Polyether polycarbonate diol and its manufacturing method
A polyether polycarbonate diol with controlled alkoxy and aryloxy end groups addresses handling issues and durability challenges in polyurethane production, enabling controlled polymerization and desired molecular weights for synthetic leather applications.
Patent Information
- Application Number
- JP2020125482
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-07
- Filing Date
- 2020-07-22
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-07-22
AI Technical Summary
Existing polyurethanes derived from polytetramethylene ether glycol have high melting points and viscosities, leading to handling difficulties, and those derived from polyether polycarbonate diol suffer from low durability and uncontrollable polymerization reactivity, making it difficult to achieve a weight average molecular weight of 200,000 for applications like synthetic leather.
A polyether polycarbonate diol is developed with a controlled ratio of alkoxy and aryloxy end groups within a specific range, allowing for controlled urethane polymerization and production of polyurethane with desired molecular weights.
The solution enables easy control of polymerization reactions, producing polyurethane with targeted molecular weights suitable for various applications, including synthetic leather, by suppressing rapid reaction rates and ensuring durability.
Smart Images

Figure 0007567247000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyether polycarbonate diol which is a raw material for polyurethane, polyurethane urea, etc., and a method for producing the same. The present invention also relates to a method for producing polyurethane using the polyether polycarbonate diol. [Background technology]
[0002] Polyurethane is used in a wide range of applications, including urethane foam, paint, adhesive, sealant, and elastomer. Polyurethane is composed of a hard segment composed of isocyanate and a chain extender, and a soft segment mainly composed of polyol. Polyol, one of the main raw materials of polyurethane, is classified into polyether polyol, polyester polyol, polycarbonate polyol, polybutadiene polyol, acrylic polyol, etc. depending on the difference in molecular chain structure, and a polyol is selected according to the required performance of polyurethane. Among polyether polyols, polytetramethylene ether glycol (hereinafter sometimes abbreviated as PTMG) has high crystallinity, so polyurethane obtained by reacting with isocyanates exhibits excellent abrasion resistance, hydrolysis resistance, and tear resistance. The main applications of such polyurethanes are spandex, thermoplastic elastomers, thermosetting elastomers, artificial leather, synthetic leather, etc.
[0003] Owing to these excellent properties, polyurethanes obtained from polytetramethylene ether glycol are used in a variety of applications; however, polytetramethylene ether glycol has a high melting point and viscosity, posing problems in terms of handleability, and in some applications, there is still room for improvement in the durability, such as the chemical resistance, of the obtained polyurethane.
[0004] In Patent Document 1, a methyl group is introduced into some of the side chains of the polymer units to make the polyether polyol amorphous, thereby obtaining a polyether polyol that is liquid at room temperature. Moreover, polyether polycarbonate diol (hereinafter sometimes abbreviated as PEPCD) produced from polytetramethylene ether glycol having a small molecular weight is known as a polyol that is liquid at room temperature (Patent Document 2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 120830 / 1983 [Patent Document 2] JP 2002-256069 A Summary of the Invention [Problem to be solved by the invention]
[0006] The polyurethane obtained from the polyether polyol of Patent Document 1 has a drawback in that it has low durability. According to the PEPCD of Patent Document 2, although durability is improved, it is difficult to control the urethane polymerization reactivity, and it is not possible to obtain polyurethane with a weight average molecular weight of about 200,000, which is used for synthetic leather and the like.
[0007] The present invention has been made in view of the above problems, and an object of the present invention is to provide a polyether polycarbonate diol that can be used to produce polyurethane having a weight average molecular weight of about 200,000 and that can be used for synthetic leather, etc., by a simple method. [Means for solving the problem]
[0008] The present inventors have conducted extensive research to solve the above problems and have found that by using a polyether polycarbonate diol in which the ratio of the total number of alkoxy terminal groups and aryloxy terminal groups to the total number of terminal groups is controlled within a suitable range, the urethane polymerization reaction can be easily controlled, a rapid polymerization reaction can be suppressed, and a polyurethane having a desired molecular weight can be obtained. The present invention has been achieved based on these findings, and has the following gist.
[0009] [1] A polyether polycarbonate diol in which the ratio of the total number of alkoxy terminal groups and aryloxy terminal groups to the total number of terminal groups is 0.20% or more and 7.5% or less.
[0010] [2] The polyether polycarbonate diol according to [1], wherein the alkoxy end groups contain methoxy end groups.
[0011] [3] The polyether polycarbonate diol according to [1] or [2], wherein the alkoxy end group contains a butoxy end group.
[0012] [4] The polyether polycarbonate diol according to any one of [1] to [3], having a hydroxyl value of 11 mg-KOH / g or more and 320 mg-KOH / g or less.
[0013] [5] The polyether polycarbonate diol according to any one of [1] to [4], wherein the polyether polycarbonate diol is mixed with methanol and a 25 wt% aqueous solution of sodium hydroxide, and the mixture is heated at 75°C for 30 minutes to hydrolyze the mixture, thereby obtaining a thermal decomposition product having a hydroxyl value of 220 mg-KOH / g or more and 750 mg-KOH / g or less.
[0014] [6] A method for producing the polyether polycarbonate diol according to any one of [1] to [5], comprising a step of reacting polytetramethylene ether glycol having a hydroxyl value of 220 mg-KOH / g or more and 750 mg-KOH / g or less with a carbonate compound.
[0015] [7] A method for producing polyurethane, comprising subjecting a raw material containing the polyether polycarbonate diol according to any one of [1] to [5] and a compound having a plurality of isocyanate groups to an addition polymerization reaction.
[0016] [8] The method for producing a polyurethane according to [7], wherein the polyurethane is a polyurethane elastomer.
[0017] [9] The method for producing a polyurethane according to [8], wherein the polyurethane elastomer is a polyurethane foam. Effect of the Invention
[0018] According to the polyether polycarbonate diol of the present invention, the polymerization reaction during the production of polyurethane can be easily controlled, and polyurethane having a desired molecular weight can be produced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, the embodiments of the present invention will be described in more detail, but the present invention is not limited to the embodiments described below as long as it does not depart from the gist of the present invention.
[0020] [Polyether polycarbonate diol] The polyether polycarbonate diol of the present invention (hereinafter sometimes abbreviated as "PEPCD") is characterized in that the ratio of the total number of alkoxy terminal groups and aryloxy terminal groups to the total number of terminal groups (hereinafter sometimes referred to as "terminal alkoxy / aryloxy ratio") is 0.20% or more and 7.5% or less.
[0021] In the present invention, the polyether polycarbonate diol refers to a "compound having a polyether polycarbonate repeating unit", and the polyether polycarbonate diol of the present invention usually has a polyether polycarbonate repeating unit and is constituted as a mixture of a plurality of compounds having different terminal groups.
[0022] PEPCD is produced by reacting a carbonate compound such as alkylene carbonate, dialkyl carbonate, diaryl carbonate, etc. with a polyether polyol compound, and, if necessary, with a diol compound different from the polyether polyol compound. In this reaction, the target product, PEPCD with hydroxyl groups at both ends, is produced as a by-product, along with alkoxy end groups resulting from the reaction of dialkyl carbonate with polyether polyol compound and aryloxy end groups resulting from the reaction of diaryl carbonate with polyether polyol compound (hereinafter, these alkoxy end groups and aryloxy end groups may be collectively referred to as "alkoxy / aryloxy end"). Furthermore, these alkoxy / aryloxy terminals may be carried into the reaction system as impurities in polyether polyol compounds such as PTMG used as raw materials for the production of PEPCD, and may become mixed into the resulting PEPCD. Furthermore, alkoxy / aryloxy ends are also introduced into PEPCD by heating during the purification process of PEPCD. The present inventors have discovered that by controlling the amount of alkoxy / aryloxy terminals generated as reaction by-products and / or contaminating the product as a result of being mixed into the raw material compounds and brought into the reaction system so that the terminal alkoxy / aryloxy ratio is 0.2% or more and 75% or less, it becomes easier to control the urethane polymerization reaction, and rapid polymerization reactions can be suppressed, making it possible to produce polyurethanes of the desired molecular weight suitable for various polyurethane applications.
[0023] <Terminal alkoxy / aryloxy ratio> In the PEPCD of the present invention, the ratio of the total number of alkoxy terminal groups and aryloxy terminal groups to the total number of terminal groups (terminal alkoxy / aryloxy ratio) is 0.20% to 7.5%. If the terminal alkoxy / aryloxy ratio exceeds 7.5%, the urethane polymerization reaction does not proceed sufficiently, while if the terminal alkoxy / aryloxy ratio is less than 0.20%, the urethane polymerization reaction rate becomes too fast, making it difficult to control the reaction, and in either case, a polyurethane with the desired molecular weight cannot be obtained. In the PEPCD of the present invention, the terminal alkoxy / aryloxy ratio is preferably 0.20% to 7.0%, more preferably 0.30% to 6.5%, further preferably 0.30% to 6.0%, and particularly preferably 0.40% to 5.5%.
[0024] The terminal alkoxy / aryloxy ratio of PEPCD is measured by the method described in the Examples section below.
[0025] <Alkoxy / aryloxy terminal> As described above, the alkoxy / aryloxy terminals contained in the PEPCD of the present invention are mainly derived from the polyether polyol compounds and carbonate compounds which are the raw materials for producing the PEPCD.
[0026] Examples of the alkoxy end group include a methoxy end, an ethoxy end, a propoxy end, and a butoxy end. From the viewpoint of PEPCD quality, the methoxy end or the butoxy end is preferable.
[0027] Specific examples of aryloxy end groups include substituted or unsubstituted phenoxy end groups.
[0028] The PEPCD of the present invention may contain only one of these alkoxy / aryloxy termini, or may contain two or more of them. When two or more types of alkoxy / aryloxy termini are contained, the total content of them is set to be within the above-mentioned range.
[0029] <Method for Controlling the Ratio of Terminal Alkoxy / Aryloxy> The method for controlling the ratio of terminal alkoxy / aryloxy of the PEPCD of the present invention is not particularly limited, but (1) A method of mixing a PEPCD containing an alkoxy / aryloxy terminal and a PEPCD not containing an alkoxy / aryloxy terminal (2) A method of adjusting the concentration of alkoxy / aryloxy terminals in a PEPCD containing alkoxy / aryloxy terminals by operations such as distillation and extraction (3) A method of controlling the content of alkoxy / aryloxy terminals in the polyether polyol compound, carbonate compound, and diol compound used as raw materials for PEPCD (4) A method of controlling the amount of alkoxy / aryloxy terminals as by-products generated by reaction during the production of PEPCD by adjusting the pH of the solution or the like and the like can be mentioned.
[0030] <Method for Producing PEPCD> The PEPCD of the present invention is produced by reacting a carbonate compound and a polyether polyol compound according to the usual method for producing PEPCD, except for controlling the ratio of the above terminal alkoxy / aryloxy. During the reaction, if necessary, a diol compound different from the polyether polyol compound may be copolymerized.
[0031] (Carbonate Compound) As the carbonate compound, alkylene carbonate, dialkyl carbonate, and diaryl carbonate can be used.
[0032] Examples of alkylene carbonate include ethylene carbonate, propylene carbonate, and butylene carbonate. Examples of dialkyl carbonate include symmetric dialkyl carbonates such as dimethyl carbonate, diethyl carbonate, and dibutyl carbonate, and asymmetric dialkyl carbonates such as methyl ethyl carbonate. Examples of diaryl carbonates include symmetric diaryl carbonates such as diphenyl carbonate and dinaphthyl carbonate, as well as asymmetric diaryl carbonates such as phenyl naphthyl carbonate. Also usable as the carbonate source are chlorocarbonates such as methyl chlorocarbonate and phenyl chlorocarbonate, phosgene and its equivalents, and carbon dioxide gas.
[0033] Among these, alkylene carbonates or dialkyl carbonates are preferred, ethylene carbonate and dimethyl carbonate are more preferred, and ethylene carbonate is even more preferred. The above carbonate compounds may be used alone or in combination of two or more.
[0034] (Polyether polyol compound) Polyether polyol compounds can be produced by ring-opening polymerization of cyclic ethers.
[0035] The cyclic ether generally has 2 to 10 carbon atoms, and preferably has 3 to 7 carbon atoms. Specific examples of cyclic ethers include tetrahydrofuran (THF), ethylene oxide, propylene oxide, oxetane, tetrahydropyran, oxepane, and 1,4-dioxane. Cyclic ethers in which a portion of the cyclic hydrocarbon chain is substituted with an alkyl group, a halogen atom, or the like can also be used. Specific examples include 3-methyl-tetrahydrofuran and 2-methyltetrahydrofuran. These cyclic ethers may be used alone or in combination of two or more, but it is preferable to use one type.
[0036] Specific polyether polyol compounds include low molecular weight polyether polyols such as diethylene glycol, triethylene glycol, tetraethylene glycol, and dipropylene glycol; polyethylene glycol, polypropylene glycol, copolymers of ethylene oxide and propylene oxide, polytetramethylene ether glycol (PTMG), copolymers of THF and 3-methyl-tetrahydrofuran, and dipropylene glycol polyethylene glycol, each having a number average molecular weight of 100 or more and 3,000 or less, determined from the hydroxyl groups.
[0037] Among these, PTMG having a hydroxyl value of 220 mg-KOH / g or more and 750 mg-KOH / g or less, particularly 280 mg-KOH / g or more and 700 mg-KOH / g or less, and particularly 370 mg-KOH / g or more and 660 mg-KOH / g or less, is preferred from the viewpoint of the tensile properties and durability of the resulting polyurethane. If the hydroxyl value of PTMG is 750 mg-KOH / g or less, the crystallinity and melting point of the resulting PEPCD can be suppressed. In addition, if the hydroxyl value of PTMG is 220 mg-KOH / g or more, the viscosity of the resulting PEPCD does not become too high, and the handling properties are excellent. In addition, it is preferable that the number average molecular weight (Mn) of this PTMG calculated from the hydroxyl groups is 100 to 3000, particularly 150 to 2000, and especially 200 to 850, from the viewpoint of the tensile properties and durability of the resulting polyurethane. If the number average molecular weight of PTMG is 100 or more, the crystallinity and melting point increase of the resulting PEPCD can be suppressed. In addition, if the number average molecular weight of PTMG is 3000 or less, the viscosity of the resulting PEPCD does not become too high, and the handling property is excellent.
[0038] Here, the hydroxyl value and the number average molecular weight (Mn) calculated from the hydroxyl value are measured, for example, by the following method. <Hydroxyl value / number average molecular weight> The hydroxyl value of a polyether polyol compound is measured by a method using an acetylation reagent in accordance with JIS K1557-1. From the measured hydroxyl value, the number average molecular weight (Mn) is calculated according to the following formula (I). Number average molecular weight = 2 × 56.1 / (hydroxyl value × 10 -3 ) …(I)
[0039] The THF used as the raw material for PTMG can be obtained by a conventionally known method. For example, there is a method in which diacetoxybutene, an intermediate obtained by carrying out an acetoxylation reaction using butadiene as raw materials, acetic acid, and oxygen, is obtained, and the diacetoxybutene is hydrogenated and hydrolyzed to obtain 1,4-butanediol, which is then cyclized and dehydrated; a method in which maleic acid, succinic acid, maleic anhydride, and / or fumaric acid are used as raw materials, and the resulting 1,4-butanediol is then cyclized and dehydrated; a method in which acetylene is used as raw material and contacted with an aqueous formaldehyde solution to obtain 1,4-butanediol, which is then cyclized and dehydrated; These include a method of obtaining 1,4-butanediol by cyclization and dehydration of the resulting 1,4-butanediol obtained by hydrogenating butynediol; a method of obtaining 1,4-butanediol by cyclization and dehydration of the resulting 1,4-butanediol obtained via the oxidation of propylene; a method of obtaining 1,4-butanediol by cyclization and dehydration of the resulting 1,4-butanediol obtained directly by fermentation of biomass such as sugar; and a method of obtaining 1,4-butanediol by decarbonylating and reducing furfural obtained from biomass.
[0040] (Diol Compound) When producing PEPCD, a diol compound other than the polyether polyol compound may be copolymerized as necessary. Examples of the diol compound include linear alkyl diols such as ethylene glycol, 1,3-propanediol, 2-methyl-1,3-propanediol, neopentyl glycol, 1,4-butanediol, 2-methyl-14-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, and 1,12-dodecanediol, and cyclic alkyl diols such as cyclohexanedimethanol and isosorbide. These other diol compounds may be used alone or in combination of two or more.
[0041] (Ratio of raw materials used) In the production of PEPCD, the amount of carbonate compound used is not particularly limited, but the molar ratio relative to 1 mole of polyether polyol compound is preferably 0.35 at the lower limit, more preferably 0.50, and even more preferably 0.60 at the upper limit, and more preferably 1.00, more preferably 0.98, and even more preferably 0.97 at the upper limit. If the amount of carbonate compound used is equal to or less than the upper limit, the proportion of PEPCD having terminal groups other than hydroxyl groups is suppressed, and the number average molecular weight is easily set within a predetermined range. If the amount of carbonate compound used is equal to or more than the lower limit, polymerization is easily allowed to proceed to a predetermined number average molecular weight.
[0042] When the above-mentioned other diol compounds are used, the amount of the other diol compounds used is, in terms of a molar ratio relative to 1 mole of the polyether polyol compound, preferably a lower limit of 0.05, more preferably 0.10, and even more preferably 0.20, and preferably an upper limit of 2.0, more preferably 1.0, and even more preferably 0.60. In this case, the amount of the carbonate compound used is preferably within the above-mentioned range in terms of a molar ratio relative to 1 mole of the total of the polyether polyol compound and the other diol compound.
[0043] (catalyst) In the production of PEPCD, it is preferable to use a catalyst used in the transesterification reaction, such as metals such as lithium, sodium, potassium, rubidium, cesium, magnesium, calcium, strontium, barium, zinc, aluminum, titanium, cobalt, germanium, tin, lead, antimony, and cerium, metal alkoxides, metal salts, and metal oxides, and preferably carbonates, carboxylates, borates, silicates, carbonates, oxides, and organometallic compounds of alkali metals, alkaline earth metals, zinc, titanium, and lead, and particularly preferably organotitanium compounds and organomagnesium compounds.
[0044] The amount of the transesterification catalyst used is usually preferably 10 μmol or more and 1500 μmol or less, more preferably 20 μmol or more, still more preferably 30 μmol or more, and particularly preferably 50 μmol or more, per 1 mol of the total of the starting polyether polyol compound and other diol compounds used as required. The upper limit is more preferably 1000 μmol, still more preferably 500 μmol, particularly preferably 300 μmol, and most preferably 200 μmol. If the amount of the catalyst is not less than the above lower limit, the reaction time can be shortened, the production efficiency can be increased, and the coloring of the obtained PEPCD can be suppressed. Also, if the amount of the catalyst is not more than the above upper limit, the coloring of PEPCD and the coloring during the production of polyurethane can be suppressed, and furthermore, the urethane polymerization reaction rate does not become too fast, and the reaction control tends to be facilitated.
[0045] (Reaction conditions) The reaction temperature during the production of PEPCD is usually 70 to 250°C, preferably 80 to 220°C. At the initial stage of the reaction, it is preferably around the boiling point of the starting carbonate compound, specifically 100 to 150°C, and as the reaction proceeds, the temperature is preferably gradually increased to further proceed the reaction. The reaction by-products such as alcohol and phenol are separated by distillation. At this time, when the starting carbonate compound is also distilled together with the distilled alcohol or the like and the loss is large, it is preferable to use a reactor equipped with a plate column or a packed column to suppress the loss amount. Also, in order to reduce the loss, the distilled starting carbonate compound may be recovered and recycled to the reaction system for use. When there is a loss of the starting carbonate compound, the theoretical molar ratio of the starting carbonate compound for the production of PEPCD to the polyether polyol compound or other diol compounds is (n + 1) mol of the polyether polyol compound or other diol compounds per n mol of the carbonate compound, but considering the loss, it is preferably 1.1 to 1.3 times the theoretical molar ratio. Incidentally, the polyether polyol compound or other diol compounds may be charged at the initial stage of the reaction or added during the process.
[0046] <Hydroxyl value, number average molecular weight, molecular weight distribution of PEPCD> The hydroxyl value of the PEPCD of the present invention is not particularly limited, but the lower limit of the hydroxyl value is usually 11 mg-KOH / g, preferably 22.4 mg-KOH / g, more preferably 28.1 mg-KOH / g, and even more preferably 37.4 mg-KOH / g, and the upper limit is usually 320 mg-KOH / g, preferably 187.0 mg-KOH / g, more preferably 140.3 mg-KOH / g, and even more preferably 112.2 mg-KOH / g. If the hydroxyl value is equal to or higher than the lower limit, the viscosity does not become too high, and handling tends to be easy when the PEPCD is used as a raw material to produce a polyurethane, and if it is equal to or lower than the upper limit, the flexibility of the resulting polyurethane tends to be good.
[0047] In addition, when the PEPCD of the present invention is mixed with methanol and a 25 wt% aqueous sodium hydroxide solution and heated at 75°C for 30 minutes to hydrolyze, the hydroxyl value of the resulting hydrolyzate is preferably 220 mg-KOH / g or more and 750 mg-KOH / g or less. If the hydroxyl value of the hydrolyzate is 220 mg-KOH / g or more, the PEPCD is prevented from increasing in crystallinity and melting point. On the other hand, if the hydroxyl value of the hydrolyzate is 750 mg-KOH / g or less, the PEPCD does not become too viscous and is excellent in handleability. From these viewpoints, the hydroxyl value of the hydrolyzate is more preferably 280 mg-KOH / g or more, even more preferably 370 mg-KOH / g or more, more preferably 700 mg-KOH / g or less, and even more preferably 660 mg-KOH / g or less. A specific method for hydrolyzing PEPCD is as described in the Examples section below.
[0048] The molecular weight of the PEPCD of the present invention is not particularly limited, but preferably the number average molecular weight (Mn) calculated from the hydroxyl groups has a lower limit of usually 600, preferably 800, more preferably 1000, and an upper limit of usually 5000, preferably 4000, more preferably 3000. If the number average molecular weight (Mn) of the PEPCD is 600 or more, the flexibility of the resulting polyurethane is sufficient, and if it is 5000 or less, the viscosity is not too high and handling is excellent.
[0049] Here, the hydroxyl value of PEPCD and its hydrolysate, and the number average molecular weight (Mn) of PEPCD are measured in the same manner as the hydroxyl value and number average molecular weight (Mn) of the polyether polyol compound described above.
[0050] The molecular weight distribution (Mw / Mn) of the PEPCD of the present invention is usually 1 or more, preferably 1.2 or more, more preferably 1.5 or more, while the upper limit is usually 3 or less, preferably 2.5 or less, more preferably 2.2 or less. If the molecular weight distribution is 3 or less, the increase in high molecular weight and the increase in viscosity are suppressed, and the polyurethane has excellent handleability and various polyurethane physical properties such as tensile strength tend to be good. On the other hand, the lower limit of the molecular weight distribution is usually 1 or more. Here, the molecular weight distribution of PEPCD is a value measured by the following method.
[0051] <Molecular weight distribution (Mw / Mn)> After preparing a solution of PEPCD in tetrahydrofuran, the weight average molecular weight (Mw) was measured using gel permeation chromatography (GPC) [Tosoh Corporation, product name "HLC-8220", column: TskgelSuperHZM-N (4 columns)], and the value (Mw / Mn) obtained by dividing the weight average molecular weight (Mw) by the number average molecular weight (Mn) was used as the molecular weight distribution of PEPCD. For calibration of the GPC, a POLYTETRAHYDROFURAN calibration kit from POLYMER LABORATORIES, UK, was used.
[0052] <Additives> Various additives can be added to the PEPCD of the present invention, if necessary. For example, an antioxidant can be added to the PEPCD of the present invention in order to suppress deterioration due to oxidation. In this case, the antioxidant is added so that the concentration of the antioxidant in the PEPCD after the addition of the antioxidant is usually 10 ppm by weight or more, preferably 50 ppm by weight or more, more preferably 100 ppm by weight or more, and usually 1000 ppm by weight or less, preferably 500 ppm by weight or less, more preferably 300 ppm by weight or less. If the antioxidant concentration is equal to or lower than the upper limit, the problem of clogging due to solid precipitation in the process can be suppressed, whereas if the antioxidant concentration is equal to or higher than the lower limit, the effect of preventing oxidation reactions is sufficient. As the antioxidant, 2,6-di-tert-butyl-p-cresol (BHT) is preferred from the viewpoints of effectiveness and stability.
[0053] [Uses of PEPCD] The PEPCD of the present invention is useful as a raw material for polyurethane suitable for applications such as elastic fibers, thermoplastic polyurethanes, and coating materials, due to its excellent controllability in urethane polymerization reactions. In such applications, a polyurethane solution or a water-based polyurethane emulsion can be produced from the PEPCD of the present invention and used. Uses of the PEPCD of the present invention are discussed further below. By modifying the terminals, the PEPCD of the present invention can be used as a raw material for UV-curable paints, electron beam-curable paints, plastic coatings, molding agents for lenses, sealants, adhesives, and the like. The PEPCD of the present invention can be used to disperse nanomaterials such as nanofiber cellulose, carbon nanofibers, and metal nanoparticles.
[0054] <Water-based polyurethane emulsion> When producing an aqueous polyurethane emulsion using the PEPCD of the present invention, when producing a prepolymer by reacting a polyol containing the PEPCD of the present invention with an excess of polyisocyanate, a compound having at least one hydrophilic functional group and at least two isocyanate-reactive groups is mixed to form a prepolymer, and the aqueous polyurethane emulsion can be produced through a neutralization / salt process of the hydrophilic functional groups, an emulsification process by adding water, and a chain extension reaction process.
[0055] The hydrophilic functional group of the compound having at least one hydrophilic functional group and at least two isocyanate-reactive groups used herein is, for example, a carboxyl group or a sulfonic acid group, which is a group that can be neutralized with an alkaline group. The isocyanate-reactive group is a group that generally reacts with isocyanate to form a urethane bond or a urea bond, such as a hydroxyl group, a primary amino group, or a secondary amino group, and these may be mixed in the same molecule.
[0056] Specific examples of compounds having at least one hydrophilic functional group and at least two isocyanate-reactive groups include 2,2'-dimethylolpropionic acid, 2,2-methylolbutyric acid, and 2,2'-dimethylolvaleric acid. In addition, diaminocarboxylic acids such as lysine, cystine, and 3,5-diaminocarboxylic acid can also be mentioned. These can be used alone or in combination of two or more. When actually using these, they can be neutralized with amines such as trimethylamine, triethylamine, tri-n-propylamine, tributylamine, and triethanolamine, or alkaline compounds such as sodium hydroxide, potassium hydroxide, and ammonia.
[0057] In producing a water-based polyurethane emulsion, the amount of the compound having at least one hydrophilic functional group and at least two isocyanate-reactive groups is preferably 1% by weight, more preferably 5% by weight, and even more preferably 10% by weight based on the total weight of the PEPCD of the present invention and other polyols in order to improve the dispersibility in water, while the upper limit is preferably 50% by weight, more preferably 40% by weight, and even more preferably 30% by weight in order to maintain the properties of the polycarbonate diol.
[0058] When producing an aqueous polyurethane emulsion, the reaction may be carried out in the prepolymer step in the presence of a solvent such as methyl ethyl ketone, acetone, or N-methyl-2-pyrrolidone, or may be carried out without a solvent. When a solvent is used, it is preferable to remove the solvent by distillation after producing the aqueous emulsion.
[0059] When an aqueous polyurethane emulsion is produced without a solvent using the PEPCD of the present invention as a raw material, the upper limit of the number average molecular weight calculated from the hydroxyl value of the PEPCD used is preferably 5000, more preferably 4500, and even more preferably 4000. The lower limit of the number average molecular weight of the PEPCD is preferably 300, more preferably 500, and even more preferably 800. If the number average molecular weight calculated from the hydroxyl value is within the above range, emulsification tends to be easier.
[0060] In addition, during synthesis or storage of the aqueous polyurethane emulsion, emulsion stability may be maintained by using in combination an anionic surfactant, such as a higher fatty acid, a resin acid, an acidic fatty alcohol, a sulfate ester, a higher alkyl sulfonate, an alkylaryl sulfonate, a sulfonated castor oil, or a sulfosuccinate; a cationic surfactant, such as a primary amine salt, a secondary amine salt, a tertiary amine salt, a quaternary amine salt, or a pyridinium salt; or a nonionic surfactant, such as a known reaction product of ethylene oxide with a long-chain fatty alcohol or a phenol.
[0061] In addition, when preparing a water-based polyurethane emulsion, the emulsion can also be produced by mechanically mixing water with an organic solvent solution of the prepolymer under high shear in the presence of an emulsifier, if necessary, without the neutralization / salting step.
[0062] The water-based polyurethane emulsions produced in this way can be used for a variety of purposes. In particular, in light of the recent demand for chemical raw materials with a low environmental impact, they can be used as a replacement for conventional products that do not use organic solvents.
[0063] Specific applications of the aqueous polyurethane emulsion include, for example, coating agents, aqueous paints, adhesives, synthetic leather, and artificial leather. In particular, the aqueous polyurethane emulsion produced using the PEPCD of the present invention is flexible and can be used more effectively as a coating agent, etc., since the PEPCD contains alkoxy / aryloxy terminals so that the PEPCD has a predetermined terminal alkoxy / aryloxy ratio, compared with aqueous polyurethane emulsions using conventional polycarbonate diol or PTMG. In particular, compared with aqueous polyurethane emulsions using conventional PTMG, the PEPCD of the present invention has a hydrophilic group, has good affinity with water, and can use a higher molecular weight PEPCD of the present invention, so that softness and transparency can be imparted to coating films, synthetic leather, artificial leather, etc. In addition, since the aqueous polyurethane emulsion has excellent dispersibility in water, the degree of freedom in molecular design of the aqueous polyurethane emulsion is increased, and it is possible to produce a matte finish by adjusting the composition.
[0064] The storage stability of the polyurethane solution and water-based polyurethane emulsion produced using the PEPCD of the present invention using an organic solvent and / or water can be measured by adjusting the concentration of polyurethane in the solution or emulsion (hereinafter sometimes referred to as "solid content concentration") to 1 to 80% by weight, storing the solution or emulsion under specific temperature conditions, and then visually checking for changes in the solution or emulsion. For example, in the case of a polyurethane solution (N,N-dimethylformamide / toluene mixture, solid content concentration 30% by weight) produced using the PEPCD of the present invention, 4,4'-dicyclohexylmethane diisocyanate, and isophorone diamine by the above-mentioned two-stage method, the period during which no changes are observed visually in the polyurethane solution when stored at 10°C is preferably 1 month, more preferably 3 months or more, and even more preferably 6 months or more.
[0065] [Polyurethane manufacturing method] The method for producing a polyurethane of the present invention is a method for producing a polyurethane (hereinafter, sometimes referred to as "the polyurethane of the present invention") by addition polymerization reaction of a raw material containing the PEPCD of the present invention and a compound having multiple isocyanate groups (hereinafter, sometimes referred to as "polyisocyanate compound" or "polyisocyanate"). The method for producing a polyurethane of the present invention is characterized by using the PEPCD of the present invention, and the polyurethane of the present invention can usually be produced by a conventional polyurethane reaction except for using the PEPCD of the present invention, a polyisocyanate compound, and a chain extender.
[0066] For example, the polyurethane of the present invention can be produced by reacting the PEPCD of the present invention with a polyisocyanate compound and a chain extender at a temperature in the range of from room temperature to 200°C. Alternatively, the polyurethane of the present invention can be produced by first reacting the PEPCD of the present invention with an excess of a polyisocyanate compound to produce a prepolymer having an isocyanate group at its terminal, and then increasing the degree of polymerization using a chain extender.
[0067] <Polyisocyanate compounds> The polyisocyanate compound used as a raw material for producing the polyurethane of the present invention may be any compound having two or more isocyanate groups, and examples of such compounds include various known aliphatic, alicyclic, or aromatic polyisocyanate compounds.
[0068] For example, aliphatic diisocyanate compounds such as tetramethylene diisocyanate, hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, and dimer diisocyanate in which the carboxyl groups of dimer acid are converted to isocyanate groups; alicyclic diisocyanate compounds such as 1,4-cyclohexane diisocyanate, isophorone diisocyanate, 1-methyl-2,4-cyclohexane diisocyanate, 1-methyl-2,6-cyclohexane diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, and 1,3-bis(isocyanatemethyl)cyclohexane; xylylene diisocyanate, 4,4'-di Examples of the aromatic diisocyanate include aromatic diisocyanate compounds such as phenyl diisocyanate, toluene diisocyanate (2,4-toluene diisocyanate, 2,6-toluene diisocyanate), m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl diisocyanate, dialkyl diphenylmethane diisocyanate, tetraalkyl diphenylmethane diisocyanate, 1,5-naphthylene diisocyanate, 3,3'-dimethyl-4,4'-biphenylene diisocyanate, polymethylene polyphenyl isocyanate, phenylene diisocyanate, and m-tetramethylxylylene diisocyanate. These may be used alone or in combination of two or more.
[0069] Among these, aromatic polyisocyanate compounds are preferred because of their reactivity with PEPCD and the high curability of the resulting polyurethane. In particular, 4,4'-diphenylmethane diisocyanate (hereinafter sometimes referred to as "MDI"), toluene diisocyanate (TDI), and xylylene diisocyanate are preferred because they are available industrially in large quantities at low cost.
[0070] <Chain extender> The chain extender used as a raw material for producing the polyurethane of the present invention is a low molecular weight compound having at least two active hydrogens that react with an isocyanate group, and is selected from polyols and polyamines.
[0071] Specific examples thereof include linear diols such as ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, and 1,12-dodecanediol; 2-methyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 2,2-diethyl-1,3-propanediol, 2-methyl-2-propyl-1,3-propanediol, and 2,4-heptanediol. Diols having branched chains such as diol, 1,4-dimethylolhexane, 2-ethyl-1,3-hexanediol, 2,2,4-trimethyl-1,3-pentanediol, 2-methyl-1,8-octanediol, 2-butyl-2-ethyl-1,3-propanediol, and dimer diol; diols having ether groups such as diethylene glycol and propylene glycol; diols having alicyclic structures such as 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, and 1,4-dihydroxyethylcyclohexane. diols having an aromatic group such as xylylene glycol, 1,4-dihydroxyethylbenzene, 4,4'-methylenebis(hydroxyethylbenzene); polyols such as glycerin, trimethylolpropane, pentaerythritol; hydroxyamines such as N-methylethanolamine, N-ethylethanolamine; ethylenediamine, 1,3-diaminopropane, hexamethylenediamine, triethylenetetramine, diethylenetriamine, isophoronediamine, 4,4'-diamino polyamines such as dicyclohexylmethane, 2-hydroxyethylpropylenediamine, di-2-hydroxyethylethylenediamine, di-2-hydroxyethylpropylenediamine, 2-hydroxypropylethylenediamine, di-2-hydroxypropylethylenediamine, 4,4'-diphenylmethanediamine, methylenebis(o-chloroaniline), xylylenediamine, diphenyldiamine, tolylenediamine, hydrazine, piperazine, and N,N'-diaminopiperazine; and the like.
[0072] These chain extenders may be used alone or in combination of two or more.
[0073] Among these, ethylene glycol, 1,4-butanediol, and 1,6-hexanediol are preferred because they provide excellent phase separation between the soft and hard segments of the resulting polyurethane, resulting in excellent flexibility and elastic recovery, and because they are available in large quantities industrially at low cost.
[0074] <Chain stopper> When producing the polyurethane of the present invention, a chain terminator having one active hydrogen group can be used as necessary for the purpose of controlling the molecular weight of the resulting polyurethane. Examples of these chain terminators include aliphatic monools having one hydroxyl group, such as methanol, ethanol, propanol, butanol, and hexanol, and aliphatic monoamines having one amino group, such as diethylamine, dibutylamine, n-butylamine, monoethanolamine, diethanolamine, and morpholine. These may be used alone or in combination of two or more.
[0075] <Catalyst> In the polyurethane-forming reaction when producing the polyurethane of the present invention, known urethane polymerization catalysts such as amine catalysts such as triethylamine, N-ethylmorpholine, triethylenediamine, etc., acid catalysts such as acetic acid, phosphoric acid, sulfuric acid, hydrochloric acid, sulfonic acid, etc., tin compounds such as trimethyltin laurate, dibutyltin dilaurate, dioctyltin dilaurate, dioctyltin dineodecane, etc., and further organometallic salts such as titanium compounds can also be used. The urethane polymerization catalysts may be used alone or in combination of two or more.
[0076] <Polyol other than PEPCD of the present invention> In the polyurethane forming reaction when producing the polyurethane of the present invention, a polyol other than the PEPCD of the present invention may be used in combination as necessary. Here, the polyol other than the PEPCD of the present invention is not particularly limited as long as it is one used in normal polyurethane production, and examples thereof include polyester polyol, polycaprolactone polyol, polycarbonate polyol, and polyether polyol. Among these, polyether polyol is preferred, and polytetramethylene ether glycol, which can obtain urethane properties similar to those of PEPCD, is particularly preferred. Here, the weight ratio of the PEPCD of the present invention to the combined weight of the PEPCD of the present invention and the other polyol is preferably 30% or more, more preferably 50% or more, and even more preferably 90% or more. If the weight ratio of the PEPCD of the present invention is the above lower limit or more, the controllability of the urethane polymerization reaction and the flexibility of the obtained polyurethane are good.
[0077] <Method of manufacturing polyurethane> As a method for producing the polyurethane of the present invention using the above-mentioned reactants, a production method generally used in experiments or industrially can be used. Examples of such a method include a method in which the PEPCD of the present invention, other polyols that are used as necessary, a polyisocyanate compound, and a chain extender are mixed together and reacted (hereinafter, sometimes referred to as a "one-step method"), and a method in which the PEPCD of the present invention, other polyols that are used as necessary, and a polyisocyanate compound are first reacted to prepare a prepolymer having isocyanate groups at both ends, and then the prepolymer is reacted with a chain extender (hereinafter, sometimes referred to as a "two-step method").
[0078] The two-stage method involves a step of preparing an intermediate having isocyanates at both ends of the part corresponding to the soft segment of polyurethane by reacting the PEPCD of the present invention and another polyol with at least one equivalent of a polyisocyanate compound in advance. In this way, if a prepolymer is prepared and then reacted with a chain extender, it may be easy to adjust the molecular weight of the soft segment part, and this is useful when it is necessary to ensure phase separation of the soft segment and the hard segment.
[0079] (One step method) The one-stage method, also called the one-shot method, is a method in which the PEPCD of the present invention, other polyol, polyisocyanate compound and chain extender are charged all at once to carry out the reaction. The amount of the polyisocyanate compound used in the one-stage process is not particularly limited, but when the total number of hydroxyl groups in the PEPCD of the present invention and the other polyol and the total number of hydroxyl groups and amino groups in the chain extender are taken as 1 equivalent, the lower limit is preferably 0.7 equivalents, more preferably 0.8 equivalents, even more preferably 0.9 equivalents, and particularly preferably 0.95 equivalents, and the upper limit is preferably 3.0 equivalents, more preferably 2.0 equivalents, even more preferably 1.5 equivalents, and particularly preferably 1.1 equivalents.
[0080] When the amount of the polyisocyanate compound used is equal to or less than the upper limit, unreacted isocyanate groups do not undergo a side reaction, and the viscosity of the resulting polyurethane does not become too high, making it difficult to handle, or the flexibility does not decrease. When the amount is equal to or more than the lower limit, the molecular weight of the polyurethane tends to be sufficiently large, and sufficient strength tends to be obtained.
[0081] The amount of the chain extender used is not particularly limited, but when the total number of hydroxyl groups of the PEPCD of the present invention and the other polyols is subtracted from the number of isocyanate groups of the polyisocyanate compound to form 1 equivalent, the lower limit is preferably 0.7 equivalents, more preferably 0.8 equivalents, even more preferably 0.9 equivalents, and particularly preferably 0.95 equivalents, and the upper limit is preferably 3.0 equivalents, more preferably 2.0 equivalents, even more preferably 1.5 equivalents, and particularly preferably 1.1 equivalents. If the amount of the chain extender used is below the above upper limit, the polyurethane obtained tends to be easily soluble in a solvent and easy to process, and if it is above the above lower limit, the polyurethane obtained is not too soft, and sufficient strength, hardness, elastic recovery performance, and elastic retention performance are obtained, and heat resistance is also good.
[0082] (Two step method) The two-stage method is also called the prepolymer method, and mainly includes the following methods. (a) A method in which the PEPCD of the present invention, the other polyol, and an excess of a polyisocyanate compound are reacted in advance at a reaction equivalent ratio of polyisocyanate compound / (PEPCD of the present invention and the other polyol) of from more than 1 to 10.0 or less to produce a prepolymer having isocyanate groups at the molecular chain terminals, and then a chain extender is added to the prepolymer to produce a polyurethane. (b) A method in which a polyisocyanate compound is reacted in advance with an excess of the PEPCD of the present invention and another polyol at a reaction equivalent ratio of the polyisocyanate compound / (PEPCD of the present invention and another polyol) of 0.1 or more and less than 1.0 to produce a prepolymer having hydroxyl groups at the molecular chain ends, and then a polyisocyanate compound having isocyanate groups at the ends is reacted as a chain extender to produce a polyurethane.
[0083] The two-stage process can be carried out in the absence of a solvent or in the presence of a solvent. The two-stage polyurethane production can be carried out by any one of the following methods (1) to (3). (1) Without using a solvent, a polyisocyanate compound is first reacted directly with the PEPCD of the present invention and another polyol to synthesize a prepolymer, which is then used as is in the chain extension reaction. (2) A prepolymer is synthesized by the method in (1), then dissolved in a solvent and used in the subsequent chain extension reaction. (3) A solvent is used from the beginning, and a polyisocyanate compound, the PEPCD of the present invention, and other polyols are reacted, followed by a chain extension reaction.
[0084] In the case of method (1), it is important to obtain the polyurethane in the coexistence with the solvent during the chain extension reaction by, for example, dissolving the chain extender in the solvent or dissolving the prepolymer and the chain extender in the solvent at the same time. The amount of the polyisocyanate compound used in the two-stage process (a) is not particularly limited, but when the total number of hydroxyl groups in the PEPCD of the present invention and the other polyol is taken as 1 equivalent, the lower limit in terms of the number of isocyanate groups is preferably an amount exceeding 1.0 equivalent, more preferably 1.2 equivalents, and even more preferably 1.5 equivalents, and the upper limit is preferably in the range of 10.0 equivalents, more preferably 5.0 equivalents, and even more preferably 3.0 equivalents.
[0085] When the amount of this polyisocyanate compound used is equal to or less than the above upper limit, there is a tendency that side reactions due to excess isocyanate groups are suppressed and it is easy to achieve the desired physical properties of the polyurethane. When the amount is equal to or more than the above lower limit, the molecular weight of the obtained polyurethane can be sufficiently increased to improve the strength and thermal stability. The amount of the chain extender used is not particularly limited, but the lower limit is preferably 0.1 equivalents, more preferably 0.5 equivalents, and even more preferably 0.8 equivalents, and the upper limit is preferably 5.0 equivalents, more preferably 3.0 equivalents, and even more preferably 2.0 equivalents, relative to 1 equivalent of the number of isocyanate groups contained in the prepolymer.
[0086] When the chain extension reaction is carried out, monofunctional organic amines or alcohols may be coexisted for the purpose of adjusting the molecular weight. The amount of polyisocyanate compound used in preparing a prepolymer having a hydroxyl group at its terminal in the two-stage process (b) is not particularly limited, but when the total number of hydroxyl groups in the PEPCD of the present invention and the other polyol is taken as 1 equivalent, the lower limit in terms of the number of isocyanate groups is preferably 0.1 equivalent, more preferably 0.5 equivalent, and even more preferably 0.7 equivalent, and the upper limit is preferably 0.99 equivalent, more preferably 0.98 equivalent, and even more preferably 0.97 equivalent.
[0087] When the amount of this polyisocyanate compound used is equal to or more than the above lower limit, the process until the desired molecular weight is obtained by the subsequent chain extension reaction is not too long, and production efficiency tends to be good. When the amount is equal to or less than the above upper limit, the viscosity is prevented from becoming too high, which reduces the flexibility of the obtained polyurethane or makes it difficult to handle, resulting in poor productivity. The amount of chain extender used is not particularly limited, but when the total number of hydroxyl groups of the PEPCD of the present invention and the other polyol used in the prepolymer is taken as 1 equivalent, the total equivalent including the equivalent of the isocyanate groups used in the prepolymer is preferably 0.7 equivalents at the lower limit, more preferably 0.8 equivalents, and even more preferably 0.9 equivalents at the upper limit, and is preferably less than 1.0 equivalent, more preferably 0.99 equivalents, and even more preferably 0.98 equivalents.
[0088] When the chain extension reaction is carried out, monofunctional organic amines or alcohols may be coexisted for the purpose of adjusting the molecular weight. The chain extension reaction is usually carried out at 0°C to 250°C, but this temperature varies depending on the amount of solvent, the reactivity of the raw materials used, the reaction equipment, etc., and is not particularly limited. If the temperature is above the lower limit above, the reaction proceeds quickly and the solubility of the raw materials and polymers is high, so the production time is shortened. If the temperature is below the upper limit above, side reactions and decomposition of the resulting polyurethane can be suppressed. The chain extension reaction may be carried out under reduced pressure while degassing.
[0089] In addition, a catalyst, a stabilizer, etc. may be added to the chain extension reaction, if necessary. Examples of catalysts include compounds such as triethylamine, tributylamine, dibutyltin dilaurate, stannous octoate, acetic acid, phosphoric acid, sulfuric acid, hydrochloric acid, and sulfonic acid, and may be used alone or in combination of two or more. Examples of stabilizers include compounds such as 2,6-dibutyl-4-methylphenol, distearyl thiodipropionate, N,N'-di-2-naphthyl-1,4-phenylenediamine, and tris(dinonylphenyl)phosphite, and may be used alone or in combination of two or more. In addition, when the chain extender is a highly reactive one such as a short-chain aliphatic amine, the reaction may be carried out without adding a catalyst. In addition, a reaction inhibitor such as tris(2-ethylhexyl) phosphite can also be used.
[0090] <Additives> Various additives such as heat stabilizers, light stabilizers, colorants, fillers, stabilizers, ultraviolet absorbers, antioxidants, anti-tack agents, flame retardants, antioxidants, and inorganic fillers can be added or mixed into the polyurethane of the present invention, as long as the properties of the polyurethane are not impaired.
[0091] Examples of compounds that can be used as heat stabilizers include aliphatic, aromatic, or alkyl group-substituted aromatic esters of phosphoric acid and phosphorous acid, hypophosphorous acid derivatives, phosphorus compounds such as phenylphosphonic acid, phenylphosphinic acid, diphenylphosphonic acid, polyphosphonates, dialkyl pentaerythritol diphosphites, and dialkyl bisphenol A diphosphites; phenol derivatives, particularly hindered phenol compounds; sulfur-containing compounds such as thioethers, dithioacid salts, mercaptobenzimidazoles, thiocarbanilides, and thiodipropionic acid esters; and tin compounds such as tin maleates and dibutyltin monoxide.
[0092] Specific examples of the hindered phenol compound include "Irganox1010" (product name: manufactured by BASF Japan Ltd.), "Irganox1520" (product name: manufactured by BASF Japan Ltd.), and "Irganox245" (product name: manufactured by BASF Japan Ltd.). Examples of phosphorus compounds include "PEP-36", "PEP-24G", and "HP-10" (all trade names: manufactured by ADEKA Corporation), and "Irgafos 168" (trade name: manufactured by BASF Japan Ltd.).
[0093] Specific examples of the sulfur-containing compound include thioether compounds such as dilauryl thiopropionate (DLTP) and distearyl thiopropionate (DSTP). Examples of light stabilizers include benzotriazole-based and benzophenone-based compounds. Specifically, usable products include "TINUVIN622LD" and "TINUVIN765" (both manufactured by Chiba Specialty Chemicals Co., Ltd.), "SANOL LS-2626" and "SANOL LS-765" (both manufactured by Sankyo Co., Ltd.).
[0094] Examples of ultraviolet absorbents include "TINUVIN328" and "TINUVIN234" (both manufactured by Chiba Specialty Chemicals Co., Ltd.).
[0095] Examples of colorants include dyes such as direct dyes, acid dyes, basic dyes, and metal complex dyes; inorganic pigments such as carbon black, titanium oxide, zinc oxide, iron oxide, and mica; and organic pigments such as coupling azo pigments, condensed azo pigments, anthraquinone pigments, thioindigo pigments, dioxazone pigments, and phthalocyanine pigments.
[0096] Examples of the inorganic filler include short glass fibers, carbon fibers, alumina, talc, graphite, melamine, and clay.
[0097] Examples of flame retardants include additive and reactive flame retardants such as phosphorus and halogen-containing organic compounds, bromine or chlorine-containing organic compounds, ammonium polyphosphate, aluminum hydroxide, and antimony oxide.
[0098] These additives may be used alone, or two or more of them may be used in any combination and in any ratio.
[0099] The amount of these additives added, in terms of weight ratio to polyurethane, has a lower limit of preferably 0.01% by weight, more preferably 0.05% by weight, and even more preferably 0.1% by weight, and an upper limit of preferably 10% by weight, more preferably 5% by weight, and even more preferably 1% by weight. If the amount of the additives added is equal to or greater than the lower limit, the additives can fully exert their effect, and if the amount is equal to or less than the upper limit, there is no risk of precipitation or turbidity occurring in the polyurethane.
[0100] <Molecular weight of polyurethane> The molecular weight of the polyurethane of the present invention is appropriately adjusted depending on the application, and is not particularly limited, but is preferably 50,000 to 400,000, and more preferably 100,000 to 300,000, in terms of polystyrene equivalent weight average molecular weight (Mw) measured by GPC. If Mw is equal to or higher than the lower limit, sufficient strength and hardness are obtained, and if it is equal to or lower than the upper limit, there is a tendency for excellent handleability, such as processability, to be obtained.
[0101] <Applications of polyurethane> The polyurethane of the present invention has excellent solvent resistance and good flexibility and mechanical strength, and therefore can be widely used in foams, elastomers, elastic fibers, paints, fibers, pressure-sensitive adhesives, adhesives, flooring materials, sealants, medical materials, artificial leather, synthetic leather, coating agents, water-based polyurethane paints, active energy radiation-curable polymer compositions, and the like.
[0102] In particular, when the polyurethane of the present invention is used for applications such as artificial leather, synthetic leather, moisture-permeable waterproof cloth, waterproof cloth, water-based polyurethane, adhesive, elastic fiber, medical material, flooring material, paint, coating agent, etc., it has a good balance of solvent resistance, flexibility, and mechanical strength, and therefore can impart good properties such as high durability in areas that come into contact with human skin or where cosmetic agents or disinfectant alcohol are used, sufficient flexibility, and resistance to physical impact, etc. In addition, it can be suitably used for automotive applications requiring heat resistance and outdoor applications requiring weather resistance.
[0103] The polyurethane of the present invention can be used for polyurethane elastomers, such as cast polyurethane elastomers.Specific applications include rolls such as rolling mill rolls, papermaking rolls, office equipment, and pretension rolls, solid tires and casters for forklifts, automobile vehicle new trams, dollies, and carriers, and industrial products such as conveyor belt idlers, guide rolls, pulleys, steel pipe linings, rubber screens for ores, gears, connection rings, liners, pump impellers, cyclone cones, cyclone liners, etc.It can also be used for office automation equipment belts, paper feed rolls, copying cleaning blades, snow plows, toothed belts, surf rollers, etc.
[0104] The polyurethane of the present invention is also applicable to applications as a thermoplastic elastomer. For example, it can be used in pneumatic equipment, painting equipment, analytical equipment, physicochemical equipment, metering pumps, water treatment equipment, tubes and hoses in industrial robots, spiral tubes, fire hoses, etc. used in the food and medical fields. It can also be used as belts such as round belts, V-belts, and flat belts in various transmission mechanisms, spinning machines, packing machines, printing machines, etc. It can also be used in footwear heel tops and soles, couplings, packing, ball joints, bushes, gears, rolls, and other equipment parts, sports goods, leisure goods, watch belts, etc. Furthermore, examples of automobile parts include oil stoppers, gear boxes, spacers, chassis parts, interior parts, tire chain replacements, etc. It can also be used in keyboard films, films for automobiles, curl cords, cable sheaths, bellows, conveyor belts, flexible containers, binders, synthetic leather, dipping products, adhesives, etc.
[0105] The polyurethane elastomer made of the polyurethane of the present invention can be further made into a foamed polyurethane elastomer or a polyurethane foam. The method for foaming or foaming the polyurethane elastomer may be, for example, any of chemical foaming using water or mechanical foaming such as mechanical froth, and other methods include hard foams obtained by spray foaming, slab, injection, or mold molding, and soft foams obtained by slab or mold molding. Specific applications of the polyurethane elastomer foam or polyurethane foam include electronic devices, heat insulating materials and vibration isolating materials for railway rails and buildings, automobile seats, automobile ceiling cushions, bedding such as mattresses, insoles, midsoles, shoe soles, etc.
[0106] The polyurethane of the present invention can also be used as a solvent-based two-liquid coating material and can be applied to wood products such as musical instruments, Buddhist altars, furniture, decorative plywood, sporting goods, etc. It can also be used as a tar epoxy urethane for automobile repair.
[0107] The polyurethane of the present invention can be used as a component of moisture-curing one-component paints, blocked isocyanate-based solvent paints, alkyd resin paints, urethane-modified synthetic resin paints, ultraviolet-curing paints, water-based urethane paints, and the like, and can be applied, for example, to paints for plastic bumpers, strippable paints, coating agents for magnetic tapes, overprint varnishes for floor tiles, flooring materials, paper, wood grain printed films, and the like, varnishes for wood, coil coats for high processing, optical fiber protective coatings, solder resists, top coats for metal printing, base coats for vapor deposition, white coats for food cans, and the like.
[0108] The polyurethane of the present invention can also be used as a pressure sensitive adhesive or bonding agent for food packaging, shoes, footwear, magnetic tape binders, decorative paper, wood, structural members, etc., and can also be used as a component of low temperature adhesives and hot melts. The polyurethane of the present invention can be used as a binder in magnetic recording media, inks, castings, burnt bricks, graft materials, microcapsules, granular fertilizers, granular agricultural chemicals, polymer cement mortar, resin mortar, rubber chip binders, recycled foams, glass fiber sizing, and the like.
[0109] The polyurethane of the present invention can be used as a component of a fiber processing agent for shrink-proofing, wrinkle-proofing, water-repellent finishing, and the like.
[0110] When the polyurethane of the present invention is used as an elastic fiber, the fiberization method can be carried out without any particular limitation as long as it can be spun. For example, a melt spinning method can be adopted in which the polyurethane is once pelletized, melted, and spun directly through a spinneret. When the polyurethane of the present invention is melt spun to obtain an elastic fiber, the spinning temperature is preferably 250°C or less, more preferably 200°C or more and 235°C or less.
[0111] The elastic fiber made of the polyurethane of the present invention can be used as it is as a bare yarn, or can be covered with other fibers to be used as a covered yarn. Examples of the other fibers include conventionally known fibers such as polyamide fibers, wool, cotton, and polyester fibers, and polyester fibers are preferably used. The elastic fiber made of the polyurethane of the present invention may contain a disperse dye of a dyeing type.
[0112] The polyurethane of the present invention can be used as a sealant or caulking in poured concrete walls, induction joints, around sashes, wall-type PC (precast concrete) joints, ALC (autoclaved lightweight concrete) joints, board joints, sealants for composite glass, heat-insulating sash sealants, automotive sealants, rooftop waterproof sheets, etc.
[0113] The polyurethane of the present invention can be used as a medical material, and can be used as a blood-compatible material for tubes, catheters, artificial hearts, artificial blood vessels, artificial valves, etc., and as a disposable material for catheters, tubes, bags, surgical gloves, artificial kidney potting materials, etc.
[0114] By modifying the ends, the polyurethane of the present invention can be used as a raw material for UV-curable coating materials, electron beam-curable coating materials, photosensitive resin compositions for flexographic printing plates, photocurable optical fiber coating material compositions, and the like.
[0115] [Polyurethane applications] The uses of the polyurethane of the present invention will be described in detail below by application.
[0116] <Breathable waterproof film, breathable waterproof membrane, breathable waterproof fabric> The polyurethane using PEPCD of the present invention has excellent performance as a moisture-permeable waterproof film. Polyester polyol and polyether polyol are mainly used as polyurethane raw materials for moisture-permeable waterproof, but polyester polyol has a fatal drawback of poor hydrolysis resistance. On the other hand, urethane using polyether polyol has a drawback of poor light resistance and heat resistance. Furthermore, recently, polyurethane for moisture-permeable waterproof cloth has been released that has improved durability such as hydrolysis resistance by using polycarbonate diol (PCD) or ester-modified polycarbonate diol. However, although moisture-permeable waterproof cloth using polycarbonate diol can be made moisture-permeable by forming micropores by a wet manufacturing method, it cannot have sufficient moisture permeability when made into a film. For this reason, polyethylene glycol (PEG) and polycarbonate diol are sometimes blended and used, but there are problems such as poor mixability, insufficient strength, poor adhesion and texture.
[0117] PEPCD is made up of ether bonds and carbonate bonds, so it has a high oxygen content and can exhibit sufficient moisture permeability even in a non-porous type. In other words, it is a polyol that combines the moisture permeability of PEG and the durability of PCD in one polyol. Therefore, it is possible to achieve a water pressure resistance of 10,000 mm or more, and even 20,000 mm or more. Furthermore, the moisture permeability is 10,000 g / m 2 -24hrs or more, even 15,000g / m 2 It can achieve performance of more than -24hrs.
[0118] In addition, PEPCD has carbonate bonds, and is therefore strong enough and able to withstand water pressure, so it can also be designed as a porous type. When made into a porous type, it has even better moisture permeability, and even if the thickness is increased, it is possible to achieve a water pressure resistance of 10,000 mm or more, or even 20,000 mm or more. Furthermore, the moisture permeability is 10,000 g / m 2 -24hrs or more, even 15,000g / m 2 It can achieve performance of more than -24hrs.
[0119] There is no particular method for forming the moisture-permeable waterproof coating film. For example, a method for manufacturing the non-porous type is to coat a polyurethane solution for the surface layer, which contains anti-blocking agents and pigments to prevent the films from sticking together, on release paper, and then dry it to form a film. On top of that, a polyurethane solution for the adhesive layer, which is made of polyurethane, crosslinking agent, solvent, catalyst, etc., is coated, and the substrate is pressed and bonded together. The solvent in the adhesive layer is volatilized in a dryer, and the hardening reaction is completed by aging. When the release paper is peeled off, a moisture-permeable waterproof fabric of the non-porous membrane type is obtained.
[0120] The polyurethane using the PEPCD of the present invention can also be applied to coating of porous type moisture-permeable waterproof fabric. For example, the porous type can be produced by coating a polyurethane solution for the surface layer on a substrate that has been pretreated to prevent the solution from penetrating more than necessary, and immersing the substrate in a coagulation bath. During immersion, the solvent in the polyurethane solution is extracted, the resin precipitates and coagulates, and a polyurethane layer with a porous structure having many voids is formed. After drying, a microporous membrane type moisture-permeable waterproof fabric is obtained. PEPCD has moderate hydrophilicity and flexibility due to the balance of carbonate bonds and ether bonds, and provides a moisture-permeable waterproof fabric that is excellent not only in moisture-permeable waterproof performance but also in terms of comfort when worn.
[0121] The moisture-permeable, waterproof fabric produced using the PEPCD of the present invention is suitable for use in outdoor rainwear, windbreakers, cold weather wear, shoes, tents, backpacks, bags, shoes, and the like.
[0122] <Cellulose nanofiber treatment agent> The polyurethane using the PEPCD of the present invention can be used as a cellulose nanofiber processing agent. Cellulose nanofiber (CNF) is an extremely fine fibrous material with a diameter of 3 to 50 nm and an aspect ratio (fiber length / fiber width) of 100 or more, and can be obtained by defibrating plant fibers derived from wood, bamboo, etc., using various methods. The advantage of CNF is its light weight (specific gravity 1.3 to 1.5 g / cm 3 , about 1 / 5 of steel), strong (strength 3 GPa, about 5 times that of steel), large specific surface area (250 m 2 / g or more), high adsorption properties, hardness (tensile modulus of elasticity of about 140 GPa, equivalent to aramid fiber), small expansion and contraction due to heat (linear expansion coefficient 0.1-0.2 ppm / K, about 1 / 50 that of glass), heat conductivity on a par with glass, excellent biocompatibility, etc., make it an extremely promising material as a reinforcing filler for various plastics. However, it is difficult to knead the highly hydrophilic CNF into normally hydrophobic plastics, which has been a major obstacle to its widespread use. The polyurethane using the PEPCD of the present invention becomes a polymer with moderate hydrophilicity by controlling the ether bond concentration in the polyol, and can be adsorbed on the surface of CNF as a polyurethane emulsion. As a result, the polarity of the CNF surface can be converted to hydrophobicity, making it possible to knead it into hydrophobic general-purpose resins such as polypropylene, polyethylene, PET, PBT, polycarbonate, polyamide, etc. CNF finely and uniformly dispersed in the resin forms a strong network, efficiently exerting a reinforcing effect, increasing strength and elastic modulus, and significantly reducing the linear expansion coefficient.
[0123] <Automotive interior paint> The polyurethane using the PEPCD of the present invention can be used in automotive interior paints. Large plastic parts used in automotive interiors are usually painted to conceal molding defects and provide design while at the same time protecting them. Since the usage environment is such that they are touched by human hands and exposed to strong direct sunlight, they require high light resistance, heat resistance, chemical resistance, and scratch resistance, as well as good tactile feel and advanced design. In addition, drying and curing at low temperatures in a short time is required to improve productivity and save energy. The polyurethane using the PEPCD of the present invention has high durability and excellent touch by controlling the concentration, molecular weight, and number of functional groups of carbonate bonds and ether bonds, and has low adhesion, so that the tack-free time is short and low-temperature curing is possible. In addition, since the compression set is small, scratches caused by fingernails or the like are naturally repaired to form a self-healing coating film. Therefore, it can be used as the main agent for paints for automotive interior parts such as instrument panels and center consoles.
[0124] <Paint for home appliance housings> The polyurethane using the PEPCD of the present invention can be used as a coating for the housing of home appliances. The plastic housing of home appliances is sometimes coated for the purpose of providing anti-glare, anti-fouling, protection, touch, and design. The coating film is required to have adhesion to substrates such as polystyrene, ABS, and polycarbonate, as well as chemical resistance to acids, alkalis, oils, and fats, spray coating properties, low-temperature drying properties, and scratch resistance during transportation by packaging materials. The polyurethane using the PEPCD of the present invention can be used as a base agent for paints for the housings of home appliances, as it has excellent chemical resistance, adhesion, and scratch resistance, achieved by controlling the carbonate bond / ether bond concentration, adjusting the molecular weight and number of functional groups, and by selecting a diisocyanate and chain extender and adjusting the hard segment content and molecular weight.
[0125] <Gravure ink> The polyurethane using the PEPCD of the present invention can be used for gravure ink. Gravure ink can print long films or papers at high speed and can produce multicolor, high-definition prints, so it is widely used for food packaging films, building materials such as wallpaper and decorative sheets. Gravure ink for packaging is required to have high printability, and particularly, the requirements for resolubility of the ink, and acid resistance, alkali resistance, and oil resistance after printing are strict. The polyurethane using the PEPCD of the present invention can be used as a binder resin for gravure ink for packaging, due to the durability derived from polycarbonate and the solubility obtained by adjusting the ether bond concentration. Furthermore, gravure inks for building materials require weather resistance, stain resistance, and blocking resistance to prevent blocking caused by winding during printing. The polyurethane using the PEPCD of the present invention has high weather resistance derived from polycarbonate, and by controlling the number of functional groups and optimizing the concentration of ether bonds, it is possible to increase resolubility and suppress blocking on the back surface of the film by controlling the concentrations of urethane bonds and urea bonds introduced by a diamine chain extender, and it can be used as a binder resin for gravure inks for printing on various films for building materials.
[0126] <Architectural exterior paint> The polyurethane using the PEPCD of the present invention can be used in architectural exterior paints. Architectural exterior paints require a high gloss appearance, stain resistance, and high weather resistance to withstand long-term wind, rain, and sunlight. On the other hand, there is a shift from conventional solvent-based paints to less irritating weak solvent-based paints, and furthermore, environmentally friendly water-based paints are progressing. The shift to water-based paints is making it difficult to maintain the required performance. The polyurethane using the PEPCD of the present invention can reduce the emulsion particle size by controlling the carbonate bond / ether bond concentration and optimizing the hydrophilicity, and when used as a water-based paint, it can achieve a high-gloss appearance with less unevenness on the coating surface. In addition, because of its high weather resistance derived from polycarbonate, it is ideal as a resin for architectural exterior paints. Furthermore, by maximizing the hydrophilicity of the coating surface, it forms a low-staining coating film that weakens the adhesion of lipophilic contaminants and makes cleaning easier.
[0127] <Rooftop waterproofing> The polyurethane using the PEPCD of the present invention can be used for rooftop waterproofing. Rooftop waterproofing treatments include sheet waterproofing and coating waterproofing. For coating waterproofing, a cured coating film made by aromatic diamine crosslinking of a prepolymer obtained from polypropylene glycol and diisocyanate has been widely used. Although these are easier to apply than sheet waterproofing, they have low weather resistance and a short service life, with the repair period being about 10 years, half that of sheet waterproofing. Polyurethanes using the PEPCD of the present invention have high weather resistance derived from polycarbonate, and by appropriately controlling the concentration of ether bonds and adjusting the number of functional groups, they can exhibit high waterproofing performance, and can be used as the main agent for rooftop coating waterproofing materials with long service lives.
[0128] <Sealant for information and electronic materials> The polyurethane using the PEPCD of the present invention can be used as a sealant for information and electronic materials. In various fields of information and electronic materials, various sealants are used to protect various functional elements from the environment. These sealants are required to have barrier properties, heat resistance, hydrolysis resistance, transparency, light resistance, adhesion, flexibility, mechanical strength, etc. The polyurethane using the PEPCD of the present invention has high weather resistance derived from polycarbonate, and by controlling the polyether bond concentration and the number of functional groups, it is possible to improve the oxygen and water vapor barrier properties, and by adjusting the diisocyanate, the type of chain extender, and the hard segment content, it is possible to adjust other required performance in a well-balanced manner, and it can be used as an encapsulant resin for light-emitting elements in flat panel displays, solar cell panels, etc.
[0129] <Ultra-low hardness, low compression set, non-foam resin> The polyurethane using the PEPCD of the present invention can be used for non-foam resins with ultra-low hardness and low compression set. To achieve low hardness, it is necessary to increase the molecular weight between crosslinks and introduce a flexible ether structure to increase the flexibility of the molecular chain. To achieve low compression set, it is necessary to increase the number of functional groups and minimize the loss of the crosslinked structure. PEG lacks mechanical properties, PTMG is difficult to multi-functionalize, and PPG has low reactivity because the terminal OH group is bonded to a secondary carbon and is olefinized at a certain ratio by dehydration, so none of them can be used for this purpose. As long as a polyfunctional alcohol having an OH group bonded to a primary carbon is used as a raw material for the PEPCD of the present invention, an OH group bonded to a highly reactive primary carbon will always remain at the end, so that a polyurethane with a completely crosslinked structure can be obtained while increasing the molecular weight between crosslinks.Since the PEPCD has high weather resistance derived from polycarbonate, it is effective as a material for various special rolls used in printers and copiers as a non-foam molded product with high durability, flexibility comparable to foam, and compression set.
[0130] <Polyurethane soft foam> The polyurethane using the PEPCD of the present invention can be used for flexible polyurethane foam. To achieve low hardness, it is necessary to increase the molecular weight between crosslinks and introduce a flexible ether structure to increase the flexibility of the molecular chain. Also, to achieve low compression set, it is necessary to increase the number of functional groups and minimize the loss of the crosslinked structure. None of the above can be used for this purpose because PEG lacks mechanical properties, PTMG is difficult to multifunctionalize, and PPG has low reactivity because the terminal OH group is bonded to the secondary carbon and is olefinized at a certain ratio by dehydration. As long as the PEPCD of the present invention uses a polyfunctional alcohol having an OH group bonded to a primary carbon as a raw material, the highly reactive OH group bonded to the primary carbon always remains at the end, so that a polyurethane having a complete crosslinked structure can be obtained while increasing the molecular weight between crosslinks, and since it has high weather resistance derived from polycarbonate, it is effective as a material for various special rolls used in printers and copiers, shoe soles, urethane batts, sleepers for railway rails, and vibration-proof materials as a foam molded product with high durability, flexibility, low compression set, and high resilience. This characteristic is particularly noticeable in high-density foams with a foam density of 0.1 g / cc or more.
[0131] [Urethane (meth)acrylate resin] The PEPCD of the present invention can be subjected to an addition reaction between a polyisocyanate and a hydroxyalkyl (meth)acrylate to produce a urethane (meth)acrylate oligomer (hereinafter, sometimes referred to as the "urethane (meth)acrylate oligomer of the present invention"). When other raw material compounds such as polyol and a chain extender are used in combination, the urethane (meth)acrylate oligomer can be produced by further adding these other raw material compounds to the polyisocyanate. The urethane (meth)acrylate of the present invention can be blended with other raw materials to give an active energy ray curable resin composition. This active energy ray curable resin composition can be widely used in various surface processing fields and for cast molding applications. When this active energy ray curable resin composition is cured to form a cured film, it has the characteristics of being excellent in balance between hardness and elongation, solvent resistance, and handling, and can be used as a raw material for UV-curable paints, electron beam curable paints, photosensitive resin compositions for flexographic printing plates, and photocurable optical fiber coating compositions.
[0132] The urethane (meth)acrylate oligomer of the present invention can be produced by adding a polyisocyanate and a hydroxyalkyl (meth)acrylate, and if necessary, other compounds, in addition to the PEPCD of the present invention. Examples of polyisocyanates that can be used when producing the urethane (meth)acrylate oligomer include the above-mentioned organic diisocyanates as well as polyisocyanates such as tris(isocyanatohexyl)isocyanurate. The hydroxyalkyl (meth)acrylate that can be used is not particularly limited as long as it is a compound having one or more hydroxyl groups and one or more (meth)acryloyl groups, such as 2-hydroxyethyl (meth)acrylate. Furthermore, in addition to the PEPCD of the present invention, compounds having at least two active hydrogens, such as other polyols and / or polyamines, may be added as necessary, and these may be used in any combination.
[0133] The active energy ray-curable resin composition containing the urethane (meth)acrylate oligomer of the present invention may be mixed with an active energy ray-reactive monomer other than the urethane (meth)acrylate oligomer of the present invention, an active energy ray-curable oligomer, a polymerization initiator, a light enhancer, and other additives.
[0134] The cured film of the active energy ray-curable resin composition containing the urethane (meth)acrylate oligomer of the present invention can be a film that has excellent stain resistance and protective properties against common household stains such as ink and ethanol. Laminates using the cured film as a coating for various substrates have excellent design properties and surface protective properties and can be used as a film to replace paint, and can be effectively applied to, for example, interior or exterior building materials and various components of automobiles and home appliances.
[0135] [Applications of polyester elastomers] The PEPCD of the present invention can be used as a polyester elastomer. A polyester elastomer is a copolymer composed of a hard segment mainly made of an aromatic polyester and a soft segment mainly made of an aliphatic polyether, an aliphatic polyester, or an aliphatic polycarbonate. When the PEPCD of the present invention is used as a constituent component of the soft segment of a polyester elastomer, the physical properties such as heat resistance and water resistance are superior to those when an aliphatic polyether or an aliphatic polyester is used. In addition, compared to known polycarbonate polyols, it is a polyether carbonate ester elastomer that has a melt flow rate suitable for blow molding and extrusion molding when melted, and is excellent in balance with mechanical strength and other physical properties, and can be suitably used for various molding materials including fibers, films, and sheets, for example, molding materials for elastic threads, boots, gears, tubes, packings, etc. Specifically, it can be effectively applied to applications such as joint boots for automobiles, home appliance parts, etc., which require heat resistance and durability, and electric wire coating materials.
[0136] [Uses of (meth)acrylic resin] The PEPCD of the present invention can be derived into a novel (meth)acrylate by (meth)acrylating one or both of the terminal hydroxyl groups. The (meth)acrylate can be produced by using any of the anhydride, halide, and ester of the corresponding (methacrylate). This (meth)acrylate can be blended with other raw materials to give an active energy ray-polymerizable composition ((meth)acrylic resin).
[0137] This active energy ray-polymerizable composition has the property of being cured by polymerization in a short time by active energy rays such as ultraviolet rays, and generally has excellent transparency, and the cured product can have excellent properties such as toughness, flexibility, scratch resistance, chemical resistance, etc. From this point of view, it can be used in various fields such as a coating agent for plastics, a molding agent for lenses, a sealant, an adhesive, etc. EXAMPLES
[0138] The present invention will be described in more detail below with reference to examples and comparative examples. However, the present invention is not limited to these examples as long as the gist of the present invention is not exceeded.
[0139] [Evaluation method] The PEPCD and polyurethane obtained in the following Examples and Comparative Examples were evaluated as follows.
[0140] [Terminal alkoxy / aryloxy ratio of PEPCD] PEPCD dissolved in CDCl3 was used for 400MHz 1 H-NMR (ECZ-400 manufactured by JEOL Ltd.) was measured, and the intensity was calculated from the integral value of the signal of each component. -OCH3 terminal group: δ3.33(s, 3H) -OCH2CH2CH2CH3 terminal group: δ0.91(t, 3H)
[0141] [Viscosity of PEPCD] 0.4 mL of PEPCD was measured using an E-type rotational viscometer (manufactured by Toki Sangyo Co., Ltd., VISCOMETER TV-22L, rotor; 3°R14) set at 40° C., and the value was taken as the viscosity of PEPCD. The PEPCD is preferably in a liquid state and has a viscosity in the range of 300 to 5000 mPa·s.
[0142] [Hydroxyl value and number average molecular weight of PEPCD] The hydroxyl value of PEPCD was measured by a method using an acetylation reagent in accordance with JIS K1557-1. The number average molecular weight (Mn) was calculated from the measured hydroxyl value according to the following formula (I). Number average molecular weight = 2 × 56.1 / (hydroxyl value × 10 -3 ) …(I)
[0143] [Hydroxyl value of PEPCD hydrolysate] 1 g of PEPCD was mixed with 45 mL of methanol and 5 mL of 25 wt% aqueous sodium hydroxide solution, and hydrolyzed by heating at 75°C for 30 minutes. After that, 7 mL of 17.5 wt% aqueous hydrochloric acid solution was added to neutralize the solution, and then methanol was added so that the total volume of the solution became 100 mL. The hydroxyl value of the obtained hydrolyzate was measured in the same manner as the hydroxyl value of PEPCD.
[0144] [Hydroxyl value / number average molecular weight of PTMG] The hydroxyl value and number average molecular weight of PEPCD were measured in the same manner as above.
[0145] [Polyurethane molecular weight] Polyurethane was dissolved in dimethylacetamide to prepare a dimethylacetamide solution with a concentration of 0.14% by weight. The dimethylacetamide solution was injected into a GPC device (Tosoh Corporation, product name "HLC-8220" (column: TskgelGMH-XL x 2)) to measure the weight average molecular weight (Mw) and number average molecular weight (Mn) of the polyurethane in terms of standard polystyrene.
[0146] [Tensile test of polyurethane] According to JIS K6301 (2010), a dumbbell-shaped test piece with a width of 10 mm and a length of 120 mm was cut out from the polyurethane elastomer sheet with a thickness of 1 mm obtained in the examples and comparative examples (Super Dumbbell Cutter, Model: SDK-100), and a tensile test was performed using a tensile tester (manufactured by Orientec, product name "Tensilon UTM-III-100") with a chuck distance of 50 mm, a tensile speed of 500 mm / min, a temperature of 23°C, and a relative humidity of 55%, to measure the breaking elongation and breaking strength of the test piece. A breaking elongation of 800% or more and a breaking strength of 20 MPa or more have a high elastic modulus.
[0147] [Compound abbreviation] The abbreviations for the compounds used in the examples and comparative examples are as follows. PTMG: Polyoxytetramethylene glycol EC: Ethylene carbonate Mg(acac)2: Magnesium(II) acetylacetonate BG: 1,4-butanediol MDI: 4,4'-diphenylmethane diisocyanate TEHP: Tris(2-ethylhexyl) phosphite
[0148] [Example 1] 515g of PTMG1 (hydroxyl value: 613.1mg-KOH / g, number average molecular weight: 183), 285g of EC, and 250mg of Mg(acac)2 were placed in a 1L glass 4-neck flask equipped with a magnetic stirrer, a distillate trap, a pressure regulator, and a 400mm Vigreux tube, and the atmosphere was replaced with nitrogen gas. The internal temperature was raised to 150°C while stirring, and the contents were heated and dissolved. After that, the reaction was carried out at normal pressure for 2 hours, and then the pressure was lowered to 80-40kPa, and the reaction was carried out for 12 hours while removing ethylene glycol and EC from the system. Next, 37g of EC was added, the pressure was lowered to 40-20kPa, and the reaction was carried out at 150°C for 8 hours. 37g of EC was further added, and the pressure was further reduced to 40-18kPa, and the reaction was continued for 10 hours. Then, 1.1 mL of an 8.5% aqueous phosphoric acid solution was added to the product to deactivate the catalyst.Then, the Vigreux flask was removed, and the residual monomer was removed at 1 kPa or less and 168 to 178°C to obtain crude PEPCD.
[0149] The obtained crude PEPCD was sent to a thin-film distillation apparatus at a flow rate of 20 g / min, and thin-film distillation (temperature: 210°C, pressure: 53 Pa) was performed to obtain PEPCD. The thin-film distillation apparatus had a diameter of 50 mm, a height of 200 mm, and an area of 0.0314 m. 2 The molecular distillation apparatus used was a special MS-300 model with an internal condenser and a jacket manufactured by Shibata Scientific Co., Ltd. The analytical values and physical properties of the obtained PEPCD and its hydrolysate are shown in Table 1.
[0150] <Production of polyurethane elastomer> In a reactor equipped with a 300 mL SUS type stirrer preheated to 90°C, 80 g of PEPCD heated to 90°C, 33.6 g of MDI, and 0.77 g of TEHP as an inhibitor for the urethane reaction were charged. The reactor was then covered and reacted for about 90 minutes under reduced pressure (10 torr or less) while stirring and mixing at 2000 rpm. After the reaction, 7.6 g of BG was gradually added to the reactor after the heat generation subsided, and after stirring for 2 minutes, the reactor lid was removed. A fluororesin sheet (fluoro tape Nitoflon 900, thickness 0.1 mm, manufactured by Nitto Denko Corporation) was attached on a glass plate, and a silicon mold (dimensions: 10 cm x 10 cm, thickness 2 mm) was placed on top of it. The reaction liquid was poured into this silicon mold, and the top of the silicon mold was covered with a glass plate with a fluororesin sheet attached to the bottom. A weight of 4.5 kg was then placed on the glass plate on the top of the mold, and it was inserted into a dryer. The mixture was dried in the dryer by heating (110° C.×1 hour) under a nitrogen atmosphere.
[0151] <Melt molding> The resulting polyurethane elastomer (dimensions: 10 cm x 10 cm, thickness: 2 mm) was left overnight and then removed from the silicon mold, and then dried at 10 torr or less and 70°C for 6 hours or more using a vacuum dryer (manufactured by Yamato Scientific Co., Ltd., product name "Vacuum Dryer ADP300").
[0152] The fluororesin sheet and the melt molding die were placed on the plate of a heating press (manufactured by Toyo Seiki Seisakusho, product name "Mini Test Press") that had been heated to 180°C in advance. The melt molding die was 20cm x 20cm x 1mm thick (hole size 15cm x 8cm x 1mm thick x 2 pieces). The polyurethane elastomer was placed in the die and covered with a fluororesin sheet. The polyurethane elastomer was melted using the plate of the heating press (pressure: 0.5MPa x temperature: 180°C x time: 5 minutes). After melting, the pressure setting of the heating press was gradually increased, and the polyurethane elastomer was heated and molded for 5 minutes at a maximum of 10MPa. The pressure of the heating press was then reduced to remove the polyurethane elastomer molded product, and the product was placed in a cooling press (manufactured by Toyo Seiki Seisakusho, product name "Mini Test Press") that had been cooled in advance by running cooling water through it, and quenched (pressure 10MPa x time 2 minutes) to obtain a sheet-shaped polyurethane elastomer molded product. The evaluation results of the physical properties of the polyurethane elastomer molded products are shown in Table 1.
[0153] [Example 2] PEPCD was obtained in the same manner as in Example 1, except that EC was not added to the reactor during the reaction. The analytical values and physical properties of the PEPCD and its hydrolysate are shown in Table 1. Further, a polyurethane elastomer was synthesized and a polyurethane elastomer molded product was obtained in the same manner as in Example 1, except that the PEPCD was used in the amounts shown in Table 1. The evaluation results of the physical properties of this molded product are shown in Table 1.
[0154] [Example 3] PEPCD was obtained in the same manner as in Example 1, except that 515 g of PTMG4 (hydroxyl value: 461.7 mg-KOH / g, number average molecular weight: 243), 285 g of EC, 250 mg of Mg(acac)2, and 74 g of additional EC were used instead of PTMG1. Analytical values and physical properties of the PEPCD and its hydrolysate are shown in Table 1. Further, a polyurethane elastomer was synthesized and a polyurethane elastomer molded product was obtained in the same manner as in Example 1, except that the PEPCD was used in the amounts shown in Table 1. The evaluation results of the physical properties of this molded product are shown in Table 1.
[0155] [Comparative Example 1] PEPCD was obtained in the same manner as in Example 1, except that 2453 g of PTMG2 (hydroxyl value: 461.5 mg-KOH / g, number average molecular weight: 243), 1022 g of EC, 360 mg of Mg(acac)2, and 667 g of additional EC were used instead of PTMG1. Analytical values and physical properties of the PEPCD and its hydrolysate are shown in Table 1. Further, a polyurethane elastomer was synthesized and a polyurethane elastomer molded product was obtained in the same manner as in Example 1, except that the PEPCD was used in the amounts shown in Table 1. The evaluation results of the physical properties of this molded product are shown in Table 1.
[0156] [Comparative Example 2] PEPCD was obtained in the same manner as in Example 1, except that 202 g of PTMG3 (hydroxyl value: 431.5 mg-KOH / g, number average molecular weight: 260), 79 g of EC, 38 mg of Mg(acac)2, and 20 g of additional EC were used instead of PTMG1. Analytical values and physical properties of the PEPCD and its hydrolysate are shown in Table 1. Further, a polyurethane elastomer was synthesized and a polyurethane elastomer molded product was obtained in the same manner as in Example 1, except that the PEPCD was used in the amounts shown in Table 1. The evaluation results of the physical properties of this molded product are shown in Table 1.
[0157] [Table 1]
[0158] The results of Examples 1, 2, and 3 and Comparative Examples 1 and 2 show that by using the PEPCD of the present invention, whose terminal alkoxy / aryloxy ratio is within the range specified by the present invention, polyurethane having excellent tensile properties and usable for synthetic leather, etc. can be easily produced.
Claims
1. A polyether polycarbonate diol having a ratio of the total number of alkoxy terminal groups and aryloxy terminal groups to the total number of terminal groups of 0.20% or more and 7.5% or less, The polyether polycarbonate diol is mixed with methanol and a 25 wt % aqueous solution of sodium hydroxide, and then heated at 75° C. for 30 minutes to effect hydrolysis, thereby obtaining polytetramethylene ether glycol having a hydroxyl value of 220 mg-KOH / g or more and 750 mg-KOH / g or less as a hydrolyzate.
2. The polyether polycarbonate diol of claim 1 , wherein the alkoxy end groups comprise methoxy end groups.
3. 3. The polyether polycarbonate diol of claim 1 or 2, wherein the alkoxy end groups comprise butoxy end groups.
4. The polyether polycarbonate diol according to any one of claims 1 to 3, having a hydroxyl value of 11 mg-KOH / g or more and 320 mg-KOH / g or less.
5. A method for producing the polyether polycarbonate diol according to any one of claims 1 to 4, comprising the steps of: A method for producing a polyether polycarbonate diol, comprising a step of reacting polytetramethylene ether glycol having a hydroxyl value of 220 mg-KOH / g or more and 750 mg-KOH / g or less with a carbonate compound.
6. A method for producing polyurethane, comprising subjecting a raw material containing the polyether polycarbonate diol according to any one of claims 1 to 4 and a compound having a plurality of isocyanate groups to an addition polymerization reaction.
7. The method for producing a polyurethane according to claim 6, wherein the polyurethane is a polyurethane elastomer.
8. The method for producing a polyurethane according to claim 7, wherein the polyurethane elastomer is a polyurethane foam.
Citation Information
Patent Citations
Production of polyether polyol
JP1986120830A
Liquid polyether carbonate diol
JP2002256069A
Polycarbonate / polyether block copolymer having hydroxy group at its terminal
JP2006124485A
Polycarbonate / polyether block copolymer having hydroxy group at its terminal
JP2006124486A
Polycarbonate diol with excellent heat stability and method for producing the same
JP2014208791A