Polyamide resin composition
The polyamide resin composition, enhanced with a metal cyanide salt and redox oxygen absorber, addresses the issue of inadequate heat aging resistance in lower temperature ranges by improving mechanical strength retention in molded products.
Patent Information
- Application Number
- JP2020177259
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-22
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-10-22
AI Technical Summary
Existing polyamide resin compositions fail to provide adequate heat aging resistance in temperature ranges below 200°C, particularly between 150°C and 180°C, leading to reduced mechanical strength in molded products.
A polyamide resin composition is developed by blending a metal cyanide salt as an oxygen barrier agent and a redox oxygen absorber, such as cerium oxide or ferric oxide, in specific ratios to enhance heat aging resistance across a wider temperature range.
The composition exhibits improved heat aging resistance from 150°C to 200°C, maintaining high tensile strength retention in molded products, especially in welded areas, by preventing oxygen ingress and suppressing oxidation reactions.
Smart Images

Figure 0007567353000003 
Figure 0007567353000001 
Figure 0007567353000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyamide resin composition having improved heat aging resistance over a wide temperature range. [Background technology]
[0002] Polyamide resins have excellent mechanical properties, chemical resistance, moldability, and the like, and therefore have been widely used as molding materials for various parts such as automobile parts, electrical and electronic parts, and industrial machine parts. Although polyamide resins are a type of resin that is relatively excellent in heat aging resistance, a decrease in strength retention due to deterioration of the resin caused by heat is inevitable. For this reason, a method of adding copper halide, potassium halide, oxazole compound, or the like as a heat stabilizer has long been known as a method for improving the heat aging resistance of polyamide resins (see, for example, Patent Document 1).
[0003] Thanks to these technologies, polyamide resins are used as molding materials for parts in the fields of automobile parts and electric and electronic parts that are exposed to high-temperature environments of about 140° C. However, for example, with regard to the engine compartment of an automobile, the environmental temperature in the engine compartment has risen in recent years due to an increase in engine output and a higher density of parts, and heat aging resistance in a temperature environment higher than that previously assumed is now required.
[0004] In response to this, methods have been proposed that incorporate fine particle elemental iron into polyamide (see Patent Document 2), that incorporate finely dispersed metal powder into polyamide (see Patent Document 3), that incorporate a copper compound and iron oxide into a mixture of two types of polyamides with different melting points (see Patent Document 4), and that incorporate a heat stabilizer such as copper iodide and potassium iodide and a complex oxide such as iron tetroxide (containing iron (II) oxide) (see Patent Document 5). These methods are said to be capable of achieving heat aging resistance even in high temperature environments of around 200°C.
[0005] However, the methods of Patent Document 2 and Patent Document 3 are not easy to manufacture due to the risk of fire during the production of the composition, the method of Patent Document 4 has the drawback that it is effective only in very limited compositions, and the method of Patent Document 5 is inferior in heat aging resistance, stability of mechanical strength, and reproducibility. In other words, no matter which method is adopted, there is room for improvement.
[0006] Therefore, in order to solve these problems, the present inventor has already proposed a method of blending a metal cyanide salt having an oxygen barrier property imparting effect (see Patent Document 6). It has been shown that a polyamide resin composition employing the method of Patent Document 6 has excellent heat aging resistance in a high-temperature environment of 200°C without the drawbacks of the methods of Patent Documents 2 to 5. However, further investigation of this polyamide resin composition after that revealed that the effect of improving heat aging resistance was surprisingly low at temperatures lower than 200°C, particularly in the temperature range of about 150 to 180°C. Therefore, there is a demand for improvement in heat aging resistance in such a low-temperature environment. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Special Publication No. 7-47690 [Patent Document 2] Special Publication No. 2006-528260 [Patent Document 3] Special Publication No. 2008-527127 [Patent Document 4] Special Publication No. 2008-527129 [Patent Document 5] JP 2010-270318 A [Patent Document 6] JP 2017-95549 A Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made in consideration of such problems in the conventional technology, and an object of the present invention is to provide a polyamide resin composition which has improved heat aging resistance not only in a high-temperature environment of about 200°C, but also at lower temperatures, particularly in a temperature range of about 150 to 180°C, and which can exhibit heat aging resistance over a wider temperature range than conventional polyamide resin compositions. [Means for solving the problem]
[0009] As a result of extensive research by the present inventors to solve the problems of the conventional technology described above, the present inventors discovered that in order to improve the heat aging resistance of polyamide resins not only in high temperature environments of about 200°C but also in low temperature environments of about 150 to 180°C, it is effective to blend a redox-based oxygen absorber in an appropriate ratio in addition to a metal cyanide salt as a substance that can assist the gas (oxygen) barrier properties in low temperature environments, and thus completed the present invention. That is, the present invention comprises the following (1) to (8). (1) A polyamide resin composition comprising a polyamide resin (A), an oxygen barrier property imparting agent (B), and a redox-based oxygen absorber (C), characterized in that the contents of the oxygen barrier property imparting agent (B) and the redox-based oxygen absorber (C) are 0.1 to 5 parts by mass and 0.1 to 5 parts by mass, respectively, per 100 parts by mass of the polyamide resin (A). (2) The polyamide resin composition according to (1), wherein the oxygen barrier property imparting agent (B) is a metal cyanide salt represented by the following general formula: A x [M(CN) y ] In the formula, M is at least one of transition metal elements in groups 5 to 10 and periods 4 to 6 of the periodic table, A is at least one of alkali metals and alkaline earth metals, y is an integer from 3 to 6, x is a number calculated by (ym) / a, m is the valence of M, and a is the valence of A. (3) The polyamide resin composition according to (1) or (2), wherein M in the general formula is iron. (4) The polyamide resin composition according to any one of (1) to (3), wherein the metal cyanide salt represented by the general formula is selected from the group consisting of alkali metal hexacyanoferrate(II) and alkali metal hexacyanoferrate(III). (5) The polyamide resin composition according to any one of (1) to (4), wherein the redox-based oxygen absorber (C) is selected from the group consisting of oxides, hydroxides, halides, oxyhalides, various acid salts, and alcoholate compounds containing an iron element, oxides, hydroxides, halides, oxyhalides, various acid salts, and alcoholate compounds containing a cerium element, sodium dithionite (Na2S2O4), and oxides, hydroxides, halides, oxyhalides, various acid salts, and alcoholates of lanthanoid compounds. (6) The polyamide resin composition according to (5), wherein the redox-based oxygen absorber (C) is selected from the group consisting of ferric oxide, cerium oxide, and cerium hydroxide. (7) The polyamide resin composition according to any one of (1) to (6), further comprising a copper compound (D), the content of the copper compound (D) being 0.0001 to 1 part by mass in terms of elemental copper per 100 parts by mass of the polyamide resin (A). (8) The polyamide resin composition according to any one of (1) to (7), wherein the polyamide resin (A) is polyhexamethylene adipamide. Effect of the Invention
[0010] According to the present invention, it is possible to provide a polyamide resin composition having improved heat aging resistance over a range from a relatively low temperature of about 150 to 180° C. to a high temperature of about 200° C. As a result, a molded article made from the polyamide resin composition of the present invention exhibits high strength retention over a wide temperature range, and in particular, even in the welds of the molded article, which are generally considered to have inferior strength due to their structure, they can exhibit sufficient strength retention over a wide temperature range. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a diagram showing the shape of a molded product of a weld portion produced in the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The polyamide resin composition of the present invention contains a polyamide resin (A), an oxygen barrier property imparting agent (B), and a redox-based oxygen absorber (C), and is characterized in that the contents of the oxygen barrier property imparting agent (B) and the redox-based oxygen absorber (C) are 0.1 to 5 parts by mass and 0.1 to 5 parts by mass, respectively, per 100 parts by mass of the polyamide resin (A).
[0013] The polyamide resin (A) in the present invention is not particularly limited, and examples thereof include ring-opening polymers of cyclic lactams, polycondensates of aminocarboxylic acids, and polycondensates of dibasic acids and diamines. Specific examples thereof include aliphatic polyamides such as polycaproamide (polyamide (PA) 6), polyhexamethylene adipamide (polyamide 66), polytetramethylene adipamide (polyamide 46), polyhexamethylene sebacamide (polyamide 610), polyhexamethylene dodecamide (polyamide 612), poly-lauryllactam (polyamide 12), and poly-11-aminoundecanoic acid (polyamide 11); Examples of the polyamide resin suitable for the present invention include aliphatic-aromatic polyamides such as poly(metaxylene adipamide) (hereinafter abbreviated as MXD6), poly(hexamethylene terephthalamide) (hereinafter abbreviated as 6T), poly(hexamethylene isophthalamide) (hereinafter abbreviated as 6I), poly(nonamethylene terephthalamide) (hereinafter abbreviated as 9T), and poly(tetramethylene isophthalamide) (hereinafter abbreviated as 4I), as well as copolymers and mixtures thereof. Examples of the polyamide resin suitable for the present invention include polyamide 6, polyamide 66, polyamide 6 / 66 copolymer, polyamide 66 / 6T copolymer, polyamide 6T / 12 copolymer, polyamide 6T / 11 copolymer, polyamide 6T / 6I copolymer, polyamide 6T / 6I / 12 copolymer, polyamide 6T / 610 copolymer, and polyamide 6T / 6I / 6 copolymer.
[0014] The molecular weight of the polyamide resin (A) is not particularly limited, but the relative viscosity measured in 98% (98% by mass) sulfuric acid at a concentration of 1% by mass and at 25° C. is preferably 1.70 to 4.50. The relative viscosity of the polyamide resin (A) is more preferably 2.00 to 4.00, and further preferably 2.00 to 3.50.
[0015] The oxygen barrier agent (B) in the present invention is a substance capable of lowering the oxygen transmission rate (permeability) of the polyamide resin composition when added to the polyamide resin composition. Specifically, when the oxygen barrier agent (B) is contained in the polyamide resin composition at 5% by mass, the oxygen transmission rate of the polyamide resin composition measured by the method shown in the Examples can be lowered to 1 / 5 or less of the oxygen transmission rate of the polyamide resin itself. In this way, the oxygen barrier agent (B) capable of lowering the oxygen transmission rate is distributed on the surface of the molded body, and the molded body molded from the polyamide resin composition of the present invention effectively prevents oxygen from penetrating from the surface of the molded body into the inside of the molded body, and the oxygen concentration inside the molded body does not increase. Therefore, even if the molded body is exposed to a high-temperature environment of about 200°C, the oxidation reaction inside the molded body at high temperatures is suppressed, and as a result, the heat aging resistance of the molded body is improved.
[0016] The oxygen transmission rate of polyamide resins and polyamide resin compositions can be determined based on the gas permeability data described in the Polyamide Handbook (published January 30, 1988, edited by Osamu Fukumoto, p. 305), the Permacall values taught in M. Salame, "Prediction of gas barrier properties of high polymers," Polymer Engineering and Science, Vol. 26, No. 22, pp. 1543-1546, 1986, and JY Park, DRPoul, "Correlation and prediction of gas permeability in glassy polymer membrane materials via a modified free volume based group contribution method," Journal of Membrane Science, Vol. 125, pp. 23-39, 1997, and the like.
[0017] Specific examples of the oxygen barrier agent (B) include phenol resins, polyacrylonitrile, polyvinyl alcohol, metal cyanide salts, etc. Among these, metal cyanide salts are particularly preferred because they have excellent heat aging resistance in high temperature environments.
[0018] The metal cyanide salt is represented by the following general formula: A x [M(CN) y ] (In the formula, M is at least one of transition metal elements in groups 5 to 10 and periods 4 to 6 of the periodic table, A is at least one of alkali metals and alkaline earth metals, y is an integer of 3 to 6, and x is a number calculated by (ym) / a. Here, m is the valence of M, and a is the valence of A.) The metal cyanide salt may be in the form of a hydrate.
[0019] Examples of M in the above formula include Fe, Co, Cr, Mn, Ir, Rh, Ru, V, and Ni. Considering the valence of the metal element, Fe(II), Fe(III), Co(III), Cr(III), Mn(II), Mn(III), Ir(III), Rh(III), Ru(II), V(IV), V(V), Co(II), Ni(II), and Cr(II) are preferred, more preferably Co(II), Co(III), Fe(II), Fe(III), Cr(III), Ir(III), and Ni(II), and particularly preferably Fe(II) and Fe(III). M is not limited to one type, and two or more types of metal elements may be present in the metal cyanide salt, such as potassium hexacyanocobalt(II)ferrate(II). Examples of A include alkali metals Li, Na, and K, and alkaline earth metals Ca and Ba. y is an integer of 3 to 6. x is selected so that the metal cyanide salt is electrically neutral as a whole. In other words, x is a number calculated by (ym) / a (where m is the valence of M, and a is the valence of A). In particular, y corresponds to the coordination number of M, and is preferably 4 to 6, and more preferably 6.
[0020] Preferred examples of metal cyanide salts that can be used in the present invention include potassium hexacyanoferrate(II), potassium hexacyanoferrate(III), sodium hexacyanoferrate(II), sodium hexacyanoferrate(III), potassium hexacyanocobaltate(III), sodium hexacyanocobaltate(III), potassium hexacyanoruthenate(II), calcium hexacyanocobaltate(III), potassium tetracyanonickelate(II), potassium hexacyanochromate(III), potassium hexacyanoiridate(III), calcium hexacyanoferrate(II), potassium hexacyanocobaltate(II), and lithium hexacyanocobaltate(III). More preferred from the standpoint of ease of handling and safety are alkali metal hexacyanoferrate(II), such as potassium hexacyanoferrate(III), sodium hexacyanoferrate(II), and sodium hexacyanoferrate(III), and alkali metal hexacyanoferrate(III).
[0021] The redox-based oxygen absorber (C) in the present invention has a role of supporting the heat aging resistance improving action of the oxygen barrier property imparting agent (B), and particularly contributes to improving heat aging resistance under a low temperature environment of about 150 to 180 ° C that cannot be covered by the oxygen barrier property imparting agent (B). As described above, in the molded body molded from the polyamide resin composition of the present invention, the oxygen barrier property imparting agent (B) is distributed on the surface of the molded body, so that the intrusion of oxygen from the surface of the molded body into the inside of the molded body is effectively prevented, but there is still a possibility that oxygen may invade the inside of the molded body to a certain extent. In the present invention, this invaded oxygen is effectively absorbed by the redox-based oxygen absorber (C) distributed inside the molded body, and the increase in the oxygen concentration inside the molded body is suppressed. Therefore, the oxidation reaction inside the molded body at a low temperature of about 150 to 180 ° C is also suppressed, and as a result, the heat aging resistance of the molded body is improved over a wide temperature range. With regard to the effective temperature, the oxygen barrier agent (B) contributes to heat aging resistance mainly in high-temperature environments of about 200°C, while the redox-based oxygen absorber (C) contributes to heat aging resistance mainly in low-temperature environments of about 150 to 180°C. The reason for this is believed to be that in low-temperature environments of about 150 to 180°C, the rate of oxygen absorption by the redox-based oxygen absorber (C) exceeds the rate of reaction between the polyamide resin and oxygen.
[0022] Examples of the redox-based oxygen absorber (C) include oxides, hydroxides, halides, oxyhalides, various acid salts, and alcoholates containing iron such as iron element, ferric oxide, iron hydroxide, and iron pentacarbonyl; oxides, hydroxides, halides, oxyhalides, various acid salts, and alcoholates containing cerium such as cerium oxide and cerium hydroxide; sodium dithionite (Na2S2O4); oxides, hydroxides, halides, oxyhalides, various acid salts, and alcoholates of lanthanoid compounds (lanthanum, praseodymium, neodymium, promethium, samarium, europium, galidolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, etc.). Among these, ferric oxide, cerium oxide, and cerium hydroxide are particularly preferred because they have excellent heat aging resistance in a low-temperature environment.
[0023] In the polyamide resin composition of the present invention, it is important that the content of the oxygen barrier property imparting agent (B) and the redox-based oxygen absorber (C) are 0.1 to 5 parts by mass and 0.1 to 5 parts by mass, respectively, relative to 100 parts by mass of the polyamide resin (A). The content of the oxygen barrier property imparting agent (B) is preferably 0.3 to 4.5 parts by mass, more preferably 0.4 to 4.2 parts by mass, relative to 100 parts by mass of the polyamide resin (A). The content of the redox-based oxygen absorber (C) is preferably 0.3 to 4.5 parts by mass, more preferably 0.4 to 4.2 parts by mass, relative to 100 parts by mass of the polyamide resin (A). If the content of the oxygen barrier agent (B) and the redox oxygen absorber (C) is less than the lower limit, the effect of improving heat aging resistance over a wide temperature range may be poor, while if the content of the oxygen barrier agent (B) and the redox oxygen absorber (C) exceeds the upper limit, the effect of improving heat aging resistance will plateau and no further increase will be observed. In addition, when glass fibers are added to the polyamide resin composition for reinforcement, if the content of the redox oxygen absorber (C) exceeds the upper limit, the glass fibers may be broken due to the high hardness of the redox oxygen absorber (C), and the initial mechanical strength may be lower than the intended level. A similar tendency is also observed to some extent when the content of the oxygen barrier agent (B) exceeds the upper limit. The blending ratio of the oxygen barrier property imparting agent (B) and the redox-based oxygen absorber (C) is not particularly limited, but in order to effectively improve heat aging resistance in both high-temperature and low-temperature environments, it is preferable to blend the oxygen barrier property imparting agent (B) and the redox-based oxygen absorber (C) in a mass ratio of 6:1 to 1:6.
[0024] In the polyamide resin composition of the present invention, it is preferable to further blend a copper compound (D) in addition to the oxygen barrier agent (B) and the redox oxygen absorber (C) described above. The copper compound has a thermal stabilizing effect, and therefore can prevent or reduce discoloration of molded products in high-temperature environments.
[0025] Examples of the copper compound (D) that can be used in the present invention include copper acetate, copper iodide, copper bromide, copper chloride, copper fluoride, copper laurate, and copper stearate. These copper compounds may be used alone or in combination. Copper acetate, copper iodide, and copper bromide are preferred, and cupric bromide is particularly preferred. When the copper compound (D) is used, the amount of the copper compound (D) is 0.0001 to 1.0 part by mass as copper element in the copper compound (D) per 100 parts by mass of the polyamide resin (A). A more preferred amount is 0.0005 to 0.03 parts by mass, and a further more preferred amount is 0.0005 to 0.02 parts by mass. If the amount of the copper compound (D) is less than the above lower limit, the discoloration prevention effect may be poor in a more severe environment such as a high-temperature atmosphere and exposure to ultraviolet light. On the other hand, if the amount of the copper compound (D) is more than the above upper limit, the discoloration prevention effect in the above-mentioned severe environment may reach a plateau, and further, problems such as corrosion of the screw, cylinder, etc. of the mold, extruder, or molding machine may occur.
[0026] In addition, when the copper compound (D) is blended, it is preferable to use an alkali metal halide compound such as potassium iodide or potassium bromide in combination in order to prevent copper precipitation. The method of blending the copper compound (D) may be added at any stage of the production of the polyamide resin (A), and the method of addition is not limited. For example, it may be added to the raw material salt aqueous solution of polyamide, or it may be added by injecting into the molten polyamide during melt polymerization, or it may be melt-kneaded using an extruder, a molding machine, or the like after blending the powder or master batch of the copper compound with the polyamide pellets granulated after the polymerization is completed.
[0027] Furthermore, the polyamide resin composition of the present invention may contain auxiliary stabilizers such as antioxidants, such as hindered phenol-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, and amine-based antioxidants, and light stabilizers, such as hindered amine light stabilizers (HALS). These antioxidants and light stabilizers can prevent or reduce discoloration of molded products in high-temperature environments.
[0028] Known compounds can be used as the hindered phenol-based antioxidant. These compounds can be used alone or in combination. Among such hindered phenol-based antioxidants, phenols having two or more functional groups are preferred, such as 3,9-bis[2-{3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]2,4,8,10-tetraoxaspiro[5,5]undecane, N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxycinnamamide), 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)propionyloxy, and 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)propionyloxy. n-octadecyl-3-(4'-hydroxy-3',5'-di-tert-butylphenyl)propionate, and triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate] are particularly preferred, and semi-hindered types such as triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate] (IRGANOX245) are preferred because of their excellent discoloration prevention effect.
[0029] When a hindered phenol-based antioxidant is blended, the blending amount is preferably 0.05 to 3 parts by mass, more preferably 0.1 to 2 parts by mass, based on 100 parts by mass of the polyamide resin (A). If the blending amount of the hindered phenol-based antioxidant is less than the lower limit, the effect of preventing thermal discoloration may be insufficient, whereas if it exceeds the upper limit, the effect may reach saturation or blooming may occur on the surface of the molded article.
[0030] The phosphorus-based antioxidant may be at least one selected from inorganic and organic phosphorus-based antioxidants. Examples of inorganic phosphorus-based stabilizers include hypophosphites such as sodium hypophosphite, phosphites, and the like. As organic phosphorus-based stabilizers, commercially available organic phosphorus-based antioxidants of the phosphite type may be used, but organic phosphorus-containing compounds that do not generate phosphoric acid upon thermal decomposition are preferred. Examples of such organic phosphorus-containing compounds include triphenyl phosphite, diphenyl isodecyl phosphite, trisnonyl phosphite, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (HCA), 10-(3,5-di-tert-butyl-4-hydroxybenzyl)-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 10-decyloxy-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, and the like.
[0031] When a phosphorus-based antioxidant is blended, the blending amount is preferably 0.05 to 3 parts by mass, more preferably 0.1 to 2 parts by mass, based on 100 parts by mass of the polyamide resin (A). If the blending amount of the phosphorus-based antioxidant is less than the lower limit, the effect of preventing thermal discoloration may be insufficient, while if it exceeds the upper limit, flash may occur in the molded product. If an inorganic and an organic phosphorus-based antioxidant are used in combination, the blending amount of the antioxidant can be reduced.
[0032] Known compounds can be used as the amine antioxidant. Secondary arylamines can also be mentioned as the amine antioxidant. Secondary arylamines refer to amine compounds that contain two carbon radicals chemically bonded to a nitrogen atom, and at least one, preferably both, of the carbon radicals are aromatic.
[0033] When an amine-based antioxidant is blended, the blending amount is preferably 0.05 to 3 parts by mass, more preferably 0.1 to 2 parts by mass, based on 100 parts by mass of the polyamide resin (A). If the blending amount of the amine-based antioxidant is less than the lower limit, the effect of preventing thermal discoloration may be insufficient, whereas if the blending amount exceeds the upper limit, the effect may reach saturation or blooming may occur on the surface of the molded article.
[0034] Known compounds can be used as the sulfur-based antioxidant. When a sulfur-based antioxidant is used, the amount is preferably 0.05 to 3 parts by mass, more preferably 0.1 to 2 parts by mass, based on 100 parts by mass of the polyamide resin (A). If the amount of the sulfur-based antioxidant is less than the lower limit, the effect of preventing thermal discoloration may be insufficient, while if the amount exceeds the upper limit, the effect may reach saturation or blooming may occur on the surface of the molded article.
[0035] The light stabilizer is preferably one or more hindered amine light stabilizers (HALS).Preferably, the HALS is a compound derived from a substituted piperidine compound, particularly an alkyl-substituted piperidyl, piperidinyl or piperazinone compound, and a compound derived from a substituted alkoxy piperidinyl compound.As such a compound, known compounds can be used.
[0036] In the present invention, a mixture of a secondary arylamine and HALS can be used. A preferred embodiment contains at least two kinds of co-stabilizers, at least one of which is selected from the group of secondary arylamines and at least one of which is selected from the group of HALS. When a co-stabilizer mixture is blended, the total blend amount is preferably 0.5 to 10 parts by mass, more preferably 0.5 to 3 parts by mass, based on 100 parts by mass of the polyamide resin (A). If the total blend amount is less than the lower limit, the effect of improving heat aging resistance may be insufficient, while if it exceeds the upper limit, the effect may be saturated or blooming may occur on the surface of the molded article.
[0037] In the polyamide resin composition of the present invention, a filler can be further blended. This can significantly improve the strength, rigidity, heat resistance, etc. of a molded article obtained from the polyamide resin composition. Examples of the filler include glass fiber, carbon fiber, metal fiber, aramid fiber, asbestos, potassium titanate whisker, wollastonite, glass flakes, glass beads, talc, mica, clay, calcium carbonate, barium sulfate, titanium oxide, and aluminum oxide, and among them, chopped strand type glass fiber is preferably used. The blending amount of the filler is preferably 5 to 140 parts by mass, particularly preferably 5 to 100 parts by mass, based on 100 parts by mass of the polyamide resin (A).
[0038] Furthermore, one or more of conventional additives such as an ultraviolet absorber (e.g., resorcinol, salicylate, benzotriazole, benzophenone, etc.), a lubricant and a release agent, a nucleating agent, a plasticizer, an antistatic agent, and a colorant including a dye or pigment may be blended into the polyamide resin composition of the present invention in an amount of up to 5 parts by mass per 100 parts by mass of polyamide resin (A), within a range that does not impair the object of the present invention.
[0039] The polyamide resin composition of the present invention can contain each of the components described above. In the composition excluding the filler, the polyamide resin (A), the oxygen barrier property imparting agent (B) and the redox-based oxygen absorber (C) preferably account for 90 mass% or more in total, and more preferably 95 mass% or more.
[0040] The polyamide resin composition of the present invention can be prepared by incorporating or mixing the oxygen barrier property imparting agent (B), the redox oxygen absorber (C), and other additives into or with the polyamide resin (A). There are no particular limitations on the method, and examples of the method that can be used include a method in which all components are premixed and then kneaded in an extruder or kneader, and a method in which any part of the components is premixed in an extruder or kneader to obtain pellets, and then other components are kneaded and blended therewith.
[0041] The polyamide resin composition of the present invention can be made into a molded article by injection molding, extrusion molding, thermoforming, compression molding, or a so-called hollow process such as blow molding or die slide molding. In addition, the molded article can also be made into a molded article by subjecting the molded article to secondary processing, such as a welding process including vibration welding, hot plate welding, ultrasonic welding, etc. The molded article is preferably an injection molded or blow molded article, or a molded article obtained by secondary processing thereof.
[0042] Examples of applications of the molded article of the polyamide resin composition of the present invention include, in the automobile and vehicle fields, for example, cylinder head covers, engine covers, housings for intercoolers, valves, end caps, casters, trolley parts, etc., as well as intake system parts such as intake pipes (air ducts), especially intake manifolds, connectors, gears, fan wheels, coolant storage containers, housings or housing members for heat exchangers, radiators, thermostats, coolant and water pumps, heaters, fastening elements, oil pans, exhaust systems such as mufflers, housings for catalytic converters, timing chain belt front covers, gear boxes, bearing retainers, gasoline caps, seat parts, headrests, door handles, wiper parts, etc. In the electrical / electronics field, examples include circuit board parts, housings, films, conductors, switches, terminal strips, relays, resistors, capacitors, coils, lamps, diodes, LEDs, transistors, connectors, controllers, memories, bolts, coil bobbins, plugs, plug parts, mechatronics parts, home appliance parts such as cooking appliances, washing machines, refrigerators, air conditioners, sensors, etc. In the fields related to daily life and furniture and building materials, examples include parts for wheelchairs, stroller parts, chair legs, armrests, handrails, window frames, doorknobs, etc.
[0043] Since the polyamide resin composition of the present invention has the configuration as described above, a molded article formed therefrom can have excellent heat aging resistance, in which the tensile strength retention rate is 70% or more in both general parts and weld parts even after heat treatment for 1,000 hours at a wide high temperature range of 150°C, 180°C, and 200°C in the heat aging resistance test described in the Examples section below. EXAMPLES
[0044] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The measured values described in the examples were measured by the following methods.
[0045] (2) Heat aging resistance As an index of heat aging resistance, molded articles were prepared from each of the resin compositions of the Examples and Comparative Examples, and the tensile strength retention was measured after treatment for 1000 hours at 200° C., 180° C., or 150° C. Two types of molded articles were prepared: a molded article of a general portion having no welds, and a molded article of a weld portion having a weld.
[0046] Specifically, for the molded products of the general parts, a Toshiba Machine IS-100 was used, the cylinder temperature was set to 280°C, and a mold temperature was set to 90°C to obtain molded products (shape conforming to ISO178: thickness 4mm, width 10mm), which were used as test samples. For the molded products of the welded parts, a Toshiba Machine IS-100 was used, the cylinder temperature was set to 280°C, and a mold temperature was set to 90°C to obtain ISO dumbbell molded products (thickness 4mm, width 10mm: shape see Figure 1) with a weld in the center, which were used as test samples. Next, the test samples were heat-treated in a recirculating air oven (Hot air circulation dryer NH-401S, Nagano Scientific Machinery Works) at 200°C, 180°C, or 150°C for a specified test time (1000 hours) according to the procedure detailed in ISO2578. After treatment, the test samples were removed from the oven, cooled to room temperature, and sealed in aluminum-lined bags until they were ready for tensile strength measurements. The tensile strength of the test samples was then measured according to ISO 527-1,2. The average value obtained from the three test samples was taken as the tensile strength. The tensile strength retention was then calculated as the percentage (%) of the tensile strength at the time point after heat treatment relative to the tensile strength at the initial time point without heat treatment.
[0047] Examples 1 to 17, Comparative Examples 1 to 7 Raw materials used Polyamide resin (A) Polyamide 66: Relative viscosity RV=2.7 Rhodia Stabamid 27AE1K Polyamide 6: Relative viscosity RV=2.7 Shuseisha TP-4208 Polyamide MXD-6: Relative viscosity RV=2.1 Toyobo T-600 Polyamide 6I / 6T: Relative viscosity RV=2.1 EMS Grivory G21 Oxygen barrier agent (B) Potassium ferrocyanide trihydrate (potassium hexacyanoferrate(II) trihydrate): Manufactured by Wako Pure Chemical Industries, Ltd., purity 99% Potassium ferricyanide (potassium hexacyanoferrate(III)): Manufactured by Wako Pure Chemical Industries, purity 99% Redox oxygen absorber (C) Cerium oxide: Wako Pure Chemical Industries, purity 99.9% Cerium hydroxide: Wako Pure Chemical Industries, purity 99.9% Ferric oxide: Wako Pure Chemical Industries, purity 99.9% Copper compound (D) Cupric bromide: Wako Pure Chemical Industries, purity 99.9% Antioxidants Hindered phenol stabilizer: BASF Irganox 245 filling material Glass fiber: Nippon Electric Glass Co., Ltd. T-275H Carbon fiber: TENAX-J HT C413 manufactured by Teijin Fibers
[0048] The above raw materials were blended in the ratios (parts by mass) shown in Table 1 below using a twin-screw extruder (STS35 manufactured by Coperion), melt-kneaded, and pellets (diameter about 2.5 mm x length about 2.5 mm) of the resin compositions of Examples 1 to 17 and Comparative Examples 1 to 7 were obtained. The obtained pellets were dried at 100°C for 4 hours or more in a hot air circulation dryer, and then used to prepare molded products, and the oxygen permeability and heat aging resistance were evaluated by the above-mentioned methods. The results are shown in Table 2 below.
[0049] [Table 1]
[0050] The full names of the abbreviations in Table 1 are as follows: PA66: Polyamide 66 PA6: Polyamide 6 MXD6: Poly(metaxylene adipamide) PA6I / 6T: Poly(hexamethylene isophthalamide) / Poly(hexamethylene terephthalamide)
[0051] [Table 2]
[0052] As is clear from Tables 1 and 2, in Examples 1 to 17 which satisfy all the requirements of the present invention, the tensile strength retention rate after 200°C, 180°C, or 150°C x 1000 hours treatment is 70% or more in both the general part and the weld part, achieving a high tensile strength retention rate over a wide temperature range and improving heat aging resistance. On the other hand, in Comparative Example 1, which has a too small content of oxygen barrier property imparting agent (B) compared to Example 1, the tensile strength retention rate after 200°C x 1000 hours treatment is low, especially in the weld part compared to the general part, and the heat aging resistance in a high temperature environment is poor. In Comparative Example 2, which has a too small content of redox-based oxygen absorber (C) compared to Example 1, the tensile strength retention rate after 150°C and 180°C x 1000 hours treatment is low, especially in the weld part compared to the general part, and the heat aging resistance in a low temperature environment is poor. Comparative Example 3, in which the content of the oxygen barrier property imparting agent (B) is too high compared to Example 1, is almost equal to or better than Example 1 in terms of the effect of improving heat aging resistance, but has inferior initial tensile strength. Comparative Example 4, in which the content of the redox-based oxygen absorber (C) is too high compared to Example 1, is almost equal to or better than Example 1 in terms of the effect of improving heat aging resistance, but has inferior initial tensile strength. Comparative Example 5, in which the content of the oxygen barrier property imparting agent (B) and the content of the redox-based oxygen absorber (C) are both too low compared to Example 1, has a lower tensile strength retention rate after 1000 hours of treatment than Example 1 under all temperature conditions of 200°C, 180°C, and 150°C, and is inferior in heat aging resistance both under high temperature and low temperature environments. Comparative Example 6, in which the content of both the oxygen barrier property imparting agent (B) and the content of the redox-based oxygen absorber (C) are too high compared to Example 1, is almost equal to or better than Example 1 in terms of the effect of improving heat aging resistance, but has inferior initial tensile strength. Comparative Example 7, which does not contain either the oxygen barrier property imparting agent (B) or the redox-based oxygen absorber (C) compared to Example 1, has a significantly lower tensile strength retention rate after 1000 hours of treatment compared to Example 1 under all temperature conditions of 200°C, 180°C, and 150°C, and is significantly inferior in heat aging resistance under both high temperature and low temperature environments. [Industrial Applicability]
[0053] According to the present invention, it is possible to provide a polyamide resin composition having improved heat aging resistance over a range from about 150 to 180° C. to a high temperature of about 200° C. Molded articles made from the polyamide resin composition of the present invention exhibit high strength retention over a wide temperature range, and in particular, even in welds of molded articles that are generally considered to have poor strength due to their structure, they can exhibit sufficient strength retention over a wide temperature range. Therefore, the polyamide resin composition of the present invention is extremely useful as a molding material for parts of automobiles and electric / electronic products that are constantly exposed to high temperatures.
Claims
1. A polyamide resin composition comprising a polyamide resin (A), an oxygen barrier property imparting agent (B), and a redox-based oxygen absorber (C), wherein the contents of the oxygen barrier property imparting agent (B) and the redox-based oxygen absorber (C) are 0.1 to 5 parts by mass and 0.1 to 5 parts by mass, respectively, relative to 100 parts by mass of the polyamide resin (A); The oxygen barrier property imparting agent (B) is a metal cyanide salt represented by the following general formula: A x [M(CN) y ] In the formula, M is at least one of transition metal elements in Groups 5 to 10 and Periods 4 to 6 of the Periodic Table, A is at least one of alkali metals and alkaline earth metals, y is an integer from 3 to 6, x is a number determined by (y-m) / a, m is the valence of M, and a is the valence of A. A polyamide resin composition, wherein the redox type oxygen absorber (C) is selected from the group consisting of ferric oxide, cerium oxide, and cerium hydroxide.
2. 2. The polyamide resin composition according to claim 1, wherein M in the general formula is iron.
3. 3. The polyamide resin composition according to claim 1, wherein the metal cyanide salt represented by the general formula is selected from the group consisting of alkali metal hexacyanoferrate (II) and alkali metal hexacyanoferrate (III).
4. The polyamide resin composition according to any one of claims 1 to 3, further comprising a copper compound (D), the content of the copper compound (D) being 0.0001 to 1 part by mass in terms of elemental copper per 100 parts by mass of the polyamide resin (A).
5. 5. The polyamide resin composition according to claim 1, wherein the polyamide resin (A) is polyhexamethylene adipamide.
Citation Information
Patent Citations
Polyamide stabilization, stabilizing composition therefor and stabilized polyamide
JP1985208357A
Ink jet unit
JP1995047690A
Heat stable molding composition
JP2006528260A
Heat stabilized molding composition
JP2008527127A
Heat stabilized molding composition
JP2008527129A