Thermoplastic polyester elastomer resin composition and foamed molded article made from same

A thermoplastic polyester elastomer resin composition with controlled soft segment molecular weight and balanced content, combined with a specific molding process, achieves lightweight and resilient foam molded products with high impact modulus and heat resistance, addressing the challenge of low-temperature molding.

JP7567589B2Active Publication Date: 2024-10-16TOYOBO MC CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021044015
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-17
Publication Date
2024-10-16
Estimated Expiration
2041-03-17

AI Technical Summary

Technical Problem

Existing thermoplastic polyester elastomer resin compositions face challenges in achieving high impact modulus and excellent mechanical properties while allowing for molding at lower temperatures, which is crucial for applications requiring lightweight and resilient foam molded products.

Method used

A thermoplastic polyester elastomer resin composition is developed with a specific molecular weight range for soft segments (less than 1000) and a balanced content (10 to 80% by mass) combined with a hard segment made of aromatic dicarboxylic acid and aliphatic diol, along with a process that includes injection molding and cavity expansion using a core back method.

Benefits of technology

The composition enables molding at lower temperatures with high impact modulus, resulting in lightweight, resilient, and uniformly foamed products with high heat resistance and water resistance, suitable for applications demanding high reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567589000002
    Figure 0007567589000002
  • Figure 0007567589000001
    Figure 0007567589000001
Patent Text Reader

Abstract

To provide a thermoplastic polyester elastomer resin composition for foam molding which is excellent in lightweight property and impact elastic modulus, and can be molded at lower temperatures, and a foam molding formed from the same.SOLUTION: There are provided a thermoplastic polyester elastomer resin composition for foam molding containing a thermoplastic polyester elastomer which is obtained by coupling a hard segment formed from polyester containing an aromatic dicarboxylic acid, and aliphatic and / or alicyclic diol as components, and at least one soft segment selected from aliphatic polyether, aliphatic polyester and aliphatic polycarbonate, wherein a number average molecular weight of the soft segment is less than 1,000, and a content of the soft segment is 10-80 mass%; and a foam molding formed from the same.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoplastic polyester elastomer resin composition having a high resilience modulus and excellent mechanical properties, and to a foam molded article thereof. More specifically, the present invention relates to a thermoplastic polyester elastomer resin composition having excellent foam moldability, and the foam molded article obtained from the thermoplastic polyester elastomer composition of the present invention is lightweight and has high resilience, and further, it is possible to provide a good quality foam molded article by molding at a low temperature. [Background technology]

[0002] Thermoplastic polyester elastomers have excellent injection and extrusion moldability, high mechanical strength, and rubber-like properties such as elastic recovery, impact resistance, and flexibility, as well as excellent cold resistance. As such, they are used in applications such as automotive parts, electrical and electronic parts, fibers, films, and sports parts.

[0003] Thermoplastic polyester elastomers have excellent heat aging resistance, light resistance, and abrasion resistance, and are therefore used in automobile parts, particularly parts used in high-temperature environments and automobile interior parts. Furthermore, in recent years, efforts have been made to reduce the weight of resin parts, and the application of foam moldings can be cited as one of the means to achieve this goal.

[0004] There are various foam molding techniques depending on the application, and foaming is achieved by using chemical or physical foaming agents, but the melting point and molding temperature are important in achieving high-fold foaming. In foaming using supercritical fluids, the solubility of the foaming agent in the resin generally increases with lower temperatures and higher pressures, so high-fold foaming can be achieved by molding at low temperatures.

[0005] In addition, in the in-mold foaming process in which foaming is performed by heated water vapor pressure, molding at lower temperatures is required due to the recent rise in fuel prices. Patent Document 1 proposes a polypropylene-based resin that has two melting peaks, making it possible to mold at lower temperatures.

[0006] In addition, when the melting point is high, there are limitations in the selection of the foaming agent. Patent Document 2 proposes a thermally expandable microcapsule with excellent heat resistance and a maximum foaming temperature of 180°C or more as a foaming agent. However, when using a resin with a melting point higher than that, the molding temperature becomes high, causing the expanded microcapsules to burst or shrink, resulting in a decrease in the foaming ratio.

[0007] Patent Document 3 proposes a thermoplastic polyester elastomer resin composition for foam molding, and although it produces high-quality foam molded articles, it makes no mention of the melting point or the temperature during molding. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Patent No. 5841076 [Patent Document 2] JP 2011-74282 A [Patent Document 3] Patent No. 6358368 Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention has been made in consideration of the current state of the prior art, and an object of the present invention is to provide a thermoplastic polyester elastomer resin composition for foam molding which is lightweight and has an excellent rebound resilience and can be molded at a lower temperature, and a foam molded article made from the same. [Means for solving the problem]

[0010] In order to achieve the above object, the present inventors have intensively studied the composition of thermoplastic polyester elastomers. As a result, they have found that by using a thermoplastic polyester elastomer with a number average molecular weight of less than 1000 as the soft segment and setting the content of the soft segment within a specific range, molding at low temperatures while maintaining a high rebound resilience is possible. Furthermore, they have found that by applying a process of filling a mold with resin by injection molding and then expanding the cavity by core-backing the mold, it is possible to easily produce and provide a high-quality polyester elastomer foam molded product, which has led to the completion of the present invention.

[0011] That is, the present invention constitutes [1] to [5]. [1] A thermoplastic polyester elastomer resin composition for foam molding, comprising a thermoplastic polyester elastomer in which a hard segment made of a polyester having an aromatic dicarboxylic acid and an aliphatic and / or alicyclic diol as constituent components is bonded to at least one soft segment selected from an aliphatic polyether, an aliphatic polyester, and an aliphatic polycarbonate, the soft segment having a number average molecular weight of less than 1,000, and the soft segment content is 10 to 80 mass%. [2] A foam molded article made from the thermoplastic polyester elastomer resin composition described in [1]. [3] The foam molded article according to [2], characterized in that the rebound resilience is 50 to 90%. [4] A foam layer having independent foam cells with an average cell diameter of 10 to 400 μm and a maximum cell diameter of 10 to 500 μm, and a density of 0.01 to 0.40 g / cm 3 The foamed molded article according to [2] or [3], [5] The foam molded article according to any one of [2] to [4], which has a non-foamed skin layer having a thickness of 100 to 800 μm as a surface layer, and a foamed layer consisting of foamed cells having an average cell diameter of 10 to 400 μm that are independent of the resin continuous phase as an inner layer, and has a sandwich structure of the non-foamed skin layer and the foamed layer in the thickness direction. Effect of the Invention

[0012] The thermoplastic polyester elastomer resin composition for foam molding of the present invention can be molded at a lower temperature, and therefore has excellent moldability in various foam molding techniques. The foam molded article of the present invention is not only lightweight, but also exhibits high resilience. Furthermore, the foam molded article has a uniform foaming state, high heat resistance, water resistance, and molding stability despite a high expansion ratio, and therefore can be used for parts that require high reliability. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a schematic diagram for explaining an example of a method for producing a foamed molded article of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The thermoplastic polyester elastomer resin composition for foam molding of the present invention and the foam molded article using the same will be described in detail below.

[0015] [Thermoplastic polyester elastomer (A)] The thermoplastic polyester elastomer (A) used in the present invention is formed by bonding hard segments and soft segments. The hard segments are made of polyester. As the aromatic dicarboxylic acid constituting the polyester of the hard segments, ordinary aromatic dicarboxylic acids are widely used and are not particularly limited, but it is desirable that the main aromatic dicarboxylic acid is terephthalic acid or naphthalenedicarboxylic acid (among isomers, 2,6-naphthalenedicarboxylic acid is preferred). The content of these aromatic dicarboxylic acids is preferably 70 mol% or more, more preferably 80 mol% or more, of the total dicarboxylic acids constituting the polyester of the hard segments. Other dicarboxylic acid components include aromatic dicarboxylic acids such as diphenyldicarboxylic acid, isophthalic acid, and 5-sodium sulfoisophthalic acid, alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid and tetrahydrophthalic anhydride, and aliphatic dicarboxylic acids such as succinic acid, glutaric acid, adipic acid, azelaic acid, sebacic acid, dodecanedioic acid, dimer acid, and hydrogenated dimer acid. These can be used in an amount that does not significantly lower the melting point of the resin, and the amount is 30 mol % or less, preferably 20 mol % or less, of the total acid components.

[0016] In the thermoplastic polyester elastomer (A) used in the present invention, the aliphatic or alicyclic diol constituting the polyester of the hard segment is generally aliphatic or alicyclic diol, and is not particularly limited, but is preferably an alkylene glycol having 2 to 8 carbon atoms. Specific examples include ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, and 1,4-cyclohexanedimethanol. Among these, either ethylene glycol or 1,4-butanediol is preferable.

[0017] As the component constituting the polyester of the above hard segment, those consisting of butylene terephthalate units (units consisting of terephthalic acid and 1,4-butanediol) or butylene naphthalate units (units consisting of 2,6-naphthalenedicarboxylic acid and 1,4-butanediol) are preferred from the viewpoints of physical properties, moldability, and cost performance.

[0018] In addition, when an aromatic polyester suitable as a polyester constituting a hard segment in the thermoplastic polyester elastomer (A) used in the present invention is produced in advance and then copolymerized with a soft segment component, the aromatic polyester can be easily obtained according to a normal polyester production method. In addition, such a polyester preferably has a number average molecular weight of 10,000 to 40,000.

[0019] The soft segment of the thermoplastic polyester elastomer (A) used in the present invention is at least one selected from aliphatic polyethers, aliphatic polyesters, and aliphatic polycarbonates.

[0020] Examples of aliphatic polyethers include poly(ethylene oxide) glycol, poly(propylene oxide) glycol, poly(tetramethylene oxide) glycol, poly(hexamethylene oxide) glycol, poly(trimethylene oxide) glycol, copolymers of ethylene oxide and propylene oxide, ethylene oxide adducts of poly(propylene oxide) glycol, copolymers of ethylene oxide and tetrahydrofuran, etc. Among these, poly(tetramethylene oxide) glycol and ethylene oxide adducts of poly(propylene oxide) glycol are preferred from the viewpoint of elastic properties.

[0021] Examples of the aliphatic polyester include poly(ε-caprolactone), polyenantholactone, polycaprylolactone, polybutylene adipate, etc. Among these, poly(ε-caprolactone) and polybutylene adipate are preferred from the viewpoint of elasticity characteristics.

[0022] The aliphatic polycarbonate is preferably composed mainly of an aliphatic diol residue having 2 to 12 carbon atoms. Examples of these aliphatic diols include ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 2,2-dimethyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 1,9-nonanediol, and 2-methyl-1,8-octanediol. In particular, from the viewpoint of flexibility and low-temperature properties of the resulting thermoplastic polyester elastomer, an aliphatic diol having 5 to 12 carbon atoms is preferred. These components may be used alone or in combination of two or more kinds as necessary, based on the examples described below.

[0023] The aliphatic polycarbonate diol having good low-temperature properties and constituting the soft segment of the thermoplastic polyester elastomer (A) used in the present invention preferably has a low melting point (for example, 70°C or less) and a low glass transition temperature. In general, the aliphatic polycarbonate diol made of 1,6-hexanediol used to form the soft segment of the thermoplastic polyester elastomer has a low glass transition temperature of about -60°C and a melting point of about 50°C, so that it has good low-temperature properties. In addition, the aliphatic polycarbonate diol obtained by copolymerizing the above aliphatic polycarbonate diol with an appropriate amount of 3-methyl-1,5-pentanediol, for example, has a slightly higher glass transition point than the original aliphatic polycarbonate diol, but has a lower melting point or is amorphous, so that it corresponds to an aliphatic polycarbonate diol having good low-temperature properties. For example, an aliphatic polycarbonate diol made of 1,9-nonanediol and 2-methyl-1,8-octanediol has a melting point of about 30° C. and a glass transition temperature of about −70° C., which are sufficiently low, and therefore corresponds to an aliphatic polycarbonate diol with good low-temperature properties.

[0024] The number average molecular weight of the soft segment of the thermoplastic polyester elastomer (A) used in the present invention is less than 1000. The number average molecular weight of the soft segment is preferably 300 or more and less than 1000, more preferably 400 or more and 950 or less, and even more preferably 500 or more and 900 or less. In general, those having a number average molecular weight of 1000 or more and 2500 or less are often used, but by using those having a number average molecular weight of less than 1000, it is possible to lower the melting point without impairing the high rebound resilience. On the other hand, if the number average molecular weight is less than 300, it may be difficult to express the elastomer properties. The number average molecular weight of the soft segment may be adjusted by using a mixture of soft segments having different number average molecular weights. For example, a number average molecular weight of 700 may be achieved by using a soft segment having a number average molecular weight of 500 and a soft segment having a number average molecular weight of 900 in a 50 / 50 mass ratio.

[0025] From the viewpoint of solving the problems of the present invention, the soft segment of the thermoplastic polyester elastomer (A) used in the present invention is preferably an aliphatic polyether.

[0026] The thermoplastic polyester elastomer (A) used in the present invention is preferably a copolymer mainly composed of terephthalic acid, 1,4-butanediol, and poly(tetramethylene oxide) glycol. In the dicarboxylic acid component constituting the thermoplastic polyester elastomer (A), terephthalic acid is preferably 40 mol% or more, more preferably 70 mol% or more, even more preferably 80 mol% or more, and particularly preferably 90 mol% or more. In the glycol component constituting the thermoplastic polyester elastomer (A), the total of 1,4-butanediol and poly(tetramethylene oxide) glycol is preferably 40 mol% or more, more preferably 70 mol% or more, even more preferably 80 mol% or more, and particularly preferably 90 mol% or more.

[0027] In the thermoplastic polyester elastomer (A) used in the present invention, the soft segment content is preferably 10 to 80 mass%, more preferably 20 to 80 mass%, and further preferably 30 to 75 mass%. If the soft segment content is less than 10 mass%, the crystallinity is too high and the resilience is poor, whereas if it exceeds 80 mass%, the crystallinity is too low and the foam moldability tends to be poor.

[0028] The melting point of the thermoplastic polyester elastomer (A) used in the present invention is preferably not more than 205°C, more preferably 120 to 205°C, and even more preferably 130 to 195°C.

[0029] The thermoplastic polyester elastomer (A) used in the present invention can be produced by a known method, for example, a method of transesterifying a lower alcohol diester of a dicarboxylic acid, an excess amount of a low molecular weight glycol, and a soft segment component in the presence of a catalyst and polycondensing the resulting reaction product, a method of esterifying a dicarboxylic acid, an excess amount of a glycol, and a soft segment component in the presence of a catalyst and polycondensing the resulting reaction product, a method of preparing a hard segment polyester in advance, adding a soft segment component to the polyester, and randomizing the polyester by transesterification, a method of connecting a hard segment and a soft segment with a chain linking agent, and further, when poly(ε-caprolactone) is used for the soft segment, a method of adding an ε-caprolactone monomer to the hard segment, or the like, may be used.

[0030] [Other ingredients] A crosslinking agent may be blended into the thermoplastic polyester elastomer (A) as necessary, as long as it does not impair the effects of the present invention. Such a crosslinking agent is not particularly limited as long as it is a crosslinking agent that reacts with the hydroxyl group or carboxyl group of the thermoplastic polyester elastomer (A), and examples thereof include epoxy-based crosslinking agents, carbodiimide-based crosslinking agents, isocyanate-based crosslinking agents, acid anhydride-based crosslinking agents, silanol-based crosslinking agents, melamine resin-based crosslinking agents, metal salt-based crosslinking agents, metal chelate-based crosslinking agents, and amino resin-based crosslinking agents. The crosslinking agents may be used alone or in combination of two or more.

[0031] The epoxy crosslinking agent is not particularly limited as long as it is a multifunctional epoxy compound having two or more epoxy groups (glycidyl groups) in the molecule. Specifically, 1,6-dihydroxynaphthalene diglycidyl ether and 1,3-bis(oxiranylmethoxy)benzene having two epoxy groups, 1,3,5-tris(2,3-epoxypropyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione and diglycerol triglycidyl ether having three epoxy groups, and 1-chloro-2,3-epoxypropane-formaldehyde-2,7-naphthalene diol polycondensate and pentaerythritol polyglycidyl ether having four epoxy groups are listed. Among them, a multifunctional epoxy compound having heat resistance in the skeleton is preferable. In particular, a bifunctional or tetrafunctional epoxy compound having a naphthalene structure as the skeleton, or a trifunctional epoxy compound having a triazine structure as the skeleton is preferable. Considering the degree of increase in the solution viscosity of the thermoplastic polyester elastomer (A), the effect of efficiently reducing the acid value of the thermoplastic polyester elastomer (A), and the degree of gelation caused by aggregation and solidification of the epoxy itself, a difunctional or trifunctional epoxy compound is preferred.

[0032] Other examples include styrene copolymers that contain two or more glycidyl groups per molecule, have a weight average molecular weight of 4000 to 25000, and are composed of 20 to 99% by mass of vinyl aromatic monomer (X), 1 to 80% by mass of glycidyl (meth)acrylate (Y), and 0 to 79% by mass of vinyl group-containing monomer other than (X) that does not contain an epoxy group. More preferred are copolymers that contain 20 to 99% by mass of (X), 1 to 80% by mass of (Y), and 0 to 40% by mass of (Z), and even more preferred are copolymers that contain 25 to 90% by mass of (X), 10 to 75% by mass of (Y), and 0 to 35% by mass of (Z). Examples of the vinyl aromatic monomer (X) include styrene and α-methylstyrene. Examples of the (Y) glycidyl alkyl (meth)acrylate include glycidyl (meth)acrylate, (meth)acrylic acid esters having a cyclohexene oxide structure, and (meth)acrylic glycidyl ethers. Among these, glycidyl (meth)acrylate is preferred in terms of its high reactivity. Examples of the (Z) other vinyl group-containing monomers include (meth)acrylic acid alkyl esters having an alkyl group having 1 to 22 carbon atoms (the alkyl group may be linear or branched), such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, stearyl (meth)acrylate, and methoxyethyl (meth)acrylate; (meth)acrylic acid polyalkylene glycol esters; (meth)acrylic acid alkoxyalkyl esters; (meth)acrylic acid hydroxyalkyl esters; (meth)acrylic acid dialkylaminoalkyl esters; (meth)acrylic acid benzyl esters; (meth)acrylic acid phenoxyalkyl esters; (meth)acrylic acid isobornyl esters; and (meth)acrylic acid alkoxysilylalkyl esters. In addition, (meth)acrylamide, (meth)acryldialkylamide, vinyl esters such as vinyl acetate, vinyl ethers, (meth)allyl ethers and other aromatic vinyl monomers, and α-olefin monomers such as ethylene and propylene can also be used as the (Z) other vinyl group-containing monomer. The weight average molecular weight of the copolymer is preferably 4000 to 25000. The weight average molecular weight is more preferably 5000 to 15000. The epoxy value of the copolymer is 400 to 2500 equivalents / 1×10 6 g, and more preferably 500 to 1500 equivalents / 1×10 6 g, and more preferably 600 to 1000 equivalents / 1×10 6 g.

[0033] The carbodiimide crosslinking agent is not particularly limited as long as it is a polycarbodiimide having two or more carbodiimide groups (-N=C=N- structure) in one molecule, and examples thereof include aliphatic polycarbodiimides, alicyclic polycarbodiimides, aromatic polycarbodiimides, and copolymers thereof. Preferred are aliphatic polycarbodiimide compounds or alicyclic polycarbodiimide compounds.

[0034] The polycarbodiimide compound can be obtained, for example, by the decarbonation reaction of a diisocyanate compound. Examples of the diisocyanate compound that can be used here include 4,4'-diphenylmethane diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 1,5-naphthylene diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, cyclohexane-1,4-diisocyanate, xylylene diisocyanate, isophorone diisocyanate, methylcyclohexane diisocyanate, tetramethylxylylene diisocyanate, and 1,3,5-triisopropylphenylene-2,4-diisocyanate. These may be used alone or in the form of copolymerization of two or more. In addition, a branched structure may be introduced, or a functional group other than a carbodiimide group or an isocyanate group may be introduced by copolymerization. Furthermore, the terminal isocyanate may be used as it is, but the degree of polymerization may be controlled by reacting the terminal isocyanate, or a part of the terminal isocyanate may be blocked.

[0035] As the polycarbodiimide compound, in particular, alicyclic polycarbodiimides derived from dicyclohexylmethane diisocyanate, cyclohexane-1,4-diisocyanate, isophorone diisocyanate, etc. are preferred, and polycarbodiimides derived from dicyclohexylmethane diisocyanate or isophorone diisocyanate are particularly preferred.

[0036] The polycarbodiimide compound preferably contains 2 to 50 carbodiimide groups per molecule in terms of stability and handling. More preferably, the polycarbodiimide compound contains 5 to 30 carbodiimide groups per molecule. The number of carbodiimides in a polycarbodiimide molecule (i.e., the number of carbodiimide groups) corresponds to the degree of polymerization in the case of a polycarbodiimide obtained from a diisocyanate compound. For example, the degree of polymerization of a polycarbodiimide obtained by linking 21 diisocyanate compounds in a chain is 20, and the number of carbodiimide groups in the molecular chain is 20. Usually, a polycarbodiimide compound is a mixture of molecules of various lengths, and the number of carbodiimide groups is expressed as an average value. If the polycarbodiimide compound has the number of carbodiimide groups in the above range and is solid around room temperature, it can be powdered, so it is excellent in workability and compatibility when mixed with the thermoplastic polyester elastomer (A), and is also preferable in terms of uniform reactivity and bleed-out resistance. The number of carbodiimide groups can be measured, for example, by a conventional method (a method of dissolving in an amine and performing back titration with hydrochloric acid).

[0037] The polycarbodiimide compound has an isocyanate group at its terminal, and the isocyanate group content is preferably 0.5 to 4 mass% from the viewpoint of stability and ease of handling. More preferably, the isocyanate group content is 1 to 3 mass%. In particular, it is preferable that the polycarbodiimide is derived from dicyclohexylmethane diisocyanate or isophorone diisocyanate and has an isocyanate group content in the above range. The isocyanate group content can be measured by a conventional method (a method of dissolving in an amine and performing back titration with hydrochloric acid).

[0038] Examples of the isocyanate-based crosslinking agent include the above-mentioned polycarbodiimide compounds containing an isocyanate group and the above-mentioned isocyanate compounds which are raw materials for the polycarbodiimide compounds.

[0039] As the acid anhydride crosslinking agent, a compound containing 2 to 4 anhydrides per molecule is preferred in terms of stability and ease of handling. Examples of such compounds include phthalic anhydride, trimellitic anhydride, and pyromellitic anhydride.

[0040] The amount (content) of the crosslinking agent used is appropriately adjusted depending on the extrusion conditions, the desired expansion ratio, etc., and is, for example, preferably 0.1 to 4.5 parts by mass, more preferably 0.1 to 4 parts by mass, and even more preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the thermoplastic polyester elastomer (A).

[0041] As the crosslinking agent, an epoxy-based crosslinking agent is preferred, in particular, a styrene-based copolymer containing two or more glycidyl groups per molecule, a weight average molecular weight of 4000 to 25000, and consisting of (X) 20 to 99% by mass of a vinyl aromatic monomer, (Y) 1 to 80% by mass of glycidyl (meth)acrylate, and (Z) 0 to 79% by mass of a vinyl group-containing monomer other than (X) that does not contain an epoxy group. However, when a compound having a functional group with high reactivity such as a carbodiimide group is used in combination with an epoxy compound, the molecular weight distribution of the resin composition after crosslinking tends to become narrow. Therefore, the injection pressure during injection molding may increase, the foam nucleus may disappear, and the foaming ratio may decrease. Therefore, in the resin composition used in the present invention, it is preferable not to use an epoxy-based crosslinking agent and a carbodiimide-based crosslinking agent in combination as crosslinking agents.

[0042] Furthermore, in addition to the crosslinking agent, various additives can be blended into the thermoplastic polyester elastomer (A) used in the present invention depending on the purpose. The type of such additives is not particularly limited, and various additives usually used in foam molding can be used. Specifically, additives include known hindered phenol-based, sulfur-based, phosphorus-based, and amine-based antioxidants, hindered amine-based, as well as benzotriazole-based, benzophenone-based, benzoate-based, triazole-based, nickel-based, and salicylic light stabilizers, lubricants, fillers, flame retardants, flame retardant assistants, mold release agents, antistatic agents, molecular regulators such as peroxides, metal deactivators, organic and inorganic nucleating agents, neutralizing agents, antacids, antibacterial agents, fluorescent brighteners, organic and inorganic pigments, as well as organic and inorganic phosphorus compounds used for the purpose of imparting flame retardancy and thermal stability. The amount of additives added can be appropriately selected within a range that does not impair the formation of bubbles, and the amount used in molding of ordinary thermoplastic resins can be adopted.

[0043] [Thermoplastic polyester elastomer resin composition] In the present invention, the foamed molded product may be formed by only the thermoplastic polyester elastomer (A) or by containing the above-mentioned crosslinking agent or additives in the thermoplastic polyester elastomer (A). Therefore, for convenience, the thermoplastic polyester elastomer (A) or the thermoplastic polyester elastomer (A) containing the above-mentioned crosslinking agent or additives is called a "thermoplastic polyester elastomer resin composition". When the thermoplastic polyester elastomer (A) contains the above-mentioned crosslinking agent or additives, the thermoplastic polyester elastomer resin composition preferably contains 70% by mass or more of the thermoplastic polyester elastomer (A), more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more.

[0044] [Foam molded body] The foamed molded article of the present invention is obtained by using the polyester elastomer resin composition of the present invention described above. The foaming method of the present invention is not particularly limited, but a foaming method in which the resin composition is impregnated with a high-pressure gas and then the pressure is reduced (pressure is released) is preferred. Among them, a method in which the foamed molded article is obtained by expanding the volume of the cavity when melt-mixing the foaming agent and the polyester elastomer resin composition of the present invention and injection-molding the mixture, as a molding method that can obtain a homogeneous foam in terms of molding cycle property, cost, etc., is preferred. Specifically, as shown in FIG. 1, a polyester elastomer resin composition in a molten state is injected and filled into a cavity 3 formed by a plurality of molds 1 and 2 that are clamped together with a chemical foaming agent and / or a supercritical inert gas (hereinafter, these may be collectively referred to as "foaming agent"). At the stage when a non-foamed skin layer having a thickness of 100 to 800 μm is formed on the surface layer, at least one mold 2 is moved in the mold opening direction to expand the volume of the cavity 3, thereby obtaining a foamed molded article. Specifically, after the polyester elastomer resin composition and the foaming agent are filled into the cavity 3, the cavity 3 is cooled at a predetermined temperature to form a non-foamed skin layer on the surface of the polyester elastomer resin composition filled into the cavity 3. When the non-foamed skin layer reaches a predetermined thickness (100 to 800 μm), the mold 2 is moved in the mold opening direction to expand the volume of the cavity 3. The thermoplastic polyester elastomer resin composition for foam molding and the foaming agent can be mixed in the plasticization area 4a of the injection molding machine 4 before filling the cavity 3. The foam molded product of the present invention usually has a sandwich structure in which non-foamed skin layers are provided on both sides of the foam layer (in other words, a structure in which the foam layer is sandwiched between non-foamed skin layers from both sides). There is no particular restriction on the size of the foam molded product, but the thickness of the sandwich structure is expected to be about 1 to 30 mm.

[0045] The foam layer is composed of a resin continuous phase and independent foam cells. Here, the resin continuous phase means a portion formed of a cured polyester elastomer resin composition that has no cavities. The diameter of the foam cells (cell diameter) varies depending on the size, as long as it is uniform and does not vary. In order to achieve high resilience, a smaller cell diameter is advantageous, and specifically, the average cell diameter is preferably 10 to 400 μm. More preferably, it is 100 to 400 μm, and even more preferably, it is 200 to 400 μm. When the average cell diameter is less than 10 μm, the internal pressure of the molded body is low and the pressure during the formation of the non-foamed skin layer is insufficient, which tends to deteriorate the appearance, such as sink marks. On the other hand, when the average cell diameter exceeds 400 μm, the load resistance and resilience tend to be low.

[0046] The foamed molded article of the present invention has a maximum cell diameter of 10 to 500 μm, more preferably 400 μm or less. Since the foamed molded article of the present invention has a maximum cell diameter of 500 μm or less, it has excellent uniformity of cell structure and does not contain coarse cells, and therefore has excellent resilience.

[0047] The non-foamed skin layer is laminated on the foamed layer and preferably has a thickness of 100 to 800 μm. If the thickness of the non-foamed skin layer is less than 100 μm, a good appearance tends not to be obtained, while if it exceeds 800 μm, the specific gravity of the foamed layer becomes too low, and the foamed molded article as a whole has a density of 0.01 to 0.40 g / cm3 (described later). 3 In such a case, it is difficult to obtain a foamed structure having uniform cells. The thickness of the non-foamed skin layer is more preferably 200 to 600 μm, and further preferably 300 to 450 μm.

[0048] The density of the foamed molded article of the present invention is 0.01 to 0.40 g / cm 3 The density of a typical polyester elastomer is about 1.0 to 1.4 g / cm. 3 Therefore, it can be said that the foamed molded article of the present invention is sufficiently lightweight. More preferably, it is 0.1 to 0.35 g / cm. 3 and more preferably 0.18 to 0.30 g / cm 3The density is 0.01g / cm 3 If it is less than 0.40 g / cm, sufficient resilience and strength are not obtained, and the mechanical properties tend to be inferior. 3 If the density exceeds 0.01, sufficient flexibility tends not to be obtained. To achieve both excellent high resilience and flexibility, the density of the foamed molded product should be 0.01 to 0.25 g / cm. 3 It is more preferable that:

[0049] The foamed molded article of the present invention has a uniform and fine cell structure because the average cell size is within a specific range, the maximum cell size is within a specific range, no coarse cells are contained, and the density is within a specific range. As a result, the high resilience modulus, which is a characteristic of the polyester elastomer resin composition of the present invention, can be achieved even during foaming. The foamed molded article of the present invention has a resilience modulus of 40 to 90%. The resilience modulus is preferably 50 to 90%, more preferably 60 to 90%.

[0050] The chemical foaming agent that can be used to obtain the foamed molded article of the present invention is added to the molten resin in the resin melting zone of a molding machine as a gas component that becomes the foaming nucleus or as a source of the gas component. Specifically, the chemical foaming agent may be an inorganic compound such as ammonium carbonate or sodium bicarbonate, or an organic compound such as an azo compound, a sulfohydrazide compound, a nitroso compound, or an azide compound. Examples of the azo compound include diazocarbonamide (ADCA), 2,2-azoisobutyronitrile, azohexahydrobenzonitrile, and diazoaminobenzene, among which ADCA is preferably used. Examples of the sulfohydrazide compound include benzenesulfohydrazide, benzene 1,3-disulfohydrazide, diphenylsulfone-3,3-disulfonehydrazide, and diphenyloxide-4,4-disulfonehydrazide. Examples of the nitroso compound include N,N-dinitrosopentaethylenetetramine (DNPT), and examples of the azide compound include terephthalazide and p-tert-butylbenzazide.

[0051] When a chemical foaming agent is used as a foaming agent, the chemical foaming agent can be used as a foaming agent masterbatch based on a thermoplastic resin having a melting point lower than the decomposition temperature of the chemical foaming agent in order to disperse the chemical foaming agent uniformly in the polyester elastomer resin composition of the present invention. The base thermoplastic resin is not particularly limited as long as it has a melting point lower than the decomposition temperature of the chemical foaming agent, and examples thereof include polystyrene (PS), polyethylene (PE), and polypropylene (PP). In this case, the compounding ratio of the chemical foaming agent to the thermoplastic resin is preferably 10 to 100 parts by mass of the chemical foaming agent per 100 parts by mass of the thermoplastic resin. If the chemical foaming agent is less than 10 parts by mass, the amount of the masterbatch relative to the polyester elastomer resin composition of the present invention may be too large, resulting in a decrease in physical properties. If the amount exceeds 100 parts by mass, it becomes difficult to make a masterbatch due to the problem of dispersibility of the chemical foaming agent.

[0052] When a supercritical inert gas is used as a foaming agent, carbon dioxide and / or nitrogen can be used as the inert gas. When supercritical carbon dioxide and / or nitrogen are used as a foaming agent, the amount is preferably 0.05 to 30 parts by mass, more preferably 0.1 to 20 parts by mass, per 100 parts by mass of the polyester elastomer resin composition of the present invention. If the amount of supercritical carbon dioxide and / or nitrogen is less than 0.05 parts by mass, it becomes difficult to obtain uniform and fine foam cells, and if it exceeds 30 parts by mass, the appearance of the molded product surface tends to be impaired.

[0053] In addition, the supercritical carbon dioxide or nitrogen used as the foaming agent can be used alone, but carbon dioxide and nitrogen may be mixed and used. Nitrogen tends to be suitable for forming finer cells in the polyester elastomer resin composition, and carbon dioxide is suitable for obtaining a higher expansion ratio because it can relatively increase the amount of gas injected, so they may be mixed arbitrarily depending on the state of the adjusted foam structure, and the mixing ratio when mixed is preferably in the range of 1:9 to 9:1 in molar ratio.

[0054] Other examples of the blowing agent include hydrocarbon-based blowing agents such as propane, n-butane, i-butane, n-pentane, i-pentane, and neopentane, and ether-based blowing agents such as dimethyl ether, diethyl ether, methyl ethyl ether, isopropyl ether, n-butyl ether, diisopropyl ether, furan, furfural, 2-methylfuran, tetrahydrofuran, and tetrahydropyran. The blowing agent may be encapsulated in a thermally expandable microcapsule.

[0055] As the foaming agent used in the present invention, from the viewpoint of uniform fine foaming, nitrogen in a supercritical state is more preferable.

[0056] In order to inject the polyester elastomer resin composition in a molten state together with a blowing agent into the cavity 3, the polyester elastomer resin composition in a molten state and the blowing agent may be mixed in a plasticization region 4a of an injection molding machine 4. In particular, when carbon dioxide and / or nitrogen in a supercritical state are used as the blowing agent, a method of injecting gaseous carbon dioxide and / or nitrogen directly from a gas cylinder 5 into the injection molding machine 4 or pressurizing the gaseous carbon dioxide and / or nitrogen with a booster pump 6 as shown in Fig. 1 can be employed. The carbon dioxide and / or nitrogen must be in a supercritical state inside the molding machine from the viewpoint of solubility, permeability, and diffusibility in the polyester elastomer resin composition in a molten state.

[0057] Here, the supercritical state refers to a state in which, when the temperature and pressure of a substance that has gas and liquid phases are increased, the distinction between the gas and liquid phases can be eliminated in a certain temperature and pressure range, and the temperature and pressure at this time are called the critical temperature and critical pressure. That is, in the supercritical state, a substance has the properties of both gas and liquid, so the fluid that occurs in this state is called a critical fluid. Such a critical fluid has a higher density than a gas and a lower viscosity than a liquid, so it has the property of being very easy to diffuse in a substance. EXAMPLES

[0058] In order to demonstrate the effects of the present invention, examples are given below, but the present invention is not limited to these examples in any way.

[0059] In the following examples and comparative examples, the following raw materials were used. [Thermoplastic polyester elastomer (A)] (Polyester elastomer A-1) According to the method described in JP-A-9-59491, a thermoplastic polyester elastomer having a soft segment content of 44 mass% was produced using dimethyl terephthalate, 1,4-butanediol, and poly(tetramethylene oxide) glycol (PTMG) having a number average molecular weight of 450 as raw materials, and this was named polyester elastomer A-1. (Polyester elastomer A-2) According to the method described in JP-A-9-59491, a thermoplastic polyester elastomer having a soft segment content of 44 mass% was produced using dimethyl terephthalate, 1,4-butanediol, and poly(tetramethylene oxide) glycol having a number average molecular weight of 650 as raw materials, and this was named polyester elastomer A-2. (Polyester elastomer A-3) According to the method described in JP-A-9-59491, a thermoplastic polyester elastomer having a soft segment content of 44 mass% was produced using dimethyl terephthalate, 1,4-butanediol, and poly(tetramethylene oxide) glycol having a number average molecular weight of 850 as raw materials, and this was named polyester elastomer A-3. (Polyester elastomer A-4) According to the method described in JP-A-9-59491, a thermoplastic polyester elastomer having a soft segment content of 72% by mass was produced using dimethyl terephthalate, 1,4-butanediol, and poly(tetramethylene oxide) glycol having a number average molecular weight of 850 as raw materials, and this was named polyester elastomer A-4. (Polyester elastomer A-5) According to the method described in JP-A-9-59491, a thermoplastic polyester elastomer having a soft segment content of 25% by mass was produced using dimethyl terephthalate, 1,4-butanediol, and poly(tetramethylene oxide) glycol having a number average molecular weight of 450 as raw materials, and this was designated as polyester elastomer A-5. (Polyester elastomer A-6) According to the method described in JP-A-9-59491, a thermoplastic polyester elastomer having a soft segment content of 25% by mass was produced using dimethyl terephthalate, 1,4-butanediol, and poly(tetramethylene oxide) glycol having a number average molecular weight of 650 as raw materials, and this was named polyester elastomer A-6. (Polyester elastomer A-7) According to the method described in JP-A-9-59491, a thermoplastic polyester elastomer having a soft segment content of 44 mass% was produced using dimethyl terephthalate, 1,4-butanediol, and poly(tetramethylene oxide) glycol having a number average molecular weight of 1000 as raw materials, and this was named polyester elastomer A-7. (Polyester elastomer A-8) According to the method described in JP-A-9-59491, a thermoplastic polyester elastomer having a soft segment content of 44% by mass was produced using dimethyl terephthalate, 1,4-butanediol, and poly(tetramethylene oxide) glycol having a number average molecular weight of 2000 as raw materials, and this was named polyester elastomer A-8. (Polyester elastomer A-9) According to the method described in JP-A-9-59491, a thermoplastic polyester elastomer having a soft segment content of 44% by mass was produced using dimethyl terephthalate, dimethyl isophthalate, 1,4-butanediol, and poly(tetramethylene oxide) glycol having a number average molecular weight of 2000 as raw materials, and this was named polyester elastomer A-9. The dicarboxylic acid components had a terephthalic acid component / isophthalic acid component ratio of 75 / 25 (molar ratio). (Polyester elastomer A-10) According to the method described in JP-A-9-59491, a thermoplastic polyester elastomer having a soft segment content of 25% by mass was produced using dimethyl terephthalate, 1,4-butanediol, and poly(tetramethylene oxide) glycol having a number average molecular weight of 2000 as raw materials, and this was designated as polyester elastomer A-10. The number average molecular weight of poly(tetramethylene oxide) glycol (PTMG) is a value determined by quantifying the amount of terminal hydroxyl groups.

[0060] [Crosslinking agent (B)] (Styrene-based copolymer 1 (B-1)) The oil jacket temperature of a 1-liter pressurized stirred tank reactor equipped with an oil jacket was kept at 200°C. Meanwhile, a monomer mixture consisting of 89 parts by mass of styrene (St), 11 parts by mass of glycidyl methacrylate (GMA), 15 parts by mass of xylene (Xy), and 0.5 parts by mass of ditertiary butyl peroxide (DTBP) as a polymerization initiator was charged into a raw material tank. This was continuously fed from the raw material tank to the reactor at a constant feed rate (48 g / min, residence time: 12 min), and the reaction liquid was continuously extracted from the outlet of the reactor so that the content liquid mass of the reactor was constant at about 580 g. The temperature inside the reactor at that time was kept at about 210°C. After 36 minutes had elapsed since the temperature inside the reactor stabilized, the extracted reaction liquid was introduced into a thin-film evaporator kept at a reduced pressure of 30 kPa and a temperature of 250°C, and the volatile components were continuously removed to obtain a styrene-based copolymer (B-1). According to GPC analysis (polystyrene equivalent), this styrene copolymer (B-1) had a weight average molecular weight of 8500 and a number average molecular weight of 3300. According to the following measurement method, the epoxy value was 670 equivalents / 1×10 6 g, the epoxy valence (the average number of epoxy groups per molecule) is 2.2, and each molecule has two or more glycidyl groups.

[0061] [Epoxy value measurement method] The sample was weighed into a 100 ml ethylene Mayer flask, 10-15 ml of methylene chloride was added, and the mixture was stirred and dissolved using a magnetic stirrer. 10 ml of tetraethyleneammonium bromide reagent was added, followed by 6-8 drops of crystal violet indicator, and neutralized with 0.1 N perchloric acid. The end point was the point at which the color changed from blue to green and remained stable for 2 minutes. The amount of perchloric acid required for titration (ml) was A, the mass of the sample was W (g), and the normality of the perchloric acid reagent was N. The epoxy value was calculated based on the following formula. Epoxy value (equivalent / 1×10 6 g) = (N x A x 1000) / W

[0062] Examples 1 to 6, Comparative Examples 1 to 4 According to the compounding composition shown in Table 1, various components were melt-kneaded with 100 parts by mass of thermoplastic polyester elastomer using a twin-screw extruder, and then pelletized to obtain pellets of Examples 1-6 and Comparative Examples 1-4.

[0063] Next, the thermoplastic polyester elastomer resin composition obtained above was used to produce a foamed molded product by the above-mentioned mold expansion method. As the mold, a mold for producing a flat plate was used, which is composed of a fixed mold and a working mold, and can form a cavity with a width of 100 mm, a length of 100 mm, and a thickness of 3 mm when the mold is clamped, and can form a cavity with the same width and length and a thickness of 3 mm + core back amount (mm) when the mold is cored back in the mold opening direction. Specifically, in the plasticization region of an electric injection molding machine having a mold clamping force of 1800 kN, a screw diameter of 40 mm, and a screw stroke of 180 mm, nitrogen in a supercritical state was injected, and the mold, whose surface temperature was controlled to 50 ° C., was injected and filled, and at the stage where a non-foamed skin layer of 100 to 800 μm was formed by the injection external pressure and the foaming pressure from the inside, the working mold was moved in the mold opening direction by the length shown as the core back amount (mm) in Table 1 to expand the volume of the cavity, and a foamed molded product was obtained.

[0064] The thermoplastic polyester elastomer resin compositions for foam molding obtained in Examples 1 to 6 and Comparative Examples 1 to 4 and the foam molded articles obtained from the resin compositions were evaluated as follows. The results are shown in Table 1.

[0065] [Melting point] Using a differential scanning calorimeter "DSC220" manufactured by Seiko Denshi Kogyo Co., Ltd., 5 mg of the measurement sample was placed in an aluminum pan, the lid was pressed down and sealed, and the sample was melted in nitrogen at 250°C for 2 minutes. The temperature was then lowered to 50°C at a rate of 20°C / min, and the temperature was then increased from 50°C to 250°C at a rate of 20°C / min. The endothermic peak due to melting from the obtained thermogram curve was taken as the melting point.

[0066] [Density (apparent density)] The dimensions of the foamed molded product were measured with a vernier caliper, and the mass was measured with an electronic balance, and calculated according to the following formula. Density (g / cm 3 ) = mass of test piece / volume of test piece

[0067] [Average cell diameter] The cross-section of the foamed sample was photographed with a scanning electron microscope (SU1510, Hitachi High-Technologies Corporation), and the cell diameter was determined by measuring the circle-equivalent diameter of at least 100 adjacent cells with a caliper. The average of the 100 cells was calculated, and this was done at three random locations. The average of the three average values ​​was taken as the average cell diameter.

[0068] [Skin thickness] A photograph of the foamed cross section of the sample for cross-sectional observation taken with a scanning electron microscope SU1510 manufactured by Hitachi High-Technologies was processed, and the thickness of the integrated non-foamed layer observed in the surface layer was measured as the skin layer thickness.

[0069] [Rebound elasticity] The measurement was carried out according to the method described in JIS K 6400. Using a manual measuring tester, a steel ball was dropped onto the test piece from a specified height, and the maximum height of the rebound was read. Three measurements were taken within one minute, and the median value was calculated to calculate the rebound resilience.

[0070] [Table 1]

[0071] The thermoplastic polyester elastomer resin composition of the present invention can be molded at low temperatures, and the obtained foamed molded article is lightweight and exhibits a high rebound resilience, but depending on the application, various other properties such as mechanical properties are required. Therefore, the evaluation results are compared between compositions having the same soft segment amount. As is clear from Table 1, all of Examples 1 to 6 within the scope of the present invention are lightweight and exhibit high resilience while being moldable at lower temperatures. In particular, Examples 1 to 4 have an excellent balance of these properties. In contrast, Comparative Examples 1 and 2 have the same soft segment amount as Examples 1 to 3, and are lightweight and exhibit high resilience, but have high melting points, which increases the molding temperature. In Comparative Example 3, dimethyl isophthalate is used to lower the melting point to the same level as Example 1 with the same soft segment amount, but the resilience is poor. Comparative Example 4 has the same soft segment amount as Examples 5 and 6, and is lightweight and exhibits high resilience, but has a very high melting point. [Industrial Applicability]

[0072] The thermoplastic polyester elastomer resin composition for foam molding of the present invention and the foam molded article made therefrom can be molded at a lower temperature, and therefore have excellent moldability in various foam molding techniques. The foam molded article is not only lightweight, but also has high resilience. Furthermore, the polyester foam molded article has a uniform foaming state, high heat resistance, water resistance, and molding stability despite a high expansion ratio, and therefore can be used for parts that require high reliability. [Explanation of symbols]

[0073] 1 Mold (for fixing) 2. Mold (for operation) 3 Cavity 4 Injection molding machine 4a Plasticization region 5 Gas Cylinders 6 Booster Pump 7 Pressure Control Valve

Claims

1. A thermoplastic polyester elastomer resin composition for foam molding, comprising a thermoplastic polyester elastomer in which a hard segment made of a polyester having as its constituent components an aromatic dicarboxylic acid and an aliphatic and / or alicyclic diol is bonded to at least one soft segment selected from an aliphatic polyether, an aliphatic polyester, and an aliphatic polycarbonate, the soft segment having a number average molecular weight of less than 1,000 and a soft segment content of 10 to 80 mass%.

2. A foamed molded article comprising the thermoplastic polyester elastomer resin composition according to claim 1.

3. 3. The foam molded article according to claim 2, characterized in that the rebound resilience is 50 to 90%.

4. It has a foam layer made of independent foam cells having an average cell diameter of 10 to 400 μm and a maximum cell diameter of 10 to 500 μm, and has a density of 0.01 to 0.40 g / cm 3 4. The foamed molded article according to claim 2 or 3,

5. 5. The foam molded article according to claim 2, which has a non-foamed skin layer having a thickness of 100 to 800 μm as a surface layer, a foamed layer composed of foamed cells having an average cell diameter of 10 to 400 μm independent of a resin continuous phase as an inner layer, and has a sandwich structure of the non-foamed skin layer and the foamed layer in the thickness direction.

Citation Information

Patent Citations

  • Thermoplastic polyester elastomer foaming precursor and foaming body

    CN110128639A

  • Molded polyester block copolymer containing foaming agents

    JP1977058767A

  • Seal of floating roof of tank

    JP1983041076A

  • Abnormality display device for business equipment

    JP1988058368A

  • Foamed polyester resin sheet

    JP1998067878A