Acrylic rubber, method for producing acrylic rubber, rubber composition and cross-linked rubber
By using a (meth)acrylic acid ester monomer unit with a phenolic anti-aging agent to maintain a specific temperature difference, acrylic rubber is enhanced for reduced coloring and odor, improved processability, and increased elongation, addressing storage and molding challenges.
Patent Information
- Application Number
- JP2020079193
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-04-28
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-04-28
AI Technical Summary
Acrylic rubber experiences issues with coloring and odor generation during storage, and requires improved processability for blending with compounding agents to form various molded products.
Incorporating a (meth)acrylic acid ester monomer unit as the main component with a phenolic anti-aging agent, maintaining a difference between oxidation initiation temperature and glass transition temperature of 250°C or more, and using specific monomer compositions to enhance processability and suppress coloring and odor.
The solution results in acrylic rubber with suppressed coloring and odor generation, excellent processability, and high elongation at break, producing crosslinked rubber products with improved mechanical properties and resistance to heat, oil, and ozone.
Smart Images

Figure 0007567197000001 
Figure 0007567197000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an acrylic rubber, a method for producing an acrylic rubber, a rubber composition and a cross-linked rubber, and more specifically to an acrylic rubber which is suppressed in terms of generation of coloration and odor, has excellent processability and is capable of giving a cross-linked rubber having large elongation at break, and a method for producing the same, as well as a rubber composition and a cross-linked rubber obtained by using such an acrylic rubber. [Background technology]
[0002] Acrylic rubber is a polymer whose main component is units derived from (meth)acrylic acid ester monomers, such as (meth)acrylic acid alkyl ester monomers and (meth)acrylic acid alkoxyalkyl ester monomers. It is generally known as a rubber with excellent heat resistance, oil resistance, and ozone resistance, and is widely used in fields such as the automotive industry.
[0003] Such acrylic rubber is usually produced by emulsion polymerizing a monomer component mainly composed of a (meth)acrylic acid ester monomer, such as a (meth)acrylic acid alkyl ester monomer or a (meth)acrylic acid alkoxyalkyl ester monomer, coagulating the obtained emulsion polymerization liquid by adding a coagulant, and drying the water-containing crumbs obtained by the coagulation (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2018 / 079783 Summary of the Invention [Problem to be solved by the invention]
[0005] On the other hand, acrylic rubbers such as the acrylic rubber disclosed in Patent Document 1 have problems such as discoloration and odor generation during storage. In addition, acrylic rubbers are required to have excellent processability from the viewpoint of being used by blending various compounding agents and molding them into various molded products.
[0006] The present invention has been made in consideration of the above circumstances, and has an object to provide an acrylic rubber which is suppressed in terms of coloration and odor generation, has excellent processability, and is capable of giving a cross-linked rubber product with large breaking elongation, and a method for producing the same, as well as a rubber composition and a cross-linked rubber product obtained using such an acrylic rubber. [Means for solving the problem]
[0007] As a result of intensive research into achieving the above-mentioned object, the present inventors have found that the above-mentioned object can be achieved by making the acrylic rubber containing (meth)acrylic acid ester monomer units as a main component contain a phenol-based antioxidant as an antioxidant and by setting the difference between the oxidation onset temperature and the glass transition temperature (Tg) measured by differential scanning calorimetry to be 250°C or more, thereby completing the present invention.
[0008] That is, according to the present invention, there is provided an acrylic rubber which contains (meth)acrylic acid ester monomer units as a main component, contains a phenol-based antioxidant as an antioxidant, and has a difference between the oxidation onset temperature and the glass transition temperature (Tg) measured by differential scanning calorimetry of 250°C or more. In the acrylic rubber of the present invention, the phenol-based antioxidant is preferably a doubly hindered phenol-based antioxidant. In the acrylic rubber of the present invention, the molecular weight of the phenol-based antioxidant is preferably 470 or less. In the acrylic rubber of the present invention, the difference between the oxidation onset temperature and the glass transition temperature (Tg) is preferably 265 to 370°C. In the acrylic rubber of the present invention, the difference between the oxidation onset temperature and the glass transition temperature (Tg) is preferably 270 to 370°C. The acrylic rubber of the present invention contains at least a (meth)acrylic acid alkoxyalkyl ester monomer unit as the (meth)acrylic acid ester monomer unit, and it is preferable that the content of the (meth)acrylic acid alkoxyalkyl ester monomer unit in all monomer units is 1 to 60% by weight. The acrylic rubber of the present invention preferably has a glass transition temperature (Tg) of 0° C. or lower.
[0009] According to the present invention, there is provided a rubber composition comprising a rubber component containing the above-described acrylic rubber, a filler, and a crosslinking agent. According to the present invention, there is also provided a cross-linked rubber product obtained by cross-linking the above-described rubber composition.
[0010] Further, according to the present invention, there is provided a method for producing any one of the above acrylic rubbers, comprising the steps of: an emulsion polymerization step of emulsion-polymerizing a monomer component mainly composed of a (meth)acrylic acid ester in the presence of a polymerization catalyst to obtain an emulsion polymerization liquid; an antioxidant addition step of adding a phenol-based antioxidant to the emulsion polymerization liquid; A coagulation step of contacting the emulsion polymerization liquid obtained in the antiaging agent addition step with a coagulant to generate water-containing crumbs, The antioxidant addition step comprises: adding the phenol-based antiaging agent to the emulsion polymerization liquid under a temperature condition equal to or higher than the melting point of the phenol-based antiaging agent; or The present invention provides a method for producing an acrylic rubber, comprising the steps of: contacting the phenol-based antiaging agent with an aqueous solution of an emulsifier under a temperature condition equal to or higher than the melting point of the phenol-based antiaging agent to obtain a dispersion; and adding the phenol-based antiaging agent in the form of the dispersion to the emulsion polymerization liquid. Effect of the Invention
[0011] According to the present invention, it is possible to provide an acrylic rubber that is suppressed in terms of coloration and odor generation, has excellent processability, and is capable of giving a cross-linked rubber product with large breaking elongation, and a production method therefor, as well as a rubber composition and a cross-linked rubber product obtained using such an acrylic rubber. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] <Acrylic rubber> The acrylic rubber of the present invention is an acrylic rubber containing a (meth)acrylic acid ester monomer unit as a main component, Contains a phenol-based antioxidant as an antioxidant, The difference between the oxidation onset temperature and the glass transition temperature (Tg) measured by differential scanning calorimetry is in the range of 250°C or more.
[0013] The acrylic rubber of the present invention is a rubber-like polymer containing (meth)acrylic acid ester monomer units (meaning acrylic acid ester monomers and / or methacrylic acid ester monomers; hereinafter, the same applies to methyl (meth)acrylate, etc.) as the main component in the molecule (preferably accounting for 30% by weight or more of all monomer units constituting the acrylic rubber).
[0014] The (meth)acrylic acid ester monomer forming the (meth)acrylic acid ester monomer unit which is the main component of the acrylic rubber of the present invention is not particularly limited, but examples thereof include (meth)acrylic acid alkyl ester monomers and (meth)acrylic acid alkoxyalkyl ester monomers.
[0015] The (meth)acrylic acid alkyl ester monomer is not particularly limited, but is preferably an ester of an alkanol having 1 to 12 carbon atoms and (meth)acrylic acid (a (meth)acrylic acid ester having an alkyl group having 1 to 12 carbon atoms), more preferably an ester of an alkanol having 1 to 8 carbon atoms and (meth)acrylic acid (a (meth)acrylic acid ester having an alkyl group having 1 to 8 carbon atoms), and even more preferably an ester of an alkanol having 2 to 6 carbon atoms and (meth)acrylic acid (a (meth)acrylic acid ester having an alkyl group having 2 to 6 carbon atoms).
[0016] Specific examples of the (meth)acrylic acid alkyl ester monomer include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate. Among these, ethyl (meth)acrylate and n-butyl (meth)acrylate are preferred, and ethyl acrylate and n-butyl acrylate are more preferred. These can be used alone or in combination of two or more.
[0017] The (meth)acrylic acid alkoxyalkyl ester monomer is not particularly limited, but is preferably an ester of an alkoxyalkyl alcohol having 2 to 12 carbon atoms and (meth)acrylic acid (a (meth)acrylic acid ester having an alkoxyalkyl group having 2 to 12 carbon atoms), more preferably an ester of an alkoxyalkyl alcohol having 2 to 8 carbon atoms and (meth)acrylic acid (a (meth)acrylic acid ester having an alkoxyalkyl group having 2 to 8 carbon atoms), and even more preferably an ester of an alkoxyalkyl alcohol having 2 to 6 carbon atoms and (meth)acrylic acid (a (meth)acrylic acid ester having an alkoxyalkyl group having 2 to 6 carbon atoms).
[0018] Specific examples of the (meth)acrylic acid alkoxyalkyl ester monomer include methoxymethyl (meth)acrylate, ethoxymethyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-propoxyethyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, and 4-methoxybutyl (meth)acrylate. Among these, 2-ethoxyethyl (meth)acrylate and 2-methoxyethyl (meth)acrylate are preferred, and 2-ethoxyethyl acrylate and 2-methoxyethyl acrylate are particularly preferred. These can be used alone or in combination of two or more.
[0019] The content of (meth)acrylic acid ester monomer units in all monomer units constituting the acrylic rubber of the present invention is preferably 50% by weight or more, more preferably 60% by weight or more, even more preferably 70 to 99.9% by weight, even more preferably 80 to 99.5% by weight, and particularly preferably 90 to 99% by weight. If the content of (meth)acrylic acid ester monomer units is too low, the weather resistance, heat resistance, and oil resistance of the obtained cross-linked rubber may decrease.
[0020] In addition, the acrylic rubber of the present invention preferably contains at least a (meth)acrylic acid alkoxyalkyl ester monomer unit as a (meth)acrylic acid ester monomer unit, and by containing the (meth)acrylic acid alkoxyalkyl ester monomer unit, the obtained rubber cross-linked product can be excellent in cold resistance and engine oil resistance. In addition, by containing the (meth)acrylic acid alkoxyalkyl ester monomer unit, the effect of suppressing coloration and odor generation can be further improved. The content of the (meth)acrylic acid alkoxyalkyl ester monomer unit in the total monomer units constituting the acrylic rubber of the present invention is preferably 1 to 60% by weight, more preferably 1 to 55% by weight, even more preferably 5 to 40% by weight, and particularly preferably 5 to 30% by weight.
[0021] The acrylic rubber of the present invention may contain a crosslinkable monomer unit, if necessary, in addition to the (meth)acrylic acid ester monomer unit. The crosslinkable monomer forming the crosslinkable monomer unit is not particularly limited, but examples thereof include monomers having a reactive polar functional group, such as α,β-ethylenically unsaturated carboxylic acid monomers, monomers having an epoxy group, and monomers having a halogen atom; diene monomers; and the like. As the crosslinkable monomer, from the viewpoint of crosslinkability, a monomer having a reactive polar functional group is preferable, and among the monomers having a reactive polar functional group, an α,β-ethylenically unsaturated carboxylic acid monomer, a monomer having an epoxy group, and a monomer having a halogen atom are more preferable, an α,β-ethylenically unsaturated carboxylic acid monomer, and a monomer having a halogen atom are even more preferable, and an α,β-ethylenically unsaturated carboxylic acid monomer is particularly preferable.
[0022] The α,β-ethylenically unsaturated carboxylic acid monomer is not particularly limited, and examples thereof include α,β-ethylenically unsaturated monocarboxylic acids, α,β-ethylenically unsaturated dicarboxylic acids, and α,β-ethylenically unsaturated dicarboxylic acid monoesters, etc. By using an α,β-ethylenically unsaturated carboxylic acid monomer, the acrylic rubber can be made into a carboxyl group-containing acrylic rubber having a carboxyl group as a crosslinking point, and this can further improve the compression set resistance when made into a rubber crosslinked product.
[0023] The α,β-ethylenically unsaturated monocarboxylic acid is not particularly limited, but is preferably an α,β-ethylenically unsaturated monocarboxylic acid having 3 to 12 carbon atoms, and specific examples thereof include acrylic acid, methacrylic acid, α-ethylacrylic acid, crotonic acid, and cinnamic acid. The α,β-ethylenically unsaturated dicarboxylic acid is not particularly limited, but is preferably an α,β-ethylenically unsaturated dicarboxylic acid having 4 to 12 carbon atoms, and specific examples thereof include butenedioic acids such as fumaric acid and maleic acid; itaconic acid; citraconic acid; and chloromaleic acid. The α,β-ethylenically unsaturated dicarboxylic acid monoester is not particularly limited, but is preferably a monoester of an α,β-ethylenically unsaturated dicarboxylic acid having 4 to 12 carbon atoms and an alkanol having 1 to 12 carbon atoms, more preferably a monoester of an α,β-ethylenically unsaturated dicarboxylic acid having 4 to 6 carbon atoms and an alkanol having 2 to 8 carbon atoms, and even more preferably a monoester of butenedioic acid having 4 carbon atoms and an alkanol having 2 to 6 carbon atoms. Specific examples of the α,β-ethylenically unsaturated dicarboxylic acid monoester include butenedioic acid mono-chain alkyl esters such as monomethyl fumarate, monoethyl fumarate, mono-n-butyl fumarate, monomethyl maleate, monoethyl maleate, and mono-n-butyl maleate; butenedioic acid monoesters having an alicyclic structure such as monocyclopentyl fumarate, monocyclohexyl fumarate, monocyclohexenyl fumarate, monocyclopentyl maleate, monocyclohexyl maleate, and monocyclohexenyl maleate; and itaconic acid monoesters such as monomethyl itaconate, monoethyl itaconate, mono-n-butyl itaconate, and monocyclohexyl itaconate.
[0024] Among these, α,β-ethylenically unsaturated dicarboxylic acid monoesters are preferred, butenedioic acid monochain alkyl esters or butenedioic acid monoesters having an alicyclic structure are more preferred, mono-n-butyl fumarate, mono-n-butyl maleate, monocyclohexyl fumarate, and monocyclohexyl maleate are even more preferred, and mono-n-butyl fumarate is particularly preferred. These α,β-ethylenically unsaturated carboxylic acid monomers can be used alone or in combination of two or more. Among the above monomers, dicarboxylic acids also include those that exist as anhydrides.
[0025] The monomer having an epoxy group is not particularly limited, but examples thereof include epoxy group-containing (meth)acrylic acid esters such as glycidyl (meth)acrylate; epoxy group-containing ethers such as allyl glycidyl ether and vinyl glycidyl ether; and the like.
[0026] The monomer having a halogen atom is not particularly limited, and examples thereof include unsaturated alcohol esters of halogen-containing saturated carboxylic acids, (meth)acrylic acid haloalkyl esters, (meth)acrylic acid haloacyloxyalkyl esters, (meth)acrylic acid (haloacetylcarbamoyloxy)alkyl esters, halogen-containing unsaturated ethers, halogen-containing unsaturated ketones, halomethyl group-containing aromatic vinyl compounds, halogen-containing unsaturated amides, and haloacetyl group-containing unsaturated monomers. Note that the monomer having a halogen atom is preferably one that contains a chlorine atom as the halogen atom.
[0027] Specific examples of unsaturated alcohol esters of halogen-containing saturated carboxylic acids include vinyl chloroacetate, vinyl 2-chloropropionate, and allyl chloroacetate. Specific examples of (meth)acrylic acid haloalkyl esters include chloromethyl (meth)acrylate, 1-chloroethyl (meth)acrylate, 2-chloroethyl (meth)acrylate, 1,2-dichloroethyl (meth)acrylate, 2-chloropropyl (meth)acrylate, 3-chloropropyl (meth)acrylate, and 2,3-dichloropropyl (meth)acrylate. Specific examples of (meth)acrylic acid haloacyloxyalkyl esters include 2-(chloroacetoxy)ethyl (meth)acrylate, 2-(chloroacetoxy)propyl (meth)acrylate, 3-(chloroacetoxy)propyl (meth)acrylate, and 3-(hydroxychloroacetoxy)propyl (meth)acrylate. Specific examples of (meth)acrylic acid (haloacetylcarbamoyloxy)alkyl esters include 2-(chloroacetylcarbamoyloxy)ethyl (meth)acrylate and 3-(chloroacetylcarbamoyloxy)propyl (meth)acrylate.
[0028] Specific examples of halogen-containing unsaturated ethers include chloromethyl vinyl ether, 2-chloroethyl vinyl ether, 3-chloropropyl vinyl ether, 2-chloroethyl allyl ether, and 3-chloropropyl allyl ether. Specific examples of halogen-containing unsaturated ketones include 2-chloroethyl vinyl ketone, 3-chloropropyl vinyl ketone, and 2-chloroethyl allyl ketone. Specific examples of the halomethyl group-containing aromatic vinyl compound include p-chloromethylstyrene, m-chloromethylstyrene, o-chloromethylstyrene, and p-chloromethyl-α-methylstyrene.
[0029] A specific example of the halogen-containing unsaturated amide is N-chloromethyl(meth)acrylamide. Specific examples of the haloacetyl group-containing unsaturated monomer include 3-(hydroxychloroacetoxy)propyl allyl ether, p-vinylbenzyl chloroacetic acid ester, and the like.
[0030] The diene monomer includes a conjugated diene monomer and a non-conjugated diene monomer. Specific examples of conjugated diene monomers include 1,3-butadiene, isoprene, and piperylene. Specific examples of non-conjugated diene monomers include ethylidene norbornene, dicyclopentadiene, dicyclopentadienyl (meth)acrylate, and 2-dicyclopentadienylethyl (meth)acrylate.
[0031] The content of the crosslinkable monomer units in the total monomer units constituting the acrylic rubber of the present invention is preferably 0.01% by weight or more, more preferably 0.01 to 20% by weight, even more preferably 0.1 to 10% by weight, even more preferably 0.5 to 5% by weight, and particularly preferably 1 to 3% by weight. By setting the content of the crosslinkable monomer units within the above range, it is possible to improve the mechanical properties and heat resistance of the obtained crosslinked rubber product, while more appropriately increasing the compression set resistance.
[0032] In addition to the (meth)acrylic acid ester monomer units and the crosslinkable monomer units used as necessary, the acrylic rubber of the present invention may have units of other monomers copolymerizable therewith. Such copolymerizable other monomers are not particularly limited, but may include aromatic vinyl monomers, α,β-ethylenically unsaturated nitrile monomers, acrylamide monomers, α,β-ethylenically unsaturated dicarboxylic acid diester monomers, other olefin monomers, and the like.
[0033] Examples of the aromatic vinyl monomer include styrene, α-methylstyrene, and divinylbenzene.
[0034] Examples of the α,β-ethylenically unsaturated nitrile monomer include acrylonitrile and methacrylonitrile. Examples of the acrylamide monomer include acrylamide and methacrylamide. Examples of the α,β-ethylenically unsaturated dicarboxylic acid diester monomer include dialkyl maleates such as dimethyl maleate and di-n-butyl maleate, in which the alkyl group has 1 to 18 carbon atoms; dialkyl fumarate esters such as dimethyl fumarate and di-n-butyl fumarate, in which the alkyl group has 1 to 18 carbon atoms; dicycloalkyl maleates such as dicyclopentyl maleate and dicyclohexyl maleate, in which the cycloalkyl group has 4 to 16 carbon atoms; dicycloalkyl fumarate esters such as dicyclopentyl fumarate and dicyclohexyl fumarate, in which the cycloalkyl group has 4 to 16 carbon atoms; dialkyl itaconate esters such as dimethyl itaconate and di-n-butyl itaconate, in which the alkyl group has 1 to 18 carbon atoms; and dicycloalkyl itaconate esters such as dicyclohexyl itaconate, in which the cycloalkyl group has 4 to 16 carbon atoms. Other olefin monomers include ethylene, propylene, vinyl chloride, vinylidene chloride, vinyl acetate, ethyl vinyl ether, and butyl vinyl ether.
[0035] Among these copolymerizable other monomers, styrene, acrylonitrile, methacrylonitrile, ethylene and vinyl acetate are preferred, and acrylonitrile, methacrylonitrile and ethylene are more preferred.
[0036] The copolymerizable other monomers can be used alone or in combination of two or more. The content of the units of these copolymerizable other monomers in the monomer units constituting the acrylic rubber of the present invention is preferably 49.9% by weight or less, more preferably 29.9% by weight or less, even more preferably 15% by weight or less, even more preferably 9% by weight or less, and particularly preferably 4.5% by weight or less.
[0037] In the case where the acrylic rubber of the present invention contains units of other copolymerizable monomers, the content of the units may be within the above range, but in particular, in the case where the acrylic rubber of the present invention contains ethylene units, the content of the ethylene units in the monomer units constituting the acrylic rubber of the present invention is preferably 9% by weight or less, more preferably 4.5% by weight or less. Similarly, in the case where the acrylic rubber of the present invention contains acrylonitrile units or methacrylonitrile units, the total content of the acrylonitrile units and methacrylonitrile units is preferably 9% by weight or less, more preferably 4.5% by weight or less.
[0038] The acrylic rubber of the present invention contains a phenol-based antioxidant as an antioxidant. The phenol-based antioxidant is not particularly limited as long as it is a compound having a phenol structure (i.e., a structure having a benzene ring and an OH group bonded to the benzene ring). Examples of the phenol-based antioxidant include a doubly hindered phenol-based antioxidant, a semi-hindered phenol-based antioxidant, a less hindered phenol-based antioxidant, and a phenol-based antioxidant without a hindered group.
[0039] The double hindered phenol-based antioxidant is a phenol-based compound in which both the 2-position and the 6-position (i.e., two ortho-positions) of the OH group (phenolic hydroxyl group) constituting the phenol structure are hindered groups. The hindered group may be any bulky group, and is not particularly limited, but examples thereof include substituents having 4 or more carbon atoms. Specific examples of the hindered group include tertiary alkyl groups such as t-butyl, t-pentyl, and t-hexyl groups; secondary alkyl groups such as sec-butyl and sec-pentyl groups; branched primary alkyl groups such as i-butyl and i-pentyl groups; cycloalkyl groups such as cyclohexyl and cyclopentyl groups; and alkyl groups in which alkylthio groups are substituted so that the total number of carbon atoms is 4 or more, such as octylthio and octylthiomethyl groups.
[0040] Specific examples of the doubly hindered phenol-based antioxidant include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (e.g., trade name "Irganox 1010" manufactured by BASF), 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate (e.g., trade name "Irganox 3114" manufactured by BASF), 2,4,6-tris(4-hydroxy-3,5-di-tert-butylbenzyl)mesitylene (e.g., trade name "Irganox 1330" manufactured by BASF), 6-(4-hydroxy-3,5-di-tert-butylanilino)-2,4-bis(octylthio)-1,3,5-triazine (e.g., trade name "Irganox 565, manufactured by BASF), 2,2'-thiodiethyl bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (e.g., trade name "Irganox 1035", manufactured by BASF), 1,2-bis[3-(4-hydroxy-3,5-di-tert-butylphenyl)propionyl]hydrazine (trade name "Irganox MD1024", manufactured by BASF), 3-(3,5-di-tert-butyl-4-hydroxyphenyl)octyl propionate (trade name "Irganox Examples of such esters include N,N'-hexamethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propanamide] (trade name "Irganox 1098", manufactured by BASF), 1,6-hexanediol bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (trade name "Irganox 259", manufactured by BASF), and 3-(3,5-di-tert-butyl-4-hydroxyphenyl)stearyl propionate (trade name "Irganox 1076", manufactured by BASF).
[0041] The semi-hindered phenol-based antioxidant is a phenol-based compound in which either one of the 2-position and 6-position of the OH group (phenolic hydroxyl group) constituting the phenol structure is a hindered group, and the other is an alkyl group having 3 or less carbon atoms, such as a methyl group (preferably a methyl group).
[0042] Specific examples of semi-hindered phenol-based antioxidants include 4,6-bis(octylthiomethyl)-o-cresol (trade name "Irganox 1520L", manufactured by BASF), 1,3,5-tris[[4-(1,1-dimethylethyl)-3-hydroxy-2,6-dimethylphenyl]methyl]-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (trade name "Irganox 1790", manufactured by BASF), 3,9-bis[2-{3-(3-tertiarybutyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5,5 ]undecane (for example, trade name "ADK STAB AO-80" manufactured by ADEKA Corporation), ethylene bis(oxyethylene) bis[3-(5-tert-butyl-hydroxy-m-tolyl)propionate] (for example, trade name "Irganox 245" manufactured by BASF Corporation), triethylene glycol bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate] (for example, trade name "ADK STAB AO-70" manufactured by ADEKA Corporation).
[0043] The less hindered phenol-based antioxidant is a phenol-based compound in which either one of the 2-position and 6-position of the OH group (phenolic hydroxyl group) constituting the phenol structure is a hindered group, and the other is a hydrogen atom.
[0044] Specific examples of the unhindered phenol-based antioxidant include 1,1,3-tris-(2-methyl-4-hydroxy-5-tert-butylphenyl)butane (for example, trade name "ADK STAB AO-30", manufactured by ADEKA Corporation), 4,4'-butylidenebis(6-t-butyl-3-methylphenol) (for example, trade name "ADK STAB AO-40", manufactured by ADEKA Corporation), and 4,4'-thiobis(6-t-butyl-3-methylphenol) (for example, trade name "Sumilizer WX-R", manufactured by Sumitomo Chemical Co., Ltd.).
[0045] The phenol-based antiaging agent can be used alone or in combination of two or more. Among the phenol-based antiaging agents, a doubly hindered phenol-based antiaging agent and a semi-hindered phenol-based antiaging agent are preferred, and from the viewpoint of being able to further enhance the effect of suppressing the generation of coloring and odor and the effect of improving processability, a doubly hindered phenol-based antiaging agent is preferred.
[0046] Moreover, the phenol-based antiaging agent preferably has a molecular weight of 470 or less, more preferably has a molecular weight of 100 to 450, and even more preferably has a molecular weight of 150 to 400. By using a phenol-based antiaging agent having a molecular weight of 500 or less, it is possible to further enhance the effect of suppressing the generation of coloration and odor, and the effect of improving processability.
[0047] The content of the phenol-based antiaging agent is preferably 0.1 to 5 parts by weight, more preferably 0.2 to 3.0 parts by weight, and further preferably 0.3 to 2.0 parts by weight, based on 100 parts by weight of the acrylic rubber component. By setting the content of the phenol-based antiaging agent within the above range, it is possible to further enhance the effect of suppressing the generation of coloring and odor, and the effect of improving processability.
[0048] Since the acrylic rubber of the present invention contains the above-mentioned phenol-based antioxidant, it can also be said to be an acrylic rubber composition containing an acrylic rubber component and a phenol-based antioxidant. The content of the acrylic rubber component in the acrylic rubber of the present invention is preferably 95% by weight or more.
[0049] In addition, the acrylic rubber of the present invention has a difference between the oxidation onset temperature measured by differential thermal analysis and the glass transition temperature (Tg) of 250°C or more. The oxidation onset temperature can be measured, for example, by measuring the acrylic rubber using a simultaneous differential thermal and thermogravimetric analyzer, and reading the peak value corresponding to the oxidation onset temperature from the DTA curve obtained by the measurement. In addition, the glass transition temperature (Tg) can be measured, for example, by measuring the acrylic rubber using a differential scanning calorimeter at a temperature rise of 10°C / min from -80°C to 50°C, and reading the peak value of the differential curve. The difference between the oxidation onset temperature and the glass transition temperature (Tg) is 250°C or more, preferably 265 to 370°C, and more preferably 270 to 350°C. If the difference between the oxidation onset temperature and the glass transition temperature (Tg) is too small, the acrylic rubber is likely to become discolored and emit an odor, and the processability is deteriorated, and further, the resulting rubber cross-linked product has poor breaking elongation. In the present invention, the method of controlling the difference between the oxidation onset temperature and the glass transition temperature (Tg) of the acrylic rubber within the above range is not particularly limited, but includes a method of adjusting the type and amount of the monomer unit constituting the acrylic rubber, and a method of adding a phenolic antioxidant to an emulsion polymerization liquid of an acrylic rubber obtained by emulsion polymerization of a monomer component mainly composed of a (meth)acrylic acid ester when producing the acrylic rubber in such a manner that the phenolic antioxidant is uniformly dispersed. Examples of the method of adding the phenolic antioxidant in such a manner that the phenolic antioxidant is uniformly dispersed include a method of contacting the phenolic antioxidant with an aqueous solution of an emulsifier under a temperature condition equal to or higher than the melting point of the phenolic antioxidant to obtain a dispersion, and adding the phenolic antioxidant in the dispersion state to the emulsion polymerization liquid of the acrylic rubber, and a method of adding the phenolic antioxidant to the emulsion polymerization liquid of the acrylic rubber under a temperature condition equal to or higher than the melting point of the phenolic antioxidant.For example, the more carbon atoms of a (meth)acrylic acid ester monomer is used as a monomer unit constituting the acrylic rubber, the lower the glass transition temperature (Tg) tends to be, and the more the amount of (meth)acrylic acid alkoxyalkyl ester monomer units in the monomer units constituting the acrylic rubber is increased, the lower the glass transition temperature (Tg) tends to be. Furthermore, by adding a phenol-based antiaging agent to the emulsion polymerization liquid of the acrylic rubber in such a manner that the phenol-based antiaging agent is uniformly dispersed, the oxidation onset temperature can be made higher.
[0050] The oxidation onset temperature of the acrylic rubber of the present invention may be within the above-mentioned range in relation to the glass transition temperature (Tg); however, in order to make the effects of the present invention more pronounced, the oxidation onset temperature is preferably 230°C or higher, more preferably 245°C or higher, even more preferably 245 to 350°C, and particularly preferably 245 to 300°C.
[0051] The glass transition temperature (Tg) of the acrylic rubber of the present invention may be within the above range in relation to the oxidation onset temperature, but is preferably 0° C. or lower, more preferably −10° C. or lower, even more preferably −12° C. or lower, and particularly preferably −15° C. or lower. The lower limit of the glass transition temperature (Tg) is not particularly limited, but is preferably −80° C. or higher, preferably −60° C. or higher, and more preferably −40° C. or higher. By setting the glass transition temperature (Tg) within the above range, the acrylic rubber can have a better balance of heat resistance and cold resistance.
[0052] The acrylic rubber of the present invention has a Mooney viscosity (ML1+4, 100°C) in the range of 10 to 150, preferably in the range of 20 to 100, and more preferably in the range of 25 to 70. By setting the Mooney viscosity in the above range, it is possible to achieve a high level of balance between the processability and strength properties of the acrylic rubber.
[0053] Furthermore, the pH of the acrylic rubber of the present invention is not particularly limited, but is preferably 6 or less, more preferably 2 to 6, even more preferably 2.5 to 5.5, and particularly preferably 3 to 5. By setting the pH within the above range, the storage stability of the acrylic rubber can be further improved.
[0054] The weight average molecular weight (Mw) of the acrylic rubber of the present invention is not particularly limited, but from the viewpoint of improving mechanical strength and processability, it is preferably 800,000 or more, more preferably 800,000 to 2,600,000, even more preferably 900,000 to 2,300,000, and particularly preferably 1,000,000 to 2,000,000. The molecular weight distribution of the acrylic rubber is not particularly limited, but the value of Mw / Mn is preferably 1.50 to 10.0, more preferably 1.70 to 8.00, and even more preferably 2.00 to 6.00, and the value of Mz / Mw is preferably 1.30 to 3.00, more preferably 1.45 to 2.70, and even more preferably 1.60 to 2.50. The weight average molecular weight and molecular weight distribution of the acrylic rubber can be determined as the absolute molecular weight and absolute molecular weight distribution, for example, by a GPC-MALS method using a GPC (Gel Permeation Chromatography) device incorporating a multi-angle laser light scattering photometer (MALS).
[0055] <Acrylic rubber manufacturing method> The method for producing the acrylic rubber of the present invention is not particularly limited and any method may be adopted, but for example, the following method is preferable. an emulsion polymerization step of emulsion-polymerizing a monomer component mainly composed of a (meth)acrylic acid ester in the presence of a polymerization catalyst to obtain an emulsion polymerization liquid; an antioxidant addition step of adding a phenol-based antioxidant to the emulsion polymerization liquid; A coagulation step of contacting the emulsion polymerization liquid obtained in the antiaging agent addition step with a coagulant to generate water-containing crumbs, The antioxidant addition step comprises: adding the phenol-based antiaging agent to the emulsion polymerization liquid under a temperature condition equal to or higher than the melting point of the phenol-based antiaging agent; or A preferred method for producing an acrylic rubber includes a step of contacting the phenol-based antiaging agent with an aqueous solution of an emulsifier under a temperature condition equal to or higher than the melting point of the phenol-based antiaging agent to obtain a dispersion, and then adding the phenol-based antiaging agent in the state of the dispersion to the emulsion polymerization liquid.
[0056] (Emulsion polymerization process) The emulsion polymerization step in the production method of the present invention is a step of obtaining an emulsion polymerization liquid by emulsion polymerizing a monomer component mainly composed of a (meth)acrylic acid ester in the presence of a polymerization catalyst.
[0057] The monomer components used in the emulsion polymerization may include the above-mentioned monomers, and the preferred monomers are also as described above. The amount of each monomer used may be appropriately selected so as to be within the above-mentioned composition range.
[0058] As the emulsion polymerization method in the emulsion polymerization step, a conventional method may be used, and an emulsifier, a polymerization initiator, a polymerization terminator, etc. may be used in accordance with a conventional method.
[0059] The emulsifier is not particularly limited, but a phosphate ester salt can be suitably used. As the phosphate ester salt, a compound represented by the following general formula (1) can be preferably used. [ka] (In the above general formula (1), R 1 represents a linear or branched alkyl group having 4 to 20 carbon atoms, an alkylphenyl group, or an unsaturated alkyl group having 4 to 20 carbon atoms; R 2 represents a linear or branched alkylene group having 2 or 3 carbon atoms, M represents an alkali metal, and m is an integer of 1 to 20. When m is 2 or more, R 2 may have multiple different groups as, n is 1 or 2, p is 1 or 2, and n+p is 3.
[0060] In the above general formula (1), R 1 R represents a linear or branched alkyl group having 4 to 20 carbon atoms, an alkylphenyl group, or an unsaturated alkyl group having 4 to 20 carbon atoms. 1 R preferably has 4 or more and 18 or less carbon atoms, more preferably has 5 or more and 16 or less carbon atoms, and even more preferably has 6 or more and 14 or less carbon atoms. 1 Specific examples include an n-octyl group, an n-decyl group, an n-dodecyl group, an n-tridecyl group, an n-tetradecyl group, an isooctyl group, an isotridecyl group, an n-octadecyl group, and a nonylphenyl group.
[0061] In the above general formula (1), R 2 R represents a linear or branched alkylene group having 2 or 3 carbon atoms. 2 Specific examples of the alkyl group include an ethylene group and a propylene group, and among these, an ethylene group is more preferred.
[0062] In the above general formula (1), M represents an alkali metal, and specific examples of M include sodium, potassium, lithium, rubidium, cesium, etc. Among these, sodium and potassium are preferable as M.
[0063] In the above general formula (1), m is an integer of 1 to 20, preferably an integer of 2 or more and 15 or less, more preferably an integer of 2 or more and 13 or less, and even more preferably an integer of 2 or more and 11 or less. When m is 2 or more, R 2 For example, R 2 The alkyl group may have both an ethylene group and a propylene group.
[0064] In the above general formula (1), n is 1 or 2, and preferably 1. Furthermore, p is 1 or 2, and preferably 2. Note that n+p is 3.
[0065] These phosphate salts can be used alone, or in combination of two or more different n numbers, or in combination of two or more different ester types. Among these combinations, a mixture of phosphate salts with different n numbers is preferred, and a mixture of phosphate salts with the same ester type but different n numbers is more preferred. The mixing ratio in the mixture of phosphate salts with different n numbers is not particularly limited. The amount of the phosphate salt used is preferably 0.01 to 10 parts by weight, more preferably 0.1 to 5 parts by weight, and even more preferably 1 to 3 parts by weight, based on 100 parts by weight of the monomer component used in the polymerization.
[0066] Examples of the phosphate salts represented by the above general formula (1) include octyloxydi(oxyethylene)phosphate, dodecyloxydi(oxyethylene)phosphate, tridecyloxytri(oxyethylene)phosphate, hexyloxytetra(oxyethylene)phosphate, heptylhexaoxytetra(oxyethylene)phosphate, octyloxytetra(oxyethylene)phosphate, nonyloxytetra(oxyethylene)phosphate, decyloxytetra(oxyethylene)phosphate, decyloxytetra(oxyethylene)phosphate, octadecyloxytetra(oxyethylene)phosphate, oct ... Examples of the alkali metal salts of oxytetra(oxyethylene)phosphate, nonylphenyloxytetra(oxyethylene)phosphate, tridecyloxytetra(oxyethylene)phosphate, octyloxyhexa(oxyethylene)phosphate, decyloxyhexa(oxyethylene)phosphate, tridecyloxyhexa(oxyethylene)phosphate, nonylphenyloxyhexa(oxyethylene)phosphate, octadecyloxyhepta(oxyethylene)phosphate, and tridecyloxydeca(oxyethylene)phosphate (e.g., Na salt, K salt, etc.). The structure of the hydrophobic group of these phosphate salts is not limited, and may be either a straight chain or a branched chain, or may contain an unsaturated structure.
[0067] In the present invention, an emulsifier other than the phosphoric acid ester salt can be used together with the phosphoric acid ester salt or instead of the phosphoric acid ester salt. Examples of the emulsifier other than the phosphoric acid ester salt include anionic emulsifiers other than the phosphoric acid ester salt, cationic emulsifiers, and nonionic emulsifiers. Among these, anionic emulsifiers other than the phosphoric acid ester salt and nonionic emulsifiers are preferred, and it is preferred to use an anionic emulsifier other than the phosphoric acid ester salt in combination with a nonionic emulsifier.
[0068] Examples of anionic emulsifiers other than phosphate ester salts include, but are not limited to, salts of fatty acids such as myristic acid, palmitic acid, oleic acid, and linolenic acid; alkylbenzenesulfonates such as sodium dodecylbenzenesulfonate; sulfate salts such as sodium lauryl sulfate; and alkylsulfosuccinates.
[0069] The cationic emulsifier is not particularly limited, but examples thereof include alkyltrimethylammonium chloride, dialkylammonium chloride, and benzylammonium chloride.
[0070] The nonionic emulsifier is not particularly limited, but examples thereof include polyoxyalkylene fatty acid esters such as polyoxyethylene stearic acid ester, polyoxyalkylene alkyl ethers such as polyoxyethylene dodecyl ether, polyoxyalkylene alkylphenol ethers such as polyoxyethylene nonylphenyl ether, polyoxyethylene sorbitan alkyl esters, etc. Among these, polyoxyalkylene alkyl ethers and polyoxyalkylene alkylphenol ethers are preferred, and polyoxyethylene alkyl ethers and polyoxyethylene alkylphenol ethers are more preferred.
[0071] The emulsifiers other than the phosphate ester salts may be used alone or in combination of two or more.
[0072] In the production method of the present invention, the amount of emulsifier used is preferably 0.01 to 10 parts by weight, more preferably 0.1 to 5 parts by weight, and even more preferably 1 to 3 parts by weight, based on 100 parts by weight of the monomer component used in polymerization. In addition, when an anionic emulsifier other than a phosphoric acid ester salt is used in combination with a nonionic emulsifier, the amount of the nonionic emulsifier used is more than 0 parts by weight and 4 parts by weight or less, preferably 0.1 to 3 parts by weight, more preferably 0.5 to 2 parts by weight, and even more preferably 0.7 to 1.7 parts by weight, based on 100 parts by weight of the monomer used in polymerization, and the amount of the anionic emulsifier other than a phosphoric acid ester salt used is more than 0 parts by weight and 4 parts by weight or less, preferably 0.1 to 3 parts by weight, more preferably 0.5 to 2 parts by weight, and even more preferably 0.35 to 0.75 parts by weight, based on 100 parts by weight of the monomer used in polymerization. When an anionic emulsifier other than a phosphate ester salt is used in combination with a nonionic emulsifier, the weight ratio of the emulsifier to the anionic emulsifier other than a phosphate ester salt is preferably from 1 / 99 to 99 / 1, more preferably from 10 / 90 to 80 / 20, even more preferably from 25 / 75 to 75 / 25, even more preferably from 50 / 50 to 75 / 25, and particularly preferably from 65 / 35 to 75 / 25.
[0073] In the emulsion polymerization step, it is preferable to emulsify the monomer component mainly composed of (meth)acrylic acid ester with water and an emulsifier in advance to obtain an emulsion, and then emulsion-polymerize the obtained emulsion in the presence of a polymerization catalyst. In this case, the method of emulsifying the monomer component mainly composed of (meth)acrylic acid ester with water and an emulsifier is not particularly limited, but a method of mixing the monomer component, water, and an emulsifier is preferable, and a method of stirring the monomer component, water, and an emulsifier with a stirrer such as a homogenizer or a disk turbine is more preferable.
[0074] The amount of water used when emulsifying the monomer components is preferably 5 to 500 parts by weight, more preferably 10 to 300 parts by weight, and further preferably 20 to 200 parts by weight, based on 100 parts by weight of the monomer components used in the polymerization.
[0075] The polymerization catalyst is not particularly limited, and any catalyst that is commonly used in emulsion polymerization can be used without any restrictions. For example, a redox catalyst consisting of a radical generator and a reducing agent can be used as the polymerization catalyst.
[0076] Examples of the radical generator include peroxides and azo compounds, and among these, peroxides are preferred. As the peroxide, either an inorganic peroxide or an organic peroxide may be used.
[0077] Examples of inorganic peroxides include sodium persulfate, potassium persulfate, hydrogen peroxide, ammonium persulfate, etc. Among these, potassium persulfate, hydrogen peroxide, and ammonium persulfate are preferred, and potassium persulfate is particularly preferred.
[0078] Examples of organic peroxides include 2,2-di(4,4-di(t-butylperoxy)cyclohexyl)propane, 1-di(t-hexylperoxy)cyclohexane, 1,1-di(t-butylperoxy)cyclohexane, 4,4-di(t-butylperoxy)n-butyl valerate, 2,2-di(t-butylperoxy)butane, t-butyl hydroperoxide, cumene hydroperoxide, diisopropylbenzene hydroperoxide, paramenthane hydroperoxide, benzoyl peroxide, and 1,1,3,3-tetramethylphenylacetate. tetraethylbutyl hydroperoxide, t-butylcumyl peroxide, di-t-butyl peroxide, di-t-hexyl peroxide, di(2-t-butylperoxyisopropyl)benzene, dicumyl peroxide, diisobutyryl peroxide, di(3,5,5-trimethylhexanoyl) peroxide, dilauroyl peroxide, disuccinic acid peroxide, dibenzoyl peroxide, di(3-methylbenzoyl) peroxide, benzoyl(3-methylbenzoyl) peroxide, diisobutyryl peroxide dika peroxydicarbonate, di-n-propyl peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, di-sec-butyl peroxydicarbonate, 1,1,3,3-tetramethylbutyl peroxyneodecanate, t-hexyl peroxypivalate, t-butyl peroxyneodecanate, t-hexyl peroxypivalate, t-butyl peroxypivalate, 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanate, t-hexyl Examples of peroxyalkylene oxides include tert-butylperoxy-2-ethylhexanate, t-butylperoxy-3,5,5-trimethylhexanate, t-hexylperoxyisopropyl monocarbonate, t-butylperoxyisopropyl monocarbonate, t-butylperoxy-2-ethylhexyl monocarbonate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-butylperoxyacetate, t-hexylperoxybenzoate, t-butylperoxybenzoate, and 2,5-dimethyl-2,5-di(t-butylperoxy)hexane.Among these, diisopropylbenzene hydroperoxide, cumene hydroperoxide, paramenthane hydroperoxide, and benzoyl peroxide are preferable.
[0079] Examples of the azo compound include azobisisobutyronitrile, 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis[2-(2-imidazolin-2-yl)propane, 2,2'-azobis(propane-2-carboxamidine), 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropanamide], 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane}, 2,2'-azobis(1-imino-1-pyrrolidino-2-methylpropane), and 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propanamide}.
[0080] These radical generators can be used alone or in combination of two or more. The amount of the radical generator used is preferably 0.0001 to 5 parts by weight, more preferably 0.0005 to 1 part by weight, and further preferably 0.001 to 0.5 part by weight, based on 100 parts by weight of the monomer components used in the polymerization.
[0081] The reducing agent used in combination with the radical generator can be any reducing agent that can be used as a redox catalyst for emulsion polymerization without any restrictions. As the reducing agent, it is preferable to use at least two reducing agents, and among them, a combination of a metal ion compound in a reduced state and another reducing agent is preferable.
[0082] The reduced metal ion compound is not particularly limited, but examples thereof include ferrous sulfate, sodium iron hexamethylenediaminetetraacetate, cuprous naphthenate, etc. Among these, ferrous sulfate is preferred.
[0083] The reduced metal ion compound may be used alone or in combination of two or more. The amount of the reduced metal ion compound used is preferably 0.000001 to 0.01 parts by weight, more preferably 0.00001 to 0.001 parts by weight, and even more preferably 0.00005 to 0.0005 parts by weight, based on 100 parts by weight of the monomer component used in the polymerization.
[0084] Examples of reducing agents other than metal ion compounds in a reduced state include, but are not limited to, ascorbic acid or a salt thereof such as ascorbic acid, sodium ascorbate, or potassium ascorbate; erythorbic acid or a salt thereof such as erythorbic acid, sodium erythorbate, or potassium erythorbate; sulfinates such as sodium hydroxymethanesulfinate (sodium formaldehyde sulfoxylate); sulfites such as sodium sulfite, potassium sulfite, sodium hydrogensulfite, aldehyde sodium hydrogensulfite, or potassium hydrogensulfite; pyrosulfites such as sodium pyrosulfite, potassium pyrosulfite, sodium hydrogensulfite, or potassium pyrosulfite; thiosulfates such as sodium thiosulfate or potassium thiosulfate; phosphorous acid or a salt thereof such as sodium phosphite, potassium phosphite, sodium hydrogen phosphite, or potassium hydrogen phosphite; pyrophosphorous acid or a salt thereof such as pyrophosphorous acid, sodium pyrophosphite, potassium pyrophosphite, sodium hydrogen pyrophosphite, or potassium hydrogen pyrophosphite; Among these, ascorbic acid or a salt thereof, and sodium hydroxymethanesulfinate (sodium formaldehyde sulfoxylate) are preferred, with ascorbic acid or a salt thereof being particularly preferred.
[0085] The reducing agent other than the reduced metal ion compound may be used alone or in combination of two or more. The amount of the reducing agent other than the reduced metal ion compound to be used is preferably 0.001 to 1 part by weight, more preferably 0.005 to 0.5 parts by weight, and even more preferably 0.01 to 0.1 parts by weight, based on 100 parts by weight of the monomer component used in the polymerization.
[0086] A preferred combination of a metal ion compound in a reduced state and a reducing agent other than a metal ion compound in a reduced state is a combination of ferrous sulfate and ascorbic acid or a salt thereof and / or sodium hydroxymethanesulfinate (sodium formaldehyde sulfoxylate), with a more preferred combination being ferrous sulfate and an ascorbate salt and / or sodium hydroxymethanesulfinate (sodium formaldehyde sulfoxylate), and a particularly preferred combination being ferrous sulfate and an ascorbate salt. In this case, the amount of ferrous sulfate used is preferably 0.000001 to 0.01 parts by weight, more preferably 0.00001 to 0.001 parts by weight, and even more preferably 0.00005 to 0.0005 parts by weight, relative to 100 parts by weight of the monomer components used in the polymerization, and the amount of ascorbic acid or a salt thereof and / or sodium hydroxymethanesulfinate (sodium formaldehyde sulfoxylate) used is preferably 0.001 to 1 part by weight, more preferably 0.005 to 0.5 parts by weight, and even more preferably 0.01 to 0.1 part by weight, relative to 100 parts by weight of the monomer components used in the polymerization.
[0087] The amount of water used in emulsion polymerization is preferably 10 to 1000 parts by weight, more preferably 50 to 800 parts by weight, further preferably 80 to 600 parts by weight, and particularly preferably 100 to 400 parts by weight, relative to 100 parts by weight of the monomer components used in polymerization. The amount of water used in emulsion polymerization may be adjusted so that the amount taken into consideration of the amount of water used in emulsifying the monomer components described above falls within the above range, and emulsion polymerization may be performed using only the water used in emulsifying the monomer components, or emulsion polymerization may be performed after further adding water.
[0088] In the emulsion polymerization, polymerization auxiliary materials such as a molecular weight regulator, a particle size regulator, a chelating agent, and an oxygen scavenger can be used as necessary.
[0089] The emulsion polymerization may be carried out by any of a batch system, a semi-batch system, and a continuous system, but the semi-batch system is preferred.
[0090] The polymerization temperature and polymerization time are not particularly limited and may be appropriately selected depending on the type of polymerization catalyst used, but the polymerization temperature is preferably 0 to 100° C., more preferably 5 to 80° C., and even more preferably 10 to 50° C. The polymerization time is preferably 0.5 to 100 hours, and more preferably 1 to 10 hours. The polymerization conversion is not particularly limited, but is preferably 80% by weight or more, more preferably 90% by weight or more, and even more preferably 95% by weight or more.
[0091] In addition, when terminating the polymerization reaction, a polymerization terminator can be used. Examples of the polymerization terminator include hydroxylamine, hydroxylamine sulfate, diethylhydroxyamine, hydroxylamine sulfonic acid and its alkali metal salts, sodium dimethyldithiocarbamate, and hydroquinone. The amount of the polymerization terminator used is not particularly limited, but is preferably 0.1 to 2 parts by weight based on 100 parts by weight of the monomer component used in the polymerization.
[0092] (Anti-aging agent addition process) In the production method of the present invention, the antioxidant addition step is a step of adding a phenol-based antioxidant to the emulsion polymerization liquid obtained in the above emulsion polymerization step.
[0093] In the antioxidant addition step, the phenol-based antioxidant is added to the emulsion polymerization liquid of the acrylic rubber by either the following addition method (1) or addition method (2). Method of addition (1): Add the phenolic antioxidant to the emulsion polymerization liquid of acrylic rubber at a temperature above the melting point of the phenolic antioxidant. Addition method (2): A method in which a phenolic antioxidant is brought into contact with an aqueous solution of an emulsifier at a temperature equal to or higher than the melting point of the phenolic antioxidant to obtain a dispersion, and the phenolic antioxidant is added in the form of a dispersion to the emulsion polymerization liquid of acrylic rubber.
[0094] When the phenolic antioxidant is added to the emulsion polymerization liquid of acrylic rubber, by adopting either of the addition methods (1) and (2), the phenolic antioxidant can be uniformly dispersed in the emulsion polymerization liquid, and as a result, the dispersion of the phenolic antioxidant in the acrylic rubber after solidification can be made uniform, and the effect of adding the phenolic antioxidant can be made sufficient. Specifically, the difference between the differential thermal measurement value and the glass transition temperature (Tg) of the acrylic rubber after solidification can be made 250°C or more, and thus the acrylic rubber can be effectively prevented from coloring and generating odor, and has excellent processability, and furthermore, the obtained cross-linked rubber can have excellent elongation at break.
[0095] In the addition method (1), the specific addition method when adding the phenolic antioxidant to the emulsion polymerization liquid of the acrylic rubber under the temperature condition of the melting point or higher of the phenolic antioxidant is not particularly limited, but a method in which the emulsion polymerization liquid is kept at a temperature of the melting point or higher of the phenolic antioxidant and the phenolic antioxidant is added to the emulsion polymerization liquid is preferred. In particular, since the amount of the phenolic antioxidant added to the emulsion polymerization liquid is usually very small compared to the amount of the emulsion polymerization liquid, it is simple and preferred to set the temperature of the emulsion polymerization liquid to a temperature of the melting point or higher of the phenolic antioxidant used in the antioxidant addition step.
[0096] In the addition method (1), the phenol-based antiaging agent may be added to the emulsion polymerization liquid under temperature conditions of not less than the melting point of the phenol-based antiaging agent used, but the addition is more preferably carried out under temperature conditions of not less than the melting point of the phenol-based antiaging agent used + 10°C, and even more preferably carried out under temperature conditions of not less than the melting point of the phenol-based antiaging agent used + 15°C.
[0097] In the addition method (2), a phenolic antioxidant is first contacted with an aqueous solution of an emulsifier at a temperature equal to or higher than the melting point of the phenolic antioxidant to obtain a dispersion of the phenolic antioxidant.
[0098] The emulsifier is not particularly limited, but from the viewpoint of dispersibility when the dispersion of the phenol-based antiaging agent is added to the emulsion polymerization liquid, it is preferable to use the same emulsifier as the one used in the emulsion polymerization step described above. In addition, when two or more kinds of emulsifiers are used in the emulsion polymerization step, it is preferable to use at least one of the two or more kinds of emulsifiers.
[0099] The amount of the emulsifier used is preferably an amount such that the concentration of the emulsifier in the dispersion of the phenolic antioxidant is 0.5 to 20% by weight, more preferably an amount such that the concentration is 1.0 to 15% by weight, and even more preferably an amount such that the concentration is 2.0 to 10% by weight. By setting the amount of the emulsifier to be within the above range, the dispersion of the phenolic antioxidant in the dispersion of the phenolic antioxidant can be made sufficient, and thus, when the dispersion of the phenolic antioxidant is added to the emulsion polymerization liquid, the phenolic antioxidant can be more uniformly dispersed.
[0100] The method for contacting the phenolic antioxidant with the aqueous solution of the emulsifier under temperature conditions equal to or higher than the melting point of the phenolic antioxidant is not particularly limited, but a preferred method is to bring both the phenolic antioxidant and the aqueous solution of the emulsifier to a state in which the temperatures are equal to or higher than the melting point of the phenolic antioxidant, and then add the phenolic antioxidant to the aqueous solution of the emulsifier under stirring.
[0101] In the addition method (2), the phenolic antioxidant may be brought into contact with the aqueous solution of the emulsifier under temperature conditions that are equal to or higher than the melting point of the phenolic antioxidant used. However, the addition is more preferably carried out under temperature conditions that are 10°C higher than the melting point of the phenolic antioxidant used, and even more preferably carried out under temperature conditions that are 15°C higher than the melting point of the phenolic antioxidant used.
[0102] The content of the phenolic antioxidant in the dispersion of the phenolic antioxidant is not particularly limited, but is preferably an amount such that the concentration of the phenolic antioxidant is 10 to 80% by weight, more preferably an amount such that the concentration is 25 to 75% by weight, and even more preferably an amount such that the concentration is 30 to 70% by weight. By setting the content of the phenolic antioxidant within the above range, the phenolic antioxidant can be more uniformly dispersed when the dispersion of the phenolic antioxidant is added to the emulsion polymerization liquid.
[0103] In the addition method (2), the dispersion of the phenolic antioxidant thus prepared is added to the emulsion polymerization liquid of the acrylic rubber.
[0104] The amount of the phenolic antioxidant added to the emulsion polymerization liquid in the antioxidant addition step may be an amount that results in the content in the acrylic rubber within the above-mentioned range, and the specific amount added is preferably 0.1 to 5 parts by weight, more preferably 0.2 to 3 parts by weight, and even more preferably 0.3 to 2 parts by weight, relative to 100 parts by weight of the acrylic rubber component contained in the emulsion polymerization liquid. The phenolic antioxidant added in the antioxidant addition step usually remains in the solidified acrylic rubber even after undergoing the coagulation step described below, and the amount of the phenolic antioxidant added may be determined taking this into consideration.
[0105] (solidification process) The coagulation step in the production method of the present invention is a step of producing hydrous crumbs by contacting the emulsion polymerization liquid to which the phenol-based antiaging agent has been added, obtained in the antiaging agent addition step described above, with a coagulant.
[0106] The coagulant is not particularly limited, but examples thereof include monovalent to trivalent metal salts. The monovalent to trivalent metal salts are salts containing metals that become monovalent to trivalent metal ions when dissolved in water, and are not particularly limited, but examples thereof include salts of inorganic acids selected from hydrochloric acid, nitric acid, and sulfuric acid, and organic acids such as acetic acid, and metals selected from sodium, potassium, lithium, magnesium, calcium, zinc, titanium, manganese, iron, cobalt, nickel, aluminum, and tin. Hydroxides of these metals can also be used.
[0107] Specific examples of monovalent to trivalent metal salts include metal chlorides such as sodium chloride, potassium chloride, lithium chloride, magnesium chloride, calcium chloride, zinc chloride, titanium chloride, manganese chloride, iron chloride, cobalt chloride, nickel chloride, aluminum chloride, and tin chloride; nitrates such as sodium nitrate, potassium nitrate, lithium nitrate, magnesium nitrate, calcium nitrate, zinc nitrate, titanium nitrate, manganese nitrate, iron nitrate, cobalt nitrate, nickel nitrate, aluminum nitrate, and tin nitrate; sulfates such as sodium sulfate, potassium sulfate, lithium sulfate, magnesium sulfate, calcium sulfate, zinc sulfate, titanium sulfate, manganese sulfate, iron sulfate, cobalt sulfate, nickel sulfate, aluminum sulfate, and tin sulfate; and the like. Among these, calcium chloride, sodium chloride, aluminum sulfate, magnesium chloride, magnesium sulfate, zinc chloride, zinc sulfate, and sodium sulfate are preferred. Among these, monovalent or divalent metal salts are preferred, divalent metal salts are more preferred, magnesium salts are more preferred, inorganic magnesium salts are even more preferred, and magnesium sulfate is particularly preferred. These can be used alone or in combination.
[0108] The amount of the coagulant used is preferably 0.01 to 100 parts by weight, more preferably 0.1 to 50 parts by weight, and even more preferably 1 to 30 parts by weight, relative to 100 parts by weight of the monomer components used in the polymerization. By setting the amount of the coagulant used within the above range, the acrylic rubber can be sufficiently coagulated in the coagulation step, and the obtained acrylic rubber can have excellent water resistance.
[0109] In the production method of the present invention, the method of contacting the emulsion polymerization liquid with the coagulant is not particularly limited, but examples thereof include a method of adding the emulsion polymerization liquid to an aqueous solution containing a coagulant while stirring the aqueous solution containing the coagulant, and a method of adding an aqueous solution containing a coagulant to the emulsion polymerization liquid while stirring the emulsion polymerization liquid. Alternatively, a method of simply adding the emulsion polymerization liquid to an aqueous solution containing a coagulant without stirring, or a method of adding an aqueous solution containing a coagulant to the emulsion polymerization liquid may be adopted. Among these, a method of adding the emulsion polymerization liquid to an aqueous solution containing a coagulant while stirring the aqueous solution containing the coagulant is preferred, and by adopting such a method to perform the coagulation operation, the particle size of the water-containing crumbs generated by coagulation can be controlled to a relatively uniform range, and thus the washing efficiency of the generated water-containing crumbs can be improved.
[0110] The concentration of the magnesium salt in the aqueous solution containing the coagulant used in the coagulation step is not particularly limited, but from the viewpoint of more appropriately controlling the particle size of the hydrous crumbs produced by coagulation, it is preferably 0.1 to 20% by weight, more preferably 0.5 to 10% by weight, and even more preferably 1 to 5% by weight.
[0111] The temperature of the aqueous solution containing the coagulant in the coagulation step (i.e., the coagulation temperature) is not particularly limited, but from the viewpoint of more appropriately controlling the particle size of the water-containing crumbs produced by coagulation, it is preferably 40°C or higher, more preferably 40 to 90°C, and even more preferably 50 to 80°C.
[0112] In the solidification step, the stirring method for stirring the aqueous solution containing the coagulant is not particularly limited, but may be a method using a stirring device that stirs with a stirring blade. In this case, it is preferable to employ a method in which the aqueous solution containing the coagulant is contained in a stirring tank, and the emulsion polymerization liquid is added while stirring the aqueous solution containing the coagulant in the stirring tank with a stirring blade.
[0113] Furthermore, in the coagulation step, the solids concentration of the emulsion polymerization liquid used for coagulation is not particularly limited, and may be used as obtained in the emulsion polymerization step and the antioxidant addition step. However, from the viewpoint of more appropriately controlling the particle size of the water-containing crumbs generated by coagulation, it is preferable to adjust the solids concentration to a range of 5 to 50% by weight, more preferably to a range of 10 to 45% by weight, and particularly preferably to a range of 20 to 40% by weight.
[0114] (Cleaning process) In addition, the production method of the present invention preferably further includes a washing step of washing the water-containing crumbs obtained in the above-mentioned solidification step.
[0115] The washing method in the washing step is not particularly limited, but may be, for example, a method of washing the water-containing crumb obtained in the above-mentioned coagulation step with water, preferably a method of mixing the water-containing crumb obtained in the above-mentioned coagulation step with water, etc. The temperature during washing is not particularly limited, but is preferably 5 to 60°C, more preferably 10 to 50°C, and the mixing time is 1 to 60 minutes, more preferably 2 to 30 minutes.
[0116] In addition, the amount of water to be mixed with the water-containing crumbs in the washing step is not particularly limited, but from the viewpoint of further increasing the efficiency of water washing, it is preferably an amount of 50 parts by weight or more relative to 100 parts by weight of the monomer components used in the polymerization, more preferably an amount of 50 to 15,000 parts by weight, even more preferably an amount of 100 to 10,000 parts by weight, and particularly preferably an amount of 500 to 5,000 parts by weight.
[0117] The water washing time is not particularly limited, but is preferably 1 to 120 minutes, more preferably 2 to 60 minutes, and further preferably 3 to 30 minutes.
[0118] The number of water washings in the washing step is not particularly limited, and is preferably 1 to 10 times, more preferably 1 to 5 times, and even more preferably 1 to 3 times. In the present invention, the number of water washings is the number of times when the operation of adding water to the wet crumbs, mixing for a predetermined time, and then separating the wet crumbs from the water used for water washing is defined as one water washing. That is, for example, the number of water washings twice means that the operation of adding water to the wet crumbs, mixing for a predetermined time, and then separating the wet crumbs from the water used for water washing is performed, and then, water is further added to the wet crumbs, mixing for a predetermined time, and then separating the wet crumbs from the water used for water washing. In the case of performing water washing twice or more, the temperature of the water used for water washing, the amount of water, and the time of water washing may be the same or different.
[0119] In the present invention, after the water washing, an acid washing may be further performed using an acid as a washing liquid. After the acid washing, it is preferable to further perform water washing, and the water washing conditions may be the same as those described above.
[0120] (drying process) The above-mentioned production method may further include a drying step of drying the hydrous crumbs washed in the washing step.
[0121] The method for drying the hydrous crumbs is not particularly limited and may be any conventional method, for example, a method using a dryer such as a hot air dryer, a reduced pressure dryer, an expander dryer, a kneader type dryer, or a screw type extruder.
[0122] The drying temperature for the hydrous crumb is not particularly limited, but is preferably 80 to 250°C, more preferably 100 to 200°C, and further preferably 120 to 180°C.
[0123] The method of dehydrating the hydrous crumb is not particularly limited, but includes a method of draining water from the hydrous crumb using a dehydrator such as a centrifuge, a squeezer, or a screw-type extruder. From the viewpoint of further reducing the moisture content of the hydrous crumb, a method using a squeezer or a screw-type extruder is preferred, and a method using a screw-type extruder is particularly preferred. By using a screw-type extruder, the hydrous crumb can be dehydrated and dried in a continuous process, thereby increasing productivity.
[0124] As the screw-type extruder, a twin-screw extruder having a barrel unit consisting of a plurality of barrel blocks and a pair of screws rotatably disposed inside the barrel unit can be suitably used.
[0125] The barrel unit may include, in order from the supply side of the water-containing crumb, a supply barrel section consisting of one or more supply barrel blocks, a dehydration barrel section consisting of one or more dehydration barrel blocks, and a drying barrel section consisting of one or more drying barrel blocks. A die for extruding the dehydrated and dried acrylic rubber into a sheet shape is connected to the downstream side of the drying barrel section.
[0126] The supply barrel section is a region where the wet crumbs are supplied to the inside of the barrel unit. The dehydration barrel section is a region where the liquid (serum water) containing the coagulant and the like is separated and discharged from the wet crumbs. At least a part of the dehydration barrel blocks constituting the dehydration barrel section is provided with a slit for discharging the water generated by the dehydration. The drying barrel section is a region where the crumbs dehydrated by the dehydration barrel section are dried.
[0127] The temperature set in the dehydration barrel is preferably 60 to 150° C., more preferably 70 to 140° C., and even more preferably 80 to 130° C. The temperature set in the drying barrel is preferably 100 to 250° C., more preferably 110 to 200° C., and even more preferably 120 to 180° C.
[0128] The screw length (L) of a pair of screws arranged inside the barrel unit constituting the screw type extruder is not particularly limited, but is preferably 3000 to 15000 mm, more preferably 4000 to 10000 mm, and even more preferably 4500 to 8000 mm. The screw diameter (D) of the screw is not particularly limited, but is preferably 50 to 250 mm, more preferably 100 to 200 mm, and even more preferably 120 to 160 mm. The ratio (L / D) of the screw length (L) to the screw diameter (D) of the screw is not particularly limited, but is preferably 10 to 100, more preferably 20 to 80, and even more preferably 30 to 60. By setting the screw length (L) and screw diameter (D) in the above ranges, it is possible to efficiently perform dehydration and drying while effectively suppressing the molecular weight reduction and the occurrence of scorching of the acrylic rubber.
[0129] In addition, the operating conditions of the screw extruder when dehydrating and drying the water-containing crumbs using the screw extruder are not particularly limited, but examples thereof include the following conditions. That is, the rotation speed N [rpm] of the pair of screws arranged inside the barrel unit is preferably 10 to 1000 rpm, and from the viewpoint of efficiently reducing the water content and gel amount of the acrylic rubber, is more preferably 50 to 750 rpm, even more preferably 100 to 500 rpm, and particularly preferably 120 to 300 rpm. The throughput Q [kg / hr] of the acrylic rubber dried per unit time in the screw extruder is preferably 100 to 1500 kg / hr, more preferably 300 to 1200 kg / hr, further preferably 400 to 1000 kg / hr, and particularly preferably 500 to 800 kg / hr.
[0130] Furthermore, the ratio (Q / N) of the amount Q of acrylic rubber dried per unit time to the number of rotations N of the screw is not particularly limited, but is preferably 1 to 20, more preferably 2 to 10, even more preferably 3 to 8, and particularly preferably 4 to 6. By setting "Q / N" within the above range, acrylic rubber with an appropriately reduced moisture content can be produced with high productivity. In addition, the rubber pressure (resin pressure or discharge pressure) in the die connected downstream of the drying barrel section is not particularly limited, but from the viewpoint of effectively suppressing air entrainment while realizing high productivity, it is preferably 0.1 to 10 MPa, more preferably 0.5 to 5 MPa, and even more preferably 1 to 3 MPa.
[0131] The temperature of the water-containing crumbs supplied to the screw-type extruder is not particularly limited, but it is preferable to set the temperature at 60°C or higher from the viewpoint of increasing the efficiency of dehydration and drying, thereby further increasing the water resistance of the obtained acrylic rubber.
[0132] According to the production method of the present invention, the acrylic rubber can be produced as described above. In the present invention, the acrylic rubber may be obtained in the form of crumbs, or may be obtained as baled rubber, that is, acrylic rubber bales (acrylic rubber formed into chunks of a specified shape).
[0133] <Rubber composition> The rubber composition of the present invention contains a rubber component containing the above-mentioned acrylic rubber of the present invention, a filler, and a crosslinking agent. The content of the acrylic rubber component of the present invention in the rubber component may be appropriately selected depending on the purpose of use, but is preferably 30% by weight or more, more preferably 50% by weight or more, even more preferably 70% by weight or more, and particularly preferably 100% by weight (i.e., an embodiment in which the rubber component is substantially composed of only the acrylic rubber component).
[0134] The rubber other than the acrylic rubber of the present invention that constitutes the rubber component is not particularly limited, but examples thereof include acrylic rubber other than the acrylic rubber of the present invention, natural rubber, polybutadiene rubber, polyisoprene rubber, styrene-butadiene rubber, acrylonitrile-butadiene rubber, silicone rubber, fluororubber, olefin-based elastomers, styrene-based elastomers, vinyl chloride-based elastomers, polyester-based elastomers, polyamide-based elastomers, polyurethane-based elastomers, polysiloxane-based elastomers, and the like.
[0135] The rubber other than the acrylic rubber of the present invention may be used alone or in combination of two or more. The shape of the acrylic rubber of the present invention and the shape of the rubber other than the acrylic rubber of the present invention are not particularly limited, but may be any shape such as a veil, a sheet, or a powder.
[0136] The filler is not particularly limited, but examples thereof include reinforcing fillers and non-reinforcing fillers, and among these, reinforcing fillers are preferred.
[0137] Examples of reinforcing fillers include carbon blacks such as furnace black, acetylene black, thermal black, channel black, and graphite; silicas such as wet silica, dry silica, and colloidal silica; and examples of non-reinforcing fillers include quartz powder, clays such as diatomaceous earth, zinc oxide, basic magnesium carbonate, activated calcium carbonate, magnesium silicate, aluminum silicate, titanium dioxide, talc, aluminum sulfate, calcium sulfate, and barium sulfate.
[0138] These fillers can be used alone or in combination of two or more. The content of the filler in the rubber composition of the present invention is not particularly limited, but is preferably 1 to 200 parts by weight, more preferably 10 to 150 parts by weight, and further preferably 20 to 100 parts by weight, based on 100 parts by weight of the rubber component containing the acrylic rubber of the present invention.
[0139] The crosslinking agent is not particularly limited, but may be, for example, a polyamine compound such as a diamine compound and its carbonate; sulfur; a sulfur donor; a triazine thiol compound; a polyepoxy compound; an organic carboxylic acid ammonium salt; an organic peroxide; a dithiocarbamic acid metal salt; a polycarboxylic acid; a quaternary onium salt; an imidazole compound; an isocyanuric acid compound; or other conventionally known crosslinking agents. These crosslinking agents may be used alone or in combination of two or more. It is preferable to select the crosslinking agent appropriately according to the type of crosslinkable monomer unit.
[0140] Among these, when the acrylic rubber of the present invention has an α,β-ethylenically unsaturated carboxylic acid monomer unit as a crosslinkable monomer unit, it is preferable to use a polyamine compound and a carbonate thereof as a crosslinking agent.
[0141] The polyamine compound and the carbonate thereof are not particularly limited, but are preferably a polyamine compound having 4 to 30 carbon atoms and a carbonate thereof. Examples of such polyamine compounds and carbonates thereof include aliphatic polyamine compounds and carbonates thereof, and aromatic polyamine compounds.
[0142] The aliphatic polyamine compounds and carbonates thereof are not particularly limited, but examples thereof include hexamethylenediamine, hexamethylenediamine carbamate, and N,N'-dicinnamylidene-1,6-hexanediamine, etc. Among these, hexamethylenediamine carbamate is preferred.
[0143] The aromatic polyamine compound is not particularly limited, but examples thereof include 4,4'-methylenedianiline, p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-(m-phenylenediisopropylidene)dianiline, 4,4'-(p-phenylenediisopropylidene)dianiline, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-diaminobenzanilide, 4,4'-bis(4-aminophenoxy)biphenyl, m-xylylenediamine, p-xylylenediamine, and 1,3,5-benzenetriamine. Among these, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane is preferred.
[0144] In addition, when the acrylic rubber of the present invention has a monomer unit having an epoxy group as a crosslinkable monomer unit, the crosslinking agent may be an aliphatic polyamine compound such as hexamethylenediamine, hexamethylenediamine carbamate, and the like, and a carbonate thereof; an aromatic polyamine compound such as 4,4'-methylenedianiline; an ammonium carboxylate salt such as ammonium benzoate, ammonium adipate, and the like; a metal dithiocarbamate salt such as zinc dimethyldithiocarbamate; a polycarboxylic acid such as tetradecanedioic acid; a quaternary onium salt such as cetyltrimethylammonium bromide; an imidazole compound such as 2-methylimidazole; an isocyanuric acid compound such as ammonium isocyanurate; and the like. Among these, ammonium carboxylate salts and metal dithiocarbamate salts are preferred, and ammonium benzoate is more preferred.
[0145] Furthermore, when the acrylic rubber of the present invention has a monomer unit having a halogen atom as a crosslinkable monomer unit, it is preferable to use sulfur, a sulfur donor, or a triazine thiol compound as a crosslinking agent. Examples of the sulfur donor include dipentamethylene thiuram hexasulfide and triethylthiuram disulfide. Examples of triazine compounds include 2,4,6-trimercapto-s-triazine, 2-anilino-4,6-dithiol-s-triazine, 2-dibutylamino-4,6-dithiol-s-triazine, 1-hexylamino-3,5-dimercaptotriazine, etc. Among these, 2,4,6-trimercapto-s-triazine is preferred.
[0146] The content of the crosslinking agent in the rubber composition of the present invention is preferably 0.001 to 20 parts by weight, more preferably 0.1 to 10 parts by weight, further preferably 0.1 to 5 parts by weight, and particularly preferably 0.2 to 4 parts by weight, based on 100 parts by weight of the rubber component containing the acrylic rubber of the present invention. By setting the content of the crosslinking agent within the above range, it is possible to ensure sufficient rubber elasticity while providing excellent mechanical strength as a crosslinked rubber product.
[0147] In addition, the rubber composition of the present invention preferably further contains a crosslinking accelerator. The crosslinking accelerator is not particularly limited, but when the acrylic rubber of the present invention has a carboxyl group as a crosslinkable group and the crosslinking agent is a polyvalent amine compound or a carbonate thereof, a guanidine compound, a diazabicycloalkene compound, an imidazole compound, a quaternary onium salt, a tertiary phosphine compound, an aliphatic monovalent secondary amine compound, and an aliphatic monovalent tertiary amine compound can be used. Among these, a guanidine compound, a diazabicycloalkene compound, and an aliphatic monovalent secondary amine compound are preferred, and a guanidine compound and a diazabicycloalkene compound are particularly preferred. These basic crosslinking accelerators can be used alone or in combination of two or more.
[0148] Specific examples of guanidine compounds include 1,3-di-o-tolylguanidine and 1,3-diphenylguanidine. Specific examples of diazabicycloalkene compounds include 1,8-diazabicyclo[5.4.0]undec-7-ene and 1,5-diazabicyclo[4.3.0]non-5-ene. Specific examples of imidazole compounds include 2-methylimidazole and 2-phenylimidazole. Specific examples of quaternary onium salts include tetra-n-butylammonium bromide and octadecyltri-n-butylammonium bromide. Specific examples of tertiary phosphine compounds include triphenylphosphine and tri-p-tolylphosphine.
[0149] The aliphatic monovalent secondary amine compound is a compound in which two hydrogen atoms of ammonia are replaced with an aliphatic hydrocarbon group. The aliphatic hydrocarbon group replacing the hydrogen atom preferably has 1 to 30 carbon atoms. Specific examples of the aliphatic monovalent secondary amine compound include dimethylamine, diethylamine, dipropylamine, diallylamine, diisopropylamine, di-n-butylamine, di-t-butylamine, di-sec-butylamine, dihexylamine, diheptylamine, dioctylamine, dinonylamine, didecylamine, diundecylamine, didodecylamine, ditridecylamine, ditetradecylamine, dipentadecylamine, dicetylamine, di-2-ethylhexylamine, and dioctadecylamine.
[0150] The aliphatic monovalent tertiary amine compound is a compound in which all three hydrogen atoms of ammonia are substituted with an aliphatic hydrocarbon group. The aliphatic hydrocarbon group that substitutes the hydrogen atom preferably has 1 to 30 carbon atoms. Specific examples of the aliphatic monovalent tertiary amine compound include trimethylamine, triethylamine, tripropylamine, triallylamine, triisopropylamine, tri-n-butylamine, tri-t-butylamine, tri-sec-butylamine, trihexylamine, triheptylamine, trioctylamine, trinonylamine, tridecylamine, triundecylamine, and tridodecylamine.
[0151] The content of the crosslinking accelerator in the rubber composition of the present invention is preferably 0.1 to 10 parts by weight, more preferably 0.5 to 7.5 parts by weight, and particularly preferably 1 to 5 parts by weight, based on 100 parts by weight of the rubber component containing the acrylic rubber of the present invention. By setting the content of the crosslinking accelerator within the above range, the tensile strength and compression set resistance of the obtained crosslinked rubber product can be further improved.
[0152] The rubber composition of the present invention may contain an antioxidant as required. That is, in addition to the phenolic antioxidant contained in the acrylic rubber, an additional antioxidant may be added. The antioxidant is not particularly limited, but may be any of the above-mentioned phenolic antioxidants; phosphite ester antioxidants such as tris(nonylphenyl)phosphite, diphenylisodecylphosphite, and tetraphenyldipropylene glycol diphosphite; sulfur ester antioxidants such as dilauryl thiodipropionate; phenyl-α-naphthylamine, phenyl-β-naphthylamine, p-(p-toluenesulfonylamido)-diphenylamine, 4,4'-bis(α,α-dimethylamine), and the like. Examples of the antiaging agents include amine-based antiaging agents such as N,N-diphenyl-p-phenylenediamine, N-isopropyl-N'-phenyl-p-phenylenediamine, and butyraldehyde-aniline condensates; imidazole-based antiaging agents such as 2-mercaptobenzimidazole; quinoline-based antiaging agents such as 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline; and hydroquinone-based antiaging agents such as 2,5-di-(t-amyl)hydroquinone.
[0153] The antioxidant can be used alone or in combination of two or more. The content of the antioxidant in the rubber composition of the present invention is not particularly limited, but is preferably 0.01 to 15 parts by weight, more preferably 0.05 to 10 parts by weight, and further preferably 0.1 to 5 parts by weight, based on 100 parts by weight of the rubber component containing the acrylic rubber of the present invention.
[0154] In addition to the above-mentioned components, the rubber composition of the present invention may contain compounding agents that are commonly used in the field of rubber processing. Examples of such compounding agents include light stabilizers, scorch inhibitors, plasticizers, processing aids, tackifiers, slip agents, lubricants, flame retardants, antifungal agents, antistatic agents, colorants, and crosslinking retarders. The amount of these compounding agents is not particularly limited as long as it is within a range that does not impair the purpose and effects of the present invention, and they can be appropriately compounded in an amount according to the purpose of compounding.
[0155] The rubber composition of the present invention is prepared by blending a crosslinking agent and various other compounding ingredients used as necessary with a rubber component containing the acrylic rubber of the present invention described above, mixing and kneading the mixture with an open roll, a Banbury mixer, various kneaders, or the like, and then further kneading the mixture with a kneading roll.
[0156] The order of mixing the components is not particularly limited, but it is preferable to thoroughly mix the components that are unlikely to react or decompose when heated, and then mix the crosslinking agent and other components that are likely to react or decompose when heated for a short period of time at a temperature at which they will not react or decompose.
[0157] <Rubber cross-linked products> The cross-linked rubber product of the present invention is obtained by cross-linking the above-mentioned rubber composition of the present invention. The cross-linked rubber product of the present invention can be produced by using the acrylic rubber composition of the present invention, molding the composition into a desired shape using a molding machine such as an extruder, an injection molding machine, a compressor, and a roll, and then heating the composition to cause a cross-linking reaction and fix the shape as a cross-linked rubber product. In this case, the composition may be cross-linked after molding in advance, or may be cross-linked simultaneously with molding. The molding temperature is usually 10 to 200°C, preferably 25 to 120°C. The cross-linking temperature is usually 130 to 220°C, preferably 150 to 190°C, and the cross-linking time is usually 2 minutes to 10 hours, preferably 3 minutes to 5 hours. As the heating method, a method used for cross-linking rubber, such as press heating, steam heating, oven heating, and hot air heating, may be appropriately selected.
[0158] Depending on the shape, size, etc. of the cross-linked rubber product, the cross-linked rubber product of the present invention may be further heated to carry out secondary cross-linking. The secondary cross-linking time varies depending on the heating method, cross-linking temperature, shape, etc., but is preferably carried out for 1 to 48 hours. The heating method and heating temperature may be appropriately selected.
[0159] The cross-linked rubber product of the present invention thus obtained is suitably used as sealing materials such as O-rings, packings, diaphragms, oil seals, shaft seals, bearing sheaths, mechanical seals, well head seals, seals for electric and electronic devices, and seals for air compressors; various gaskets such as a cylinder head gasket attached to the connecting portion between a cylinder block and a cylinder head, a rocker cover gasket attached to the connecting portion between a rocker cover and a cylinder head, an oil pan gasket attached to the connecting portion between an oil pan and a cylinder head or a transmission case, a gasket for a fuel cell separator attached between a pair of housings sandwiching a unit cell having a positive electrode, an electrolyte plate, and a negative electrode, and a gasket for the top cover of a hard disk drive; cushioning materials, vibration-proofing materials; wire covering materials; industrial belts, tubes, hoses, sheets, and the like.
[0160] Furthermore, the cross-linked rubber product of the present invention can be suitably used as extrusion molded articles and cross-linked products for automotive applications, for example, various hoses such as fuel oil hoses for fuel tanks, such as fuel hoses, filler neck hoses, vent hoses, vapor hoses and oil hoses, air hoses, such as turbo air hoses and mission control hoses, radiator hoses, heater hoses, brake hoses and air conditioner hoses. EXAMPLES
[0161] The present invention will be described in more detail below with reference to examples and comparative examples. In each example, "parts" is by weight unless otherwise specified. Various physical properties were evaluated according to the following methods.
[0162] [Monomer composition of acrylic rubber] The monomer composition of the acrylic rubber was calculated from the amount of each monomer used in the polymerization reaction and the polymerization conversion rate. Specifically, in the emulsion polymerization reaction in each Example and Comparative Example, no unreacted monomer was found, and the polymerization conversion rate was approximately 100%, so the amount of each monomer used in the polymerization reaction was determined to be the same as the content ratio of each monomer unit constituting the acrylic rubber.
[0163] [Glass transition temperature (Tg) of acrylic rubber] The glass transition temperature (Tg) of the acrylic rubber was measured using a differential scanning calorimeter (DSC, product name "X-DSC7000", manufactured by Hitachi High-Tech Science Corporation) by increasing the temperature from -80°C to 50°C at a rate of 10°C / min and reading the peak value of the differential curve.
[0164] [Oxidation start temperature of acrylic rubber] The oxidation onset temperature of the acrylic rubber was measured using a thermogravimetry / differential thermal analyzer (Tg / DTA, product name "STA-7200", manufactured by Hitachi High-Tech Science Corporation) and was measured by reading the peak value corresponding to the oxidation onset temperature from the DTA curve obtained by the measurement.
[0165] [Weight average molecular weight of acrylic rubber (Mw)] The weight average molecular weight (Mw) of the acrylic rubber was measured by the following method. That is, using a GPC system (Tosoh Corporation's "HLC-8220GPC" and two Tosoh Corporation separation columns "TSKgel α-M (φ7.8mm × 30cm)" connected in series) incorporating a multi-angle laser light scattering photometer (MALS: Wyatt Corporation's "DAWN HELEOS-II"), GPC measurement was performed under the following conditions: column temperature 40°C, 0.01% concentrated hydrochloric acid as developing solvent, 0.05M lithium chloride-added dimethylformamide, flow rate 0.8mL / min, injection volume 0.2mL. The measurement sample was dissolved in the developing solvent to a concentration of 2.0mg / mL, and passed through a 0.5μm filter to remove high molecular weight components outside the GPC measurement range. The results obtained were measured by the GPC-MALS method and can be considered as absolute molecular weights.
[0166] [Antioxidant content in acrylic rubber] The acrylic rubber was dissolved in a developing solvent, and the acrylic rubber dissolved in the developing solvent was subjected to GPC measurement to measure the content of the antioxidant in the acrylic rubber. Specifically, the integral value of the peak corresponding to the molecular weight of the antioxidant used in the production was obtained from the chart obtained by GPC measurement, and these integral values were compared with the integral value of the peak of the acrylic rubber, and the weight ratio was calculated from these integral values and the corresponding molecular weight to calculate the content of the antioxidant. Note that tetrahydrofuran or dimethylformamide was used as the developing solvent.
[0167] [Acrylic rubber heat stability test (color change and odor generation)] The acrylic rubber was placed in a mold measuring 15 cm in length, 15 cm in width, and 0.2 cm in depth, compressed at 150°C for 10 minutes while applying a pressure of 10 MPa, and then cooled while still in the mold to obtain an acrylic rubber sheet. The obtained acrylic rubber sheet was cut into pieces of 3 cm x 3 cm and subjected to a thermal stability test under the following two conditions in accordance with JIS K7212. In this test, discoloration and odor modes were observed and evaluated according to the following criteria. (Heating conditions) Heating condition 1: 50℃, 168 hours Heating condition 2: 190℃, 24 hours (evaluation) ◎: Colorless, transparent and odorless ○: Yellow color and odorless △: Yellow color and odor generation ×: Colored brown to black
[0168] [Mixing and processing evaluation (BIT)] In the kneading process for preparing the acrylic rubber composition (1) for evaluation, the time required for the powder-like compounding agents, etc., taken into the raw rubber by shear force or elongation force to be dispersed and finely dispersed in the rubber composition, that is, the BIT (Black Incorporation Time: the time from the time when the compounding agent is added to the time when the torque reaches the maximum value point when the kneaded dough is integrated), was observed and evaluated. That is, the time (seconds) at which the torque reaches the maximum value observed when kneading with a Banbury type mixer as the kneading machine and a charge factor of 70% was evaluated as the BIT value. The smaller the BIT, the shorter the time it takes for the entire kneaded dough to be integrated, and the better the processability, which improves productivity. In addition, the smaller the BIT, the more it is possible to prevent excessive shear and temperature from being applied to the rubber composition, and the more effectively it is possible to suppress adverse effects on storage stability, scorch properties, normal physical properties, and heat aging properties.
[0169] [Extrusion processability evaluation (surface smoothness)] The acrylic rubber composition for evaluation (1) was extrusion molded using a single screw extruder and a Garvey die, and the surface smoothness was evaluated in accordance with ASTM D2230. The surface smoothness was evaluated according to the following criteria. It is to be noted that the smoother the surface, the better the extrusion processability. : The surface of the extrudate is smooth and glossy. Δ: The surface of the extrudate is smooth but lacks luster. ×: Irregularities or small wrinkles are observed on the surface of the extruded product.
[0170] [Elongation at break] The acrylic rubber composition (2) for evaluation was placed in a mold 15 cm long, 15 cm wide, and 0.2 cm deep, and compressed at 170°C for 20 minutes while applying a pressure of 10 MPa to perform primary crosslinking. The primary crosslinked product was then heated in a gear oven at 170°C for 4 hours to perform secondary crosslinking, thereby obtaining a sheet-like crosslinked rubber product. The crosslinked rubber product was punched out with a No. 3 dumbbell to prepare a test piece. The test piece was then used to measure the breaking elongation according to JIS K6251.
[0171] [Example 1] (Production of Acrylic Rubber (A-1)) A mixing vessel equipped with a homomixer was charged with 46.294 parts of ion-exchanged water, 74.5 parts of ethyl acrylate, 17 parts of n-butyl acrylate, 7 parts of 2-methoxyethyl acrylate, and 1.5 parts of mono-n-butyl fumarate as monomer components, and 1.8 parts of tridecyloxyhexa(oxyethylene) phosphate sodium salt (anionic emulsifier), as an emulsifier, and stirred to obtain a monomer emulsion.
[0172] Next, 170.853 parts of pure water and 2.962 parts of the monomer emulsion obtained above were put into a polymerization reaction tank equipped with a thermometer and a stirrer, and cooled to 12°C under a nitrogen stream. Next, 145.132 parts of the monomer emulsion obtained above, 0.00033 parts of ferrous sulfate (reducing agent), 0.264 parts of sodium ascorbate (reducing agent), and 7.72 parts of a 2.85 wt% aqueous potassium persulfate solution (polymerization initiator) (0.22 parts as the amount of potassium persulfate) were continuously dropped into the polymerization reaction tank over a period of 3 hours while maintaining the temperature at 12°C. Thereafter, the reaction was continued for 1 hour while maintaining the temperature in the polymerization reaction tank at 23°C, and it was confirmed that the polymerization conversion rate reached approximately 100%, and hydroquinone was added as a polymerization terminator to terminate the polymerization reaction, thereby obtaining an emulsion polymerization liquid.
[0173] Next, separately from the above, 50 parts of a 12 wt % aqueous solution of tridecyloxyhexa(oxyethylene) phosphate sodium salt (anionic emulsifier) and 50 parts of octyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (product name "Irganox 1135", manufactured by BASF, doubly hindered phenol-based antioxidant, molecular weight: 390, melting point: 10° C.) were mixed and stirred at a temperature of 25° C. to obtain an antioxidant dispersion (concentration of tridecyloxyhexa(oxyethylene) phosphate sodium salt as emulsifier: 6 wt %, concentration of phenol-based antioxidant: 50 wt %).
[0174] Next, 0.36 parts of the antioxidant dispersion liquid prepared above (an amount such that the phenol-based antioxidant was 0.5 parts per 100 parts of the rubber component in the emulsion polymerization liquid) was added to 100 parts of the emulsion polymerization liquid obtained above (temperature: 25°C), and the mixture was stirred.
[0175] Next, 60 parts of a 30 wt % aqueous magnesium sulfate solution adjusted to 85° C. was added to a coagulation tank equipped with a thermometer and a stirrer, and stirred with a stirring blade while heating to 85° C. Then, 100 parts of the emulsion polymerization liquid to which the antioxidant dispersion liquid had been added, prepared as above, was continuously added to the aqueous magnesium sulfate solution while stirring, whereby the polymer was coagulated and filtered to obtain hydrous crumbs.
[0176] Next, 388 parts of industrial water was added to 100 parts of the solid content of the hydrous crumb obtained above, and the mixture was stirred at room temperature for 5 minutes in a coagulation tank, after which the water was discharged from the coagulation tank to wash the hydrous crumb. The hydrous crumb after washing was dried in a hot air dryer at 110°C for 1 hour to obtain a solid acrylic rubber (A-1) with a recovery rate of 100%. The monomer composition, glass transition temperature (Tg), oxidation onset temperature, and weight average molecular weight (Mw) of the obtained acrylic rubber (A-1) were measured according to the above-mentioned methods, and a thermal stability test (color change and odor generation) was also performed according to the above-mentioned methods. The results are shown in Table 1. Furthermore, when the amount of the antioxidant in the acrylic rubber (A-1) was measured, it was found to be almost the same amount as the amount of the antioxidant that was blended (95 to 100% by weight of the antioxidant that was blended) (the same applies to Examples 2 to 10 and Comparative Examples 1, 3, and 4 described later).
[0177] (Preparation of Acrylic Rubber Composition (1) for Evaluation) Using a Banbury mixer, 100 parts of the acrylic rubber (A-1) obtained above was mixed with 60 parts of carbon black (trade name "Seat SO", manufactured by Tokai Carbon Co., Ltd.), 1 part of stearic acid, 1 part of ester wax (trade name "Grec 8205", manufactured by DIC Corporation), and 2 parts of 4,4'-bis(α,α-dimethylbenzyl)diphenylamine (trade name "Nocrac CD", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) at 50°C for 5 minutes to obtain an acrylic rubber composition (1) for evaluation. When preparing the acrylic rubber composition (1) for evaluation, the kneading processability evaluation (BIT) was performed according to the above-mentioned method. In addition, the obtained acrylic rubber composition (1) for evaluation was used to perform an extrusion processability evaluation (surface smoothness) according to the above-mentioned method. The results are shown in Table 1.
[0178] (Preparation of Acrylic Rubber Composition (2) for Evaluation) A part of the acrylic rubber composition for evaluation (1) obtained above was transferred to a roll at 50°C, and 100 parts of the acrylic rubber (A-1) contained in the acrylic rubber composition for evaluation (1) were mixed with 0.5 parts of hexamethylenediamine carbamate (trade name "Diak#1", manufactured by DuPont Dow Elastomers) and 2 parts of 1,3-di-o-tolylguanidine (trade name "Noccela DT", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) and kneaded to obtain an acrylic rubber composition for evaluation (2). The acrylic rubber composition for evaluation (2) obtained was used to evaluate the elongation at break. The results are shown in Table 1.
[0179] [Example 2] (Production of acrylic rubber (A-2)) An acrylic rubber (A-2) was obtained in the same manner as in Example 1, except that octyloxydi(oxyethylene) phosphate sodium salt (anionic emulsifier) was used instead of tridecyloxyhexa(oxyethylene) phosphate sodium salt as the emulsifier used in obtaining the monomer emulsion and the emulsifier used in obtaining the antioxidant dispersion. The obtained acrylic rubber (A-2) was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0180] (Preparation of Acrylic Rubber Composition (1) and Acrylic Rubber Composition (2) for Evaluation) In addition, except for using the acrylic rubber (A-2) obtained above, an acrylic rubber composition for evaluation (1) and an acrylic rubber composition for evaluation (2) were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0181] [Example 3] (Production of acrylic rubber (A-3)) An acrylic rubber (A-3) was obtained in the same manner as in Example 1, except that the amount of ethyl acrylate used as the monomer component was changed to 65.5 parts, the amount of n-butyl acrylate used was changed to 8 parts, and the amount of 2-methoxyethyl acrylate used was changed to 25 parts. The obtained acrylic rubber (A-3) was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0182] (Preparation of Acrylic Rubber Composition (1) and Acrylic Rubber Composition (2) for Evaluation) In addition, except for using the acrylic rubber (A-3) obtained above, an acrylic rubber composition for evaluation (1) and an acrylic rubber composition for evaluation (2) were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0183] [Example 4] (Production of acrylic rubber (A-4)) Emulsion polymerization was carried out in the same manner as in Example 1 to obtain an emulsion polymerization liquid, except that, as the emulsifier used in obtaining the monomer emulsion, 0.567 parts of sodium lauryl sulfate (trade name "EMAL 2FG", manufactured by Kao Corporation, anionic emulsifier) and 1.4 parts of polyoxyethylene dodecyl ether (trade name "EMAL 2FG", manufactured by Kao Corporation, nonionic emulsifier) were used instead of 1.8 parts of tridecyloxyhexa(oxyethylene) phosphate sodium salt (anionic emulsifier). Next, separately from the above, 50 parts of an aqueous solution of 12% by weight sodium lauryl sulfate (trade name "EMAL 2FG", manufactured by Kao Corporation, anionic emulsifier) and 50 parts of octyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (trade name "Irganox 1135", manufactured by BASF, doubly hindered phenol-based antioxidant, molecular weight: 390, melting point: 10°C) were mixed and stirred at a temperature of 25°C to obtain an antioxidant dispersion (sodium lauryl sulfate concentration as emulsifier: 6% by weight, phenol-based antioxidant concentration: 50% by weight). Then, except for using the emulsion polymerization liquid and the antioxidant dispersion liquid obtained above, an acrylic rubber (A-4) was obtained in the same manner as in Example 1. The obtained acrylic rubber (A-4) was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0184] (Preparation of Acrylic Rubber Composition (1) and Acrylic Rubber Composition (2) for Evaluation) In addition, except for using the acrylic rubber (A-4) obtained above, an acrylic rubber composition for evaluation (1) and an acrylic rubber composition for evaluation (2) were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0185] [Example 5] (Production of Acrylic Rubber (A-5)) An acrylic rubber (A-5) was obtained in the same manner as in Example 1, except that 1.5 parts of vinyl chloroacetate was used instead of 1.5 parts of mono-n-butyl fumarate as the monomer component. The obtained acrylic rubber (A-5) was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0186] (Preparation of Acrylic Rubber Composition (1) for Evaluation) In addition, except for using the acrylic rubber (A-5) obtained above, an acrylic rubber composition (1) for evaluation was prepared and evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0187] (Preparation of Acrylic Rubber Composition (2) for Evaluation) A part of the acrylic rubber composition for evaluation (1) obtained above was transferred to a roll at 50 ° C., and 100 parts of the acrylic rubber (A-5) contained in the acrylic rubber composition for evaluation (1) was mixed with 3.0 parts of semi-hardened beef tallow fatty acid soda soap (product name "NS Soap", manufactured by Kao Corporation), 0.5 parts of stearic acid (product name "Non-Sal SK-1", manufactured by NOF Corporation), and 0.3 parts of sulfur (product name "Sulfax PMC", manufactured by Tsurumi Chemical Industry Co., Ltd.) and kneaded to obtain an acrylic rubber composition for evaluation (2). The acrylic rubber composition for evaluation (2) obtained was used to evaluate the elongation at break. The results are shown in Table 1.
[0188] [Example 6] (Production of Acrylic Rubber (A-6)) To the emulsion polymerization liquid obtained in the same manner as in Example 1, an antioxidant was added in the following manner. That is, the emulsion polymerization liquid obtained by the same method as in Example 1 was heated to 70°C, and 0.5 parts of octyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (product name "Irganox 1135", manufactured by BASF) was added to 100 parts of the rubber component in the emulsion polymerization liquid, and the mixture was thoroughly stirred to add an antioxidant. The emulsion polymerization liquid to which the antioxidant dispersion liquid was added thus obtained was coagulated and dried in the same manner as in Example 1 to obtain an acrylic rubber (A-6). The obtained acrylic rubber (A-6) was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0189] (Preparation of Acrylic Rubber Composition (1) and Acrylic Rubber Composition (2) for Evaluation) In addition, except for using the acrylic rubber (A-6) obtained above, an acrylic rubber composition for evaluation (1) and an acrylic rubber composition for evaluation (2) were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0190] [Example 7] (Production of Acrylic Rubber (A-7)) In obtaining the monomer emulsion, the amount of sodium lauryl sulfate used was 0.709 parts, and the amount of polyoxyethylene dodecyl ether used was 1.82 parts. Except for this, emulsion polymerization was carried out in the same manner as in Example 4 to obtain an emulsion polymerization liquid. Next, separately from the above, 50 parts of an aqueous solution of 12% by weight sodium lauryl sulfate (trade name "EMAL 2FG", manufactured by Kao Corporation, anionic emulsifier) and 50 parts of 4,6-bis(octylthiomethyl)-o-cresol (trade name "Irganox 1520L", manufactured by BASF, semi-hindered phenol-based antiaging agent, molecular weight: 425, melting point: 14°C) were mixed and stirred at a temperature of 30°C to obtain an antiaging agent dispersion (sodium lauryl sulfate concentration as emulsifier: 6% by weight, phenol-based antiaging agent concentration: 50% by weight). Then, except for using the emulsion polymerization liquid and antioxidant dispersion liquid obtained above, an acrylic rubber (A-7) was obtained in the same manner as in Example 1. The obtained acrylic rubber (A-7) was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0191] (Preparation of Acrylic Rubber Composition (1) and Acrylic Rubber Composition (2) for Evaluation) In addition, except for using the acrylic rubber (A-7) obtained above, an acrylic rubber composition for evaluation (1) and an acrylic rubber composition for evaluation (2) were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0192] [Example 8] (Manufacture of acrylic rubber (A-8)) The antioxidant dispersion was prepared under the following conditions. That is, 50 parts of a 12 wt % aqueous solution of sodium lauryl sulfate heated to 70°C and 50 parts of 3-(3,5-di-tert-butyl-4-hydroxyphenyl)stearyl propionate (product name "Irganox 1076", manufactured by BASF, doubly hindered phenol-based antioxidant, molecular weight: 561, melting point: 50 to 55°C) heated to 70°C were mixed and stirred under heating at 70°C to obtain an antioxidant dispersion (sodium lauryl sulfate concentration as emulsifier: 6 wt %, phenol-based antioxidant concentration: 50 wt %). Then, except for using the obtained antioxidant dispersion liquid, an acrylic rubber (A-8) was obtained in the same manner as in Example 4. The obtained acrylic rubber (A-8) was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0193] (Preparation of Acrylic Rubber Composition (1) and Acrylic Rubber Composition (2) for Evaluation) In addition, except for using the acrylic rubber (A-10) obtained above, an acrylic rubber composition for evaluation (1) and an acrylic rubber composition for evaluation (2) were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0194] [Comparative Example 1] (Production of Acrylic Rubber (A-9)) An emulsion polymerization liquid was obtained in the same manner as in Example 4, except that the amounts of ethyl acrylate, n-butyl acrylate, and mono-n-butyl fumarate used as monomer components were changed to 49.3 parts, 49.3 parts, and 1.4 parts, respectively, and that 2-methoxyethyl acrylate was not used.
[0195] In addition, when preparing the antioxidant dispersion, the antioxidant dispersion was obtained under the following conditions. That is, 50 parts of an aqueous solution of 0.2 wt % sodium lauryl sulfate and 50 parts of stearyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (trade name "Irganox 1076", manufactured by BASF, doubly hindered phenol-based antioxidant, molecular weight: 561, melting point: 50-55° C.) were mixed and stirred at a temperature of 25° C. to obtain an antioxidant dispersion (concentration of sodium lauryl sulfate as an emulsifier: 0.1 wt %, concentration of phenol-based antioxidant: 50 wt %). Note that the obtained antioxidant dispersion was one in which the dispersion of stearyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate as a phenol-based antioxidant was insufficient, and some of it was localized in the antioxidant dispersion. Then, except for using the emulsion polymerization liquid and the antioxidant dispersion liquid obtained above, an acrylic rubber (A-9) was obtained in the same manner as in Example 4. The obtained acrylic rubber (A-9) was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0196] (Preparation of Acrylic Rubber Composition (1) and Acrylic Rubber Composition (2) for Evaluation) In addition, except for using the acrylic rubber (A-9) obtained above, an acrylic rubber composition for evaluation (1) and an acrylic rubber composition for evaluation (2) were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0197] [Comparative Example 2] The antioxidant dispersion was prepared under the following conditions. That is, 50 parts of a 0.2 wt % aqueous solution of sodium lauryl sulfate salt and 50 parts of 4,4'-bis(α,α-dimethylbenzyl)diphenylamine (product name "Nocrac CD", manufactured by Ouchi Shinko Chemical Industry Co., Ltd., molecular weight: 405.58, melting point: 90°C or higher) were mixed and stirred at a temperature of 25°C to obtain an antioxidant dispersion (concentration of sodium lauryl sulfate as an emulsifier: 0.1 wt %, concentration of phenolic antioxidant: 50 wt %). Note that the obtained antioxidant dispersion was one in which the dispersion of 4,4'-bis(α,α-dimethylbenzyl)diphenylamine as a phenolic antioxidant was insufficient, and some of it was localized in the antioxidant dispersion. Then, except for using the antioxidant dispersion liquid obtained above, an acrylic rubber (A-10) was obtained in the same manner as in Example 1. The obtained acrylic rubber (A-10) was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0198] [Comparative Example 3] (Manufacture of Acrylic Rubber (A-11)) The antioxidant dispersion was prepared under the following conditions. That is, 50 parts of a 12 wt % aqueous solution of sodium lauryl sulfate and 50 parts of stearyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (product name "Irganox 1076", manufactured by BASF, doubly hindered phenol-based antioxidant, molecular weight: 561, melting point: 50 to 55° C.) were mixed and stirred at a temperature of 25° C. to obtain an antioxidant dispersion (sodium lauryl sulfate concentration as emulsifier: 6 wt %, phenol-based antioxidant concentration: 50 wt %). Then, except for using the obtained antioxidant dispersion liquid, an acrylic rubber (A-11) was obtained in the same manner as in Comparative Example 1. The obtained acrylic rubber (A-11) was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0199] (Preparation of Acrylic Rubber Composition (1) and Acrylic Rubber Composition (2) for Evaluation) In addition, except for using the acrylic rubber (A-11) obtained above, an acrylic rubber composition for evaluation (1) and an acrylic rubber composition for evaluation (2) were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0200] [Table 1]
[0201] As shown in Table 1, when an acrylic rubber containing a phenol-based antioxidant as an antioxidant and having a difference between the oxidation onset temperature and the glass transition temperature (Tg) measured by differential scanning calorimetry of 250°C or more is used, the generation of coloring and odor is suppressed, and the kneading processability and extrusion processability are excellent. Furthermore, the obtained cross-linked rubber has high breaking strength (Examples 1 to 8).
[0202] On the other hand, when the difference between the oxidation onset temperature and the glass transition temperature (Tg) was less than 250°C, or when no phenol-based antioxidant was used, such as when 4,4'-bis(α,α-dimethylbenzyl)diphenylamine was used instead of a phenol-based antioxidant, coloring and odor were generated, and the kneading processability and extrusion processability, as well as the breaking strength when made into a cross-linked rubber, were poor (Comparative Examples 1 to 3).
Claims
1. An acrylic rubber containing 50% by weight or more of (meth)acrylic acid ester monomer units, The antioxidant contains a double hindered phenol-based antioxidant, the content of each of the hindered phenol-based antioxidants is 0.1 to 5 parts by weight based on 100 parts by weight of the acrylic rubber component, The oxidation onset temperature measured by differential scanning calorimetry is 230°C to 350°C, a glass transition temperature (Tg) of −80° C. to 0° C.; An acrylic rubber having a difference between its oxidation onset temperature and its glass transition temperature (Tg) of 250°C or more as measured by differential scanning calorimetry.
2. 2. The acrylic rubber according to claim 1, wherein the molecular weights of both of the hindered phenol-based antioxidants are 470 or less.
3. The acrylic rubber according to claim 1 or 2, wherein the difference between the oxidation onset temperature and the glass transition temperature (Tg) is 265 to 370°C.
4. The acrylic rubber according to any one of claims 1 to 3, wherein the difference between the oxidation onset temperature and the glass transition temperature (Tg) is 270 to 350°C.
5. The (meth)acrylic acid ester monomer unit contains at least a (meth)acrylic acid alkoxyalkyl ester monomer unit, 5. The acrylic rubber according to claim 1, wherein the content of the (meth)acrylic acid alkoxyalkyl ester monomer units in all monomer units is 1 to 60% by weight.
6. A rubber composition comprising a rubber component containing the acrylic rubber according to any one of claims 1 to 5, a filler, and a crosslinking agent.
7. A cross-linked rubber product obtained by cross-linking the rubber composition according to claim 6.
8. A method for producing the acrylic rubber according to any one of claims 1 to 5, an emulsion polymerization step of emulsion-polymerizing a monomer component containing a (meth)acrylic acid ester in a proportion of 50% by weight or more in the presence of a polymerization catalyst to obtain an emulsion polymerization liquid; an antioxidant addition step of adding a doubly hindered phenol-based antioxidant to the emulsion polymerization liquid; a coagulation step of contacting the emulsion polymerization liquid containing the two hindered phenol-based antiaging agents added thereto, obtained in the antiaging agent adding step, with a coagulant to produce water-containing crumbs, The antioxidant addition step adding the two hindered phenol-based antioxidants to the emulsion polymerization liquid at a temperature equal to or higher than the melting points of the two hindered phenol-based antioxidants; or a step of bringing both hindered phenol-based antiaging agents into contact with an aqueous solution of an emulsifier at a temperature equal to or higher than the melting points of the both hindered phenol-based antiaging agents to obtain a dispersion, and then adding the both hindered phenol-based antiaging agents in the state of the dispersion to the emulsion polymerization liquid.
Citation Information
Patent Citations
Process for producing acrylic rubber, and acrylic rubber obtained by said production process
JP2019189835A
Process for producing acrylic rubber, and acrylic rubber, rubber composition and rubber cross-linked product obtained by said production process
JP2019189838A
Acrylic rubber and crosslinked rubber