Hydrous gel

A hydrogel with modified polyvinyl alcohol and controlled functional group modification achieves both high water resistance and reduced yellowing, addressing the limitations of existing hydrogels by optimizing irradiation conditions and composition.

JP7567193B2Active Publication Date: 2024-10-16MITSUBISHI CHEM CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020060380
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-30
Publication Date
2024-10-16
Estimated Expiration
2040-03-30

AI Technical Summary

Technical Problem

Existing hydrogels made from modified polyvinyl alcohol suffer from poor water resistance and yellowing issues, particularly when irradiated with active energy rays, and existing methods either lack evaluation of water resistance or require high energy or long irradiation times, leading to increased yellowing.

Method used

A hydrogel comprising a resin composition with modified polyvinyl alcohol containing active energy ray-curable functional groups, specifically designed to have a yellowness index of 1.0 or less and a dissolution rate of 30% or less after immersion in water for 1 hour, achieved by controlling the amount of modification and using a photopolymerization initiator.

Benefits of technology

The hydrogel exhibits excellent water resistance and suppressed yellowing, with a yellowness index of 1.0 or less and a dissolution rate of 30% or less, making it suitable for applications requiring high durability and transparency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567193000001
    Figure 0007567193000001
Patent Text Reader

Abstract

To provide a water-containing gel which has excellent water resistance and also excellent yellowing resistance.SOLUTION: There is provided a water-containing gel composed of a resin composition containing a modified polyvinyl alcohol-based resin having an active energy ray-curable functional group. The water-containing gel has a yellowness index (YI) of 1.0 or less according to JIS K7373 reflection measurement, and has an elution rate of 30% or less after immersion for 1 hour in water at 80°C.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hydrogel, and more particularly to a hydrogel containing a modified polyvinyl alcohol having excellent water resistance and yellowing resistance and having a functional group that can be cured by irradiation with active energy rays. [Background technology]

[0002] Polyvinyl alcohol is a water-soluble polymer that has excellent film-forming properties and low toxicity, but has the drawback of being soluble in water, and therefore improvement therein is desired.

[0003] As an attempt to make polyvinyl alcohol slightly soluble in water, a method is known in which a functional group curable with active energy rays is introduced into polyvinyl alcohol to prepare a modified polyvinyl alcohol, an aqueous solution of the modified polyvinyl alcohol is applied to a substrate, the substrate is dried to remove water, and then the substrate is irradiated with active energy rays to obtain a cured product.

[0004] For example, Patent Document 1 discloses a method for obtaining a (meth)acrylic group-modified polyvinyl alcohol by reacting polyvinyl alcohol with (meth)acrylic anhydride in an organic solvent in which polyvinyl alcohol is insoluble and (meth)acrylic anhydride is soluble. Furthermore, Patent Document 2 discloses a gel containing a polyvinyl alcohol crosslinked product obtained by crosslinking polyvinyl alcohol having a radical polymerizable group, and a water-soluble polymer crosslinked product obtained by crosslinking a water-soluble polymer having a carboxy group with a metal ion. Patent Document 3 discloses a vinyl alcohol copolymer containing a structural unit consisting of a diazonium salt group. Furthermore, Patent Document 4 discloses a hydrogel containing water and a cured product obtained by curing a photocurable composition containing a hydrophilic monomer having one (meth)acryloyl structure, a crosslinking agent having two or more (meth)acryloyl structures, an inorganic ultraviolet shielding agent, and a photopolymerization initiator. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 13803 / 1983 [Patent Document 2] JP 2019-85521 A [Patent Document 3] Japanese Patent Application Publication No. 11-199634 [Patent Document 4] JP 2019-44135 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, although the above-mentioned Patent Document 1 discloses a method for obtaining a cured product of modified polyvinyl alcohol by drying water from an aqueous solution of modified polyvinyl alcohol and then irradiating the solution with ultraviolet light, it does not evaluate the water resistance of the cured product when irradiated with ultraviolet light while the cured product still contains a large amount of water. Furthermore, although Patent Document 2 discloses a water-containing gel containing methacryl-modified polyvinyl alcohol, the water resistance of the gel is not evaluated. The above-mentioned Patent Document 3 discloses a modified polyvinyl alcohol having water resistance, but the synthesis is complicated and the storage stability is poor, so that further improvement is required. In the technique disclosed in Patent Document 4, high energy or long-term irradiation is required to obtain a thick ultraviolet-cured product, and further improvement is required.

[0007] In addition, the cured product thus obtained is often colored yellow, and there is a demand for reducing the coloration. In order to obtain a hydrogel having high water resistance, it is sufficient to irradiate the active energy rays with a high intensity, but there is a problem in that the gel turns more yellow when the irradiation with the active energy rays is intensified.

[0008] Therefore, an object of the present invention is to provide a hydrogel that is excellent in water resistance and also excellent in yellowing resistance. [Means for solving the problem]

[0009] Means of the Invention The present inventors have conducted intensive research in light of the above circumstances and have found that the above problems can be solved by specifying the degree of modification of a modified polyvinyl alcohol having an active energy ray-curable functional group.

[0010] That is, the gist of the present invention is a hydrogel made of a resin composition containing a modified polyvinyl alcohol-based resin having an active energy ray-curable functional group, the hydrogel having a yellowness index (YI) of 1.0 or less as measured by JIS K7373 reflection measurement and an elution rate of 30% by weight or less after immersion in water at 80°C for 1 hour. Effect of the Invention

[0011] As described above, the hydrogel of the present invention is a hydrogel made of a resin composition containing a modified polyvinyl alcohol resin having an active energy ray-curable functional group, and has a yellowness index (YI) of 1.0 or less as measured by reflection measurement according to JIS K7373, and a dissolution rate of 30% by weight or less after immersion in water at 80° C. for 1 hour. Therefore, it is a gel of excellent quality that achieves a high level of two contradictory physical properties, namely, high water resistance and suppressed yellow coloration. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The configuration of the present invention will be described in detail below, but these are examples of preferred embodiments. In this specification, "(meth)acrylic" includes "acrylic" and "methacrylic", and "(meth)acryloyl" includes "acryloyl" and "methacryloyl".

[0013] The hydrogel of the present invention is made of a resin composition containing a modified polyvinyl alcohol (hereinafter, polyvinyl alcohol will be referred to as "PVA")-based resin having an active energy ray-curable functional group.

[0014] [Modified PVA resin having active energy ray-curable functional groups] The modified PVA resin having an active energy ray-curable functional group can be obtained, for example, by a method of introducing an active energy ray-curable functional group via a side chain or a terminal functional group of a raw material PVA resin, or by a method of copolymerizing a compound having an active energy ray-curable functional group during the production process of the PVA resin to introduce an active energy ray-curable functional group, etc. Among these, the method of introducing an active energy ray-curable functional group via a side chain or a terminal functional group of a raw material PVA resin is preferred. The PVA-based resin used as the raw material (hereinafter referred to as the "raw PVA-based resin") will be described below.

[0015] [Raw material PVA resin] The raw material PVA resin is usually preferably an unmodified PVA resin, but a copolymer-modified PVA resin may also be used.

[0016] The unmodified PVA resin can usually be produced by polymerizing a vinyl ester monomer and then saponifying the polymer.

[0017] Examples of the vinyl ester monomer include aliphatic vinyl esters such as vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl versatate, and vinyl trifluoroacetate, and aromatic vinyl esters such as vinyl benzoate. Among these, aliphatic vinyl esters having 3 to 20 carbon atoms, more preferably 4 to 10 carbon atoms, and particularly preferably 4 to 7 carbon atoms, and particularly preferably vinyl acetate. These are usually used alone, but multiple types may be used simultaneously as necessary.

[0018] The copolymer modified PVA resin can be produced by saponifying a polymer of the vinyl ester monomer and another unsaturated monomer. The amount of the other unsaturated monomer introduced in the copolymer modified PVA resin is usually 20 mol % or less, preferably 10 mol % or less, and particularly preferably 5 mol % or less.

[0019] Examples of the other unsaturated monomers include olefins such as ethylene, propylene, isobutylene, α-octene, α-dodecene, and α-octadecene; unsaturated acids such as (meth)acrylic acid, crotonic acid, maleic acid, maleic anhydride, and itaconic acid, or their salts or mono- or dialkyl esters; nitriles such as (meth)acrylonitrile; amides such as (meth)acrylamide; olefin sulfonic acids such as ethylene sulfonic acid, allyl sulfonic acid, and methallyl sulfonic acid, or their salts; alkyl vinyl ethers; N-acrylamidomethyltrimethylammonium chloride, allyl trimethylammonium chloride, dimethylallyl vinyl ketone, N-vinylpyrrolidone, vinyl chloride, vinylidene chloride, polyoxyethylene (meth)allyl ether, and the like. Examples of the polyoxyalkylene (meth)allyl ether include polyoxyalkylene (meth)acrylates such as polyoxyethylene (meth)acrylate and polyoxypropylene (meth)acrylate, polyoxyalkylene (meth)acrylamides such as polyoxyethylene (meth)acrylamide and polyoxypropylene (meth)acrylamide, polyoxyethylene (1-(meth)acrylamide-1,1-dimethylpropyl) ester, polyoxyethylene vinyl ether, polyoxypropylene vinyl ether, polyoxyethylene allylamine, polyoxypropylene allylamine, polyoxyethylene vinylamine, polyoxypropylene vinylamine, 3,4-diacetoxybutene, etc. These may be used alone or in combination of two or more.

[0020] The raw material PVA resin can be obtained by any known polymerization method, saponification method, and post-modification method.

[0021] The average saponification degree of the raw material PVA resin is usually 50 to 99 mol%, preferably 60 to 95 mol%, and particularly preferably 65 to 90 mol%. If the average saponification degree is too low, it tends to be difficult to dissolve in water, and if the average saponification degree is too high, it tends to be difficult to handle when preparing a hydrogel because the viscosity becomes too high. The average saponification degree is measured in accordance with JIS K 6726.

[0022] The average degree of polymerization of the raw material PVA resin is usually 100 to 4000, preferably 200 to 3000, and particularly preferably 250 to 2500. If the average degree of polymerization is too low, the hydrogel tends to be brittle, and if the average degree of polymerization is too high, the viscosity of the hydrogel becomes too high during preparation, making it difficult to handle. The average degree of polymerization is measured in accordance with JIS K 6726.

[0023] Furthermore, as the raw material PVA-based resin, two or more kinds of resins differing in the type of modification, the amount of modification, the average degree of saponification, the average degree of polymerization, etc. may be used in combination.

[0024] [Compounds having active energy ray-curable functional groups] In the present invention, as described above, a method of introducing an active energy ray-curable functional group via a side chain or a terminal functional group of the raw material PVA-based resin is preferred, more preferably a method of reacting a compound having an active energy ray-curable functional group with a hydroxyl group or a 1,3-diol group in a side chain of the raw material PVA-based resin, and particularly preferably a method of reacting a compound having an active energy ray-curable functional group with a hydroxyl group in a side chain of the raw material PVA-based resin.

[0025] Examples of the functional group curable with active energy rays include a (meth)acryloyl group, a vinyl group, a (meth)acryloylamino group, a vinylphenyl group, a cyclohexenyl group, a cyclopentenyl group, a norbornenyl group, a dicyclopentenyl group, etc. Among these, a (meth)acryloyl group is preferred from the viewpoint of reactivity.

[0026] Examples of the compound having a (meth)acryloyl group include (meth)acrylic acids such as (meth)acrylic acid, (meth)acrylic anhydride, (meth)acrylic acid halide, and (meth)acrylic acid ester, and among these, (meth)acrylic anhydride is preferred.

[0027] The reaction between the raw PVA resin and the compound having a (meth)acryloyl group can be carried out by reacting the compound having a (meth)acryloyl group in the presence of a base catalyst in a solvent in which the raw PVA resin is dispersed. This causes an esterification reaction or an ester exchange reaction between the hydroxyl group of the raw PVA resin and the carboxylic acid of the compound having a (meth)acryloyl group, and a modified PVA resin having a (meth)acryloyl group can be obtained.

[0028] The amount of the compound having the (meth)acryloyl group is usually 60 to 140 parts by weight, preferably 70 to 130 parts by weight, and particularly preferably 80 to 120 parts by weight, based on 100 parts by weight of the raw material PVA resin. If the amount of the compound having the (meth)acryloyl group is too small, a sufficient amount of (meth)acryloyl group cannot be introduced into the PVA resin, and the water resistance tends to be poor when the water-containing gel is formed. If the amount is too large, the compound dissolves in the solvent during the reaction, and it tends to be difficult to separate the modified PVA resin having the (meth)acryloyl group.

[0029] The above-mentioned solvent is preferably a solvent in which the raw material PVA resin does not dissolve but a compound having a functional group curable by active energy rays is soluble, and examples of the solvent include lower halogenated hydrocarbons, lower aliphatic ketones, aliphatic hydrocarbons, alicyclic hydrocarbons, aromatic hydrocarbons, etc. These may be used alone or in combination of two or more kinds.

[0030] Specific examples include methylene chloride, chloroform, tetrachlorohydrocarbon, trichloroethane, acetone, methyl ethyl ketone, methyl isobutyl ketone, hexane, cyclohexane, benzene, acetone, dimethyl sulfoxide, N-methylpyrrolidone, dimethylformamide, dimethylacetamide, etc. Among these, acetone is preferable.

[0031] The amount of the solvent is not particularly limited, but is usually 30 to 100 parts by weight, and preferably 40 to 70 parts by weight, per 100 parts by weight of the total of the raw material PVA resin and the compound having a (meth)acryloyl group.

[0032] Examples of the base catalyst include tertiary amines such as triethylamine, tetramethylethylenediamine, tributylamine, tri-n-octylamine, N,N-dimethylbenzylamine, and pyridine, quaternary ammonium salts such as tetramethylammonium chloride, tetramethylammonium bromide, tetraethylammonium bromide, and tetrabutylammonium bromide, and phosphorus compounds such as triphenylphosphine and tributylphosphine. These may be used alone or in combination of two or more. Among them, tertiary amines are preferred, and N,N-dimethylbenzylamine is particularly preferred.

[0033] The amount of the basic catalyst is usually 0.1 to 1 part by weight, and preferably 0.2 to 0.7 parts by weight, based on 100 parts by weight of the raw material PVA resin.

[0034] The reaction temperature is not particularly limited, but is usually 10 to 100°C, and preferably 40 to 80°C.

[0035] The reaction time is not particularly limited, but is usually 2 to 40 hours, preferably 4 to 20 hours.

[0036] The post-treatment of the reaction solution after the reaction and the isolation of the reaction product [(meth)acryloyl group-containing modified PVA-based resin] may be carried out according to a known method. For example, the reaction solution is filtered to obtain the (meth)acryloyl group-containing modified PVA-based resin as a residue. The (meth)acryloyl group-containing modified PVA-based resin obtained may be dried and used as it is, but in order to increase the purity, it is preferable to dry the resin after carrying out a purification operation such as washing or Soxhlet extraction.

[0037] The modification amount of the modified PVA resin having a (meth)acryloyl group thus obtained is preferably 2.5 to 10 mol%, more preferably 3 to 8 mol%, and particularly preferably 3.5 to 6 mol%. If the modification amount is too small, the water resistance of the hydrogel tends to be poor, whereas if the modification amount is too large, the volumetric shrinkage of the gel due to irradiation with active energy rays tends to be too large.

[0038] The modified PVA-based resin having an active energy ray-curable functional group is the main component of the resin composition, and its content is 50% by weight or more of the resin composition, preferably 70% by weight or more, and more preferably 90% by weight or more.

[0039] [Photopolymerization initiator] In addition to the modified PVA resin having an active energy ray-curable functional group, the resin composition preferably contains a photopolymerization initiator, which can accelerate the reaction upon irradiation with active energy rays.

[0040] The photopolymerization initiator is not particularly limited as long as it generates radicals by the action of light, and examples thereof include photopolymerization initiators such as acetophenones, benzoins, benzophenones, thioxanthones, and acylphosphine oxides. These photopolymerization initiators can be used alone or in combination of two or more. In the present invention, the aqueous solution of the resin composition is irradiated with active energy rays to obtain a hydrous gel, so the photopolymerization initiator is preferably water-soluble.

[0041] The amount of the photopolymerization initiator is preferably 0.01 to 20 parts by weight, particularly preferably 0.1 to 10 parts by weight, and further preferably 0.5 to 5 parts by weight, based on 100 parts by weight of the modified PVA resin having an active energy ray-curable functional group. If the amount is too small, the curing speed tends to decrease or the curing tends to be insufficient, whereas if the amount is too large, the curability does not improve any more and the economical efficiency tends to decrease.

[0042] [Other optional ingredients] The resin composition used in the present invention may contain other optional components in addition to the modified PVA resin having an active energy ray-curable functional group and the photopolymerization initiator.

[0043] Examples of other optional components include antioxidants, plasticizers, tackifiers, crosslinking agents, crosslinking accelerators, silane coupling agents, antistatic agents, and functional dyes. These can be used alone or in combination of two or more. The content of other optional components may be within a range that does not impair the effects of the present invention, and is preferably 0.1 to 10% by weight in the resin composition.

[0044] The hydrogel of the present invention can be obtained by preparing an aqueous solution of the above-mentioned resin composition and irradiating the aqueous solution with active energy rays.

[0045] The concentration of the resin composition in the aqueous solution is preferably 5 to 30% by weight, and more preferably 10 to 20% by weight from the viewpoints of water resistance and ease of application.

[0046] The aqueous solution of the resin composition may be irradiated with active energy rays as it is to form a hydrous gel, but it is preferable to coat the aqueous solution and then irradiate it with active energy rays to form a thin-film hydrous gel. By irradiating with active energy rays, the functional groups of the modified PVA having active energy ray-curable functional groups form a crosslinked structure at least either intramolecularly or intermolecularly, thereby forming a hydrous gel.

[0047] The method for applying the resin composition is not particularly limited as long as it is a common application method, and examples thereof include methods using an applicator, roll coating, die coating, gravure coating, comma coating, and screen printing.

[0048] Examples of the active energy rays that can be used include light rays such as far ultraviolet rays, ultraviolet rays, near ultraviolet rays, and infrared rays, electromagnetic waves such as X-rays and gamma rays, as well as electron beams, proton beams, and neutron beams. In view of the curing speed, availability of irradiation equipment, cost, and the like, ultraviolet rays are preferred.

[0049] When curing by irradiating ultraviolet light, high pressure mercury lamps, ultra-high pressure mercury lamps, carbon arc lamps, metal halide lamps, xenon lamps, chemical lamps, electrodeless discharge lamps, LED lamps, etc. are used, usually at 30 to 3000 mJ / cm. 2 , preferably 100 to 1500 mJ / cm 2 The ultraviolet light may be irradiated at 100 nm.

[0050] The thickness of the hydrogel of the present invention thus obtained is usually 1 to 1000 μm, preferably 10 to 800 μm, and more preferably 20 to 700 μm.

[0051] The water content of the hydrogel of the present invention is preferably 30% by weight or more, and particularly preferably 60 to 90% by weight. If the water content is too low, the conformability to the substrate tends to decrease, and if the water content is too high, the gel tends to have difficulty in maintaining its shape.

[0052] The hydrogel has a yellowness index (YI) of 1.0 or less, preferably 0.7 or less, and more preferably 0.5 or less, as measured by reflection measurement according to JIS K7373. That is, the hydrogel of the present invention has a low yellowness after curing and is excellent in transparency. The above yellowness index is the yellowness index of a hydrogel prepared by the following method. That is, a 15% by weight aqueous solution of the resin composition used in the present invention is prepared, and this is coated so that the film thickness after irradiation with active energy rays is 30 μm, and then 200 mJ / cm is applied. 2The hydrogel is prepared by irradiating the gel with ultraviolet light of 1000 nm. The yellowness index (YI) of the hydrogel is calculated as the value.

[0053] Furthermore, the hydrogel of the present invention has an elution rate of 30% by weight or less, preferably 25% by weight or less, and more preferably 20% by weight or less after immersion in water at 80°C for 1 hour. The hydrogel of the present invention has excellent water resistance because the elution rate is low even when immersed in water at 80°C for 1 hour. The elution rate is determined by the following method. That is, a 15% by weight aqueous solution of the resin composition used in the present invention is prepared, coated to a liquid layer thickness of 500 μm, and immediately subjected to 200 mJ / cm 2 A hydrous gel is prepared by irradiating the hydrous gel with ultraviolet rays of 100 nm. The hydrous gel is heated and dried under reduced pressure, and the amount of the resin composition before immersion is determined. The hydrous gel is also immersed in water at 80°C for 1 hour, and then heated and dried under reduced pressure, and the amount of the resin composition after immersion is determined. The elution rate is determined from the amount of the resin composition before immersion and the amount of the resin composition after immersion according to the following formula. Dissolution rate (wt%)=(amount of resin composition before immersion−amount of resin composition after immersion) / Amount of resin composition before immersion × 100

[0054] The hydrogel of the present invention is expected to be used in contact lenses and the like because it has excellent water resistance and resistance to yellowing. EXAMPLES

[0055] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. In the examples, "parts" and "%" are by weight unless otherwise specified.

[0056] <Example 1> 50 g of a partially saponified polyvinyl alcohol resin (saponification degree 87.5 mol %) was dispersed in a mixture of 50 g of methacrylic anhydride, 50 g of acetone, and 0.2 g of N,N-dimethylbenzylamine, and the mixture was allowed to react under reflux for 6 hours. After the reaction was completed, the product was filtered off, subjected to Soxhlet extraction with acetone, and then dried to obtain a methacrylic group-modified polyvinyl alcohol resin (I). The obtained methacrylic group-modified polyvinyl alcohol resin (I) 1 1 H-NMR was measured, and the introduction rate (modification amount) of methacryl groups was calculated from the integral ratio, and was found to be 4 mol %.

[0057] The above methacrylic group-modified polyvinyl alcohol-based resin (I) was dissolved in water to prepare a 15% aqueous solution. 2 parts of 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one (Omnirad 2959, manufactured by IGM Resins BV) were added to this aqueous solution per 100 parts of the methacrylic group-modified polyvinyl alcohol-based resin (I) to obtain an aqueous solution of a resin composition. This aqueous solution of the resin composition was transparent, and its viscosity measured with a rotational rheometer was 220 mPa·s at 20°C. In addition, the appearance and viscosity of this aqueous solution did not change even after it was stored at room temperature (23°C) for 6 months.

[0058] [Preparation of hydrogel for measuring yellowness] The aqueous solution of the above resin composition was applied onto a substrate (polyethylene terephthalate film, thickness 100 μm) with an applicator, and 200 mJ / cm 2 The substrate was irradiated with ultraviolet light of 1000 ohms to obtain a coating film on the substrate. The thickness of the coating film was measured to be 30 μm.

[0059] [Preparation of hydrogel for measuring dissolution rate] In addition, the aqueous solution of the resin composition was applied to a substrate (polyethylene terephthalate film, thickness 100 μm) with an applicator so that the liquid layer was 500 μm thick, and immediately after application, 200 mJ / cm 2 A hydrous gel was prepared by irradiating the solution with ultraviolet light.

[0060] <Comparative Example 1> A methacrylic group-modified polyvinyl alcohol resin (II) was obtained in the same manner as in Example 1, except that the amount of methacrylic anhydride was changed to 25 g. The obtained methacrylic group-modified polyvinyl alcohol resin (II) 1 1 H-NMR was measured, and the introduction rate (modification amount) of methacryl groups was calculated from the integral ratio, and was found to be 2 mol %.

[0061] The above-mentioned methacrylic group-modified polyvinyl alcohol-based resin (II) was dissolved in water to prepare a 15% aqueous solution. 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one (Omnirad 2959, manufactured by IGM Resins BV) was added to this aqueous solution in an amount of 10 parts per 100 parts of the methacrylic group-modified polyvinyl alcohol-based resin (II) to obtain an aqueous solution of a resin composition. Using the aqueous solution of the above resin composition, a hydrous gel for measuring yellowness and a hydrous gel for measuring dissolution rate were prepared in the same manner as in Example 1.

[0062] <Comparative Example 2> The above-mentioned methacrylic group-modified polyvinyl alcohol-based resin (II) was dissolved in water to prepare a 15% aqueous solution. To this aqueous solution, 2 parts of 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one (Omnirad 2959, manufactured by IGM Resins BV) were added per 100 parts of the methacrylic group-modified polyvinyl alcohol-based resin (II) to obtain an aqueous solution of a resin composition. Using the aqueous solution of the above resin composition, a hydrous gel for measuring yellowness and a hydrous gel for measuring dissolution rate were prepared in the same manner as in Example 1.

[0063] <Comparative Example 3> The reaction was carried out in the same manner as in Example 1, except that the amount of methacrylic anhydride was changed to 150 g. However, a part of the reaction product dissolved and could not be separated by filtration.

[0064] The following measurements of water content, yellowness and dissolution rate were carried out using the thus obtained hydrous gels for yellowness measurement and hydrous gels for dissolution rate measurement of Example 1 and Comparative Examples 1 and 2. The results are shown in Table 1 below.

[0065] [Moisture content] The weight of the hydrogel for measuring the dissolution rate in each of the examples and comparative examples was measured and designated as the weight before drying (W1).The hydrogel was then dried under reduced pressure (95°C, 100 Pa, 8 hours), and the weight after drying was measured and designated as the weight after drying (W2).The moisture content (%) was calculated from the weight before drying (W1) and the weight after drying (W2) obtained by the following formula. Moisture content (%) = [Weight before drying (W1) - Weight after drying (W2)] / Weight after drying (W2) x 100

[0066] [Measurement of YI value] The yellowness index (YI) of each of the hydrous gels for yellowness measurement of the Examples and Comparative Examples was measured using a spectrophotometer (SE6000, manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS K7373 reflection measurement.

[0067] [Elution rate] The hydrous gels for measuring the elution rate of the examples and comparative examples were dried under reduced pressure (95°C, 100 Pa, 8 hours), and the weight after drying was measured to calculate the amount of the resin composition before immersion. In addition, the hydrous gels for measuring the elution rate were immersed in water at 80°C for 1 hour, then pulled out, dried under reduced pressure, and the weight after drying was measured to calculate the amount of the resin composition after immersion. The amount of elution was calculated from the amount of the resin composition before immersion and the amount of the resin composition after immersion according to the following formula. Amount of elution (wt%)=(amount of resin composition before immersion−amount of resin composition after immersion) / Amount of resin composition before immersion × 100

[0068] [Table 1]

[0069] From the results in Table 1 above, the hydrogel of Example 1 had a yellowness index of 0.33 and an elution rate of 17.3%, and therefore was excellent in yellowing resistance and water resistance. On the other hand, the hydrogel of Comparative Example 1 had a higher yellowness and dissolution rate than the hydrogel of Example 1. Moreover, the hydrogel of Comparative Example 2 had a yellowness equivalent to that of Example 1, but had a higher dissolution rate and poorer water resistance. In Comparative Example 3, the amount of methacrylic anhydride used in the reaction was large, and part of the reaction product was dissolved in the reaction liquid, so that a modified polyvinyl alcohol resin could not be obtained. [Industrial Applicability]

[0070] Since the hydrogel of the present invention has excellent water resistance and resistance to yellowing, it is expected to be used, for example, in contact lenses.

Claims

1. A method for producing a hydrogel made of a resin composition containing a modified polyvinyl alcohol-based resin having an active energy ray-curable functional group, comprising: The hydrous gel is obtained by irradiating a resin composition containing a modified polyvinyl alcohol-based resin having an active energy ray-curable functional group obtained by reacting a polyvinyl alcohol-based resin with a compound having an active energy ray-curable functional group in a solvent in which the polyvinyl alcohol-based resin does not dissolve but the compound having an active energy ray-curable functional group dissolves, with active energy rays; the modified amount of the modified polyvinyl alcohol resin having an active energy ray-curable functional group is 2.5 to 10 mol %, The hydrogel has a yellowness index (YI) of 1.0 or less as measured by reflection measurement according to JIS K7373; The method for producing a hydrogel, wherein the hydrogel has an elution rate of 30% by weight or less after immersion in water at 80° C. for 1 hour.

2. 2. The method for producing a hydrogel according to claim 1, wherein the functional group curable by active energy rays is a (meth)acryloyl group.

3. 3. The method for producing a hydrogel according to claim 1, wherein the hydrogel has a water content of 30% by weight or more.

Citation Information

Patent Citations

  • Acylation of polyvinyl alcohol

    JP1985013803A

  • crosslinked polymer

    JP1998513408A

  • Vinyl alcohol-based polymer

    JP1999199634A

  • Method for decoloring treatment and ophthalmic lens

    JP2001139693A

  • Photo-curing type composition, hydrogel, and molded product of the same

    JP2019044135A