Method for producing polyalkylene ether glycol
By adding a compound with a specific solubility parameter difference to the polyalkylene ether glycol and alkanol mixture, the method addresses foam suppression and alkanol removal inefficiencies, enhancing the production efficiency of polyalkylene ether glycol.
Patent Information
- Application Number
- JP2021015953
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-03
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-02-03
AI Technical Summary
Existing methods for producing polyalkylene ether glycol face challenges with insufficient foam suppression and inefficient removal of alkanols during the alcoholysis reaction, leading to prolonged processing times and equipment complexity.
A specific compound is added to the mixture of polyalkylene ether glycol and alkanol to suppress foaming and enhance alkanol removal, using a method that includes specific solubility parameter differences and controlled reaction conditions.
The method effectively suppresses foaming and efficiently removes alkanol from the mixture, improving the production process by ensuring rapid and complete alkanol extraction.
Smart Images

Figure 0007567526000002 
Figure 0007567526000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyalcohol, which is a raw material for polyurethane, polyurethane urea, polyester, etc. The present invention relates to a method for producing polyethylene ether glycol. [Background technology]
[0002] Polyalkylene ether glycols, especially polytetramethylene ether glycols PTMG (hereinafter sometimes abbreviated as "PTMG") is a thermosetting polyurethane, thermoplastic Used as raw material for polyesters such as urethane, polyurethane urea, and thermoplastic elastomers It has been done.
[0003] A method for producing polyalkylene ether glycol includes, for example, using an acid catalyst and acetic anhydride. In the presence of a carboxylic acid anhydride such as and reacting the resulting diester with a tert-butyl glycol dicarboxylic acid ester of the tert-butyl glycol. Polyalkylene ether glycol is produced by alcoholysis reaction with an alkanol such as methanol. The diester of glycol was converted to polyalkylene ether glycol, and the resulting polyalkyne The alkanol contained in the alkylene ether glycol is distilled off. In Patent Document 1, diesters of polyalkylene ether glycols are reacted in the presence of a catalyst. is converted to polyalkylene ether glycol by alcoholysis reaction with alkanols. In the method, the alkanoic acid contained in the produced polyalkylene ether glycol is It is disclosed that the water content of the cellulose is returned to the reaction system.
[0004] In Patent Document 2, the reaction of acyloxy group-containing polytetrahydrofuran with alcohol is carried out. Method for producing polytetrahydrofuran having terminal hydroxyl groups by transesterification The process describes the use of a specific reactor for foam suppression. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2006-291189 A [Patent Document 2] Japanese Patent Application Publication No. 11-158263 Summary of the Invention [Problem to be solved by the invention]
[0006] However, in the previously known methods, polyalkylene ethylene obtained by the alcoholysis reaction When removing alkanol from a mixture containing ether glycol and alkanol, Foam control may be insufficient and require removal in small amounts over a long period of time, or may be inappropriate for certain manufacturing facilities. It was necessary to use equipment to suppress and eliminate foaming under certain manufacturing conditions.
[0007] The present invention has been made in view of the above problems, and provides a method for performing alcoholysis by a simple operation. From the mixture containing the polyalkylene ether glycol and the alkanol obtained by the reaction, Polyalkylene ether that can suppress foaming and efficiently remove alkanol The present invention aims to provide a method for producing glycol. [Means for solving the problem]
[0008] As a result of investigations aimed at solving the above problems, the present inventors have found that poly(ethylene glycol) obtained by alcoholysis reaction A mixture containing alkylene ether glycol and alkanol contains a specific compound in a specific amount. By adding this, it is possible to suppress the occurrence of problems such as foaming, and the alkali from the mixture can be prevented. The present invention has been accomplished based on the discovery that the above-mentioned method can efficiently remove alcohol. The present invention was achieved based on such findings and includes the following features [1] to [4]. This is our intention.
[0009] [1] Alcoholization of diesters of polyalkylene ether glycols with alkanols A process for producing a mixture containing polyalkylene ether glycol and an alkanol by a reaction with an alkylene glycol. In the process, a compound is added to the mixture to remove alkanol to produce a crude alkylene ether glycol. In a method for producing a polyalkylene ether glycol, the method comprises the steps of: The solubility parameter SP a of the polyalkylene ether glycol The absolute value of the difference between the polyamine and the compound b is 12.9 or more, and the amount of the compound added is The amount of polyalkyne ether glycol is 3% by mass or more and 20% by mass or less. A method for producing xylene ether glycol. [2] The polyalkylene ether glycol is polytetramethylene ether glycol. The method for producing a polyalkylene ether glycol according to [1], [3] The alkanol according to [1] or [2], wherein the alkanol is a C1 to C4 alkanol. A method for producing polyalkylene ether glycol. [4] The temperature for removing the alkanol is 60°C or higher and 250°C or lower. 4. A method for producing the polyalkylene ether glycol according to any one of claims 1 to 3. [5] The concentration of polyalkylene ether glycol in the mixture is 30% by mass or more and 90% by mass or more. The polyalkylene ether glycol according to any one of [1] to [4], A method for producing the [6] The number average molecular weight of the polyalkylene ether glycol is 600 or more and 8000 or less. The present invention relates to a method for producing a polyalkylene ether glycol according to any one of [1] to [5] below. Construction method. Effect of the Invention
[0010] By carrying out the method for producing polyalkylene ether glycol of the present invention, it is possible to obtain a wide range of products, such as foaming, The occurrence of the above problems is suppressed, and the polyalkylene ether glycol and the alkanol are contained. It is possible to efficiently remove the alkanol from the mixture. [Brief description of the drawings]
[0011] [Figure 1] Schematic diagram of a glass heating type low boiling separation device used in the examples DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The manufacturing method of the present invention will be described in detail below. Although the present invention has been described based on exemplary embodiments, it is not limited to such embodiments. In this specification, the numerical ranges expressed using "~" do not necessarily mean "~" This means a range that includes the numbers written before and after as the lower and upper limits.
[0013] As the diester of polyalkylene ether glycol used in the production method of the present invention, Any conventionally known polyalkylene ethers can be used. The diester of terglycol is easily soluble in alkanol, and the effect of the present invention is evident. Since the dicarboxylic acid ester of polyalkylene ether glycol is preferable, Hereinafter, the diester of polyalkylene ether glycol will be referred to as polyalkylene ether. An example of a dicarboxylic acid ester of terglycol will be described.
[0014] The method for producing a dicarboxylic acid ester of a polyalkylene ether glycol is Once the dicarboxylic acid ester of the ethylene ether glycol is prepared, it can be produced by any suitable method. The dicarboxylic acid ester of polyalkylene ether glycol is, for example, It can be obtained by ring-opening polymerization of a cyclic ether in the presence of a carboxylic acid anhydride and an acid catalyst.
[0015] Cyclic ethers have a lower polymerizability if the ring that constitutes them has a large number of carbon atoms. The number of carbon atoms constituting the ring is usually 2 to 10, and preferably 2 to 6. Ethers include, specifically, tetrahydrofuran (THF), ethylene oxide, propylene oxide, and ethylene glycol. oxetane, tetrahydropyran, oxepane, 1,4-dioxane, etc. Cyclic ethers, and one or more selected from these and their derivatives Used in combination. When two or more cyclic ethers are combined, one of them is difficult to polymerize. Even if the cyclic ether derivative is a cyclic ether, it is preferable because the polymerization proceeds easily. The cyclic ether is substituted with an alkyl group, an aryl group, an acyl group, a halogen atom, or the like. Here, the alkyl group, aryl group, acyl group, etc. may be further substituted. The alkyl group, aryl group, acyl group, etc. may further have a substituent. Examples of the aryloxy group include an alkoxy group, an aryloxy group, an acyloxy group, and an arylalkyl group. , acylalkyl group, alkoxyalkyl group, acyloxyalkyl group, aryloxy group Examples of the cyclic ether include alkyl groups and halogenated alkyl groups. More specifically, the derivatives of tetrahydrofuran, 3-methyloxetane, 3,3-dimethyloxetane, 3-chloromethyl ethyl-3-ethyloxetane, 3,3-bischloromethyloxetane, and the like. Among these, it is known to be easy to polymerize and has excellent physical properties when made into polyurethane resins. Therefore, tetrahydrofuran is preferred.
[0016] The carboxylic acid used is an aliphatic or aromatic carboxylic acid. The number of carbon atoms in the carboxylic acid is The number of carbon atoms is usually 2 to 12, preferably 2 to 8. Specific examples of the carboxylic acid include Examples include acetic acid, propionic acid, butyric acid, maleic acid, succinic acid, phthalic acid, and benzoic acid. Among these, acetic acid, which has a small molecular weight, is preferred because it can control the molecular weight with a small amount. Used.
[0017] Examples of the carboxylic acid anhydride include the anhydrides of the above-mentioned carboxylic acids. Water may react with the trace amount of water in the reaction system and some of it may become carboxylic acid. In order not to complicate the reaction system, a carboxylic acid-free compound corresponding to the carboxylic acid used in the present invention is used. It is preferable to use a diester of polyalkylene ether glycol. The carboxylic acid and carboxylic anhydride used in the production of the acetic acid are acetic acid and acetic anhydride. is particularly preferred.
[0018] The concentration of the carboxylic acid anhydride in the raw material solution is adjusted to the desired concentration of the polyalkylene ether glycol. The lower limit varies depending on the molecular weight of the catalyst and the type of catalyst, but is usually 0.1 mass %, preferably 0.5 mass %. The upper limit is usually 30% by mass, preferably 15% by mass. The ratio (molar ratio) of the carboxylic acid to the carboxylic acid anhydride is usually 0-50. Acid catalysts are used in a wide range of applications, including activated clay, zeolite, and super-strong acid ion exchange, because they are easy to separate and remove after polymerization. A solid acid catalyst such as an ion exchange resin or a composite metal oxide is preferably used. The catalyst concentration in the reaction solution is For example, when the reaction is carried out in a suspension bed, the concentration is usually 0.1 to 20% by mass.
[0019] The reactor used for producing the diester of polyalkylene ether glycol is Any type of reactor can be used to produce diesters of ethylene ether glycols. As a reactor for producing a diester of a polyalkylene ether glycol For example, a known system such as a fixed bed or a suspended bed can be used. The reaction temperature may be appropriately set, but the lower limit is usually 10° C., preferably 30° C. The upper limit is usually 80° C., preferably 50° C. If the reaction temperature is higher than the lower limit, the reaction If the reaction temperature is lower than the upper limit, the cyclic ether will not boil. This is preferable because it is difficult to
[0020] The reaction pressure may be appropriately selected within a range in which the reaction liquid remains liquid. The reaction pressure is usually normal pressure. The pressure is preferably from normal pressure to 0.5 MPa, and more preferably from normal pressure to 0.3 MPa. However, construction costs are high and the equilibrium conversion rate decreases as the temperature increases. The reaction can also be carried out under reduced pressure. The reaction is usually carried out under an inert gas such as nitrogen. The reaction is carried out in an atmosphere that does not inhibit the reaction. The residence time of the liquid is determined by the activity and concentration of the catalyst. If the residence time of the reaction liquid in the reactor is short, the conversion rate will be low, and if it is long, the conversion rate will approach equilibrium and will not appear to be high. Since the reaction rate decreases with time, the reaction time is usually 0.5 to 15 hours.
[0021] The polymerized reaction solution contains the desired polyalkylene ether glycol diester as well as Since unreacted raw materials are contained in the reaction mixture, they are usually removed by distillation. The reaction is usually carried out under normal pressure or reduced pressure. The material may be purified and reused as necessary. The polyalkylene ether glycol diester used in the present invention is, for example, TH Dicarboxylic acids of polytetramethylene ether glycol (PTMG) obtained by ring-opening polymerization of F The ester (PTME) is particularly preferred.
[0022] The mixture containing the polyalkylene ether glycol and the alkanol in the present invention is A diester of polyalkylene ether glycol and an alkanol are mixed to obtain an alcohol. The alcoholysis reaction is carried out in the presence of a catalyst for the alcoholysis reaction (hereinafter sometimes referred to as the "catalyst"). This is obtained by The alkanol is preferably a C1 to C4 alkanol, and the smaller the molecular weight, the greater the difference in molecular weight. Methanol, ethanol, and propane are preferred because they have a large number of moles by mass and are favorable for the progress of the reaction. Alcohol is preferred, methanol and ethanol are more preferred, and methanol is particularly preferred. The ratio of the alkanol to the diester of polyalkylene ether glycol in the raw liquid is The lower limit of the mass ratio is preferably 0.3, more preferably 0.6, and the upper limit is preferably 0.5. The limit is preferably 3.0, more preferably 2.0. If the content is equal to or higher than the lower limit, the reaction solution will have a suitable viscosity and the reaction will proceed smoothly. When the amount of alkanoate is equal to or less than the upper limit, the scale of the apparatus can be kept reasonable, and excessive alkanoate can be avoided. It is easy to remove the grease.
[0023] The catalyst is preferably an alkali metal alkoxide. Specific examples of the sodium methoxide include sodium ethoxide, sodium isopropyl Sodium compounds such as potassium propoxide, potassium methoxide, potassium ethoxide, potassium Among these, sodium compounds such as potassium compounds, In addition, since the smaller the molecular weight, the cheaper it is in small quantities, sodium methoxide is particularly preferred. The amount of the alkali metal alkoxide used is preferably 100 to 2000 ppm based on the reaction solution. Usually 0.002% by mass, preferably 0.005% by mass, more preferably 0.01% by mass, The upper limit is usually 0.1 mass%, preferably 0.03 mass%, and more preferably 0.02 mass%. If the amount of alkali metal alkoxide used is more than the above lower limit, the reaction rate is low. It is preferable that the content is equal to or less than the upper limit above, and it is preferable in that the remaining catalyst can be easily removed.
[0024] Specific examples of the method for supplying each raw material and catalyst to the reactor include The liquids in each tank are pumped to the mixing tank while controlling the flow rate, and mixed. One method is to mix the liquid in the tank until it becomes uniform, and then subject it to the alcoholysis reaction. Here, the catalyst is usually used in a small amount in a solid state, so the alkanol of the catalyst It is preferable to provide the catalyst as a solution. The catalyst solution in alkanol is commercially available sodium methoxide. It is convenient to use a solution of the toxide in methanol.
[0025] The type of reactor used in the alcoholysis reaction is a reactor for producing polyalkylene ether glycol. Preferably, any type of reactor may be used, and multiple reactors may be combined. The reactors used in the alcoholysis reaction are such that at least one of the reactors is a heating source. It is preferable that the reactor is provided with a reboiler. Specific examples of reactors include batch reactors, continuous stirring tanks, tubular reactors, and reactive distillation columns. Among these, reactive distillation columns equipped with a heater at the bottom are known to be efficient. Therefore, it is preferable to carry out at least a part of the alcoholysis reaction in a reactive distillation vessel. preferable.
[0026] In addition, before the reactive distillation, an alcoholysis reaction is carried out in a pre-stage reactor such as a tubular reactor or a continuous stirring tank. After partial completion of the alcoholysis reaction, the alcoholysis reaction may be completed in the reactive distillation column. When using a pre-stage reactor, the load on the reactive distillation column decreases as the conversion rate in the pre-stage reactor increases. It is preferable to carry out the reaction so that the ester exchange rate is 85% or more of the equilibrium conversion rate. When a reactor is used, the alkyl carboxylate by-produced in the reactor is removed by a known method such as distillation. As a pre-reactor, a tubular reactor is used because of its low construction cost. When the reaction is carried out in a first-stage reactor, the temperature is increased as the pressure increases. The reaction rate can be increased, but the higher the pressure, the higher the reactor construction costs. The pressure during reaction is usually 0.1 MPa, preferably 0.5 MPa, and the upper limit is usually The pressure is usually 5 MPa, preferably 3 MPa. The lower limit of the temperature during the first stage reaction is usually 4 0°C, preferably 110°C, and the upper limit is usually 250°C, preferably 180°C. In the case of a tubular reactor, the residence time during the first stage reaction is usually 2 minutes, preferably 5 minutes. The residence time during the first stage reaction is usually 60 minutes, and preferably 20 minutes. In the case of a continuous stirring tank, the lower limit is usually 0.5 hours, preferably 1 hour, and the upper limit is usually 15 hours. The heating time during the first stage reaction is preferably 10 hours. A tubular reactor can be used as the first reactor. When using a heat exchanger, the reaction liquid is heated to the reaction temperature in a heat exchanger and fed to a reactor insulated with a heat insulating material. This is simple and preferable.
[0027] When a reactive distillation column is used as a reactor, the reactive distillation column is provided with a reflux device at the top and a reboiler at the bottom. A commonly used column such as a packed column or a plate column equipped with a filter can be used. In order to ensure sufficient reaction time for the reaction to proceed, the reaction distillation column is placed below the feed tray. For the recovery stage, it is preferable to use a tray tower equipped with trays. Trays, perforated trays, valve trays, etc. are used. Bubble cap trays have a wide range of stable operation. However, the structure is complicated and the cost tends to be high. Perforated trays have a simple structure and low pressure loss. Although the loss is small, it has the disadvantage of a narrow range of stable operation. As a form, a bubble tray, which has the advantages of both, is particularly suitable. Above the feed tray (concentration tray), the distillation of by-produced alkyl carboxylate and alkanol is mainly performed. Since this is the part where separation takes place, any ordinary distillation equipment will do, and it does not necessarily have to be a tray column. The more theoretical plates in the distillation column, the easier it is to complete the reaction, but Since the cost of purification increases, the number of plates in the enrichment section is preferably 1 to 10 and the number of plates in the stripping section is preferably 5 to 40.
[0028] The heating device at the bottom of the reactive distillation column is specifically a forced circulation reboiler or a steam boiler. A known method such as a natural circulation reboiler using a mosiphon is used. In the evaporator, the viscosity of the reaction liquid increases due to the evaporation of alkanol, so forced circulation is required. A reboiler type is preferred. The reaction pressure of the reactive distillation column may be appropriately selected within a range in which the reaction liquid remains liquid. In terms of being able to increase the reaction temperature to increase the reaction rate and suppressing foaming of the reaction solution, On the other hand, from the viewpoint of the construction cost of the equipment, it is preferable that the reaction pressure is low. When a stage reactor is used, the reactive distillation column usually has a more complicated structure than the pre-stage reactor, so It is easier to reduce construction costs by setting the reaction pressure lower in the reactive distillation column than in the pre-reactor. If the pressure of the reactive distillation column is set lower than that of the upstream reactor, the carvone produced as a by-product in the upstream reactor This is also preferred in that the alkyl acid can be flash evaporated when it is fed to the reactive distillation column. The reaction pressure of the reactive distillation column is usually normal pressure, preferably 0.2 MPa. More preferably, it is 0.5 MPa. The upper limit is usually 2.0 MPa, preferably 1.0 MPa. It's better to be a.
[0029] The reaction temperature of the reactive distillation column may be appropriately set depending on the reaction pressure. Typically, for example, the lower limit of the column bottom temperature is usually 60° C., preferably 100° C., and the upper limit is The reaction temperature is usually 180° C., preferably 160° C. If the reaction temperature is equal to or higher than the lower limit, This is preferred because the reaction rate is fast. In addition, when the reaction temperature is equal to or lower than the upper limit, the temperature is maintained. This is preferable in terms of reducing construction costs because the pressure required for the reaction can be low. This can be adjusted by adjusting the flow rate or temperature of the heat medium, which is the heat source of the heat exchanger.
[0030] The reaction is usually carried out in an atmosphere that does not inhibit the reaction of the present invention, such as an inert gas such as nitrogen. When a reaction is carried out continuously, the residence time of the reaction liquid in the reactor depends on the activity and concentration of the catalyst, etc. In the case of a continuous reaction, the residence time of the reaction liquid in the reactor is determined by Therefore, it usually takes 10 to 30 minutes. The reflux ratio during the reaction varies depending on the raw material composition and the number of stages in the distillation column, but is usually 0.5 to 20. The reflux ratio is preferably 1.0 to 10.0. If the reflux ratio is less than the upper limit, the liquid on the tray may become oxidized. Since the solvent concentration is high, the reaction rate is high, which is preferable. When the reflux ratio is equal to or higher than the lower limit, the carbo This is preferred because it makes it easier to completely separate the alkyl phosphate and drive off the reaction.
[0031] In the reactive distillation column, the alcoholysis reaction of polyalkylene ether glycol with alkanol is carried out. When the reaction is carried out, alkanol and alkyl carboxylate are distilled from the top of the reactive distillation column and Mixtures containing polyalkylene ether glycols and alkanols (hereinafter referred to as "mixtures") Sometimes referred to as "can".
[0032] To obtain the desired polyalkylene ether glycol, the mixture is diluted with an alkanol. It is necessary to remove the above to obtain a crude polyalkylene ether glycol. In the process of the present invention, a compound is added to the mixture to remove alkanol from the mixture. The process includes a step of obtaining a crude polyalkylene ether glycol by subjecting the compound to the above-mentioned reaction. and the solubility parameter SPa of the polyalkylene ether glycol contained in the mixture. The absolute value of the difference with the solubility parameter SPb (hereinafter referred to as the "difference in solubility parameters") The compound is a compound having a molecular weight of 12.9 or more, and the amount of the compound added is The amount is 3% by mass or more and 20% by mass or less with respect to the amount of polyalkylene ether glycol. The difference in solubility parameters is preferably 13.0 or more, more preferably 13.1 or more, and even more preferably The solubility parameter is preferably 13.2 or more, and particularly preferably 13.3 or more. The upper limit of the difference in solubility parameters is preferably 15.0. This makes it possible to suppress foaming and efficiently remove the alkanol. The amount of the compound added is 3 to 100% based on the amount of polyalkylene ether glycol in the mixture. It is preferably from 4% to 16% by mass, more preferably from 4% to 18% by mass. More preferably, the content is 5% by mass or more and 14% by mass or less, and even more preferably 6% by mass or more. It is particularly preferable that the amount of the compound added is in the above range. This makes it possible to suppress foaming and efficiently remove the alkanol. The compound may be a single compound or a mixture of multiple compounds.
[0033] The solubility parameter of the polyalkylene ether glycol in the present invention (hereinafter referred to as "SP "SP Value" is written as "SP Value Basics and Applications" by Hideki Yamamoto, published in 2005 (Joho Kikko Co., Ltd.) The calculation was based on "2. Fedor's estimation method" on pages 66-67 of the "Calculation Method" The SP value in the dor estimation method is (cohesive energy [J / mol]) / (molecular volume [cm 3This value is defined as the square root of the solubility of the polymer in various solvents. It is a useful physical property value used to predict dissolution. The SP value of the compound in the present invention is calculated by the method proposed by Fedors et al. Specifically, the "POLYMER ENGINEERING AND S CIENCE,FEBRUARY,1974,Vol.14,No.2,ROBERT This value can be obtained by referring to "F.FEDORS. (pages 147-154)". For example, toluene (SP value: 9.1), xylene (SP value: 9.1), ethyl acetate (SP value: 8.7 ), butyl acetate (SP value: 8.7), cyclohexanone (SP value: 9.8), methylethyl Methyl isobutyl ketone (SP value: 9.0), Methyl isobutyl ketone (SP value: 8.7), N-methyl Pyrrolidone (SP value: 11.2), tetrahydrofuran (SP value: 9.1), isopropyl Examples include diethyl alcohol (SP value: 11.5) and water (SP value: 23.4). Furthermore, when the compound is a mixture of multiple types, Based on "2.5 Calculation of Solubility Parameter (SP) Values" in (1997) (page 317), It can be calculated based on various mole fractions.
[0034] The compound may be either solid or liquid, but is preferably liquid from the standpoint of homogenization with the mixture. It is preferable that Also, the compound is added to the mixture, but in the step of removing the alkanol, It is preferable that the crude polyalkylene ether obtained is removed together with the isol. It is preferable that the content of said compound in the glycol is small.
[0035] The mixture obtained from the bottom of the reactive distillation column is sent to the alkanol removal facility after removing the catalyst. The alkanol removal equipment is generally A light boiling point removal equipment such as a distillation tower or a mixing tank with a temperature-controlled jacket can be used. The heating type low boiling separation unit will be described below as an alkanol removal facility. The addition of a compound to the mixture may be performed before the mixture is sent to the heated low boiling separator. may be sent to the heated low boiling separation device.
[0036] The removal of the alkanol may be carried out in a batch or continuous manner. In the batch method, a desired amount of the mixture and a desired amount of the compound are charged into the heated low boiling separation device. The pressure and heating temperature are appropriately set to vaporize the alkanol, and the resulting mixture is distilled from the heated low boiling point separation apparatus. The alkanol is removed from the mixture by heating the mixture at a low pressure. If the pressure is too low, foaming is likely to occur. If the pressure is too high, the heating temperature must be increased to vaporize the alkanol. This may cause deterioration of the polyalkylene ether glycol. Therefore, the pressure is 0.00 The pressure is preferably 5 MPa or more and 5 MPa or less, and more preferably 0.010 MPa or more and 4 MPa or less. The heating pressure is preferably 0.0150 MPa or more and more preferably 3 MPa or less. However, the temperature is preferably 60° C. or higher and 250° C. or lower, more preferably 60° C. or higher and 210° C. or lower. ℃ or more and 180 ℃ or less are more preferable, 60 ℃ or more and 150 ℃ or less are particularly preferable, A heating temperature of 0° C. or more and 120° C. or less is particularly preferable. If the heating temperature is within the above range, foaming can be suppressed. In addition, the polyalkylene ether glycol can be efficiently removed. The heating of the heating type low boiling separation device can be carried out by a general method. Examples of such coils include a temperature-control jacket coil and an internal coil.
[0037] In the continuous type, the mixture and the compound are fed into the heating type low boiling separation device at desired flow rates. The pressure and heating temperature are appropriately set to vaporize the alkanol, and the resulting mixture is distilled from the heated low boiling point separation apparatus. The heating type low boiling separation device is used alone to remove the alkanol. Therefore, the removal of alkanol can be achieved by adjusting the pressure and heating temperature appropriately in the continuous system as well as the batch system. The alkanol is vaporized and distilled from the heating type low boiling point separation apparatus, and the akanol is separated from the mixture. If the pressure is too low, foaming will occur easily, and if the pressure is too high, In order to vaporize the alkanol, it becomes necessary to increase the heating temperature. Therefore, the pressure should be between 0.005MPa and 5MPa. The preferable range is 0.010 MPa or more and 4 MPa or less. The preferable range is 0.0150 MPa or less. The heating temperature is preferably from 60° C. to 250° C., depending on the pressure. ℃ or less is preferable, 60 ℃ or more and 210 ℃ or less is more preferable, 60 ℃ or more and 180 ℃ or less is more preferable. More preferably, the temperature is from 60° C. to 150° C., and particularly preferably from 60° C. to 120° C. If the heating temperature is within the above range, foaming can be suppressed and the alkanoate can be efficiently produced. It is possible to remove the fluorine and suppress the deterioration of polyalkylene ether glycol. The heating of the heating type low boiling separation device can be carried out by a general method, for example, by natural Examples of the heat exchanger include a circulation type heat exchanger, a forced circulation type heat exchanger, and a kettle type heat exchanger.
[0038] The mixture includes a polyalkylene ether glycol and an alkanol. Diesters of polyalkylene ether glycols, a precursor to alkylene ether glycols Since the preferred form of the polyalkylene ether glycol is PTME, The form is PTMG. EXAMPLES
[0039] The present invention will be described in more detail below with reference to examples. The following examples are not intended to be limiting. In the examples, the compounds were added to the mixture. The step of removing the alkanol to obtain a crude polyalkylene ether glycol is To clarify the effect, a small heating type low boiling separation device was used.
[0040] <Example 1-1> 100 parts by weight of tetrahydrofuran, 5.5 parts by weight of acetic anhydride, and 0.07 parts by weight of acetic acid were mixed in a distillation flask. The mixture was reacted at 35° C. for 8 hours with stirring in the presence of 4.2 parts by weight of ruthenium silica catalyst. After removing the catalyst from the reactant by filtration, the mixture was distilled in batches under a reduced pressure of 10 torr or less. Acetic anhydride and acetic acid were distilled off. A small amount of nitrogen was introduced under reduced pressure to remove volatile matter. PTME was obtained by the above procedure. The number average molecular weight was measured by gel permeation chromatography. The amount was 2788, the acetic anhydride content was 10 ppm, and the acetic acid was <10 ppm. The reactive distillation column was charged with 200 kg of PTME and 210 ppm of sodium methoxide. 460 kg of methanol was charged and the methanolysis reaction was carried out while gradually distilling off methanol, etc. The reaction pressure was normal pressure and the reaction temperature was 65° C. The reaction mixture was cooled and then eluted with a sulfonic acid type strongly acidic ion exchange resin (Mitsubishi Chemical Corporation The sodium ions dissolved in the reaction solution were removed by mixing with 100% ethanol (PK216LH, manufactured by Epson) for 1 hour. After removing the sodium ions, the reaction mixture (hereinafter referred to as "mixture A") had a PTMG of 57.7 % by mass, and methanol 42.3% by mass. The number average molecular weight measured by precipitation chromatography was 2612, and the SP value was 9.2. there were. Mixture A (760 g) was placed in a 100 mm inner diameter glass heating type low boiling point separator shown in Figure 1. (hereinafter referred to as "light boiling separator"). Next, the rotation speed was set to 150 rpm and the stirring blade 2 was While rotating, 31.6 g of water was added to the mixed solution A. The rotation of the stirring blade 2 was stopped, and the measurement was performed. The static liquid level was 109 mm. The rotation of the agitator 2 was restarted at 150 rpm. At normal pressure, the inner temperature is raised to 68°C by the jacket 1, and nitrogen gas is introduced into the nitrogen gas inlet 3. While introducing nitrogen gas into the liquid in the low boiling point separation device at 1000 ml / min, methanol was removed. After one minute had elapsed since the distillation of the distillate into the distillate container 6 had started, the low boiling point fraction was The length from the top of the liquid surface in the separation device to the top of the foam was measured with a ruler and found to be 7 mm. . The SP value of the added compound, water, is 23.4. In addition, the amount of water to be added relative to the amount of PTMG contained in the mixture can be calculated as follows. 31.6g÷(760g×57.7% by mass)=7.2% by mass The results are summarized in Table 1.
[0041] <Comparative Example 1-1> Mixture A (760 g) produced in the same manner as in Example 1-1 was subjected to a low-boiling point extraction in the same manner as in Example 1-1. The static liquid level measured after the injection was 105 mm. The stirring blade 2 was rotated at 150 rpm, and the internal temperature was kept at 68°C by the jacket 1 at normal pressure. As the temperature rises, nitrogen is introduced into the liquid in the low boiling point separation device at a rate of 1000 ml / min through the nitrogen gas introduction part 3. While introducing nitrogen gas, removal of methanol was started. Distillation of the distillate into the distillate container 6 started. After one minute had passed since the start of the experiment, the length from the top of the liquid surface in the low boiling separator to the top of the foam was measured. Measurement with a ruler revealed that it was 28 mm, and the foamed top surface reached near the bottom end of the distillation tube 5. Ta. The results are summarized in Table 1.
[0042] <Comparative Example 1-2> Mixture A (760 g) produced in the same manner as in Example 1-1 was subjected to a low-boiling point extraction in the same manner as in Example 1-1. Next, the rotation speed was set to 150 rpm, and the stirring blade 2 was rotated while stirring the water. A mixture of 17.6 g of tetrahydrofuran and 14.0 g of tetrahydrofuran was added to the mixed solution A. The rotation was stopped and the static liquid level was measured to be 109 mm. The rotation speed was then increased to 150 rpm. The stirring blade 2 is rotated at m, and the internal temperature is raised to 68°C by the jacket 1 at normal pressure. In addition, nitrogen gas is introduced into the liquid in the low boiling separation device at 1000 ml / min through the nitrogen gas introduction part 3. After the distillate started to be discharged into the distillate container 6, After 1 minute, measure the length from the top of the liquid surface in the light boiling separator to the top of the foam with a ruler. The measurement revealed that the diameter was 40 mm, and the upper surface of the foam reached the inside of the distillation tube 5. In addition, the compounds water (SP value: 23.4) and tetrahydrofuran (SP value: 9.1) The SP value of the mixture can be calculated as follows: First, calculate the total number of moles of the mixture as follows: 17.6g÷18.01528g / mol+14.0g÷72.11g / mol=1. 1711mol The mole fraction of water and tetrahydrofuran is calculated from the total number of moles, and the mole fraction of water is 83. The mole fraction of tetrahydrofuran is 16.6%. From the mole fraction, the SP value is It can be calculated using the formula below. 23.4×83.4%+9.1×16.6%=21.0 The results are summarized in Table 1.
[0043] <Example 2-1> 100 parts by weight of tetrahydrofuran, 5.5 parts by weight of acetic anhydride, and 0.07 parts by weight of acetic acid were mixed in a distillation flask. The mixture was reacted at 35° C. for 8 hours with stirring in the presence of 4.2 parts by weight of ruthenium silica catalyst. After removing the catalyst from the reactant by filtration, the mixture was distilled in batches under a reduced pressure of 10 torr or less. Acetic anhydride and acetic acid were distilled off. A small amount of nitrogen was introduced under reduced pressure to remove volatile matter. PTME was obtained by the above procedure. The number average molecular weight was measured by gel permeation chromatography. The amount was 2788, the acetic anhydride content was 10 ppm, and the acetic acid was <10 ppm. The reactive distillation column was charged with 200 kg of PTME and 210 ppm of sodium methoxide. 440 kg of methanol was charged and the methanolysis reaction was carried out while gradually distilling off methanol, etc. The reaction pressure was normal pressure and the reaction temperature was 65° C. The reaction mixture was cooled and then eluted with a sulfonic acid type strongly acidic ion exchange resin (Mitsubishi Chemical Corporation The sodium ions dissolved in the reaction solution were removed by mixing with 100% ethanol (PK216LH, manufactured by Epson) for 1 hour. The reaction solution after removing the sodium ions (hereinafter referred to as "mixture B") had a PTMG of 61.8 % by mass, and methanol 38.2% by mass. The number average molecular weight measured by precipitation chromatography was 2612, and the SP value was 9.2. there were. Mixture B (760 g) was placed in the low boiling point separator. Then, the rotation speed was set to 150 rpm. Then, 28.7 g of water was added to the mixed solution B while rotating the stirring blade 2. The rotation of the stirring blade 2 was stopped. The static liquid level was measured at 109 mm. The rotation of the furnace was resumed, and the internal temperature was raised to 68°C by jacket 1 at normal pressure. At the same time, nitrogen gas was introduced. While introducing nitrogen gas into the liquid in the low boiling point separation apparatus at 1000 ml / min through the gas introduction part 3, The removal of methanol was started. One minute had passed since the distillate started to be discharged into the distillate container 6. After that, the length from the top of the liquid surface in the light boiling separator to the top of the foam was measured with a ruler. It was 7mm. The SP value of the compound water is 23.4. In addition, the amount of water to be added relative to the amount of PTMG contained in the mixture can be calculated as follows. 28.7g÷(760g×61.8% by mass)=6.1% by mass The results are summarized in Table 1.
[0044] <Comparative Example 2-1> Mixture B (760 g) produced in the same manner as in Example 2-1 was subjected to a centrifugation reaction for 10 minutes at 20° C. to 120° C. for 1 hour. The static liquid level after the injection was 105 mm. The rotation speed was then increased to 150 Rotate the stirring blade 2 at rpm and raise the internal temperature to 68°C using the jacket 1 at normal pressure. At the same time, nitrogen gas is introduced into the liquid in the low boiling point separation device at a rate of 1000 ml / min through the nitrogen gas introduction part 3. While introducing the distillate into the distillate container 6, the removal of methanol was started. After one minute had passed, the length from the top of the liquid surface in the low boiling separator to the top of the foam was measured with a ruler. When measured, it was 26 mm, and the upper surface of the foam reached near the lower end of the distillation tube 5. The results are summarized in Table 1.
[0045] <Comparative Example 2-2> Mixture B (760 g) produced in the same manner as in Example 2-1 was subjected to a centrifugation reaction for 10 minutes at 20° C. to 120° C. for 1 hour. Next, the rotation speed was set to 150 rpm, and the stirring blade 2 was rotated while stirring the water. A mixture of 17.4 g of tetrahydrofuran and 11.3 g of tetrahydrofuran was added to the mixed solution B. The rotation was stopped and the static liquid level was measured to be 109 mm. The rotation speed was then increased to 150 rpm. The stirring blade 2 is rotated at m, and the internal temperature is raised to 68°C by the jacket 1 at normal pressure. In addition, nitrogen gas is introduced into the liquid in the low boiling separation device at 1000 ml / min through the nitrogen gas introduction part 3. After the distillate started to be discharged into the distillate container 6, After 1 minute, measure the length from the top of the liquid surface in the light boiling separator to the top of the foam with a ruler. The measured height was 26 mm, and the foaming top surface reached near the bottom end of the distillation tube 5. The SP value of the compound was calculated in the same manner as in Example 1-2 and was found to be 21.4. The results are summarized in Table 1.
[0046] <Example 3-1> 100 parts by weight of tetrahydrofuran, 5.5 parts by weight of acetic anhydride, and 0.07 parts by weight of acetic acid were mixed in a distillation flask. The mixture was reacted at 35° C. for 8 hours with stirring in the presence of 4.2 parts by weight of ruthenium silica catalyst. After removing the catalyst from the reactant by filtration, the mixture was distilled in batches under a reduced pressure of 10 torr or less. Acetic anhydride and acetic acid were distilled off. A small amount of nitrogen was introduced under reduced pressure to remove volatile matter. PTME was obtained by the above procedure. The number average molecular weight was measured by gel permeation chromatography. The amount was 2788, the acetic anhydride content was 10 ppm, and the acetic acid was <10 ppm. The reactive distillation column was charged with 200 kg of PTME and 210 ppm of sodium methoxide. 420 kg of methanol was charged and the methanolysis reaction was carried out while gradually distilling off methanol, etc. The reaction pressure was normal pressure and the reaction temperature was 65° C. The reaction mixture was cooled and then eluted with a sulfonic acid type strongly acidic ion exchange resin (Mitsubishi Chemical Corporation The sodium ions dissolved in the reaction solution were removed by mixing with 100% ethanol (PK216LH, manufactured by Epson) for 1 hour. The reaction solution after removing sodium ions (hereinafter referred to as "mixture C") had a PTMG of 66.1 % by mass, and methanol 33.9% by mass. The number average molecular weight measured by precipitation chromatography was 2612, and the SP value was 9.2. there were. Mixture C (760 g) was placed in the low boiling point separator. Then, the rotation speed was set to 150 rpm. Then, while rotating the stirring blade 2, 34.2 g of water was added to the mixed liquid C. The rotation of the stirring blade 2 was stopped. The static liquid level was measured at 109 mm. The rotation of the furnace was resumed, and the internal temperature was raised to 69°C by jacket 1 at normal pressure. While introducing nitrogen gas into the liquid in the low boiling point separation apparatus at 1000 ml / min through the gas introduction part 3, The removal of methanol was started. One minute had passed since the distillate started to be discharged into the distillate container 6. After that, the length from the top of the liquid surface in the light boiling separator to the top of the foam was measured with a ruler. It was 8mm. The SP value of the compound water is 23.4. In addition, the amount of water to be added relative to the amount of PTMG contained in the mixture can be calculated as follows. 34.2g÷(760g×66.1% by mass)=6.8% by mass The results are summarized in Table 1.
[0047] <Comparative Example 3-1> Mixture C (760 g) produced in the same manner as in Example 3-1 was subjected to a low-boiling point extraction in the same manner as in Example 3-1. The static liquid level after the injection was 105 mm. The rotation speed was then increased to 150 Rotate the stirring blade 2 at rpm and raise the internal temperature to 69°C using the jacket 1 at normal pressure. At the same time, nitrogen gas is introduced into the liquid in the low boiling point separation device at a rate of 1000 ml / min through the nitrogen gas introduction part 3. While introducing the distillate into the distillate container 6, the removal of methanol was started. After one minute had passed, the length from the top of the liquid surface in the low boiling separator to the top of the foam was measured with a ruler. When measured, it was 22 mm, and the upper surface of the foam reached near the lower end of the distillation tube 5. The results are summarized in Table 1.
[0048] <Comparative Example 3-2> Mixture C (760 g) produced in the same manner as in Example 3-1 was subjected to a low-boiling point extraction in the same manner as in Example 3-1. Next, the rotation speed was set to 150 rpm, and the stirring blade 2 was rotated while stirring the water. A mixture of 25.2 g of tetrahydrofuran and 9.0 g of tetrahydrofuran was added to the mixed solution C. The rotation was stopped and the static liquid level was measured to be 110 mm. The rotation speed was then increased to 150 rpm. The stirring blade 2 was rotated under normal pressure, and the internal temperature was raised to 69°C by the jacket 1. Nitrogen gas is introduced into the liquid in the low boiling point separation device at a rate of 1000 ml / min through the nitrogen gas introduction part 3. While distilling the distillate into the distillate container 6, the removal of methanol was started. After 10 minutes had passed, the length from the top of the liquid surface in the light boiling separator to the top of the foam was measured with a ruler. The height was 24 mm, and the foamed top surface reached near the bottom end of the distillation tube 5. The SP value of the compound was calculated in the same manner as 1-2 and was found to be 21.7. The results are summarized in Table 1.
[0049] <Example 4-1> 100 parts by weight of tetrahydrofuran, 5.5 parts by weight of acetic anhydride, and 0.07 parts by weight of acetic acid were mixed in a distillation flask. The mixture was reacted at 35° C. for 8 hours with stirring in the presence of 4.2 parts by weight of ruthenium silica catalyst. After removing the catalyst from the reactant by filtration, the mixture was distilled in batches under a reduced pressure of 10 torr or less. Acetic anhydride and acetic acid were distilled off. A small amount of nitrogen was introduced under reduced pressure to remove volatile matter. PTME was obtained by the above procedure. The number average molecular weight was measured by gel permeation chromatography. The amount was 2788, the acetic anhydride content was 10 ppm, and the acetic acid was <10 ppm. The reactive distillation column was charged with 200 kg of PTME and 210 ppm of sodium methoxide. 400 kg of methanol was charged and the methanolysis reaction was carried out while gradually distilling off methanol, etc. The reaction pressure was normal pressure and the reaction temperature was 65° C. The reaction mixture was cooled and then eluted with a sulfonic acid type strongly acidic ion exchange resin (Mitsubishi Chemical Corporation The sodium ions dissolved in the reaction solution were removed by mixing with 100% ethanol (PK216LH, manufactured by Epson) for 1 hour. The reaction solution after removing the sodium ions (hereinafter referred to as "mixture D") had a PTMG of 70.4 The PTMG contained 29.6% by mass of methanol and 29.6% by mass of gel permeation medium. The number average molecular weight measured by precipitation chromatography was 2612, and the SP value was 9.2. there were. Mixture D (760 g) was charged into the low boiling point separator. Then, the rotation speed was set to 150 rpm. Then, 24.6 g of water was added to the mixed solution D while rotating the stirring blade 2. The rotation of the stirring blade 2 was stopped. The static liquid level was measured at 108 mm. The rotation of the furnace was resumed, and the internal temperature was raised to 74°C by jacket 1 at normal pressure. While introducing nitrogen gas into the liquid in the low boiling point separation apparatus at 1000 ml / min through the gas introduction part 3, The removal of methanol was started. One minute had passed since the distillate started to be discharged into the distillate container 6. After that, the length from the top of the liquid surface in the light boiling separator to the top of the foam was measured with a ruler. It was 13mm. The SP value of the compound water is 23.4. In addition, the amount of water to be added relative to the amount of PTMG contained in the mixture can be calculated as follows. 24.6g÷(760g×70.4% by mass)=4.6% by mass The results are summarized in Table 1.
[0050] <Comparative Example 4-1> Mixture D (760 g) produced in the same manner as in Example 4-1 was subjected to a low-boiling point extraction in the same manner as in Example 4-1. The static liquid level after the injection was 105 mm. The rotation speed was then increased to 150 Rotate the stirring blade 2 at rpm and raise the internal temperature to 74°C using the jacket 1 at normal pressure. At the same time, nitrogen gas is introduced into the liquid in the low boiling point separation device at a rate of 1000 ml / min through the nitrogen gas introduction part 3. While introducing the distillate into the distillate container 6, the removal of methanol was started. After one minute had passed, the length from the top of the liquid surface in the low boiling separator to the top of the foam was measured with a ruler. When measured, it was 23 mm, and the upper surface of the foam reached near the lower end of the distillation tube 5. The results are summarized in Table 1.
[0051] <Comparative Example 4-2> Mixture D (760 g) produced in the same manner as in Example 4-1 was subjected to a low-boiling point extraction in the same manner as in Example 4-1. Next, the rotation speed was set to 150 rpm, and the stirring blade 2 was rotated while stirring the water. A mixture of 17.1 g of tetrahydrofuran and 7.5 g of tetrahydrofuran was added to the mixed solution D. The rotation was stopped and the static liquid level was measured to be 108 mm. The rotation speed was then increased to 150 rpm. The stirring blade 2 was rotated under normal pressure, and the internal temperature was raised to 74°C by the jacket 1. Nitrogen gas is introduced into the liquid in the low boiling point separation device at a rate of 1000 ml / min through the nitrogen gas introduction part 3. While distilling the distillate into the distillate container 6, the removal of methanol was started. After 10 minutes had passed, the length from the top of the liquid surface in the light boiling separator to the top of the foam was measured with a ruler. The height was 26 mm, and the foamed top surface reached near the bottom end of the distillation tube 5. The SP value of the compound was calculated in the same manner as 1-2 and was found to be 22.0. The results are summarized in Table 1.
[0052] [Table 1]
[0053] As is clear from Examples 1-1 to 4-1, by adding a specific amount of a specific compound, This makes it possible to suppress foaming and efficiently remove alkanols such as methanol. Ta. [Explanation of symbols]
[0054] 1. Jacket 2 Mixing blade 3 Nitrogen gas inlet 4 Distillate tube 5 Cooler 6 Distillate container 7 Cooling water 8 Pressure Regulating System
Claims
1. A method for producing a polyalkylene ether glycol, comprising the steps of: subjecting a diester of a polyalkylene ether glycol to an alcoholysis reaction with an alkanol in the presence of an alkali metal alkoxide catalyst to obtain a mixture containing a polyalkylene ether glycol and an alkanol; removing the alkali metal alkoxide catalyst, and then adding water to the mixture and removing the alkanol to obtain a crude polyalkylene ether glycol, the absolute value of the difference between the solubility parameter SPa of the water and the solubility parameter SPb of the polyalkylene ether glycol is 12.9 or more; and the amount of water added is 3% by mass or more and 20% by mass or less based on the amount of polyalkylene ether glycol in the mixture.
2. The method for producing a polyalkylene ether glycol according to claim 1, wherein the polyalkylene ether glycol is polytetramethylene ether glycol.
3. The alkanol is 1 ~C 4 3. The method for producing a polyalkylene ether glycol according to claim 1 or 2, wherein the alkanol is of the formula:
4. The method for producing a polyalkylene ether glycol according to any one of claims 1 to 3, wherein the temperature for removing the alkanol is 60°C or higher and 250°C or lower.
5. The method for producing a polyalkylene ether glycol according to any one of claims 1 to 4, wherein a concentration of the polyalkylene ether glycol in the mixture is from 30% by mass to 90% by mass.
6. The method for producing a polyalkylene ether glycol according to any one of claims 1 to 5, wherein the polyalkylene ether glycol has a number average molecular weight of 600 or more and 8,000 or less.
Citation Information
Patent Citations
Purification of polyoxytetramethylene glycol
JP1993194723A
Continuous production of polytetrahydrofuran by transesterification cascade capable of breaking air bubble
JP1999158263A
Production of polytetramethylene ether glycol
JP2000336164A
Production of polytetramethylene ether glycol
JP2001081181A
Method for producing polyether polyols
JP2006291189A