Piezoelectric Film
A piezoelectric film made of polypropylene resin and a β-crystal nucleating agent addresses pressure resistance and piezoelectricity issues, ensuring robust performance and reduced discharge risks.
Patent Information
- Application Number
- JP2020039332
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-20
- Filing Date
- 2020-03-06
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-03-06
AI Technical Summary
Existing piezoelectric films, particularly those using microporous membranes, suffer from poor pressure resistance and deteriorating piezoelectricity under constant surface pressure, with the relationship between porosity, pore aspect ratio, and piezoelectricity not fully understood.
A piezoelectric film composed of a polypropylene resin and a β-crystal nucleating agent, with specific porosity, air permeability, and pore aspect ratio, enhancing pressure resistance and piezoelectricity.
The film exhibits excellent pressure resistance and good piezoelectricity, maintaining performance under applied pressure with improved piezoelectric constants and reduced risk of spark discharge.
Smart Images

Figure 0007567176000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a piezoelectric film, and in particular to a piezoelectric film that can be suitably used for actuators, oscillators, sonar, vibration power generation, sensors, and the like. [Background technology]
[0002] Electrets using porous resin films are known to exhibit excellent piezoelectric effects and are widely used in actuators, oscillators, sonar, vibration power generation, sensors, etc. In order to obtain an electret with excellent piezoelectricity, it is necessary to polarize the film at a higher voltage during charge injection and to inject a larger amount of charge.
[0003] As a porous resin film, a foamed film-like plastic product in which the degree of foaming is increased by introducing gas into the resin and inflating it is known (Patent Document 1). Such a film has poor surface uniformity, and when the applied voltage is increased, localized discharge concentration occurs, which exceeds the insulation resistance of the porous resin film and causes partial destruction of the film.
[0004] In response to such problems, an electret using a microporous film utilizing β crystals of a polypropylene-based resin has been proposed (Patent Document 2). Polypropylene resin is a polymer with low polarity, and since it is difficult to localize electric charge in the intramolecular skeleton due to its chemical structure, it is not possible to obtain a high piezoelectric constant by itself. Therefore, a high piezoelectric constant is achieved by introducing air, which has a different dielectric constant, into the pores and trapping the electric charge.
[0005] In addition, it is known that a microporous film using β crystals has a highly uniform porous structure and high insulation resistance, so that it can be polarized at a high voltage, and the obtained electret has excellent piezoelectric properties. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Special Publication No. 10-504853 [Patent Document 2] JP2017-055114A Summary of the Invention [Problem to be solved by the invention]
[0007] In recent years, with the development of flexible electronics, research on bendable devices using piezoelectric films as pressure-sensitive materials has been progressing. Electrets using microporous membranes are attracting attention for use in bendable devices because they can be manufactured in large areas at low cost. However, when an electret using a microporous film is used under a constant surface pressure, the piezoelectricity may deteriorate. Although the relationship between one-dimensional information such as the average pore size in the thickness direction of a resin film and piezoelectricity has been known, the relationship between parameters such as porosity and pore aspect ratio and piezoelectricity and pressure resistance has not been studied in detail.
[0008] Therefore, an object of the present invention is to provide a piezoelectric film having excellent pressure resistance and good piezoelectric properties. [Means for solving the problem]
[0009] The present inventors have conducted extensive research to achieve the above object, and as a result, have focused on solving the above object and have completed the present invention. In one aspect, the present invention is summarized as follows: [1] to [9]. [1] A piezoelectric film made of a resin composition containing a polypropylene resin and a β crystal nucleating agent, having a porosity of 0% or more and 35% or less, and an air permeability of 40,000 sec / dL or more. [2] The piezoelectric film according to [1], wherein the β-crystal nucleating agent is an amide compound. [3] The piezoelectric film according to [1] or [2], having a β crystal generation ability of 80% or more. [4] The piezoelectric film according to any one of [1] to [3], which has a total light transmittance of 30% or more. [5] The piezoelectric film according to any one of [1] to [4], having a piezoelectric constant of 50 pC / N or more and 10,000 pC / N or less. [6] The piezoelectric film according to any one of [1] to [5], which has a piezoelectric constant of 50 pC / N or more and 10,000 pC / N or less under a pressure of 50 kPa. [7] The piezoelectric film according to any one of [1] to [6], having a thickness of 1 μm or more and 100 μm or less. [8] The piezoelectric film according to any one of [1] to [7], having holes with an average aspect ratio of 4.0 or more. [9] A piezoelectric element comprising the piezoelectric film according to any one of [1] to [8]. Effect of the Invention
[0010] The piezoelectric film of the present invention has excellent pressure resistance and good piezoelectric properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described in detail. However, the content of the present invention is not limited to the embodiment described below.
[0012] 1. Piezoelectric film The piezoelectric film of the present invention is made of a resin composition containing a polypropylene resin and a β crystal nucleating agent, and has a porosity of 0% or more and 35% or less, and an air permeability of 40,000 sec / dL or more. The properties of this film are described below.
[0013] (1) Piezoelectric constant The piezoelectric constant of this film is d 33 is preferably 50 pC / N or more, more preferably 60 pC / N or more, and even more preferably 70 pC / N or more. In particular, it is more preferably 100 pC / N or more, more preferably 150 pC / N or more, and even more preferably 200 pC / N or more. On the other hand, the piezoelectric constant d 33is preferably 10,000 pC / N or less, more preferably 8,000 pC / N or less, and even more preferably 5,000 pC / N or less. Piezoelectric constant d 33 A piezoelectric constant d of 50 pC / N or more provides sufficient sensitivity when used as a sensor. 33 By keeping the resistivity at 10,000 pC / N or less, the risk of spark discharge when incorporated into a sensor or actuator can be reduced. The piezoelectric constant of the piezoelectric film of the present invention is measured by the method described below.
[0014] (2) Porosity The porosity of the present film is a numerical value indicating the ratio of the open space of the present film. The porosity of the present film is 35% or less, preferably 30% or less, and more preferably 25% or less. On the other hand, the porosity may be 0% or more, preferably 5% or more, and more preferably 10% or more. A porosity of 35% or less can provide a piezoelectric film with excellent pressure resistance. The porosity was measured by the following method. The actual mass W1 of the measurement sample is measured, and the mass W0 when the porosity is 0% is calculated based on the density of the resin composition. The porosity is calculated from these values based on the following formula. Porosity (%)={(W0-W1) / W0}×100
[0015] (3) Thickness The thickness of the present film is preferably 1 μm or more, more preferably 2 μm or more, and even more preferably 5 μm or more, while the upper limit of the thickness of the present film is preferably 100 μm or less, more preferably 80 μm or less, even more preferably 60 μm or less, even more preferably 50 μm or less, and particularly preferably 30 μm or less. If the thickness is 1 μm or more, a piezoelectric film with high piezoelectricity can be obtained, whereas if the thickness is 100 μm or less, it can be transported and wound from roll to roll, making subsequent processing easy.
[0016] (4) Air permeability The air permeability of the present film is 40000 sec / dL or more, preferably 60000 sec / dL or more, and more preferably 80000 sec / dL or more. On the other hand, the upper limit of the air permeability of the present film is not particularly limited, and it is sufficient that it is 99999 sec / dL or less. By setting the air permeability of the present film to 40,000 sec / dL or more, the pressure resistance of the present film becomes good. Air permeability indicates the difficulty of air passing through the piezoelectric film in the thickness direction, and is specifically expressed as the number of seconds required for 100 ml of air to pass through the piezoelectric film. Therefore, a smaller value means that air passes through more easily, and a larger value means that air passes through less easily. In other words, the smaller the air permeability, the better the interconnectivity of the piezoelectric film in the thickness direction, and the greater the air permeability, the worse the interconnectivity of the piezoelectric film in the thickness direction. Interconnectivity is the degree of connection of the pores in the thickness direction of the piezoelectric film. The air permeability (sec / dL) can be measured in accordance with JIS P 8117, specifically, by the method described in the examples.
[0017] (5) Piezoelectric constant under a pressure of 50 kPa The piezoelectric film of the present invention is characterized by its excellent pressure resistance, which can be evaluated by measuring the piezoelectric constant under pressure. The piezoelectric constant d of this film under a pressure of 50 kPa 33 is preferably 50 pC / N or more, more preferably 60 pC / N or more, and even more preferably 70 pC / N or more. In particular, it is more preferably 100 pC / N or more, even more preferably 150 pC / N or more, and even more preferably 200 pC / N or more. On the other hand, the piezoelectric constant d 33 is preferably 10,000 pC / N or less, more preferably 8,000 pC / N or less, and even more preferably 5,000 pC / N or less. Piezoelectric constant d under pressure of 50kPa 33 A piezoelectric constant d 33By keeping the resistivity at 10,000 pC / N or less, the risk of spark discharge when incorporated into a sensor or actuator can be reduced. The piezoelectric constant of the piezoelectric film of the present invention under a pressure of 50 kPa is measured by the method described below.
[0018] (6) Transparency The piezoelectric film of the present invention is, for example, a transparent piezoelectric film, and preferably has high transparency. Various layers are laminated on piezoelectric films by roll-to-roll printing and lamination, and the films are ultimately incorporated into piezoelectric elements and devices. For example, when a conductive layer is laminated on a piezoelectric film, the conductive layer is often opaque, making it difficult to optically check for foreign objects or defects during the process, and there is a risk of misidentification. Therefore, it is preferable for the piezoelectric film to be highly transparent, as this allows inspection to be performed from the back side of the piezoelectric film, making inspection easier. The total light transmittance of the present film is preferably 30% or more, more preferably 35% or more, even more preferably 40% or more, even more preferably 50% or more, and particularly preferably 60% or more.
[0019] (7) Average aspect ratio The piezoelectric film of the present invention preferably has holes with an average aspect ratio of 4.0 or more, more preferably 5.0 or more, and even more preferably 7.0 or more. When the average aspect ratio of the pores is 4.0 or more, the polypropylene matrix is oriented and crystallized to have high strength, so that the pores are not easily crushed even when a high pressure is applied to the piezoelectric film, and the piezoelectricity can be maintained. The upper limit of the average aspect ratio is not particularly limited, but is, for example, 30 or less, preferably 25 or less, and more preferably 20 or less. The average aspect ratio of the piezoelectric film of the present invention is measured by the method described below.
[0020] 2.Resin composition The components of the resin composition constituting the present film will be described below.
[0021] (1) Polypropylene resin The piezoelectric film of the present invention preferably contains a polypropylene resin as a main component. When the piezoelectric film contains a polypropylene resin as a main component, the content of the polypropylene resin in the piezoelectric film is 50% by mass or more, preferably 70% by mass or more and 99.9999% by mass or less, more preferably 80% by mass or more and 99.999% by mass or less, and even more preferably 90% by mass or more and 99.99% by mass or less.
[0022] Examples of the polypropylene resin in the present invention include homopolypropylene (propylene homopolymer), and random or block copolymers of propylene and α-olefins such as ethylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, or 1-decene. Among these, homopolypropylene is more preferably used from the viewpoint of mechanical strength.
[0023] Furthermore, the polypropylene resin preferably has an isotactic pentad fraction, which indicates stereoregularity, of 80% or more and 99% or less, more preferably 83% or more and 98% or less, and further preferably 85% or more and 97% or less. If the isotactic pentad fraction is 80% or more, the mechanical strength is good. On the other hand, the upper limit of the isotactic pentad fraction is set at the upper limit value that can be industrially obtained at present, but this will not apply in the future if a resin with higher regularity is developed at the industrial level. The isotactic pentad fraction refers to the three-dimensional structure or the proportion thereof in which the five methyl groups, which are side chains, are all positioned in the same direction relative to the main chain formed by carbon-carbon bonds composed of any five consecutive propylene units. The assignment of signals in the methyl group region follows A. Zambelli et al. (Macromol. 8, 687 (1975)).
[0024] Moreover, the polypropylene resin preferably has a Mw / Mn, which is a parameter indicating the molecular weight distribution, of 1.5 or more and 10.0 or less, more preferably 2.0 or more and 8.0 or less, and further preferably 2.0 or more and 6.0 or less. A smaller Mw / Mn ratio means a narrower molecular weight distribution, but by making the Mw / Mn ratio 1.5 or more, sufficient extrusion moldability is obtained and industrial mass production is possible, while by making the Mw / Mn ratio 10.0 or less, sufficient mechanical strength can be ensured. Mw / Mn is measured by GPC (gel per emission chromatography) method.
[0025] The melt flow rate (MFR) of the polypropylene resin is not particularly limited, but is preferably 0.5 g / 10 min or more and 15 g / 10 min or less, and more preferably 1.0 g / 10 min or more and 10 g / 10 min or less. By setting the MFR to 0.5 g / 10 min or more, sufficient melt viscosity can be obtained during molding and high productivity can be ensured, while by setting the MFR to 15 g / 10 min or less, sufficient strength can be ensured. The MFR is measured in accordance with JIS K7210-1 (2014) at a temperature of 230°C and a load of 2.16 kg.
[0026] The method for producing the polypropylene resin is not particularly limited, and examples thereof include known polymerization methods using known polymerization catalysts, such as a polymerization method using a multi-site catalyst represented by a Ziegler-Natta catalyst or a single-site catalyst represented by a metallocene catalyst.
[0027] Examples of polypropylene-based resins that can be suitably used in the present invention include commercially available products such as those sold under the trade names "Novatec PP," "WINTEC," and "WAYMAX" (manufactured by Japan Polypropylene Corporation), "Versify," "Notio," and "Tafmer XR" (manufactured by Mitsui Chemicals, Inc.), "Zelas" and "Thermorun" (manufactured by Mitsubishi Chemical Corporation), "Sumitomo Noblen" and "Tafthren" (manufactured by Sumitomo Chemical Co., Ltd.), "Prime Polypro" and "Prime TPO" (manufactured by Prime Polymer Co., Ltd.), "Adflex," "Adsyl," and "HMS-PP (PF814)" (manufactured by SunAllomer Co., Ltd.), and "Inspire" (Dow Chemical Co., Ltd.).
[0028] The piezoelectric film of the present invention is preferably made of a resin composition mainly composed of a polypropylene resin containing a large amount of β-crystals, which is one of the crystal forms. A non-porous film made of a resin composition mainly composed of a polypropylene resin containing a large amount of β-crystals shows excellent piezoelectricity after charging treatment, but by stretching it to form a porous structure, even better piezoelectricity can be obtained. The formation of a porous structure using β-crystals is advantageous in adjusting the porous structure because the pores are formed during the process in which the β-crystals in the polypropylene resin are transformed into α-crystals during the stretching process, and the porous structure is dense, and does not depend on the particle size or dispersion diameter compared to the conventionally known pore formation by adding inorganic fillers or incompatible organic substances.
[0029] The piezoelectric film of the present invention has β-crystal activity. The β-crystal activity of the piezoelectric film of the present invention can be regarded as an index showing that the polypropylene resin in the nonporous membrane before stretching has generated β-crystals. If the polypropylene resin in the nonporous membrane before stretching has generated β-crystals, many fine and uniform pores are formed by subsequent stretching, so that the mechanical properties are excellent and excellent voltage resistance can be obtained by forming fine and uniform pores.
[0030] The presence or absence of β-crystal activity of the piezoelectric film of the present invention is judged by whether or not a crystal melting peak temperature derived from β-crystal of polypropylene-based resin is detected by performing differential thermal analysis of the piezoelectric film using a differential scanning calorimeter. Specifically, the piezoelectric film is heated from 25°C to 240°C at a heating rate of 10°C / min and held for 1 minute, then cooled from 240°C to 25°C at a cooling rate of 10°C / min and held for 1 minute, and then heated again from 25°C to 240°C at a heating rate of 10°C / min. If a crystal melting peak temperature (Tmβ) derived from β-crystal of polypropylene-based resin is detected during reheating, it is judged to have β-crystal activity.
[0031] The presence or absence of the β crystal activity can also be determined from a diffraction profile obtained by X-ray diffraction measurement of a piezoelectric film that has been subjected to a specific heat treatment. In detail, a piezoelectric film is heat-treated at 170 to 190°C, which is a temperature exceeding the crystal melting peak temperature of polypropylene-based resin, and then slowly cooled to generate and grow β crystals. When the film is subjected to X-ray diffraction measurement and a diffraction peak derived from the (300) plane of the β crystals of the polypropylene-based resin is detected in the range of 2θ = 16.0° to 16.5°, it is determined that the film has β crystal activity. For details on the β crystal structure of polypropylene-based resin and X-ray diffraction measurement, Macromol.Chem.187,643-652(1986), Prog.Polym.Sci.Vol.16,361-404(1991), Macromol.Symp.89,499-511(1995), Macromol.Chem.75,134(1964), and references cited therein, can be referred to.
[0032] The above-mentioned methods for obtaining β-crystal activity of polypropylene resin include a method of not adding a substance that promotes the formation of α-crystals in polypropylene resin, a method of adding a polypropylene resin that has been treated to generate peroxide radicals as described in Japanese Patent No. 3739481, and a method of adding a β-crystal nucleating agent, but in the present invention, it is particularly preferable to obtain β-crystal activity by adding a β-crystal nucleating agent. By adding a β-crystal nucleating agent, it is possible to promote the formation of β-crystals in the polypropylene resin more uniformly and efficiently, and to obtain a piezoelectric film having β-crystal activity.
[0033] The degree of β-crystal activity can be quantified by measuring the β-crystal formation ability. The β-crystal formation ability of the polypropylene resin contained in the piezoelectric film is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more. When the β-crystal generating ability is 80% or more, the piezoelectric film can exhibit suitable piezoelectricity. There is no particular upper limit to the β-crystal generating ability, but it is preferably 100% or less. The β-crystal forming ability is calculated by the method described below.
[0034] (2) β-crystal nucleating agent In order to obtain excellent piezoelectricity, it is important that the piezoelectric film of the present invention contains a β-crystal nucleating agent, which allows the film to have β-crystal activity.
[0035] In the present invention, examples of the β-crystal nucleating agent include amide compounds, tetraoxaspiro compounds, quinacridones, iron oxides having nanoscale sizes, alkali or alkaline earth metal salts of carboxylic acids such as potassium 1,2-hydroxystearate, magnesium benzoate or magnesium succinate, and magnesium phthalate, aromatic sulfonic acid compounds such as sodium benzenesulfonate or sodium naphthalenesulfonate, di- or triesters of di- or tribasic carboxylic acids, phthalocyanine pigments such as phthalocyanine blue, two-component compounds consisting of component A, which is an organic dibasic acid, and component B, which is an oxide, hydroxide, or salt of a metal in Group 2 of the periodic table, and compositions consisting of a cyclic phosphorus compound and a magnesium compound. If necessary, two or more kinds of β-crystal nucleating agents from these may be mixed and used.
[0036] Among these β-crystal nucleating agents, amide compounds are preferred in terms of the piezoelectricity of the resulting piezoelectric film. As the amide compound, N,N'-dicyclohexyl-2,6-naphthalene diamine is preferred. Carboxyamide, N,N'-dicyclohexylterephthalamide, N,N'-diphenyl Among them, N,N'-dicyclohexyl-2,6-naphthalene diamide and the like are mentioned. Dicarboxyamide is preferred. It is believed that since the amide compound has an amide group with high polarity, it is possible to localize electric charges in the crystal structure, resulting in high piezoelectricity.
[0037] A compound with high polarity such as an amide compound has a problem in that it has poor dispersibility in polypropylene resins with low polarity due to electrostatic interactions, and is prone to aggregation. However, a typical β-crystal nucleating agent has the property of dissolving in a polypropylene-based resin within a certain temperature range. Due to this characteristic, the β-crystal nucleating agent is uniformly dispersed in the polypropylene-based resin, and crystals derived from the β-crystal nucleating agent tend to precipitate uniformly. It is believed that this is why crystals of the amide compound with high polarity are uniformly dispersed in the polypropylene resin with low polarity, resulting in high piezoelectricity.
[0038] Specific examples of commercially available β-crystal nucleating agents include the β-crystal nucleating agent "N-Jester NU-100" manufactured by New Japan Chemical Co., Ltd., and specific examples of propylene-based resins to which a β-crystal nucleating agent has been added include the polypropylene "Bepol B-022SP" manufactured by Aristech, the polypropylene "Beta(β)-PP BE60-7032" manufactured by Borealis, and the polypropylene "BNX BETAPP-LN" manufactured by Mayzo.
[0039] The content of the β-crystal nucleating agent in the piezoelectric film of the present invention can be appropriately adjusted depending on the type of β-crystal nucleating agent or the composition of the polypropylene-based resin, etc., but is preferably 0.0001 parts by mass or more and 5.0 parts by mass or less, more preferably 0.001 parts by mass or more and 3.0 parts by mass or less, and even more preferably 0.01 parts by mass or more and 1.0 parts by mass or less, relative to 100 parts by mass of the polypropylene-based resin. If the content of the β-crystal nucleating agent is 0.0001 parts by mass or more, the β-crystals of the polypropylene resin are sufficiently generated and grown during production, sufficient β-crystal activity is ensured, and the piezoelectric properties of the piezoelectric film are good. In addition, sufficient β-crystal activity is ensured even when the film is stretched to form a porous film, and a piezoelectric film having the desired piezoelectric properties can be obtained by charging the film. On the other hand, if the amount is 5.0 parts by mass or less, this is economically advantageous and also preferred since bleeding of the β-crystal nucleating agent onto the film surface does not occur.
[0040] 3.Other In the present invention, components other than the polypropylene resin and the β-crystal nucleating agent may be contained within the range that does not impair the effects of the present invention. For example, resins other than polypropylene-based resins may be contained, and examples of such resins include polystyrene-based resins, polyvinyl chloride-based resins, polyvinylidene chloride-based resins, chlorinated polyethylene-based resins, polyester-based resins, polycarbonate-based resins, polyamide-based resins, polyacetal-based resins, acrylic-based resins, ethylene-vinyl acetate copolymers, polymethylpentene-based resins, polyvinyl alcohol-based resins, cyclic olefin-based resins, polylactic acid-based resins, polybutylene succinate-based resins, polyacrylonitrile-based resins, and polyethylene oxide. resins, cellulose-based resins, polyimide-based resins, polyurethane-based resins, polyphenylene sulfide-based resins, polyphenylene ether-based resins, polyvinyl acetal-based resins, polybutadiene-based resins, polybutene-based resins, polyamideimide-based resins, polyamide bismaleimide-based resins, polyarylate-based resins, polyetherimide-based resins, polyetheretherketone-based resins, polyetherketone-based resins, polyethersulfone-based resins, polyketone-based resins, polysulfone-based resins, aramid-based resins, and fluorine-based resins.
[0041] The piezoelectric film of the present invention may contain additives to the extent that the properties of the film are not impaired. The additives include recycled resins generated from trimming losses such as edges, which are added for the purpose of improving and adjusting molding processability, productivity, and various physical properties of the piezoelectric film; inorganic particles such as silica, talc, kaolin, calcium carbonate, etc.; pigments such as titanium oxide and carbon black; flame retardants, weather resistance stabilizers, heat resistance stabilizers, antistatic agents, melt viscosity improvers, crosslinking agents, lubricants, nucleating agents, plasticizers, antioxidants, antioxidants, light stabilizers, ultraviolet absorbers, neutralizing agents, anti-fogging agents, anti-blocking agents, slip agents, colorants, and other additives.
[0042] Furthermore, the piezoelectric film of the present invention may be laminated with functional layers such as a protective layer and a conductive layer in addition to the layer mainly composed of a polypropylene-based resin, without departing from the spirit of the present invention.
[0043] 4. Manufacturing method of piezoelectric film A method for producing the piezoelectric film of the present invention will be described below. However, the following description is only one example of a method for producing the piezoelectric film of the present invention, and the piezoelectric film of the present invention is not limited to the piezoelectric film produced by the method described below.
[0044] The piezoelectric film of the present invention is preferably produced through a film-forming step, a stretching step, and a charging step, although the stretching step may be omitted. The film-forming step, the stretching step, and the charging step will be described below in order.
[0045] (1) Film forming process In the film-forming process, a non-porous film made of the material constituting the piezoelectric film is formed. In the film-forming process, the material constituting the piezoelectric film is formed into a film by any known method, but the method is not particularly limited. For example, the resin composition (material resin) constituting the piezoelectric film is heated and melted to form a film. Specifically, the film is formed by the T-die method, the inflation method, or the like, and among them, the T-die method is preferably used. In addition, from a practical standpoint, it is preferable to melt-extrude the material resin through a T-die and cast it using a cast roll (chill roll, cast drum, etc.).
[0046] The material constituting the piezoelectric film may be kneaded in a kneading device and then formed into a film. The kneading device used for kneading is not particularly limited. For example, a known extruder such as a single screw extruder, a twin screw extruder, or a multi-screw extruder can be used. Depending on the equipment structure and necessity, the extruder may be provided with a vent port connected to a pressure reducer to remove moisture and low molecular weight substances.
[0047] When using a casting roll as described above, the film-like molten resin (resin composition) extruded from the T-die is extruded onto the casting roll, and is taken up while being in close contact with the rotating casting roll to form a film-like material. In order to make the film-like material adhere to the casting roll, a touch roll, an air knife, an electric adhesion device, or the like may be attached to the casting roll.
[0048] In addition, when the molten resin (resin composition) is cooled and molded into a film, the temperature of the cast roll is preferably 100° C. or higher, more preferably 110° C. or higher, and even more preferably 120° C. or higher. In the present invention, since the porosity can also be increased by opening holes in the crystalline and amorphous parts of the polypropylene resin during the stretching process, it is preferable to set the temperature of the cast roll to 100° C. or higher to obtain a nonporous membrane with a high degree of crystallinity. The upper limit of the casting roll temperature is preferably 140° C. or less, more preferably 135° C. or less, and even more preferably 130° C. or less. By setting the casting roll temperature to 140° C. or less, peeling from the casting roll during film formation is easy.
[0049] In the obtained nonporous membrane, the thickness of the effective portion excluding both ends is preferably 20 μm or more and 800 μm or less, more preferably 30 μm or more, even more preferably 40 μm or more, even more preferably 50 μm or more, and more preferably 700 μm or less, even more preferably 600 μm or less, and even more preferably 500 μm or less. If the thickness of the nonporous membrane is 20 μm or more, breakage during stretching can be prevented, and if the thickness of the nonporous membrane is 800 μm or less, stretching of the nonporous membrane can be facilitated. The layer structure of the non-porous membrane of the piezoelectric film of the present invention may be not only the single layer structure described above, but also a structure in which other layers are combined.
[0050] (2) Stretching process The obtained nonporous membrane-like material may be directly charged, or may be stretched. By stretching the nonporous membrane-like material, the nonporous membrane-like material can be easily made into a porous film. In the stretching process, the nonporous membrane may be uniaxially stretched or biaxially stretched, with uniaxial stretching being preferred. The uniaxial stretching may be longitudinal uniaxial stretching or transverse uniaxial stretching. The biaxial stretching may be simultaneous biaxial stretching or sequential biaxial stretching. When sequential biaxial stretching is employed among these, it is relatively easy to control the porous structure and it is easy to balance with other physical properties such as mechanical strength and shrinkage rate. The stretching of the film in the machine direction (MD) is called "longitudinal stretching", and the stretching in the direction perpendicular to the machine direction (TD) is called "transverse stretching".
[0051] The stretching temperature must be appropriately selected depending on the composition of the resin composition used, the crystalline melting peak temperature, the crystallinity, etc., but the longitudinal stretching temperature is preferably 60°C or higher and 140°C or lower, more preferably 80°C or higher and 120°C or lower. A longitudinal stretching temperature of 140° C. or less is preferable because stretching can be performed without breakage at a temperature below the melting point of the polypropylene resin, which is the main component, whereas a longitudinal stretching temperature of 60° C. or more is preferable because breakage during stretching can be suppressed.
[0052] The transverse stretching temperature is preferably 90° C. or more and 160° C. or less, more preferably 100° C. or more and 150° C. or less. When the transverse stretching temperature is within the specified range, pores are sufficiently formed, the porosity can be increased, and sufficient piezoelectricity can be obtained. In the case of successive biaxial stretching, for example, the pores generated during longitudinal stretching are enlarged, so that the porosity of the porous layer can be increased, and sufficient piezoelectricity can be obtained.
[0053] The temperatures described above are for uniaxial stretching or sequential biaxial stretching, but simultaneous biaxial stretching From the above viewpoints, the stretching temperature in the case of axial stretching is preferably 90° C. or more and 160° C. or less, more preferably Preferably, the temperature is adjusted within the range of 100°C or higher and 150°C or lower.
[0054] The stretching ratio may be selected arbitrarily according to the desired porosity, but the stretching ratio per uniaxial stretching is preferably 1.1 to 20 times, more preferably 1.5 to 18 times, even more preferably 4 to 16 times, and still more preferably 4 to 10 times. By setting the stretching ratio per uniaxial stretching to 1.1 times or more, whitening progresses and the stretching-induced porosity occurs sufficiently, while by setting the stretching ratio to 20 times or less, the porosity is suppressed and a porous film with excellent pressure resistance can be obtained. In the case of sequential biaxial stretching, by stretching at the stretch ratio specified above for each axis, voids generated during the previous stretching are not deformed during the subsequent stretching.
[0055] (3) Charging process The piezoelectric film of the present invention can be obtained by subjecting the non-porous film obtained in the film-forming process or the porous film obtained through the stretching process to an electrification treatment. The electrification treatment may be continuous or batchwise. The electrodes used in the electrification treatment may be a needle-shaped electrode, a wire electrode, a roll-shaped electrode, a plate-shaped electrode, or the like, on the front and back of the film, and the film may be passed between the electrodes to apply an electric field between the electrodes, or an electric field may be applied after electrodes are formed directly on the front and back of the film by coating or vapor deposition. The electric field to be applied is preferably 0.1 MV / m to 10 MV / m, more preferably 0.2 MV / m to 8 MV / m, and even more preferably 0.3 MV / m to 6 MV / m. By applying an electric field of 0.1 MV / m or more, excellent piezoelectricity can be obtained. By applying an electric field of 10 MV / m or less, the effect of reducing dielectric breakdown during charging processing is achieved.
[0056] Furthermore, the piezoelectric film of the present invention can be subjected to surface treatments such as corona treatment, plasma treatment, printing, coating, vapor deposition, and even perforation, as necessary, without impairing the present invention, and several piezoelectric films of the present invention can be stacked depending on the application.
[0057] <Applications of piezoelectric film> The piezoelectric film of the present invention can be used, for example, in actuators, oscillators, sonars, vibration power generation, sensors, etc. Although there is no particular limitation on the piezoelectric film, for example, by mounting lead wires or forming an insulating film to form a piezoelectric element, the pressure acting on the piezoelectric film can be converted into a voltage, and the pressure acting on the piezoelectric film can be detected or electricity can be generated. EXAMPLES
[0058] The piezoelectric film of the present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited in any way.
[0059] The materials used in the examples and comparative examples are as follows. (Polypropylene resin) A-1: Homopolypropylene (Novatec PP FY6HA, MFR: 2.4g / 10min [230℃, 2.16kg load], Mw / Mn=3.2, Japan Polypropylene Corporation) (β crystal nucleating agent) B-1: N,N'-dicyclohexyl-2,6-naphthalenedicarboxamide (NU-100, manufactured by New Japan Chemical Co., Ltd.) B-2: 3,9-bis[4-(N-cyclohexylcarbamoyl)phenyl]-2,4,8,10-tetraoxaspiro[5,5]undecane (Antioxidants) C-1: A 1:1 mixture of tris(2,4-di-t-butylphenyl)phosphite and tetrakis[3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionic acid]pentaerythritol (IRGANOX-B225, manufactured by BASF)
[0060] Example 1 100 parts by mass of polypropylene resin (A-1), 0.2 parts by mass of β-crystal nucleating agent (B-1), and 0.1 parts by mass of antioxidant (C-1) were mixed and melt-extruded at 280° C. using a twin-screw extruder to obtain resin composition 1. The resin composition 1 was charged into the extruder connected to a T-die with a lip opening of 1 mm, and molded, and then guided to a cast roll to obtain a non-porous membrane having a thickness of 30 μm. The obtained non-porous membrane was placed on an earth plate and charged using needle electrodes with a voltage of 10 kV applied at an inter-electrode distance of 20 mm to obtain a piezoelectric film with a thickness of 30 μm.
[0061] Example 2 The resin composition 1 was charged into an extruder connected to a T-die with a lip opening of 1 mm, molded, and guided to a casting roll to obtain a non-porous membrane having a thickness of 100 μm. Thereafter, the film was stretched 7 times in the transverse direction at a stretching temperature of 100°C in a film tenter facility (manufactured by Kyoto Machinery Co., Ltd.) to obtain a porous film. The obtained porous film was placed on an earth plate, and charged with a voltage of 10 kV using needle electrodes with an inter-electrode distance of 20 mm to obtain a piezoelectric film.
[0062] Example 3 The β-crystal nucleating agent (B-2) was added in place of the β-crystal nucleating agent (B-1) to obtain a resin composition 2. Thereafter, in the same manner as in Example 1, a piezoelectric film was obtained.
[0063] Example 4 The resin composition 2 was charged into an extruder connected to a T-die with a lip opening of 1 mm, molded, and guided to a casting roll to obtain a non-porous membrane having a thickness of 120 μm. Thereafter, the film was stretched 4 times in the transverse direction at a stretching temperature of 100° C. in a film tenter facility (manufactured by Kyoto Machinery Co., Ltd.), and further stretched 4 times in the transverse direction at a stretching temperature of 150° C. to obtain a porous film. The obtained porous film was placed on an earth plate, and charged using needle electrodes with a voltage of 10 kV at an electrode distance of 20 mm to obtain a piezoelectric film.
[0064] Example 5 The resin composition 1 was charged into an extruder connected to a T-die with a lip opening of 1 mm, molded, and guided to a casting roll to obtain a non-porous membrane having a thickness of 40 μm. Thereafter, the film was stretched 3 times in the transverse direction at a stretching temperature of 100°C in a film tenter facility (manufactured by Kyoto Machinery Co., Ltd.) to obtain a porous film. The obtained porous film was placed on an earth plate, and charged with a voltage of 10 kV using needle electrodes with an inter-electrode distance of 20 mm to obtain a piezoelectric film.
[0065] Example 6 The resin composition 1 was charged into an extruder connected to a T-die with a lip opening of 1 mm, molded, and guided to a casting roll to obtain a non-porous membrane having a thickness of 55 μm. Thereafter, the film was stretched 7 times in the transverse direction at a stretching temperature of 100°C in a film tenter facility (manufactured by Kyoto Machinery Co., Ltd.) to obtain a porous film. The obtained porous film was placed on an earth plate, and charged with a voltage of 10 kV using needle electrodes with an inter-electrode distance of 20 mm to obtain a piezoelectric film.
[0066] Example 7 The resin composition 2 was charged into an extruder connected to a T-die with a lip opening of 1 mm, molded, and guided to a casting roll to obtain a non-porous membrane having a thickness of 120 μm. Thereafter, the film was stretched 4 times in the transverse direction at a stretching temperature of 100°C in a film tenter facility (Kyoto Kikai Co., Ltd.) to obtain a porous film. The obtained porous film was placed on an earth plate, and charged with a voltage of 10 kV using needle electrodes with an electrode distance of 20 mm to obtain a piezoelectric film.
[0067] Example 8 The resin composition 2 was charged into an extruder connected to a T-die with a lip opening of 1 mm, molded, and guided to a casting roll to obtain a non-porous membrane having a thickness of 120 μm. Thereafter, the film was stretched twice in the transverse direction at a stretching temperature of 100° C. in a film tenter facility (manufactured by Kyoto Machinery Co., Ltd.), and then further stretched twice in the transverse direction at a stretching temperature of 150° C. to obtain a porous film. The obtained porous film was placed on an earth plate, and charged using needle electrodes with a voltage of 10 kV at an electrode distance of 20 mm to obtain a piezoelectric film.
[0068] Comparative Example 1 The resin composition 1 was charged into an extruder connected to a T-die with a lip opening of 1 mm, molded, and guided to a casting roll to obtain a non-porous membrane having a thickness of 80 μm. Thereafter, using a longitudinal stretching machine, longitudinal stretching was performed between rolls set at 105°C at a draw ratio of 65% in three stages (longitudinal stretching ratio 4.5 times). The film after longitudinal stretching was preheated in a film tenter facility (manufactured by Kyoto Machinery Co., Ltd.) at a preheating temperature of 150°C for a preheating time of 12 seconds, then stretched 2.1 times in the transverse direction at a stretching temperature of 150°C and heat-treated at 155°C to obtain a porous film. The obtained laminated porous film was placed on an earth plate, and a needle-shaped electrode was used to apply a voltage of 10 kV at an electrode distance of 20 mm to perform charging treatment, thereby obtaining a piezoelectric film.
[0069] Comparative Example 2 A piezoelectric film was obtained in the same manner as in Example 1, except that the β crystal nucleating agent (B-1) was not added.
[0070] The piezoelectric films obtained in the examples and comparative examples were measured for thickness, porosity, β-crystal formation ability, air permeability, piezoelectricity, pressure resistance, total light transmittance, and average aspect ratio by the following methods.
[0071] (1) Thickness The thickness of the piezoelectric film was measured at 10 random points using a 1 / 1000 mm dial gauge, and the average value was calculated.
[0072] (2) Porosity The piezoelectric film was cut into a piece having a width of 100 mm and a length of 100 mm to prepare a measurement sample. The actual mass W1 of the measurement sample was measured, and the mass W0 when the porosity was 0% was calculated based on the density of the resin composition. The porosity was calculated from these values based on the following formula. Porosity (%)={(W0-W1) / W0}×100
[0073] (3) β crystal formation ability The DSC measurement of the piezoelectric film was carried out by the following method. First, the temperature was raised from 40°C to 200°C at 10°C / min in a nitrogen atmosphere, held for 1 minute, and then cooled to 40°C at 10°C / min. After holding for 1 minute, the temperature was raised again at 10°C / min. The melting peaks observed were determined as follows: the melting peaks in the temperature range of 145 to 157°C were the melting peaks of β crystals, and the melting peaks at 158°C or higher were the melting peaks of α crystals. The heat of fusion of each was calculated from the area of the region surrounded by the baseline drawn based on the flat part on the high temperature side and the heat of fusion of the α crystals was ΔHα, and the heat of fusion of the β crystals was ΔHβ, and the calculation was performed using the following formula. β crystal formation ability (%) = [ΔHβ / (ΔHα+ΔHβ)]×100
[0074] (4) Air permeability at 25°C The air permeability was measured in an air atmosphere at 25° C. in accordance with JIS P 8117. The measuring device used was a digital Oken-type dedicated air permeability measuring device (manufactured by Asahi Seiko Co., Ltd.).
[0075] (5) Piezoelectric constant The piezoelectric film was cut into a piece 50 mm wide x 50 mm long to prepare a measurement sample. Using a piezometer manufactured by Lead Techno Corporation, the piezoelectric constant (d 33 ) was measured by a quasi-static method (for convenience, surface: d A , d B , d C , d D , d E Back: d F , d G , d H , d I , d JThe terminal of the piezometer was cylindrical with a diameter of 8 mm, and measurements were performed with a clamp load of 1 N and a dynamic load of 1.3 N. Since the measured values on the front and back sides of the measurement sample were positive and negative, respectively, the average value of the piezoelectric constant was calculated by the following formula. Piezoelectric constant = |d A +d B +d C +d D +d E -d F -d G -d H -d I -d J | / 10
[0076] (6) Piezoelectric The piezoelectric properties of the piezoelectric film were evaluated according to the following criteria. A (better): The piezoelectric constant is 100 pC / N or more. B (good): The piezoelectric constant is 50 pC / N or more and less than 100 pC / N. (Within practical range) C (poor): The piezoelectric constant is less than 50 pC / N.
[0077] (7) Piezoelectric constant under a pressure of 50 kPa After applying pressure to the piezoelectric film by adjusting the clamp load and dynamic load of the piezometer, the piezoelectric constant was determined in the same manner as in (5) above. Note that the terminals of the piezometer were cylindrical with a diameter of 8 mm, and measurements were performed with a clamp load of 2.51 N and a dynamic load of 2.81 N.
[0078] (8) Pressure resistance The pressure resistance of the piezoelectric film was evaluated according to the following criteria. A (better): The piezoelectric constant is 100 pC / N or more under a pressure of 50 kPa. B (good): The piezoelectric constant under a pressure of 50 kPa is 50 pC / N or more and less than 100 pC / N. C (poor): The piezoelectric constant under a pressure of 50 kPa is less than 50 pC / N.
[0079] (9) Total light transmittance The total light transmittance was measured in accordance with JIS K 7136 using a haze meter "HM-150" (manufactured by Murakami Color Research Laboratory Co., Ltd.).
[0080] (10) Average aspect ratio of hole cross section More than 100 voids were selected from the cross-sectional SEM images of the piezoelectric films of Example 2, Examples 4 to 8, and Comparative Example 1, and the aspect ratio of each void (length in the stretching direction / length in the film thickness direction) was calculated from the length of each void in the stretching direction and the length in the film thickness direction, and the average value was calculated. When biaxial stretching was performed, the aspect ratio of the cross section of the pores in the stretching direction with the higher stretch ratio was adopted, and in Comparative Example 1, the longitudinal stretching direction was adopted.
[0081] Table 1 shows the evaluation results for the examples and comparative examples.
[0082] [Table 1]
[0083] The piezoelectric films of Examples 1 to 8 contained a polypropylene resin and a β crystal nucleating agent, had a porosity of 0% or more and 35% or less, and had an air permeability of 40,000 sec / dL or more, and thus had good piezoelectric properties and pressure resistance. In particular, the piezoelectric films of Examples 2 and 4 to 6 had better pressure resistance due to the presence of holes with an average aspect ratio of 4.0 or more. On the other hand, the porosity was too high in Comparative Example 1, and therefore the pressure resistance was insufficient. In Comparative Example 2, since no β crystal nucleating agent was included, the piezoelectricity was insufficient.
Claims
1. A piezoelectric film made of a resin composition containing a polypropylene-based resin and a β-crystal nucleating agent, having a porosity of 0% or more and 35% or less and an air permeability of 40,000 sec / dL or more, wherein the resin composition contains a polypropylene-based resin as a main component and the β-crystal nucleating agent is an amide compound.
2. A piezoelectric film as described in claim 1, wherein the content of the β crystal nucleating agent is 0.0001 parts by mass or more and 5.0 parts by mass or less per 100 parts by mass of the polypropylene-based resin.
3. The piezoelectric film according to claim 1 or 2, having a β-crystal generating ability of 80% or more.
4. 4. The piezoelectric film according to claim 1, wherein the total light transmittance is 30% or more.
5. 5. The piezoelectric film according to claim 1, having a piezoelectric constant of 50 pC / N or more and 10,000 pC / N or less.
6. 6. The piezoelectric film according to claim 1, wherein the piezoelectric constant under a pressure of 50 kPa is 50 pC / N or more and 10,000 pC / N or less.
7. The piezoelectric film according to any one of claims 1 to 6, having a thickness of 1 µm or more and 100 µm or less.
8. The piezoelectric film according to any one of claims 1 to 7, having pores with an average aspect ratio of 4.0 or more.
9. A piezoelectric element comprising the piezoelectric film according to any one of claims 1 to 8.
Citation Information
Patent Citations
Method for manufacturing foamed plastic products
JP1998504853A
Electret-converted film
JP2010089494A
Electret-converted film
JP2010089495A
Microporous film, laminated microporous film, battery separator and method for producing microporous film
JP2011074214A
Energy conversion film
JP2011084735A