Resin composition, molded article, and method for manufacturing molded article
A resin composition with tailored polycarbonate resins and (meth)acrylate polymer ratios addresses the issues of low surface hardness and whitening in polycarbonate resins, ensuring high impact and heat resistance for molded articles.
Patent Information
- Application Number
- JP2020148441
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-03
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-09-03
AI Technical Summary
Polycarbonate resins with bisphenol A exhibit low surface hardness and are prone to whitening during high-speed molding or when producing thin-walled products, compromising impact resistance and heat resistance.
A resin composition comprising specific ratios of polycarbonate resins with structural units represented by formulas (1) and (2), combined with a (meth)acrylate polymer, enhances surface hardness, impact resistance, and heat resistance while suppressing whitening.
The composition achieves high surface hardness, effective whitening suppression, and maintains excellent impact and heat resistance even during high-speed molding or thin-walled product formation.
Smart Images

Figure 0007567298000001 
Figure 0007567298000002 
Figure 0007567298000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, a molded article, and a method for producing a molded article, and in particular to a resin composition containing a polycarbonate resin as a main component. [Background technology]
[0002] Polycarbonate resin is a thermoplastic resin having excellent impact resistance, heat resistance and transparency, and has a wide range of applications, such as automobile interior panels, automobile headlamp lenses, mobile phones, personal digital assistants, liquid crystal televisions, and personal computer housings. Furthermore, since it is lighter than inorganic glass and has excellent productivity, it is also used for automobile windows, etc. Furthermore, sheets and films using polycarbonate resins are also widely used, and are often used to form laminates or to undergo additional treatments such as hard coating, and are widely used as various components for various display devices, automotive interior parts, and protective equipment components.
[0003] However, the currently widely used polycarbonate resin made from 2,2-bis(4-hydroxyphenyl)propane, i.e., bisphenol A, has the problem that, although it exhibits excellent mechanical properties, it has low surface hardness, as represented by pencil hardness.
[0004] In order to improve the surface hardness of polycarbonate resins, many polycarbonate resins or polycarbonate resin compositions have been proposed (for example, Patent Document 1). However, it has been found that the polycarbonate resin composition described in Patent Document 1 has reduced impact resistance and heat resistance, and is prone to whitening during molding, and the whitening phenomenon is particularly prominent when high-speed molding is performed or thin-walled molded products are molded. In order to solve such problems, Patent Document 2 describes blending a specific acrylic resin with 2,2-bis(3-methyl-4-hydroxyphenyl)propane, i.e., a polycarbonate resin using bisphenol C (Patent Document 2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 11-158364 [Patent Document 2] JP 2014-065901 A Summary of the Invention [Problem to be solved by the invention]
[0006] The resin composition described in Patent Document 2 is an excellent resin composition that has high surface hardness and can effectively suppress whitening even during high-speed molding or molding of thin-walled molded products. However, with recent technological innovations, there is a demand for higher performance in terms of impact resistance and heat resistance. The present invention has an object to solve the above problems, and to provide a resin composition which has high surface hardness, can effectively suppress whitening even during high-speed molding or when molding thin-walled molded products, and has excellent impact resistance and heat resistance, as well as a molded product using the resin composition and a method for manufacturing the molded product. [Means for solving the problem]
[0007] In view of the above problems, the present inventors have conducted research and found that the above problems can be solved by adjusting the ratio of polycarbonate resin using bisphenol A, polycarbonate resin using bisphenol C, and acrylic resin. Specifically, the above problems were solved by the following means. <1> A resin composition comprising a polycarbonate resin and a (meth)acrylate polymer, the polycarbonate resin comprising a structural unit represented by formula (1) and a structural unit represented by formula (2), and satisfying the following relationship: the content (parts by mass) of the structural unit represented by formula (1) ≧ the content (parts by mass) of the structural unit represented by formula (2) ≧ the content (parts by mass) of the (meth)acrylate polymer. Formula (1) [ka] (In formula (1), X 1 represents one of the following formulas: [ka] R 3 and R 4 each independently represents a hydrogen atom or a methyl group, and Z represents a group that bonds with C to form an alicyclic hydrocarbon having 6 to 12 carbon atoms which may have a substituent. Formula (2) [ka] (In formula (2), R 1 represents a methyl group, and R 2 represents a hydrogen atom or a methyl group, and X 2 represents one of the following formulas: [ka] R 3 and R 4 each independently represents a hydrogen atom or a methyl group, and Z represents a group that bonds with C to form an alicyclic hydrocarbon having 6 to 12 carbon atoms which may have a substituent. <2> The polycarbonate resin contains 53 to 90 mol % of a structural unit represented by formula (1) and 47 to 10 mol % of a structural unit represented by formula (2). <1> The resin composition according to claim 1. <3> The (meth)acrylate polymer is contained in an amount of 5 to 40 parts by mass relative to 100 parts by mass of the polycarbonate resin. <1> or <2> The resin composition according to claim 1. <4> the (meth)acrylate polymer contains an aromatic (meth)acrylate structural unit (b1) and a methyl methacrylate structural unit (b2) in a mass ratio of (b1) / (b2) of 5 to 80 / 95 to 20; <1> ~ <3> 10. The resin composition according to claim 9 . <5> The (meth)acrylate polymer has a weight average molecular weight of 5,000 to 30,000. <1> ~ <4> 10. The resin composition according to claim 9 . <6> When the resin composition is molded into a flat test piece having a thickness of 1.5 mm, the haze is 2.0% or less. <1> ~ <5> 10. The resin composition according to claim 9 . <7> The flat test piece was obtained by injection molding the resin composition at an injection speed of 500 mm / sec. <6> The resin composition according to claim 1. <8> When the resin composition is molded into an ISO multipurpose test piece (4 mm thick), the unnotched Charpy impact strength according to ISO179 is 80 kJ / m 2 That's all. <1> ~ <7> 10. The resin composition according to claim 9 . <9> When the resin composition is molded into an ISO multipurpose test piece (4 mm thick), the deflection temperature under load of 1.80 MPa in accordance with ISO 75-1 and ISO 75-2 is 98°C or higher. <1> ~ <8> 10. The resin composition according to claim 9 . <10> For injection molding with an injection speed of 200 mm / sec or more. <1> ~ <9> 10. The resin composition according to claim 9 . <11> For forming thin-walled housings for portable electronic devices. <1> ~ <10> 10. The resin composition according to claim 9 . <12> <1> ~ <11> 2. A molded article formed from the resin composition according to claim 1. <13> A thin-walled housing for a portable electronic device. <12> The molded article according to claim 1. <14> <1> ~ <11> 2. A method for producing a molded article, comprising injection molding the resin composition according to claim 1. <15> The injection molding is carried out at an injection speed of 200 mm / sec or more. <14> A method for producing the molded article according to claim 1. Effect of the Invention
[0008] The present invention makes it possible to provide a resin composition having high surface hardness, capable of effectively suppressing whitening even during high-speed molding or when molding thin-walled molded products, and excellent impact resistance and heat resistance, as well as a molded product using the resin composition and a method for manufacturing the molded product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. Note that the present embodiment is an example for explaining the present invention, and the present invention is not limited to the present embodiment. In this specification, the use of "to" means that the numerical values before and after it are included as the lower limit and upper limit. In this specification, various physical properties and characteristic values are those at 23° C. unless otherwise specified. In the description of groups (atomic groups) in this specification, when the description does not indicate whether the group is substituted or unsubstituted, the description also includes groups (atomic groups) that have a substituent as well as groups (atomic groups) that have no substituent. For example, the term "alkyl group" includes not only alkyl groups that have no substituent (unsubstituted alkyl groups), but also alkyl groups that have a substituent (substituted alkyl groups). In this specification, when the description does not indicate whether the group is substituted or unsubstituted, the description is preferably unsubstituted. In this specification, "(meth)acrylate" refers to both or either of acrylate and methacrylate.
[0010] The resin composition of the present embodiment contains a polycarbonate resin and a (meth)acrylate polymer, and the polycarbonate resin contains a structural unit represented by formula (1) and a structural unit represented by formula (2), and is characterized in that the content (parts by mass) of the structural unit represented by formula (1) ≧ the content (parts by mass) of the structural unit represented by formula (2) ≧ the content (parts by mass) of the (meth)acrylate polymer. Formula (1) [ka] (In formula (1), X 1 represents one of the following formulas: [ka] R 3 and R4 each independently represents a hydrogen atom or a methyl group, and Z represents a group that bonds with C to form an alicyclic hydrocarbon having 6 to 12 carbon atoms which may have a substituent. Formula (2) [ka] (In formula (2), R 1 represents a methyl group, and R 2 represents a hydrogen atom or a methyl group, and X 2 represents one of the following formulas: [ka] R 3 and R 4 each independently represents a hydrogen atom or a methyl group, and Z represents a group that bonds with C to form an alicyclic hydrocarbon having 6 to 12 carbon atoms which may have a substituent.
[0011] By adopting such a configuration, it is possible to provide a resin composition that has high surface hardness, can effectively suppress whitening even during high-speed molding or when molding thin-walled molded products, and has excellent impact resistance and heat resistance. The mechanism of this embodiment is presumed to be as follows. That is, it is presumed that impact resistance and heat resistance can be increased by increasing the ratio of the structural unit represented by formula (1) in the resin component. It is presumed that the surface hardness and the fluidity of the resin composition can be increased by blending a (meth)acrylate polymer. By increasing the fluidity, it is possible to improve high-speed moldability and moldability of thin-walled molded products. However, the inventors of the present invention have found that blending only the above two components causes whitening of the resin composition. As a result of various studies, it is presumed that whitening can be effectively suppressed by blending the structural unit represented by formula (2) in the resin component and precisely adjusting the blend ratio of the three components. The resin composition of the present embodiment will be described in detail below.
[0012] <Polycarbonate resin> The resin composition of the present embodiment contains a polycarbonate resin. By using the polycarbonate resin, it is possible to effectively utilize the inherent properties of the polycarbonate resin, such as impact resistance, heat resistance, and transparency. The polycarbonate resin used in this embodiment contains a constitutional unit represented by formula (1) and a constitutional unit represented by formula (2) in a blend ratio such that the content (parts by mass) of the constitutional unit represented by formula (1) ≧ the content (parts by mass) of the constitutional unit represented by formula (2). By containing the constitutional unit represented by formula (1), the impact resistance and heat resistance of the resin composition can be improved. In addition, by containing the constitutional unit represented by formula (2), the compatibility of the constitutional unit represented by formula (1) in the polycarbonate resin with the (meth)acrylate polymer can be improved, and whitening of the resin composition can be effectively suppressed. Furthermore, the surface hardness of the obtained molded article can be improved.
[0013] Formula (1) [ka] (In formula (1), X 1 represents one of the following formulas: [ka] R 3 and R 4 each independently represents a hydrogen atom or a methyl group, and Z represents a group that bonds with C to form an alicyclic hydrocarbon having 6 to 12 carbon atoms which may have a substituent. Formula (2) [ka] (In formula (2), R 1 represents a methyl group, and R 2 represents a hydrogen atom or a methyl group, and X 2 represents one of the following formulas: [ka] R 3 and R 4 each independently represents a hydrogen atom or a methyl group, and Z represents a group that bonds with C to form an alicyclic hydrocarbon having 6 to 12 carbon atoms which may have a substituent.
[0014] <<Constituent unit represented by formula (1)>> The polycarbonate resin used in this embodiment contains a constitutional unit represented by formula (1). Formula (1) [ka] (In formula (1), X 1 represents one of the following formulas: [ka] R 3 and R 4 each independently represents a hydrogen atom or a methyl group, and Z represents a group that bonds with C to form an alicyclic hydrocarbon having 6 to 12 carbon atoms which may have a substituent.
[0015] Examples of the alicyclic hydrocarbon formed by bonding Z to C include cycloalkylidene groups such as a cyclohexylidene group, a cycloheptylidene group, a cyclododecylidene group, an adamantylidene group, and a cyclododecylidene group. Examples of the alicyclic hydrocarbon having a substituent formed by bonding Z to C include the methyl- and ethyl-substituted alicyclic hydrocarbon groups described above. Among these, a cyclohexylidene group, a methyl-substituted cyclohexylidene group (preferably a 3,3,5-trimethyl-substituted cyclohexylidene group), and a cyclododecylidene group are preferred.
[0016] In formula (1), X 1 teeth, [ka] If R 3and R 4 At least one of the groups is preferably a methyl group, and it is more preferable that both of the groups are methyl groups. Also X 1 but, [ka] In this case, Z is bonded to the carbon C bonded to the two phenyl groups in the above formula (1) to form a divalent alicyclic hydrocarbon group having 6 to 12 carbon atoms. Examples of the divalent alicyclic hydrocarbon group include cycloalkylidene groups such as a cyclohexylidene group, a cycloheptylidene group, a cyclododecylidene group, an adamantylidene group, and a cyclododecylidene group. Substituted groups include those having a methyl or ethyl substituent. Among these, a cyclohexylidene group, a methyl-substituted cyclohexylidene group (preferably a 3,3,5-trimethyl-substituted cyclohexylidene group), and a cyclododecylidene group are preferred. In formula (1), X 1 is preferably the following structure: [ka]
[0017] A specific preferred example of the structural unit represented by the above formula (1) is 2,2-bis(4-hydroxyphenyl)propane, that is, a structural unit formed from bisphenol A (carbonate structural unit).
[0018] In the present embodiment, the polycarbonate resin may not contain any structural unit represented by formula (1), may contain only one type, or may contain two or more types.
[0019] <<Constituent unit represented by formula (2)>> The polycarbonate resin used in the present embodiment preferably contains a constitutional unit represented by formula (2). Formula (2) [ka] (In formula (2), R 1 represents a methyl group, and R 2 represents a hydrogen atom or a methyl group, and X 2 represents one of the following formulas: [ka] R 3 and R 4 each independently represents a hydrogen atom or a methyl group, and Z represents a group that bonds with C to form an alicyclic hydrocarbon having 6 to 12 carbon atoms which may have a substituent. The two R in Eq. (2) 2 may be the same or different, and are preferably the same. 2 is preferably a hydrogen atom.
[0020] In formula (2), X 2 teeth, [ka] If R 3 and R 4 At least one of the groups is preferably a methyl group, and it is more preferable that both of the groups are methyl groups. Also X 2 but, [ka] In this case, Z is bonded to the carbon C bonded to the two phenyl groups in the above formula (2) to form a divalent alicyclic hydrocarbon group having 6 to 12 carbon atoms. Examples of the divalent alicyclic hydrocarbon group include cycloalkylidene groups such as a cyclohexylidene group, a cycloheptylidene group, a cyclododecylidene group, an adamantylidene group, and a cyclododecylidene group. Substituted groups include those having a methyl substituent or an ethyl substituent. Among these, a cyclohexylidene group, a methyl-substituted cyclohexylidene group (preferably a 3,3,5-trimethyl-substituted cyclohexylidene group), and a cyclododecylidene group are preferred. In formula (2), X 2 is preferably the following structure: [ka]
[0021] In this embodiment, the polycarbonate resin may contain only one type of constitutional unit represented by formula (2), or may contain two or more types.
[0022] In the present embodiment, the polycarbonate resin may contain other structural units in addition to the structural unit represented by formula (1) and the structural unit represented by formula (2). Examples of other structural units include structural units derived from dihydroxy compounds shown below.
[0023] Bis(4-hydroxyphenyl)methane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)pentane, 2,2-bis(4-hydroxyphenyl)-4-methylpentane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 2,2-bis(4-hydroxy-3-(1-methylethyl)phenyl)propane, 2,2-bis(4-hydroxy-3-tert-butylphenyl)propane, 2,2-bis(4-hydroxy-3-(1-methylpropyl)phenyl)propane, 2,2-bis(4-hydroxy-3-cyclohexylphenyl)propane, 2,2-bis(4-hydroxy-3-phenylphenyl)propane, 1,1-bis(4-hydroxyphenyl)decane, 1,1-bis(4-hydroxyphenyl) Cyclohexane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 1,1-bis(4-hydroxyphenyl)phenylmethane, 1,1-bis(4-hydroxy-3-methylphenyl)cyclohexane, 1,1-bis(4-hydroxy-3,5-dimethylphenyl)cyclohexane, 1,1-bis(4-hydroxy-3-(1-methylethyl)phenyl)cyclohexane, 1,1-bis(4-hydroxy-3-tert-butylphenyl)cyclohexane, 1,1-bis(4-hydroxy-3-(1-methylpropyl)phenyl)cyclohexane, 1,1-bis(4-hydroxy-3-cyclohexylphenyl)cyclohexane, 1,1-bis(4-hydroxy-3-phenylphenyl)cyclohexane, 1,1-bis(4-hydroxy-3-methylphenyl)-1-phenylethane, 1,1-bis(4-hydroxy-3 ,5-dimethylphenyl)-1-phenylethane, 1,1-bis(4-hydroxy-3-(1-methylethyl)phenyl)-1-phenylethane, 1,1-bis(4-hydroxy-3-tert-butylphenyl)-1-phenylethane, 1,1-bis(4-hydroxy-3-(1-methylpropyl)phenyl)-1-phenylethane, 1,1-bis(4-hydroxy-3-cyclohexylphenyl)-1-phenylethane, 1,1-bis(4-hydroxy-3-phenylphenyl)-1-phenylethane, 1,1-bis(4-hydroxyphenyl)cyclopentane, 1,1-bis(4-hydroxyphenyl)cyclopentane, 1,1-bis(4-hydroxyphenyl)cyclooctane, 4,4'-(1,3-phenylenediisopropylidene)bisphenol, 4,4'-(1,4-phenylenediisopropylidene)bisphenol, 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 4,4'-dihydroxybenzophenone, 4,4'-dihydroxyphenyl ether, 4,4'-dihydroxybiphenyl, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 1,1-bis(4-hydroxy-6-methyl-3-tert-butylphenyl)butane.
[0024] In addition, as an embodiment of other structural units, the structural unit represented by formula (2) described in paragraph 0008 of WO 2017 / 099226, the description in paragraphs 0043 to 0052 of WO 2017 / 099226, and the description in JP 2011-046769 A can be referred to, the contents of which are incorporated herein by reference.
[0025] In the polycarbonate resin used in this embodiment, the ratio of the structural unit represented by formula (1) and the structural unit represented by formula (2) is not particularly determined as long as the content (parts by mass) of the structural unit represented by formula (1) is ≧ the content (parts by mass) of the structural unit represented by formula (2). Preferably, the ratio of the structural unit represented by formula (1) is 50 parts by mass or more, preferably 55 parts by mass or more, more preferably 60 parts by mass or more, and even more preferably 65 parts by mass or more, when the structural unit represented by formula (1) and the structural unit represented by formula (2) are taken as 100 parts by mass. The upper limit of the ratio of the structural unit represented by formula (1) is preferably 85 parts by mass or less. In addition, in the polycarbonate resin used in this embodiment, the ratio of the structural unit represented by formula (2) is 50 parts by mass or less, more preferably 45 parts by mass or less, even more preferably 40 parts by mass or less, and even more preferably 35 parts by mass or less, when the structural unit represented by formula (1) and the structural unit represented by formula (2) are taken as 100 parts by mass. The lower limit of the proportion of the structural unit represented by formula (2) is preferably 15 parts by mass or more when the structural unit represented by formula (1) and the structural unit represented by formula (2) are taken as 100 parts by mass.
[0026] In the polycarbonate resin used in the present embodiment, the total of the constitutional units represented by the above formula (1) and the constitutional units represented by the formula (2) preferably accounts for 90% by mass or more, more preferably 95% by mass or more, and even more preferably 99% by mass or more of all constitutional units excluding terminal groups. The upper limit of the total is 100% by mass or less.
[0027] The polycarbonate resin used in the present embodiment preferably contains 53 to 90 mol% of the structural unit represented by formula (1) and 47 to 10 mol% of the structural unit represented by formula (2). The proportion of the structural unit represented by formula (1) is preferably 58 mol% or more, more preferably 62 mol% or more, and even more preferably 67 mol% or more. The upper limit of the proportion of the structural unit represented by formula (1) is preferably 86 mol% or less. The proportion of the structural unit represented by formula (2) is preferably 42 mol% or less, more preferably 38 mol% or less, and even more preferably 33 mol% or less, when the structural unit represented by formula (1) and the structural unit represented by formula (2) are taken as 100 mol%. The lower limit of the proportion of the structural unit represented by formula (2) is preferably 14 mol% or more, when the structural unit represented by formula (1) and the structural unit represented by formula (2) are taken as 100 mol%.
[0028] In the polycarbonate resin used in the present embodiment, the total of the constitutional units represented by the above formula (1) and the constitutional units represented by the formula (2) preferably accounts for 90 mol % or more, more preferably 95 mol % or more, and even more preferably 99 mol % or more of all constitutional units excluding terminal groups. The upper limit of the total is 100 mol % or less.
[0029] The polycarbonate resin used in the present embodiment is preferably in the following form: In the present embodiment, (A1) or (A2) is preferred, and (A1) is more preferred. (A1) A blend of a polycarbonate resin containing a structural unit represented by formula (1) and a polycarbonate resin containing a structural unit represented by formula (2) (A2) A polycarbonate resin containing a structural unit represented by formula (1) and a structural unit represented by formula (2) (A3) A blend of a polycarbonate resin containing a structural unit represented by formula (1) and a polycarbonate resin containing a structural unit represented by formula (1) and a structural unit represented by formula (2). (A4) A blend of a polycarbonate resin containing a structural unit represented by formula (2) and a polycarbonate resin containing a structural unit represented by formula (1) and a structural unit represented by formula (2). (A5) A blend of a polycarbonate resin containing a structural unit represented by formula (1), a polycarbonate resin containing a structural unit represented by formula (2), and a polycarbonate resin containing a structural unit represented by formula (1) and a structural unit represented by formula (2). (A6) In the above (A1) to (A5), the polycarbonate resin or the polycarbonate resin constituting the blend thereof contains a structural unit represented by formula (1) and a structural unit other than the structural unit represented by formula (2). (A7) A blend of the polycarbonate resin or blend of the above (A1) to (A6) with a polycarbonate resin comprising other structural units.
[0030] The lower limit of the viscosity average molecular weight (Mv) of the polycarbonate resin used in this embodiment is preferably 5,000 or more, more preferably 8,000 or more, even more preferably 10,000 or more, and even more preferably 12,000 or more. The upper limit of Mv is preferably 32,000 or less, more preferably 30,000 or less, even more preferably 29,000 or less, even more preferably 27,000 or less, and even more preferably 25,000 or less. When two or more types of polycarbonate resins are contained, the total is calculated by multiplying the viscosity average molecular weight of each polycarbonate resin by the mass fraction. By setting the viscosity average molecular weight to the above lower limit or more, moldability is improved and molded articles having high mechanical strength can be obtained, while by setting the viscosity average molecular weight to the above upper limit or less, the flowability of the molded article is improved and thin-walled molded articles can be efficiently produced. In particular, the viscosity average molecular weight of the polycarbonate resin containing the structural unit represented by formula (1) is preferably 20,000 to 30,000, and more preferably 20,000 to 25,000.The viscosity average molecular weight of the polycarbonate resin containing the structural unit represented by formula (2) is preferably 12,000 to 28,000, and more preferably 18,000 to 27,000. The viscosity average molecular weight (Mv) is measured according to the method described in the Examples section below.
[0031] The polycarbonate resin used in the present embodiment (all polycarbonate resins including the constitutional units represented by formula (1) and formula (2)) has a pencil hardness of 3B to 2H, preferably 2B to 2H, as measured in accordance with ISO 15184. The pencil hardness is measured according to the method described in the examples below. In particular, the pencil hardness of the polycarbonate resin containing the constitutional unit represented by formula (1) is preferably 2B to HB, and the pencil hardness of the polycarbonate resin containing the constitutional unit represented by formula (2) is preferably H to 2H.
[0032] The method for producing the polycarbonate resin used in the present embodiment is not particularly limited, but for example, the description in paragraphs 0027 to 0043 and the Examples of JP-A-2014-065901 can be referred to, the contents of which are incorporated herein by reference.
[0033] The content of the polycarbonate resin in the resin composition of this embodiment is preferably 70% by mass or more, more preferably 75% by mass or more, and even more preferably 77% by mass or more. By making it equal to or more than the lower limit, the impact strength and heat resistance of the molded article formed from the resin composition tend to be further improved. In addition, by making it equal to or less than the upper limit, from the viewpoint of the surface hardness of the molded article formed from the resin composition and the fluidity of the resin composition, it is preferably 97% by mass or less, more preferably 95% by mass or less, even more preferably 92% by mass or less, and may be 88% by mass or less.
[0034] <(Meth)acrylate polymer> The resin composition of the present embodiment contains a (meth)acrylate polymer. By containing the (meth)acrylate polymer, the surface hardness of a molded article formed from the resin composition can be increased, and the flowability of the resin composition can be increased. In other words, the high-speed moldability and the moldability of a thin-walled molded article can be improved. The (meth)acrylate polymer used in this embodiment is not limited to a specific type, and any known (meth)acrylate polymer can be used. The (meth)acrylate polymer used in this embodiment preferably contains an aromatic (meth)acrylate structural unit and a methyl methacrylate structural unit. By containing an aromatic (meth)acrylate structural unit, the compatibility with polycarbonate resin can be improved, and by containing a methyl methacrylate structural unit, the surface hardness of a molded article formed from the resin composition can be increased.
[0035] Aromatic (meth)acrylate, which is a monomer constituting an aromatic (meth)acrylate structural unit, refers to a (meth)acrylate having an aromatic group. Examples of aromatic (meth)acrylates include phenyl (meth)acrylate and benzyl (meth)acrylate. These may be used alone or in combination of two or more. Among these, preferred are phenyl methacrylate and benzyl methacrylate, and more preferred is phenyl methacrylate.
[0036] The monomer constituting the methyl methacrylate structural unit is methyl methacrylate.
[0037] When the (meth)acrylate polymer used in the present embodiment contains an aromatic (meth)acrylate structural unit (b1) and a methyl methacrylate structural unit (b2), the mass ratio of (b1) / (b2) is preferably 5 to 80 / 95 to 20. The mass ratio of (b1) / (b2) is more preferably 20 to 60 / 80 to 40, even more preferably 25 to 50 / 75 to 50, even more preferably 25 to 45 / 75 to 55, and even more preferably 30 to 40 / 70 to 60. When the (meth)acrylate polymer used in this embodiment contains an aromatic (meth)acrylate structural unit (b1) and a methyl methacrylate structural unit (b2), it may or may not contain other structural units. When it contains other structural units, styrene structural units and (meth)acrylate structural units other than (b1) and (b2) are preferred, and (meth)acrylate structural units other than (b1) and (b2) are more preferred. Examples of (meth)acrylate structural units other than (b1) and (b2) include aliphatic (meth)acrylates other than methyl methacrylate. In the (meth)acrylate polymer used in this embodiment, the total of the aromatic (meth)acrylate structural unit (b1) and the methyl methacrylate structural unit (b2) preferably accounts for 90% by mass or more, more preferably 95% by mass or more, and even more preferably 99% by mass or more of all structural units excluding the terminal groups. The upper limit of the total may be 100% by mass or less of all structural units excluding the terminal groups.
[0038] In addition to the above, the acrylic resin used in this embodiment may be one described in WO 2014 / 038500, WO 2013 / 094898, JP 2006-199774, JP 2010-116501, JP 2014-065901, or JP 2016-27068, the contents of which are incorporated herein by reference.
[0039] The weight average molecular weight of the (meth)acrylate polymer used in this embodiment is preferably 5,000 or more, more preferably 10,000 or more, and even more preferably 13,000 or more. By making it equal to or more than the lower limit, the impact strength and heat resistance of the obtained molded article tend to be further improved. In addition, the weight average molecular weight of the (meth)acrylate polymer is preferably 30,000 or less, more preferably 25,000 or less, even more preferably 20,000 or less, and even more preferably 16,000 or less. By making it equal to or less than the upper limit, the flowability of the resin composition tends to be further improved.
[0040] The (meth)acrylate polymer used in the present embodiment preferably has a pencil hardness of 2H or harder as measured according to ISO 15184. There is no particular upper limit, but it is practical to have a pencil hardness of 4H or softer. By using a polymer having a pencil hardness harder than the above hardness, the surface hardness of the resulting molded article can be improved. The pencil hardness of the (meth)acrylate polymer measured according to ISO 15184 is preferably harder than the pencil hardness of the polycarbonate resin used in the embodiment, and more preferably 1 to 3 levels harder. By using a (meth)acrylate polymer having such a pencil hardness, the surface hardness of the obtained molded article can be improved. Furthermore, when the resin composition of the present embodiment contains two or more types of (meth)acrylate polymers, the pencil hardness of the mixture is preferably within the above range.
[0041] The content of the (meth)acrylate polymer in the resin composition of the present embodiment is preferably 5 parts by mass or more, more preferably 8 parts by mass or more, even more preferably 10 parts by mass or more, and may be 15 parts by mass or more, relative to 100 parts by mass of the polycarbonate resin. By making it equal to or more than the lower limit, the surface hardness of the molded article formed from the resin composition and the flowability of the resin composition tend to be further improved. In addition, the content of the (meth)acrylate polymer in the resin composition of the present embodiment is preferably 40 parts by mass or less, more preferably 32 parts by mass or less, even more preferably 30 parts by mass or less, even more preferably 28 parts by mass or less, and may be 24 parts by mass or less, relative to 100 parts by mass of the polycarbonate resin. By making it equal to or less than the upper limit, the impact strength of the molded article formed from the resin composition tends to be further improved, and the deterioration of the heat resistance of the resin composition tends to be effectively suppressed. In particular, by setting the content of the (meth)acrylate polymer in the resin composition of this embodiment to 24 parts by mass or less per 100 parts by mass of the polycarbonate resin, a resin composition having even better impact resistance can be obtained.
[0042] The content of the (meth)acrylate polymer in the resin composition of the present embodiment is preferably 3% by mass or more, more preferably 5% by mass or more, even more preferably 8% by mass or more, and may be 12% by mass or more. By making it equal to or more than the lower limit, the surface hardness of the molded article formed from the resin composition and the flowability of the resin composition tend to be further improved. In addition, the content of the (meth)acrylate polymer in the resin composition of the present embodiment is preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 23% by mass or less. By making it equal to or less than the upper limit, the impact strength of the molded article formed from the resin composition tends to be further improved, and the deterioration of the heat resistance of the resin composition tends to be effectively suppressed. The resin composition of the present embodiment may contain only one type of (meth)acrylate polymer, or may contain two or more types. When two or more types are contained, the total amount is preferably within the above range.
[0043] Next, the blend ratio of the constitutional unit represented by formula (1), the constitutional unit represented by formula (2), and the (meth)acrylate polymer will be described. In the resin composition of the present embodiment, the content (parts by mass) of the structural unit represented by formula (1) ≧ the content (parts by mass) of the structural unit represented by formula (2) ≧ the content (parts by mass) of the (meth)acrylate polymer is satisfied, and it is preferable that the content (parts by mass) of the structural unit represented by formula (1) ≧ the content (parts by mass) of the structural unit represented by formula (2)> the content (parts by mass) of the (meth)acrylate polymer is satisfied. In the resin composition of the present embodiment, the constitutional unit represented by formula (1), the constitutional unit represented by formula (2), and the (meth)acrylate polymer preferably account for 90% by mass or more of the resin composition in total, more preferably 95% by mass or more, and even more preferably 99% by mass or more. The upper limit of the total is 100% by mass or less.
[0044] <Other ingredients> In addition to the polycarbonate resin and the (meth)acrylate polymer, the resin composition of the present embodiment may contain other components as necessary, as long as the desired physical properties are not significantly impaired. Examples of the other components include various resin additives. Examples of resin additives include stabilizers (thermal stabilizers, antioxidants, etc.), UV absorbers, antistatic agents, flame retardants, flame retardant assistants, dyes, pigments, antifogging agents, lubricants, antiblocking agents, flow improvers, plasticizers, dispersants, and antibacterial agents. The resin additives may be contained in one type or in any combination and ratio of two or more types. For details of these, refer to the descriptions in paragraphs 0059 to 0080 of JP 2014-065901 A, the contents of which are incorporated herein by reference. The resin composition of the present embodiment is prepared so that the total amount of the polycarbonate resin, the (meth)acrylate polymer, and the resin additives (for example, stabilizers) blended as necessary is 100 mass %.
[0045] <<Stabilizer>> The stabilizers include heat stabilizers and antioxidants. As the heat stabilizer, a phosphorus-based stabilizer is preferably used. Any known phosphorus stabilizer can be used. Specific examples include phosphorus oxoacids such as phosphoric acid, phosphonic acid, phosphorous acid, phosphinic acid, and polyphosphoric acid; metal acid pyrophosphates such as sodium acid pyrophosphate, potassium acid pyrophosphate, and calcium acid pyrophosphate; phosphates of Group 1 or Group 2B metals such as potassium phosphate, sodium phosphate, cesium phosphate, and zinc phosphate; organic phosphate compounds, organic phosphite compounds, and organic phosphonite compounds, with organic phosphite compounds being particularly preferred.
[0046] Examples of organic phosphite compounds include triphenyl phosphite, tris(mononylphenyl)phosphite, tris(mononyl / dinonyl phenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, monooctyl diphenyl phosphite, dioctyl monophenyl phosphite, monodecyl diphenyl phosphite, didecyl monophenyl phosphite, tridecyl phosphite, trilauryl phosphite, tristearyl phosphite, and 2,2-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite. Specific examples of such organic phosphite compounds include "ADK STAB (registered trademark; the same applies below) 1178," "ADK STAB 2112," and "ADK STAB HP-10" manufactured by ADEKA Corporation, "JP-351," "JP-360," and "JP-3CP" manufactured by Johoku Chemical Industry Co., Ltd., and "IRGAFOS (registered trademark; the same applies below) 168" manufactured by BASF.
[0047] As the antioxidant, a hindered phenol-based stabilizer is preferably used. Specific examples of hindered phenol stabilizers include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, thiodiethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide], 2,4-dimethyl-6-(1-methylpentadecyl)phenol, diethyl[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphate, 3,3',3'',5,5',5''-hexa-tert-butyl-a,a',a''-(mesityle) 4,6-bis(octylthiomethyl)-o-cresol, ethylene bis(oxyethylene) bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate], hexamethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,3,5-tris(3,5-di-tert-butyl -4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2,6-di-tert-butyl-4-(4,6-bis(octylthio)-1,3,5-triazin-2-ylamino)phenol, 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate, and the like.
[0048] Among them, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate are preferred. Specific examples of such hindered phenol stabilizers include "Irganox (registered trademark, the same applies below) 1010" and "Irganox 1076" manufactured by BASF, and "Adeka STAB AO-50" and "Adeka STAB AO-60" manufactured by ADEKA.
[0049] The content of the stabilizer in the resin composition of the present embodiment is usually 0.001 parts by mass or more, preferably 0.005 parts by mass or more, more preferably 0.01 parts by mass or more, and usually 1 part by mass or less, preferably 0.5 parts by mass or less, more preferably 0.3 parts by mass or less, relative to 100 parts by mass of the polycarbonate resin. By setting the content of the stabilizer within the above range, the effect of adding the stabilizer is more effectively exhibited. The resin composition of the present embodiment may contain only one type of stabilizer, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0050] <Physical properties of resin composition> The resin composition of the present embodiment preferably has a high surface hardness when molded. Specifically, the resin composition of the present embodiment is molded into a flat test piece (150 mm x 100 mm x 2 mm thick) and the pencil hardness measured under a load of 750 g using a pencil hardness tester in accordance with ISO 15184 is preferably HB or harder, more preferably F or harder. The upper limit of the pencil hardness is, for example, 3H or softer. The pencil hardness is measured as described in the Examples section below.
[0051] The resin composition of the present embodiment preferably has high fluidity. Specifically, the melt volume rate (MVR, unit: cm) under the conditions of a measurement temperature of 300° C. and a load of 11.8 N in accordance with ISO1133 is 3 / 10min) is 65cm 3 / 10min or less is preferable, and 60cm 3 / 10min or less is more preferable, and 55cm 3 / 10min or less is more preferable, and 52cm 3 / 10min or less is more preferable, and 49cm 3 The lower limit of the MVR may be 25 cm / 10 min or less. 3 / 10min or more is practical, 30cm 3 / 10min or more. MVR is measured as described in the Examples section below.
[0052] The resin composition of the present embodiment preferably has excellent impact resistance. Specifically, when the resin composition of the present embodiment is molded into an ISO multipurpose test piece (thickness: 4 mm), the unnotched Charpy impact strength according to ISO179 is 80 kJ / m 2 It is preferable that the concentration is 90 kJ / m or more. 2 More preferably, it is 100 kJ / m or more. 2 More preferably, it is 110 kJ / m or more. 2 More preferably, it is 120 kJ / m or more. 2 It is even more preferable that the upper limit is equal to or greater than NB. The unnotched Charpy impact strength is measured as described in the Examples section below.
[0053] The resin composition of the present embodiment is preferably excellent in heat resistance. Specifically, when the resin composition of the present embodiment is molded into an ISO multipurpose test piece (4 mm thick), the deflection temperature under load of 1.80 MPa according to ISO75-1 and ISO75-2 is preferably 98°C or higher, more preferably 99°C or higher, even more preferably 100°C or higher, and even more preferably 102°C or higher. Although there is no particular upper limit for the deflection temperature under load, 120°C or lower is practical, and even 115°C or lower, or 112°C or lower, sufficiently meets the required performance. The deflection temperature under load is measured according to the description in the Examples section below.
[0054] The resin composition of this embodiment is preferably excellent in transparency. Specifically, when the resin composition of this embodiment is molded into a flat test piece having a thickness of 1.5 mm, the haze is preferably 2.0% or less, more preferably 1.8% or less, even more preferably 1.4% or less, even more preferably 1.2% or less, and even more preferably 1.0% or less. The lower limit of the haze is ideally 0%, but 0.1% or more is practical. In the resin composition of this embodiment, it is particularly preferable that the above haze is satisfied when the flat test piece is obtained by injection molding the resin composition at a high speed (e.g., injection speed of 500 mm / sec). It is also preferable that the above haze is satisfied when the molding temperature is high (e.g., 300°C). The haze is measured as described in the Examples section below.
[0055] <Method of producing resin composition> The method for producing the resin composition of this embodiment is not limited, and a wide variety of known methods for producing resin compositions can be used, including a method in which the polycarbonate resin, the (meth)acrylate polymer, and other components to be mixed as necessary are mixed in advance using various mixers such as a tumbler or a Henschel mixer, and then melt-kneaded using a mixer such as a Banbury mixer, a roll, a Brabender, a single-screw kneading extruder, a twin-screw kneading extruder, a kneader, etc. The temperature for melt-kneading is not particularly limited, but is usually in the range of 240 to 320°C.
[0056] <Molded products> The molded article of the present embodiment is a molded article formed from the resin composition of the present embodiment. Therefore, the molded article of the present embodiment can have high surface hardness, low haze, and excellent impact resistance and heat resistance. The shape of the molded product is not particularly limited and can be appropriately selected depending on the application and purpose of the molded product. Examples of the shape include plate-like, plate-like, rod-like, sheet-like, film-like, cylindrical, annular, circular, elliptical, polygonal, irregularly shaped, hollow, frame-like, box-like, panel-like, and special shapes. The molded product of this embodiment is suitable for a thin-walled molded product. For example, it is preferably used for a thin-walled molded product having a thin-walled portion having a thickness of 0.8 mm or less. The lower limit of the thickness of the thin-walled portion is not particularly set, but may be, for example, 0.1 mm or more.
[0057] The molded product molded from the resin composition of this embodiment has high surface hardness, low haze, and excellent impact resistance and heat resistance, and can be preferably applied to, for example, the following. That is, the resin composition of this embodiment is preferably used for molding applications such as window glass of buildings (buildings, houses, greenhouses, etc.); window glass of cars, airplanes, and construction machines; roofs of garages, arcades, etc.; sunroofs, roof panels, sunshades; various peepholes; lenses for lighting, traffic light lenses, lenses for optical instruments; lens covers; mirrors, glasses, goggles, and motorcycle windshields; solar cell covers; protective covers; various automobile lamp covers such as headlamps, inner lenses, and rear lamps; automobile interior panels; displays, display panel members, and game machine (pachinko, etc.) parts; various mobile terminals, cameras, game machines, and the like, housings of electric and electronic equipment and office automation equipment; helmets; sheets, films, and laminates thereof. The molded article of the present embodiment is preferably used for the housing of a portable electronic device (such as a mobile phone or a smartphone), and is more preferably used for a thin-walled housing of the portable electronic device. One example of the housing of a portable electronic device is a back panel.
[0058] The molded article of the present embodiment may have a cured layer on the surface. By forming the cured layer, the molded article can be given a higher surface hardness. In addition, by providing the cured layer, the surface hardness of the molded article itself formed from the resin composition of the present embodiment can be somewhat lowered, and the ratio of the structural unit represented by formula (2) and / or the ratio of the (meth)acrylic polymer in the resin composition of the present embodiment can be reduced, and the impact resistance and heat resistance of the molded article can be improved more inexpensively. An example of the cured layer is a cured layer of an energy ray-curable acrylic resin composition. For details of the cured layer, the descriptions in paragraphs 0086 to 0091 of JP 2014-065901 A can be referred to, and the contents thereof are incorporated herein.
[0059] <Method of manufacturing molded products> The resin composition of the present embodiment is pelletized and then molded into a molded product by various molding methods. Alternatively, the resin melt-kneaded in an extruder can be directly molded into a molded product without going through the pelletization process.
[0060] The method for molding the molded product is not particularly limited, and any conventionally known molding method can be used, such as injection molding, injection compression molding, extrusion molding, profile extrusion, transfer molding, hollow molding, gas-assisted hollow molding, blow molding, extrusion blow molding, IMC (in-mold coating molding), rotational molding, multi-layer molding, two-color molding, insert molding, sandwich molding, foam molding, and pressure molding. In addition, it may be used as a sheet or film by extrusion molding. For details on the use as a sheet or film, refer to paragraph 0083 of JP2014-065901A, the contents of which are incorporated herein by reference.
[0061] In this embodiment, it is preferable to produce a molded article by injection molding the resin composition of this embodiment. Therefore, the resin composition of this embodiment is preferably used for injection molding. The molded article molded from the resin composition of this embodiment has almost no problem of whitening, and a molded article with excellent appearance can be obtained. In particular, when thin-wall molding is performed at high temperature and / or high speed, the phenomenon of whitening of the edge of the molded article is likely to occur, but by using the resin composition of this embodiment, whitening can be effectively suppressed even when thin-wall molding is performed at high temperature and / or high speed. When molding the resin composition of this embodiment, even if the cylinder temperature is, for example, 260°C or more, further 270°C or more, 280°C or more, 290°C or more, or 300°C or more, the whitening phenomenon can be effectively suppressed, and a molded product with excellent appearance can be obtained. The upper limit of the cylinder temperature is preferably 330°C or less, more preferably 320°C or less. In addition, by using the resin composition of this embodiment, even under conditions where the injection speed is 200mm / sec or more, or even 500mm / sec or more, a molded product with excellent appearance can be obtained without causing the whitening phenomenon. The upper limit of the injection speed is, for example, 1,000mm / sec or less. EXAMPLES
[0062] The present invention will be described in more detail below with reference to examples. The materials, amounts, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below. If the measuring instruments used in the examples are difficult to obtain due to discontinuation or the like, measurements can be made using other instruments with equivalent performance.
[0063] 1. Raw materials <Production Example 1: Production of Polycarbonate Resin A2-1> 26.14 moles (6.75 kg) of bisphenol C (BPC) and 26.79 moles (5.74 kg) of diphenyl carbonate were placed in an aluminum (SUS) reactor (internal volume: 10 L) equipped with a stirrer and a distillate condenser. The inside of the reactor was replaced with nitrogen gas, and the temperature was raised to 220°C in a nitrogen gas atmosphere over 30 minutes. Next, the reaction liquid in the reactor was stirred, and cesium carbonate (Cs2CO3) was added as a transesterification catalyst to the molten reaction liquid at a ratio of 1.5 × 10 -6 The reaction solution was stirred and fermented in a nitrogen gas atmosphere at 220° C. for 30 minutes. Next, the pressure in the reactor was reduced to 100 Torr over 40 minutes at the same temperature, and the reaction was continued for another 100 minutes to distill off phenol. Next, the temperature in the reactor was raised to 284°C over 60 minutes, and the pressure was reduced to 3 Torr, and phenol equivalent to almost the entire theoretical amount was distilled out. Next, the pressure in the reactor was kept below 1 Torr at the same temperature, and the reaction was continued for another 60 minutes to complete the polycondensation reaction. At this time, the stirring speed of the stirrer was 38 rpm, the temperature of the reaction liquid immediately before the end of the reaction was 289°C, and the stirring power was 1.00 kW. Next, the reaction liquid in the molten state was fed into a twin-screw extruder, and p-toluenesulfonate in an amount four times by mole relative to the cesium carbonate was fed from the first feed port of the twin-screw extruder and kneaded with the reaction liquid. Thereafter, the reaction liquid was extruded into strands through the die of the twin-screw extruder and cut with a cutter to obtain pellets of polycarbonate resin A2-1.
[0064] <Production Example 2: Production of Polycarbonate Resin A2-2> 26.14 moles (6.75 kg) of bisphenol C (BPC) and 26.79 moles (5.74 kg) of diphenyl carbonate were placed in an aluminum (SUS) reactor (internal volume: 10 L) equipped with a stirrer and a distillate condenser. The inside of the reactor was replaced with nitrogen gas, and the temperature was raised to 220°C in a nitrogen gas atmosphere over 30 minutes. Next, the reaction liquid in the reactor was stirred, and cesium carbonate (Cs2CO3) was added as a transesterification catalyst to the molten reaction liquid at a ratio of 1.5 × 10-6 The reaction solution was stirred and fermented in a nitrogen gas atmosphere at 220° C. for 30 minutes. Next, the pressure in the reactor was reduced to 100 Torr over 40 minutes at the same temperature, and the reaction was continued for another 100 minutes to distill off phenol. Next, the temperature in the reactor was raised to 284°C over 60 minutes, and the pressure was reduced to 3 Torr, and phenol equivalent to almost the entire theoretical amount was distilled out. Next, the pressure in the reactor was kept below 1 Torr at the same temperature, and the reaction was continued for another 60 minutes to complete the polycondensation reaction. At this time, the stirring speed of the stirrer was 38 rpm, the temperature of the reaction liquid immediately before the end of the reaction was 289°C, and the stirring power was 0.60 kW. Next, the reaction liquid in the molten state was fed into a twin-screw extruder, and p-toluenesulfonate in an amount four times by mole relative to the cesium carbonate was fed from the first feed port of the twin-screw extruder and kneaded with the reaction liquid. Thereafter, the reaction liquid was extruded into strands through the die of the twin-screw extruder and cut with a cutter to obtain pellets of polycarbonate resin A2-2.
[0065] The raw materials listed in Table 1 below were used. [Table 1]
[0066] <Measurement of viscosity average molecular weight (Mv) of polycarbonate resin> The viscosity average molecular weight (Mv) of the polycarbonate resin was calculated from the intrinsic viscosity (η) (unit: dL / g) at 20°C using an Ubbelohde viscometer with methylene chloride as a solvent, and the viscosity average molecular weight (Mv) was calculated from the following Schnell viscosity formula. η = 1.23 × 10 -4 Mv 0.83
[0067] <Measurement of pencil hardness of polycarbonate resin> The polycarbonate resin pellets were dried at 100°C for 5 hours, and then flat test pieces (150 mm x 100 mm x 2 mm thick) were produced using an injection molding machine (FANUC Corporation's "α-2000i-150B") under conditions of a cylinder setting temperature of 260°C, a mold temperature of 70°C, a screw rotation speed of 100 rpm, and an injection speed of 30 mm / sec. The pencil hardness of the obtained flat test piece (150 mm×100 mm×2 mm thick) was measured using a pencil hardness tester in accordance with ISO 15184 under a load of 750 g to determine the hardness. The pencil hardness tester used was a product of Toyo Seiki Co., Ltd.
[0068] <Weight average molecular weight (Mw) of (meth)acrylate polymer> The weight average molecular weight of the (meth)acrylate polymer is a value calculated as polystyrene (PS) as measured by gel permeation chromatography using chloroform as a solvent.
[0069] <Measurement of pencil hardness of (meth)acrylate polymer> The (meth)acrylate polymer was dried at 80°C for 5 hours, and then a flat test piece (150 mm x 100 mm x 2 mm thick) was produced using an injection molding machine ("α-2000i-150B" manufactured by Fanuc Corporation) under conditions of a cylinder setting temperature of 240°C, a mold temperature of 70°C, a screw rotation speed of 100 rpm, and an injection speed of 30 mm / sec. The pencil hardness of the obtained flat test piece (150 mm×100 mm×2 mm thick) was measured using a pencil hardness tester in accordance with ISO 15184 under a load of 750 g to determine the hardness. The pencil hardness tester used was a product of Toyo Seiki Co., Ltd.
[0070] 2. Examples 1 to 12, Comparative Examples 1 to 5 <Production of Resin Composition Pellets> Each component described in Table 1 above was blended at the ratios shown in Tables 2 to 4 below (expressed in parts by mass unless otherwise specified), and uniformly mixed using a tumbler mixer. Then, using a twin-screw extruder (TEX30α manufactured by Nippon Steel Corporation), it was fed into the extruder from the barrel at the upstream part of the extruder at a cylinder set temperature of 260°C, a screw rotation speed of 180 rpm, and a discharge rate of 30 kg / hr, and melt-kneaded to obtain resin composition pellets.
[0071] <Ratio (mol%) of the formula (2) in the polycarbonate resin> In Tables 2 to 4 described later, the "ratio (mol%) of the formula (2) in the polycarbonate resin" is an index indicating the content of the structural unit represented by the formula (2) in 100 mol% of the polycarbonate resin, and was calculated using the mixing ratio of the resins used and the molecular weight of the structural unit represented by the formula (2).
[0072] <Measurement of the pencil hardness of the resin composition> After drying the resin composition pellets at 100°C for 5 hours, using an injection molding machine ("α-2000i-150B" manufactured by Fanuc Corporation), a flat test piece (150 mm × 100 mm × 2 mm thick) was produced under the conditions of a cylinder set temperature of 280°C, a mold temperature of 70°C, a screw rotation speed of 100 rpm, and an injection speed of 30 mm / second. Regarding the flat test piece obtained above, in accordance with ISO 15184, the pencil hardness measured at a load of 750 g was determined using a pencil hardness tester. The pencil hardness tester used was manufactured by Toyo Seiki Co., Ltd.
[0073] <Melt volume rate (MVR)> After drying the above resin composition pellets at 100°C for 5 hours, using a melt indexer, in accordance with ISO1133, under the conditions of a measurement temperature of 300°C and a load of 11.8 N, MVR (unit: cm 3 / 10 min) was measured. The melt indexer used was manufactured by Toyo Seiki Co., Ltd.
[0074] <Production of ISO multi-purpose test pieces> The above resin composition pellets were dried at 80°C for 5 hours, and then molded into ISO multipurpose test pieces (4 mm thick) using an injection molding machine (Japan Steel Works, Ltd., "J55-60H") under conditions of a cylinder setting temperature of 280°C, a mold temperature of 70°C, a screw rotation speed of 100 rpm, an injection time of 2.0 seconds, and a molding cycle of 40 seconds.
[0075] <Unnotched Charpy impact strength> In accordance with ISO179, the above ISO multipurpose test piece (4 mm thick) was subjected to the unnotched Charpy impact strength test (unit: kJ / m 2 ) was measured.
[0076] <Deflection temperature under load> Using the above ISO multipurpose test piece (4 mm thick), the deflection temperature under load (unit: °C) was measured under a load of 1.80 MPa in accordance with ISO75-1 and ISO75-2.
[0077] <Whitening haze during molding (%)> The resin composition pellets obtained above were dried at 100°C for 5 hours, and then injection molded into flat test pieces measuring 90 mm x 60 mm x 1.5 mm in thickness using an injection molding machine (Sumitomo Heavy Industries, Ltd., "SE100DU") under conditions of a cylinder set temperature of 300°C, a mold temperature of 70°C, a screw rotation speed of 100 rpm, and an injection speed of 500 mm / sec. The haze (unit: %) of the flat test piece obtained above was measured using a haze meter. The haze meter used was a NDH-2000 type haze meter manufactured by Nippon Denshoku Industries Co., Ltd.
[0078] [Table 2]
[0079] [Table 3]
[0080] [Table 4]
[0081] As is clear from the above results, the resin composition of the present invention had high surface hardness when molded into a molded product, and was able to effectively suppress whitening even during high-speed molding or when forming a thin-walled molded product, and was excellent in impact resistance and heat resistance (Examples 1 to 12). In contrast, when the polycarbonate resin did not contain the structural unit represented by formula (2) (Comparative Examples 1 and 2), whitening occurred and the haze was high. In addition, when the content of the (meth)acrylate polymer was high (Comparative Examples 3 and 4), the impact resistance was poor. Furthermore, when the proportion of the structural unit represented by formula (1) in the polycarbonate resin was low (Comparative Example 5), the impact resistance and heat resistance were poor.
Claims
1. The composition comprises a polycarbonate resin and a (meth)acrylate polymer containing an aromatic (meth)acrylate structural unit (b1) and a methyl methacrylate structural unit (b2), The (meth)acrylate polymer is a (meth)acrylate polymer in which the total of the aromatic (meth)acrylate structural units (b1) and the methyl methacrylate structural units (b2) accounts for 90 mass % or more of all structural units excluding terminal groups, The content of the (meth)acrylate polymer is 18 to 32 parts by mass based on 100 parts by mass of the polycarbonate resin, The polycarbonate resin contains a structural unit represented by formula (1) and a structural unit represented by formula (2), The content (parts by mass) of the structural unit represented by formula (1) ≧ the content (parts by mass) of the structural unit represented by formula (2) ≧ the content (parts by mass) of the (meth)acrylate polymer, A resin composition comprising: The resin composition is molded into a flat test piece (150 mm x 100 mm x 2 mm thick), and the pencil hardness measured in accordance with ISO 15184 using a pencil hardness tester under a load of 750 g is F or harder. Formula (1) [Formula 1] (In formula (1), X 1 represents one of the following formulas: [Case 2] R 3 and R 4 each independently represents a hydrogen atom or a methyl group, and Z represents a group that bonds with C to form an alicyclic hydrocarbon having 6 to 12 carbon atoms which may have a substituent. Formula (2) [C3] (In formula (2), R 1 represents a methyl group, R 2 represents a hydrogen atom or a methyl group, X 2 represents one of the following formulas: [C4] R 3 and R 4 each independently represents a hydrogen atom or a methyl group, and Z represents a group that bonds with C to form an alicyclic hydrocarbon having 6 to 12 carbon atoms which may have a substituent.
2. The polycarbonate resin contains 53 to 90 mol % of a structural unit represented by formula (1) and 47 to 10 mol % of a structural unit represented by formula (2). The resin composition according to claim 1.
3. The (meth)acrylate polymer contains an aromatic (meth)acrylate structural unit (b1) and a methyl methacrylate structural unit (b2) in a mass ratio of (b1) / (b2) of 5-80 / 95-20. The resin composition according to claim 1 or 2.
4. The resin composition according to any one of claims 1 to 3, wherein the (meth)acrylate polymer has a weight average molecular weight of 5,000 to 30,000.
5. The resin composition according to any one of claims 1 to 4, wherein the haze of the resin composition when molded into a 1.5 mm thick flat plate-shaped test piece is 2.0% or less.
6. The resin composition according to claim 5 , wherein the flat test piece is obtained by injection molding the resin composition at an injection speed of 500 mm / sec.
7. When the resin composition is molded into an ISO multipurpose test piece (4 mm thick), the unnotched Charpy impact strength according to ISO 179 is 80 kJ / m 2 The resin composition according to any one of claims 1 to 6.
8. The resin composition according to any one of claims 1 to 7, wherein the resin composition has a deflection temperature under load of 1.80 MPa in accordance with ISO 75-1 and ISO 75-2 when molded into an ISO multipurpose test piece (4 mm thick) of 98 ° C. or higher. The resin composition according to any one of claims 1 to 7.
9. The resin composition according to any one of claims 1 to 8, which is for injection molding at an injection speed of 200 mm / sec or more.
10. The resin composition according to any one of claims 1 to 9, which is used for forming a thin-walled housing for a portable electronic device.
11. A molded article formed from the resin composition according to any one of claims 1 to 10.
12. The molded article according to claim 11, which is a thin-walled housing for a portable electronic device.
13. A method for producing a molded article, comprising injection molding the resin composition according to any one of claims 1 to 10.
14. The method for producing a molded article according to claim 13, wherein the injection molding is carried out at an injection speed of 200 mm / sec or more.
Citation Information
Patent Citations
Polycarbonate resin composition and light-conducting plate
JP1999158364A
Copolymerized polycarbonate resin composition and molded article
JP2013112780A
Polycarbonate resin molded article
JP2014019843A
Polycarbonate resin composition and molded article thereof
JP2014065901A
Polycarbonate resin composition and molded product
JP2017179331A