.20 mol) of 4,4'-dichlorobenzophenone, and 304.05 g (2.20 mol) of potassium carbonate having a volume average particle size of 34.5 μm were suspended in 1152 ml of NMP under a nitrogen atmosphere.
[0132] The mixture was heated to 190° C. within 1 hour. In the following, reaction time will be understood as the time the reaction mixture was maintained at 190° C. The water formed during the reaction was continuously removed by distillation and the lost NMP was replaced.
[0133] The reaction was continued for another 5 hours at 190°C, then 1500 ml of NMP was added to the reactor and the temperature of the suspension was adjusted to 135°C (took 10 minutes). Methyl chloride was then added to the reactor over 60 minutes. N2 was then purged through the suspension for another 30 minutes. The solution was then cooled to 80°C and then transferred to a pressure filter to separate the potassium chloride formed in the reaction by filtration. The resulting polymer solution was then precipitated in water and the resulting polymer beads were separated and then extracted with hot water (85°C) over 20 hours. The beads were then dried under vacuum (<100mbar) at 120°C for 24 hours.
[0134] Amorphous polymer (P)2 In a 4 liter glass reactor equipped with a thermometer, a gas inlet tube, and a Dean-Stark trap, 508.28 g (1.77 mol) of DCDPS, 372.41 g (2.00 mol) of 4,4'-dihydroxybiphenyl, 62.78 g (0.25 mol) of 4,4'-dichlorobenzophenone, and 304.05 g (2.20 mol) of potassium carbonate having a volume average particle size of 34.5 μm were suspended in 1152 ml of NMP under a nitrogen atmosphere.
[0135] The mixture was heated to 190° C. within 1 hour. In the following, reaction time will be understood as the time the reaction mixture was maintained at 190° C. The water formed during the reaction was continuously removed by distillation and the lost NMP was replaced.
[0136] The reaction was continued for another 5 hours at 190°C, then 1500 ml of NMP was added to the reactor and the temperature of the suspension was adjusted to 135°C (took 10 minutes). Methyl chloride was then added to the reactor over 60 minutes. N2 was then purged through the suspension for another 30 minutes. The solution was then cooled to 80°C and then transferred to a pressure filter to separate the potassium chloride formed in the reaction by filtration. The resulting polymer solution was then precipitated in water and the resulting polymer beads were separated and then extracted with hot water (85°C) over 20 hours. The beads were then dried under vacuum (<100mbar) at 120°C for 24 hours.
[0137] Amorphous polymer (P)3 In a 4 liter glass reactor equipped with a thermometer, a gas inlet tube, and a Dean-Stark trap, 493.92 g (1.72 mol) of DCDPS, 372.41 g (2.00 mol) of 4,4'-dihydroxybiphenyl, 75.33 g (0.3 mol) of 4,4'-dichlorobenzophenone, and 304.05 g (2.20 mol) of potassium carbonate having a volume average particle size of 34.5 μm were suspended in 1152 ml of NMP under a nitrogen atmosphere.
[0138] The mixture was heated to 190° C. within 1 hour. In the following, reaction time will be understood as the time the reaction mixture was maintained at 190° C. The water formed during the reaction was continuously removed by distillation and the lost NMP was replaced.
[0139] The reaction was continued for another 5.5 hours at 190°C, then 1500 ml of NMP was added to the reactor and the temperature of the suspension was adjusted to 135°C (took 10 minutes). Methyl chloride was then added to the reactor over 60 minutes. N2 was then purged through the suspension for another 30 minutes. The solution was then cooled to 80°C and then transferred to a pressure filter to separate the potassium chloride formed in the reaction by filtration. The resulting polymer solution was then precipitated in water and the resulting polymer beads were separated and then extracted with hot water (85°C) over 20 hours. The beads were then dried under vacuum (<100mbar) at 120°C for 24 hours.
[0140] Amorphous polymer (P) 4 In a 4 liter glass reactor equipped with a thermometer, a gas inlet tube, and a Dean-Stark trap, 465.22 g (1.62 mol) of DCDPS, 372.41 g (2.00 mol) of 4,4'-dihydroxybiphenyl, 100.44 g (0.40 mol) of 4,4'-dichlorobenzophenone, and 304.05 g (2.20 mol) of potassium carbonate having a volume average particle size of 34.5 μm were suspended in 1152 ml of NMP under a nitrogen atmosphere.
[0141] The mixture was heated to 190° C. within 1 hour. In the following, reaction time will be understood as the time the reaction mixture was maintained at 190° C. The water formed during the reaction was continuously removed by distillation and the lost NMP was replaced.
[0142] The reaction was continued for another 6 hours at 190°C, then 1500ml of NMP was added to the reactor and the temperature of the suspension was adjusted to 135°C (took 10 minutes). Methyl chloride was then added to the reactor over 60 minutes. N2 was then purged through the suspension for another 30 minutes. The solution was then cooled to 80°C and then transferred to a pressure filter to separate the potassium chloride formed in the reaction by filtration. The resulting polymer solution was then precipitated in water and the resulting polymer beads were separated and then extracted with hot water (85°C) over 20 hours. The beads were then dried under vacuum (<100mbar) at 120°C for 24 hours.
[0143] Polymer V5 In a 4 liter glass reactor equipped with a thermometer, a gas inlet tube, and a Dean-Stark trap, 450.86 g (1.57 mol) of DCDPS, 372.41 g (2.00 mol) of 4,4'-dihydroxybiphenyl, 113.00 g (0.45 mol) of 4,4'-dichlorobenzophenone, and 304.05 g (2.20 mol) of potassium carbonate having a volume average particle size of 34.5 μm were suspended in 1152 ml of NMP under a nitrogen atmosphere.
[0144] The mixture was heated to 190° C. within 1 hour. In the following, reaction time will be understood as the time the reaction mixture was maintained at 190° C. The water formed during the reaction was continuously removed by distillation and the lost NMP was replaced.
[0145] The reaction was continued for another 6 hours at 190°C, then 1500ml of NMP was added to the reactor and the temperature of the suspension was adjusted to 135°C (took 10 minutes). Methyl chloride was then added to the reactor over 60 minutes. N2 was then purged through the suspension for another 30 minutes. The solution was then cooled to 80°C and then transferred to a pressure filter to separate the potassium chloride formed in the reaction by filtration. The resulting polymer solution was then precipitated in water and the resulting polymer beads were separated and then extracted with hot water (85°C) over 20 hours. The beads were then dried under vacuum (<100mbar) at 120°C for 24 hours.
[0146] [Table 1]
[0147] As can be seen from the results shown in Table 1, when the content of benzophenone units (BPO units) is less than 10 mol%, no improvement in Skydrol resistance can be detected. When the content of units based on BPO is more than 20 mol%, the product cannot be isolated because the filtration of the suspension exceeds 24 hours. When a small amount of material is precipitated and washed, it is not possible to obtain a homogeneous solution in NMP for VN measurement. The product is not completely soluble even in CDCl3 (H-NMR), but the spectrum obtained nevertheless allows the content of units based on BPO to be determined. A small amount of product isolated from test V5 was melt pressed at 320 °C into a thin film. The film thickness was only 50 μm, but the sample was opaque.
Claims
1. formula 【Chemistry 1】 A segment (S1); formula 【Chemistry 2】 A segment (S2); formula 【Chemistry 3】 Segment (S3) An amorphous polymer (P) comprising Based on the total number of moles of the segments (S1) and (S2) contained in the amorphous polymer (P), 80.1 to 89 mol % of segment (S1), and 11 to 19.9 mol% of segment (S2) The amorphous polymer (P) comprises:
2. The amorphous polymer (P) according to claim 1, comprising a repeating unit (RU1) obtainable by reacting at least one aromatic dihalogen compound (D1,1) containing a segment (S1) with at least one aromatic dihydroxy compound (aDHy1).
3. 3. The amorphous polymer (P) according to claim 2, wherein the aromatic dihalogen compound (D1,1) is at least one compound selected from the group consisting of 4,4'-dihalogen diphenyl sulfone and 4,4'-bis[(4-chlorophenyl)sulfonyl]-1,1'-biphenyl.
4. The amorphous polymer (P) according to any one of claims 1 to 3, comprising a repeating unit (RU2) obtainable by reacting at least one dihalogen compound (D2,1) comprising a segment (S2) with at least one aromatic dihydroxy compound (aDHy2).
5. 5. Amorphous polymer (P) according to any one of claims 1 to 4, having a polydispersity (Q) in the range of from 2.0 to ≦5.
0.
6. The average molecular weight (M) ranges from 30,000 to 120,000 g / mol as measured using gel permeation chromatography (GPC) using dimethylacetamide (DMAc) as the solvent and narrow disperse polymethyl methacrylate as the standard in the measurement. W 6. The amorphous polymer (P) according to claim 1 , wherein
7. The amorphous polymer (P) according to claim 4, wherein the dihalogen compound (D2,1) is a 4,4'-dihalogen benzophenone.
8. The amorphous polymer (P) according to any one of claims 1 to 7, comprising a repeating unit (RU3) obtainable by reacting at least one aromatic dihydroxy compound (D2,2) comprising a segment (S2) with at least one aromatic dihalogen compound (aDHa1).
9. The amorphous polymer (P) according to any one of claims 1 to 8, comprising a repeating unit (RU4) obtainable by reacting at least one aromatic dihydroxy compound (D3,1) comprising a segment (S3) with at least one aromatic dihalogen compound (aDHa2).
10. 5. The amorphous polymer (P) according to claim 2 or 4, wherein the aromatic dihydroxy compound (aDHy1) and / or (aDHy2) is 4,4'-biphenol.
11. The amorphous polymer (P) comprises repeating units (RU1) and (RU2), the repeating unit (R1) being obtainable by a reaction between at least one aromatic dihalogen compound (D1,1) comprising a segment (S1) and at least one aromatic dihydroxy compound (aDHy1), the repeating unit (RU2) being obtainable by a reaction between at least one dihalogen compound (D2,1) comprising a segment (S2) and at least one aromatic dihydroxy compound (aDHy2), and the amorphous polymer (P) does not comprise any repeating unit other than the repeating units (RU1) and (RU2). The amorphous polymer (P) according to any one of claims 1 to 7 and 10.
12. 12. Amorphous polymer (P) according to any one of claims 2, 3 and 11, wherein the repeating unit (RU1) is obtained by reaction of the monomers 4,4'-dichlorodiphenylsulfone and 4,4'-biphenol.
13. 12. Amorphous polymer (P) according to claim 4 or 11, wherein the repeating unit (RU2) is obtained by reaction of the monomers 4,4'-dichlorobenzophenone and 4,4'-biphenol.
14. (A1) at least one aromatic dihalogen sulfone compound (D1,1); (A2) at least one aromatic dihalogen ketone compound (D2,1); (B1) 4,4'-biphenol, (C) Reaction mixture (R G at least one carbonate component comprising at least 80% by weight of potassium carbonate, based on the total weight of component (C) in (D) at least one aprotic polar solvent; A reaction mixture (R G 14. A process for the preparation of an amorphous polymer (P) according to any one of claims 1 to 13, by converting
15. A composition comprising an amorphous polymer (P) according to any one of claims 1 to 13.
16. 16. An article comprising an amorphous polymer (P) according to any one of claims 1 to 13 or a composition according to claim 15.
17. 17. The article of claim 16, selected from the group consisting of fittings, pipes, valves, manifolds, aircraft interior panels or components, cookware, medical devices or device parts, medical cases or trays, laboratory animal cages, laboratory equipment, coatings, composites, fibers, and fabrics.
18. 18. The article of claim 16 or 17, which is transparent.
Citation Information
Patent Citations
High-fluidity polyphenylene ether sulfone ketone resin and industrial synthesis method thereof
CN103613763A
High-liquidity poly(phenylene ether sulfone ketone) resin and preparation method thereof
CN104497300A
High temperature resistant thermoplastic moulding masses with improved melt stability
EP0297363A2
Polyphenyl sulfone ketone copolymers
EP2225328A1
Aromatic polysulfoneetherketone polymers
GB2241245A