Integrated molding and manufacturing method thereof

By strategically positioning molten resin confluence lines between resin layers and adjusting injection conditions, the method addresses weld line strength issues in injection molding, resulting in a lightweight, thin, and structurally robust integrated molded body.

JP7567780B2Active Publication Date: 2024-10-16TORAY INDUSTRIES INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021513470
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-18
Filing Date
2021-03-09
Publication Date
2024-10-16
Estimated Expiration
2041-03-09

AI Technical Summary

Technical Problem

Existing injection molding methods result in weld lines with lower strength at confluence points, leading to reduced structural integrity and increased complexity in manufacturing processes, particularly when using fiber-reinforced resins.

Method used

The method involves interposing a resin inner material between a plate material and a resin outer material, forming molten resin confluence lines in specific positions shifted from each other, and adjusting injection conditions to ensure high bonding strength and reduced warpage, while maintaining a lightweight and thin structure.

Benefits of technology

The integrated molded body achieves high joint strength, reduced warpage, and thinner profiles by strategically positioning molten resin confluence lines to complement strength deficiencies, enhancing overall structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567780000002
    Figure 0007567780000002
  • Figure 0007567780000003
    Figure 0007567780000003
  • Figure 0007567780000004
    Figure 0007567780000004
Patent Text Reader

Abstract

An integrally molded body that is a rectangular planar structure in which a resin inner member (B1) containing a thermoplastic resin is interposed between a plate (A), the surface on one side of which is a design surface, and a resin outer member (C1), which contains a thermoplastic resin, the planar structure having a first joining part in which at least a partial region of the outer-peripheral-side surface part and / or the outer peripheral edge part of the plate (A) is joined with the resin inner member (B1), and a second joining part in which at least a partial region of the outer-peripheral-side surface part and / or the outer peripheral edge part of the resin inner member (B1) is joined with the resin outer member (C1), molten resin confluence lines being formed in at least one location on each of the resin inner member (B1) and the resin outer member (C1) on the side (non-design-surface side) of the plate (A) opposite from the design surface, and the molten resin confluence lines being in a positional relationship such that one position among molten resin confluence lines (B2) formed on the resin inner member (B1) specified along a direction parallel to the outer peripheral side of the integrally molded body, and the position of a molten resin confluence line (C2) formed on the resin outer member (C1) in the position closest to that of the molten resin confluence lines (B2), are offset from each other. Provided are an integrally molded body in which any decrease in strength is suppressed in a molded body in which molten resin confluence lines are formed in a resin member by injection molding, and a method for manufacturing the integrally molded body.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an integrally molded product suitable for applications requiring light weight, high strength, high rigidity and thin wall thickness, for use as parts or housings of personal computers, office automation equipment, mobile phones and the like. [Background technology]

[0002] Currently, as electrical and electronic devices such as personal computers, office automation equipment, audiovisual equipment, mobile phones, telephones, facsimiles, home appliances, and toys become more portable, there is a demand for them to be smaller and lighter. To meet this demand, the components that make up the devices, especially the housings, must be strong and rigid while being thin-walled so that they do not bend significantly when an external load is applied, causing contact with internal components and resulting in destruction. In addition, reliable joint strength is required for molded structures that are made smaller and lighter by integrally joining a fiber-reinforced resin structure made of reinforcing fibers and resin with another member, such as a frame member, to form a fiber-reinforced resin structure.

[0003] Patent Document 1 (WO 2018 / 110293) describes an integrally molded body in which a bonding resin (C) is interposed between a plate material (A) having a design surface on one surface and a member (B), in which at least a portion of the outer periphery of the plate material (A) has a first bonding portion that is bonded to the bonding resin (C), the plate material (A) and the member (B) are separated, and at least a portion of the surface of the design surface side of the integrally molded body has an area where the plate material (A), the member (B), and the bonding resin (C) are exposed. The patent document discloses the following effects: a plurality of structures are bonded with high bonding strength, the bonded boundary has good smoothness, and even if the molded body has a plate material component, warping can be reduced and a lighter and thinner body can be achieved.

[0004] Patent Document 2 (JP 2005-1215 A) describes a manufacturing method for injection-molded products in which parts are manufactured using a multi-point injection molding machine, the manufacturing method including a skin film placing step of placing a skin film on one of the movable and fixed molds that make up the mold of the multi-point injection molding machine, a first filling step of injecting molten resin into a cavity in the mold from a first injection gate provided on the other of the fixed and movable molds and filling and solidifying the resin while leaving at least a part of the cavity, and a second filling step of injecting molten resin into the remaining cavity from a second injection gate provided on the other mold, the same as the first injection gate, after the first filling step, and filling and solidifying the resin. The method discloses the effect of obtaining injection-molded products with invisible weld lines, even when manufacturing molded products using a multi-point injection molding machine.

[0005] In addition, Patent Document 3 (JP Patent Publication 8-318547A) discloses an injection molding method in which molten resin is injected into a mold having a cavity with two sprues, in which an injection molding machine with two injection units arranged corresponding to the positions of the two sprues is used, and the molten resin is injected into the mold from the two injection units simultaneously or with a time lag, and the injection operation and the suck-back operation of the two injection units are alternately repeated so as to be reversed from the time the molten resin is injected until it is cooled and solidified, thereby forcibly swinging the molten resin in the cavity. Therefore, the orientation of the molten resin is disturbed, and the strength of the molded product is uniform at any position. In particular, when the resin contains reinforcing materials such as glass fibers or carbon fibers, the reinforcing materials are entangled at the junction of the molten resin and are no longer oriented in one direction, so that the reduction in strength at the junction is prevented.

[0006] Patent Document 4 (JP Patent Publication 6-210669A) discloses that the mold is provided with a number of gates opening into the cavity, a number of runners connected to the gates, and a number of flow rate control mechanisms for increasing and decreasing the flow rate per hour in the runners at different times, and since the amount of resin flowing in per unit time from each gate increases and decreases at different times, the position where the multiple resin flows that flow into the cavity from the multiple gates join together in the cavity is distributed to the left and right along a line corresponding to the weld line according to the increase and decrease in the amount of resin flowing in for each gate. As a result, the weld line that should be generated at the joining part becomes a fine and intricate line on the left and right, and is essentially eliminated.

[0007] Patent Document 5 (JP Patent Publication 6-285911 A) describes a configuration having pressure detection means for detecting when the pressure of the injected molten resin exceeds a predetermined value at a point closer to the first predetermined position than a third predetermined position where the two flows of molten resin injected from the two gates meet in the resin filling space and a weld line is expected to form when molten resin is simultaneously injected from a first gate and a second gate; a small space for evacuating the molten resin injected from the first gate into the resin filling space at a point closer to the first predetermined position than the third predetermined position; and valve means for normally keeping an inlet to the resin filling space side of the small space closed, and opening the inlet to guide and evacuate a portion of the molten resin into the small space when the pressure exceeds a predetermined value in response to the pressure detection means; opening and closing the gate and opening the valve to guide and evacuate the resin in the vicinity into the small space, so that the pressure of the flow on the opposite side becomes relatively high at the portion where the weld line will be formed, causing the center of the tip of the flow to flow in and forming a deep uneven weld line. Therefore, the effect of increasing the strength of this portion is disclosed.

[0008] Patent Document 6 (JP Patent Publication No. 2000-167863) describes a method for reinforcing welds in short fiber reinforced thermoplastic resin, in which a reinforcing member made of a continuous fiber reinforced thermoplastic resin composite material having certain thermal properties is insert molded to reinforce the welds, and discloses the effect of significantly improving the strength of the welds without the need for special equipment. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] International Publication 2018 / 110293 [Patent Document 2] JP 2005-1215 A [Patent Document 3] Japanese Patent Application Publication No. 8-318547 [Patent Document 4] Japanese Patent Application Publication No. 6-210669 [Patent Document 5] Japanese Patent Application Publication No. 6-285911 [Patent Document 6] JP 2000-167863 A Summary of the Invention [Problem to be solved by the invention]

[0010] In some molds, the resin flow is forced to split in the resin filling space (cavity) inside the mold. When two or more of these split flows join together, the joining part solidifies without fully fusing with each other, forming a weld line (also called a weld part). The weld line that forms at this joining part has a problem in that its strength is weaker than other parts.

[0011] Patent Document 1 describes a method for integrally joining plate material and frame material by injection molding, but makes no mention of the weld lines that are expected to occur during injection molding, leaving room for improvement in reinforcement measures to address this issue.

[0012] In the configuration of Patent Document 2, the amount of filling in the second filling step is reduced from the total amount by the amount filled in the first filling step, so that the so-called mold clamping force can be significantly reduced compared to when it is applied to the total amount, and the skin film hides the weld lines that occur at the contact points of the molten resin from the surface. That This improves the surface appearance. However, although the skin film can hide the weld lines, there is a problem in suppressing the decrease in strength at the weld line junction.

[0013] In addition, in the configuration of Patent Document 3, in injection molding using a multi-point injection molding machine, the screws 12, 22 of each injection unit 10, 20 are moved back and forth alternately to forcibly oscillate the molten resin in the cavity 35, disturbing the orientation of the molten resin and ensuring a certain strength of the molded product. However, in order to repeat the injection operation and the suck-back operation, a control mechanism is required to move the screws 12, 22 of each injection unit 10, 20 back and forth alternately. If the molded product has a complex shape or the number of injection gate openings is increased, the number of injection units will increase, which complicates the control mechanism and results in a problem that the manufacturing process itself becomes complicated.

[0014] Furthermore, in the configuration of Patent Document 4, an extra flow control mechanism is required to adjust the amount of resin flowing from the gate per unit time during injection molding, which increases manufacturing costs. Constantly changing the amount of resin flowing in can cause unevenness in the flow of resin into the cavity during injection molding, and can even induce the generation of voids.

[0015] In addition, in the injection molding configuration of Patent Document 5, in order to form a deep uneven weld line by adjusting the pressure of the inflowing molten resin, a part of the molten resin is guided into a resin reservoir arranged outside the molding section, but this configuration requires extra space in the mold, which complicates the creation of the molding die and inevitably makes the die bulky. Also, in order to form a deep weld line more efficiently, it is necessary to detect the pressure of the molten resin and feed it back to the opening and closing of the valve, and the control of this feedback must also be considered, which results in a complicated control sequence and a problem that the manufacturing process itself becomes complicated.

[0016] In addition, the configuration of Patent Document 6 involves insert molding using a reinforcing member, and using that reinforcing member to reinforce the weld line. Since separate reinforcing members are laminated, the reinforced molded product becomes thick, posing a problem in realizing a thinner product.

[0017] In view of the problems with the conventional technology, the present invention has an object to provide an integrated molded body and a manufacturing method thereof that can maintain high joint strength and suppress a decrease in strength of the joined and integrated structure, reduce warping, and enable a reduction in weight and thickness when multiple structures are joined by injecting injection resin material from multiple injection gate openings, even if weld lines are generated where the resin materials join. [Means for solving the problem]

[0018] In order to solve the above problems, the present invention employs the following means. [1] A resin inner material (B1) containing a thermoplastic resin is interposed between a plate material (A) having a design surface on one side and a resin outer material (C1) containing a thermoplastic resin, An integrally molded body which is a rectangular planar structure having a first joint portion where at least a partial area of ​​an outer peripheral side surface portion and / or an outer peripheral edge portion of the plate material (A) is joined to the resin internal member (B1), and a second joint portion where at least a partial area of ​​an outer peripheral side surface portion and / or an outer peripheral edge portion of the resin internal member (B1) is joined to the resin external member (C1), An integrally molded body characterized in that one or more molten resin merging lines are formed in each of the internal resin component (B1) and the external resin component (C1) on the side opposite to the design surface (non-design surface side) of the plate material (A), and the position of one of the molten resin merging lines (B2) formed in the internal resin component (B1) specified along a direction parallel to the outer periphery of the integrally molded body is shifted from the position of the molten resin merging line (C2) formed in the external resin component (C1) that is closest to the position of the molten resin merging line (B2). [2] The integrally molded body according to [1], wherein the ratio M2 / M1 of the distance M2 (mm) between the molten resin merging line (B2) and the molten resin merging line (C2) closest to the molten resin merging line (B2) to the outer periphery length M1 (mm) of the integrally molded body is 0.04 to 0.4. [3] The integrally molded body according to [1] or [2], wherein the molten resin joining line (B2) is formed in a narrow portion (B1') provided in a part of the internal resin member (B1). [4] The integrally molded body according to any one of [1] to [3], wherein the molten resin joining line (C2) is formed in a narrow portion (C1') provided in a part of the outer resin member (C1). [5] The integrally molded body according to any one of [1] to [4], wherein the first joint portion is formed over the entire periphery of the outer peripheral side portion and / or outer peripheral edge portion of the plate material (A). [6] The integrally molded body according to any one of [1] to [5], wherein the second bonding portion is formed over the entire circumference of the outer circumferential side portion and / or the outer circumferential edge portion of the internal resin member (B1). [7] The integrally molded body according to any one of [1] to [6], wherein the internal resin member (B1) or the external resin member (C1) contains reinforcing fibers, the reinforcing fibers are discontinuous fibers, and the weight average fiber length of the discontinuous fibers is 0.3 to 3 mm. [8] A first step of injecting a precursor of a resin outer member (C1) from a plurality of resin injection gate openings (GC) into a molding die to form the resin outer member (C1) in advance; A second step of disposing a plate material (A) inside the resin outer member (C1) at a position spaced apart from at least a part of the resin outer member (C1); and a third step of injecting a precursor of a resin internal component (B1) from a plurality of resin injection gate ports (GB) into a gap between the plate material (A) and the resin external component (C1) to form a first joint portion that contacts at least a portion of an outer peripheral side surface portion and / or an outer peripheral edge portion of the plate material (A) with the resin internal component (B1) and a second joint portion that joins at least a portion of an outer peripheral side surface portion and / or an outer peripheral edge portion of the resin internal component (B1) with the resin external component (C1); A method for producing an integrated molded body having a rectangular planar structure, comprising the steps of: A method for manufacturing an integrally molded body, characterized in that, when viewed from the opposite side to the design surface (non-design surface side) of the plate material (A), the position of a molten resin merging line (B2) formed in the internal resin material (B1) specified along a direction parallel to the outer periphery of the integrally molded body and the position of a molten resin merging line (C2) formed in the external resin material (C1) and located closest to the molten resin merging line (B2) are shifted in at least one location or more by adjusting the injection conditions of the precursor of the internal resin material (B1) and the precursor of the external resin material (C1). [9] The method for manufacturing an integrally molded body described in [8], wherein the injection conditions are such that the position of one of the multiple resin injection gate openings (GB) for injecting the precursor of the resin inner member (B1) and the position of the resin injection gate opening (GC) for injecting the precursor of the resin outer member (C1) provided at the position closest to the position of the resin injection gate opening (GB) are set at positions shifted from a direction parallel to the outer periphery of the integrally molded body. It is. Effect of the Invention

[0019] According to the integrally molded body and its manufacturing method of the present invention, in the integrally molded body obtained by bonding a plurality of structures with injected resin, the bonds are strong and the molded body itself has high strength. Even if the molded body has plate-like components, warping can be reduced and a lightweight, thin-walled body can be achieved. [Brief description of the drawings]

[0020] [Figure 1] FIG. 2 is a perspective view of an integrally molded body according to the present invention. [Diagram 2] FIG. 2 is a plan view of an integrally molded body according to the present invention. [Diagram 3] 3 is a cross-sectional view taken along line AA' in FIG. 1 or FIG. 2. [Figure 4] FIG. 4 is an enlarged view of the region of the internal resin member (B1) or the external resin member (C1) in FIG. 3, and is a schematic cross-sectional view showing the flow state of resin proceeding inside a molding die by injection molding. [Diagram 5] FIG. 4 is an enlarged view of the region of the internal resin component (B1) or the external resin component (C1) in FIG. 3, and is a schematic cross-sectional view showing a state in which resins proceeding from the left and right collide with each other to form a molten resin confluence line. [Figure 6] This is a bottom view of the integrally molded body of the present invention, viewed from the non-design surface, showing the positional relationship of the molten resin confluence line formed by the confluence of resin parts injected from multiple resin injection gate openings. [Figure 7] FIG. 2 is a cross-sectional view of an integrally molded body according to the present invention in which a narrow width portion is provided in a part of the resin inner member (B1) and the resin outer member (C1). [Figure 8] FIG. 1 is a bottom view showing a step [1] of preforming a resin outer member (C1) by injecting a precursor of the resin outer member (C1) through a plurality of resin injection gate openings (GC) into a molding die. [Figure 9]FIG. 1 is a cross-sectional view of a molding die having a resin injection gate port (GC) for injecting the resin outer member (C1) and a space (cavity) for forming the resin outer member (C1) in the process [1] of preforming the resin outer member (C1). [Figure 10] 8 is a cross-sectional view taken along line BB' in FIG. 7, showing a state after the upper mold is removed after the resin outer member (C1) precursor is injected to form the resin outer member (C1). FIG. [Figure 11] FIG. 13 is a bottom view showing a process [2] of placing a plate material (A) having a design surface on one surface inside a molding die, with the plate material (A) being at least partially separated from the resin outer member (C1). [Figure 12] 12 is a cross-sectional view taken along CC' in FIG. 11. [Figure 13] FIG. 13 is a bottom view showing a process [3] in which a preformed resin outer component (C1) is placed in a molding die, and the precursor of the resin inner component (B1) is injected through multiple resin injection gate openings (GB) to form the resin inner component (B1). [Figure 14] FIG. 16 is a bottom view showing a process [3] in which a preformed resin outer member (C1) is placed in a molding die, and a precursor of the resin inner member (B1) is injected from multiple resin injection gate openings (GB) to form the resin inner member (B1), as an embodiment different from that shown in FIG. [Figure 15] FIG. 16 is a bottom view showing a process [3] in which a preformed resin outer member (C1) is placed in a molding die, and a precursor of the resin inner member (B1) is injected from multiple resin injection gate openings (GB) to form the resin inner member (B1), as an embodiment different from that shown in FIG. [Figure 16] FIG. 16 is a bottom view showing a process [3] in which a preformed resin outer member (C1) is placed in a molding die, and a precursor of the resin inner member (B1) is injected from multiple resin injection gate openings (GB) to form the resin inner member (B1), as an embodiment different from that shown in FIG. [Figure 17] FIG. 1 is a cross-sectional view of a molding die having a resin injection gate port (GB) for injecting the precursor of the resin internal component (B1) and a space (cavity) for forming the resin internal component (B1) in the process [3] of forming the resin internal component (B1). [Figure 18]13 is a cross-sectional view taken along the line DD' in FIG. 12, showing a state after the upper mold is removed after the internal-resin component (B1) is formed by injecting the precursor of the internal-resin component (B1). FIG. [Figure 19] FIG. 14 is a cross-sectional view including the member of FIG. 13. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, embodiments will be described with reference to the drawings. Note that the present invention is not limited to the drawings or the embodiments.

[0022] The structure of the integrally molded body 1 according to the present invention is an integrally molded body that is a rectangular planar structure having a first joint portion where a partial or entire area of ​​an outer peripheral side portion and / or an outer peripheral edge portion of the plate material (A) is joined to the resin inner member (B1) and a second joint portion where a partial or entire area of ​​an outer peripheral side portion and / or an outer peripheral edge portion of the resin inner member (B1) is joined to the resin outer member (C1), and the plate material (A) is a design surface on one side, and an inner resin member (B1) containing a thermoplastic resin is interposed between the inner resin member (B1), and the outer peripheral side portion and / or the outer peripheral edge portion of the inner resin member (B1) is joined to the resin outer member (C1). The present invention is characterized in that one or more molten resin merging lines are formed in each of the internal resin component (B1) and the external resin component (C1) on the side opposite to the design surface (non-design surface side) of the material (A), and the position of one of the molten resin merging lines (B2) formed in the internal resin component (B1) specified along a direction parallel to the outer periphery of the integrated molded body is shifted from the position of the molten resin merging line (C2) formed in the external resin component (C1) which is located in a position closest to the position of the molten resin merging line (B2).

[0023] A perspective view, a plan view, and an A-A' cross-sectional view of the integrally molded body 1 according to the present invention are shown in Fig. 1, Fig. 2, and Fig. 3, respectively. The integrally molded body 1 has a configuration in which an internal resin member (B1) 3 is interposed between a plate material (A) 2 and an external resin member (C1) 4. Here, the portion where the plate material (A) 2 and the internal resin member (B1) 3 are joined is a first joint portion 5, and the portion where the internal resin member (B1) 3 and the external resin member (C1) 4 are joined is a second joint portion 6. Note that, for the plate material (A) 2, the surface shown in Fig. 2 and the surface located at the top in Fig. 3 are the design surface.

[0024] Furthermore, at least a part of the surface on the design side of the integrally molded body 1 has an area 7 where the plate material (A) 2, the inner resin member (B1) 3 and the outer resin member (C1) 4 are exposed on the same plane.

[0025] The outer peripheral edge of the plate material (A) 2 is a flat area near the outer periphery of the plate material (A) 2 of the planar structure, and refers to an area within a width range equivalent to 0 to 15% of the length of each side constituting the outer peripheral end of the plate material (A) 2. The outer peripheral side surface portion is an end having a surface perpendicular to the flat area of ​​the outer periphery of the plate material (A) 2 of the planar structure. The same applies to the internal-resin member (B1) 3.

[0026] Next, we will explain the molten resin confluence lines (also called weld lines) that are formed in one or more locations on each of the inner resin component (B1) 3 and the outer resin component (C1) 4 on the side opposite the design surface (non-design surface side) of the plate material (A) 2.

[0027] When molten resin members 11 (precursor of the resin inner member (B1) 3 and precursor of the resin outer member (C1) 4) are injected into an injection mold through a plurality of injection resin injection gate openings, the molten resin members 11 proceed within the mold in the direction of arrow 12 along the cavity surface 10 of the mold, as shown in Figure 4. Note that resin injection gate openings are provided on both the left and right ends of Figure 4, but are omitted here.

[0028] 5, the molten resin member 11 flows through the mold while remaining in a molten state, but the leading edge of the molten resin member 11 changes from a molten state to a solidified state due to the temperature difference within the cavity over time from the time of injection. Furthermore, due to the temperature difference with the cavity surface 10 of the mold, the molten resin member 11 also changes from a molten state to a solidified state from the region close to the mold. In this partially solidified state, the molten resin members 11 flowing in the direction of the arrow 12 collide with each other in region 15.

[0029] In the collision area 15, the molten resin member 11 is partially solidified, and does not become completely molten, forming a molten resin joining line indicating the collision position. This is called a weld line, and the area where the molten resin joining line is formed is an area where the strength of the molded product formed tends to be lower than other areas.

[0030] Furthermore, when a fiber-reinforced resin is used as the molten resin member 11 as described below, it becomes difficult to arrange the reinforcing fibers across the molten resin merging line at the location where the molten resin merging line is formed, which disrupts the uniform dispersion of the reinforcing fibers near the molten resin merging line, making it easier for variations in weld strength to occur.

[0031] The integrally molded body 1 of the present invention is characterized in that one or more molten resin merging lines are formed in each of the internal resin member (B1) 3 and the external resin member (C1) 4, and the position of one of the molten resin merging lines (B2) formed in the internal resin member (B1) 3 specified along a direction parallel to the outer periphery of the integrally molded body 1 is offset from the position of the molten resin merging line (C2) formed in the external resin member (C1) 4 which is located closest to the position of the molten resin merging line (B2).

[0032] In one embodiment of the present invention shown in FIG. 6, the molten resin joining line (B2) 16 is formed on the upper and lower sides of the internal resin member (B1) 3. 2 Each one on the left and right side 1The molten resin joining lines (C2) 17 are formed in two on each of the upper and lower sides of the resin outer member (C1) 4, and in the center of the left and right sides. 2 pieces Each 6 shows a structure in which the molten resin joining line (B2) 16 and the molten resin joining line (C2) 17 are formed. In FIG. 6, when comparing the positions of the molten resin joining line (B2) 16 and the molten resin joining line (C2) 17 along a direction parallel to the outer periphery of the integrally molded body 1, both positions are shifted. In other words, the molten resin joining line (B2) 16 and the molten resin joining line (C2) 17 are arranged so as not to form a single continuous weld line. With this structure, the lack of strength at the location where the weld line, which is the molten resin joining line, is formed is complementarily compensated for by other resin members where no weld line is formed, thereby preventing a decrease in strength of the entire molded body.

[0033] In the present invention, the distance between the molten resin joining line (B2) 16 and the molten resin joining line (C2) 17 closest to the molten resin joining line (B2) 16 with respect to the outer periphery length M1 (mm) 18 of the integrally molded body 1 is away It is preferable that the ratio M2 / M1 to M2 (mm) 19 is 0.04 to 0.4.

[0034] As shown in FIG. 6, by maintaining a certain relationship between the distance between the molten resin merging line (B2) 16 and the nearest molten resin merging line (C2) 17 and the outer peripheral length of the integrally molded body 1, the strength at the position where the weld line is formed (hereinafter referred to as weld strength) can be improved compared to when the weld positions overlap.

[0035] If M2 / M1 is less than 0.04, the molten resin joining line (B2) 16 and Closest molten resin confluence line (C2) 17 and On the other hand, if M2 / M1 exceeds 0.4, the molten resin joining line (B2) 16 and Nearest molten resin confluence line ( C2)17 andHowever, this does not contribute to improving the weld strength. A more preferable range of M2 / M1 is 0.07 to 0.4, and an even more preferable range is 0.10 to 0.4.

[0036] In the present invention, it is also preferable that a molten resin merging line (B2) 16 is formed in a narrow region (B1') 18 provided in a part of the internal resin member (B1) 3. Similarly, in the present invention, it is also preferable that a molten resin merging line (C2) 17 is formed in a narrow region (C1') 19 provided in a part of the external resin member (C1) 4. Although the width is narrower, by forming the molten resin merging line in the narrow region (C1') 19, it is possible to shorten the width of the molten resin merging line, which is one factor that leads to a decrease in strength of the molded body, and thus it is possible to suppress a decrease in strength.

[0037] An example in which a narrow width portion is formed by forming the resin inner member (B1) 3 and the resin outer member (C1) 4 into a shape with repeated concave and convex shapes is shown in Figure 7. A molten resin merging line (B2) 16 is formed in the narrow width portion (B1') 24 of the resin inner member (B1) 3, and a molten resin merging line (C2) 17 is formed in the narrow width portion (C1') 25 of the resin outer member (C1) 4. Such a narrow width position can be achieved by adjusting the position of the resin injection gate opening, etc.

[0038] In the present invention, the first joint portion 5 is preferably formed over the entire circumference of the outer circumferential side surface of the plate material (A) 2. By forming the first joint portion 5 with the inner-resin member (B1) 3 over the entire circumference of the outer circumferential side surface of the plate material (A) 2, it is possible to realize high joint strength and thin-walled structure of the integrally molded body 1 as a whole.

[0039] In the present invention, the second joint portion 6 is preferably formed over the entire circumference of the outer circumferential side surface of the resin inner member (B1) 3. Second By forming the joint 6, the integrally molded body 1 as a whole can be made thin and with high joint strength.

[0040] In the present invention, it is preferable that the internal resin component (B1) 3 or the external resin component (C1) 4 contains reinforcing fibers, the reinforcing fibers are discontinuous fibers, and the weight average fiber length of the discontinuous fibers is 0.3 to 3 mm.

[0041] Here, continuous fiber and discontinuous fiber are defined. Continuous fiber means that the reinforcing fibers contained in the integrally molded body 1 are arranged substantially continuously over the entire length or width of the integrally molded body 1, and discontinuous fiber means that the reinforcing fibers are distributed intermittently. difference This refers to something that has been designed in this way.

[0042] When the weight average fiber length of the discontinuous reinforcing fibers remaining in the resin inner member (B1) 3 or the resin outer member (C1) 4 is 0.3 mm or more, the shrinkage rate of the resin inner member (B1) 3 or the resin outer member (C1) 4 can be reduced, and the warpage of the integrally molded body 1 can be further reduced. When the weight average fiber length is less than 0.3 mm, the effect of the low shrinkage rate is weak, and the warpage of the integrally molded body 1 may not be sufficiently reduced. When the weight average fiber length exceeds 3 mm, the resin viscosity increases, and it may be difficult to uniformly fill the resin inner member (B1) 3 or the resin outer member (C1) 4 up to the corners of the molding die during injection molding. The weight average fiber length of the discontinuous carbon fibers is preferably 0.4 to 2.8 mm, more preferably 0.7 to 1.5 mm, and even more preferably 0.9 to 1.2 mm.

[0043] Here, the "weight average fiber length" in the present invention refers to an average fiber length calculated by applying the method for calculating the weight average molecular weight to the calculation of the fiber length, rather than simply taking a number average, and taking into account the contribution of the fiber length, using the following formula, where the fiber diameter and density of the reinforcing fibers are considered to be constant. Weight average fiber length=Σ(Mi2×Ni) / Σ(Mi×Ni) Mi: fiber length (mm) Ni: Number of reinforcing fibers with fiber length Mi

[0044] The weight average fiber length can be measured by the following method. The molded product is heat-treated at 500°C for 60 minutes, and the reinforcing fibers in the molded product are taken out and uniformly dispersed in water. The water in which the reinforcing fibers are uniformly dispersed is sampled in a petri dish, dried, and observed under an optical microscope (50 to 200 magnifications). The lengths of 500 randomly selected reinforcing fibers are measured, and the weight average fiber length is calculated from the above formula.

[0045] In the present invention, the internal resin member (B1) 3 or the external resin member (C1) 4 preferably contains reinforcing fibers, and the reinforcing fibers are preferably discontinuous fibers having a weight average fiber content of 1 to 50% by weight. This increases the bonding strength and reduces the warping of the molded body 1. If the content is less than 1% by weight, it may be difficult to ensure the strength of the molded body 1, and if it exceeds 50% by weight, the filling of the internal resin member (B1) 3 or the external resin member (C1) 4 may be partially insufficient during injection molding. The content is preferably 5 to 40% by weight, more preferably 8 to 35% by weight, and even more preferably 12 to 30% by weight.

[0046] In the present invention, the discontinuous fibers contained in the internal resin member (B1) 3 are preferably carbon fibers from the viewpoints of rigidity and light weight.

[0047] In the present invention, the resin outer member (C1) 4 To The contained discontinuous fibers are preferably glass fibers. By using glass fibers for the resin outer member (C1) 4, the resin outer member (C1) 4 can be endowed with the function of a radio wave transmitting member.

[0048] In addition, it is preferable to use a thermoplastic resin as the resin inner member (B1) 3 or the resin outer member (C1) 4. of This results in a joint structure in which the thermoplastic resin is melted and fixed, which makes it possible to achieve higher joint strength in the integrally molded body 1. The melt-fixed joint structure refers to a joint structure in which the components are melted by heat and fixed together by cooling.

[0049] In the present invention, the plate material (A) 2 preferably includes either a metal member or a carbon fiber reinforced resin member.

[0050] From the viewpoint of increasing the strength and rigidity of the integrally molded body 1, it is preferable to use a material having high strength and rigidity, as well as excellent lightness, as the plate material (A) 2. In terms of high strength and high rigidity, a metal member or Fiber Reinforced It is preferable to use a resin member. Furthermore, in order to increase the light weight, one or more core members selected from a resin sheet, a foam, and a material obtained by expanding discontinuous fiber-reinforced resin containing discontinuous fibers in the thickness direction are used as a core layer, and a metal member or Fiber Reinforced It is more preferable to use a sandwich structure in which the resin member is used as a skin layer and both sides of the core layer are sandwiched between the skin layers. Fiber Reinforced By using carbon fiber reinforced plastic components, which use carbon fiber as the reinforcing fiber in plastic components, it is possible to achieve high rigidity, light weight, and thin wall thickness.

[0051] On the other hand, examples of the metal member include an element selected from titanium, steel, stainless steel, aluminum, magnesium, iron, silver, gold, platinum, copper, and nickel, or an alloy containing these elements as a main component. If necessary, plating treatment can be performed.

[0052] Fiber Reinforced As the resin used for the resin member, carbon fiber reinforced resin member or core member, a thermoplastic resin or a thermosetting resin can be suitably used.

[0053] There is no particular limitation on the type of thermoplastic resin that constitutes the plate material (A) 2, the resin inner member (B1) 3, or the resin outer member (C1) 4, and any of the thermoplastic resins exemplified below can be used. For example, polyethylene terephthalate (PET) resin, polybutylene terephthalate (PBT) resin, polytrimethylene terephthalate (PTT) resin, polyethylene naphthalate (PENA) resin, etc. ) resin 、 Polyester resins such as liquid crystal polyester resins and polyethylene (PE )resin 、 Polypropylene (PP ) resin 、 Polyolefin resins such as polybutylene resin, polyarylene sulfide resins such as polyoxymethylene (POM) resin, polyamide (PA) resin, polyphenylene sulfide (PPS) resin, polyketone (PK) resin, polyether ketone (PEK) resin, polyether ether ketone (PEEK) resin, polyether ketone ketone (PEKK) resin, polyether nitrile (PEN) resin, fluororesins such as polytetrafluoroethylene resin, crystalline resins such as liquid crystal polymer (LCP), styrene resins, polycarbonate (PC) resin, polymethyl methacrylate (PMMA) resin, polyvinyl chloride (PVC) Examples of the thermoplastic resin include amorphous resins such as polyphenylene ether (PPE) resin, polyimide (PI) resin, polyamideimide (PAI) resin, polyetherimide (PEI) resin, polysulfone (PSU) resin, polyethersulfone resin, and polyarylate (PAR) resin, and other thermoplastic resins such as phenolic resin, phenoxy resin, polystyrene resin, polyolefin resin, polyurethane resin, polyester resin, polyamide resin, polybutadiene resin, polyisoprene resin, fluorine resin, and acrylonitrile resin, and copolymers and modified products thereof. Among them, polyolefin resin is preferred from the viewpoint of the light weight of the molded product obtained, polyamide resin is preferred from the viewpoint of strength, and amorphous resins such as polycarbonate resin, styrene resin, and modified polyphenylene ether resin are preferred from the viewpoint of surface appearance, polyarylene sulfide resin is preferred from the viewpoint of heat resistance, and polyether ether ketone resin is preferably used from the viewpoint of continuous use temperature.

[0054] As the thermosetting resin constituting the plate material (A) 2, it is preferable to use thermosetting resins such as unsaturated polyester resin, vinyl ester resin, epoxy resin, phenol (resole type) resin, urea-melamine resin, polyimide resin, maleimide resin, benzoxazine resin, etc. These may be applied as a resin blend of two or more kinds. Among them, epoxy resin is particularly preferable from the viewpoint of mechanical properties and heat resistance of the molded body. In order to express its excellent mechanical properties, epoxy resin is preferably contained as a main component of the resin used, specifically, it is preferable to contain 60% by weight or more of the resin composition.

[0055] Plate material (A) 2 or resin Inside From the viewpoint of weight reduction, polyacrylonitrile (PAN)-, pitch-, rayon-, and other carbon fibers having excellent specific strength and specific rigidity are preferably used as the carbon fibers constituting the member (B1) 3. Polyacrylonitrile (PAN)-based carbon fibers are more preferred.

[0056] Next, a method for producing an integrally molded body according to the present invention will be described with reference to the drawings.

[0057] The method for producing an integrally molded body according to the present invention includes the steps of: [1] A step of injecting a precursor of the resin outer member (C1) 4 from a plurality of resin injection gate openings (GC) 21 into a molding die to form the resin outer member (C1) 4 in advance; [2] A step of disposing a plate material (A) inside a resin outer member (C1) 4 at a position separated from at least a part of the resin outer member (C1); and [3] A process of injecting a precursor of a resin internal component (B1) 3 from a plurality of resin injection gate ports (GB) 22 into a gap between the plate material (A) 2 and the resin external component (C1) 4 to form a first joint 5 where at least a portion of the outer peripheral side portion and / or outer peripheral edge portion of the plate material (A) 2 is joined to the resin internal component (B1) 3, and a second joint 6 where at least a portion of the outer peripheral side portion and / or outer peripheral edge portion of the resin internal component (B1) 3 is joined to the resin external component (C1) 4; A method for producing an integrated molded body 1 having a rectangular planar structure, comprising the steps of: This is a manufacturing method in which the injection conditions of the precursor of the internal resin component (B1) 3 and the precursor of the external resin component (C1) 4 are adjusted so that, when viewed from the side opposite the design surface of the plate material (A) 2 (the non-design surface side), the position of a molten resin merging line (B2) 16 formed in the internal resin component (B1) 3 specified along a direction parallel to the outer periphery of the integrated molded body 1 and the position of a molten resin merging line (C2) 17 formed in the external resin component (C1) 4 and located closest to the molten resin merging line (B2) 16 are shifted at least in one location or more.

[0058] As shown in FIG. 8 or FIG. 9, process [1] is a process of forming a resin outer member (C1) 4 by injecting a precursor of the resin outer member (C1) 4 from a plurality of resin injection gate openings (GC) 21 into a lower molding die 30 and an upper molding die 31 having a space (cavity) for forming the resin outer member (C1) 4.

[0059] In the embodiment shown in FIG. 8, the resin injection gate port (GC) 21 is provided on the upper and lower sides of the resin outer member (C1) 4. 1 Two molten resin joining lines (C2) 17 are arranged on the upper and lower sides of the resin outer member (C1) 4, and one on the left and right sides. Each The position where the molten resin joining line (C2) 17 is formed is near the middle between the adjacent resin injection gate openings (GC) 21.

[0060] After that, the resin outer member (C1) 4 is cooled, and then, as shown in FIG. On molding Remove the mold 31. Note that while Fig. 8 shows the resin injection gate opening (GC) 21 injecting resin from the side, Fig. 9 shows the resin being injected from above, but this is merely shown to make it easier to understand the injection position, and the injection form can be set appropriately depending on the shape of the mold, etc. The same applies to the following explanation.

[0061] Next, in step [2], as shown in Fig. 11 or 12, a plate material (A) 2 is disposed inside the resin outer member (C1) 4 at a position separated from at least a part of the resin outer member (C1) 4. Here, the plate material (A) 2 is prepared in advance so that one surface thereof becomes a design surface.

[0062] Next, in step [3], as shown in FIG. 13 or 14, a precursor of the inner-resin component (B1) 3 is injected from multiple resin injection gate openings (GB) 22 into the gap between the plate material (A) 2 and the resin outer component (C1) 4 in a lower molding die 30 and an upper molding die 32 having a space (cavity) for forming the inner-resin component (B1) 3, thereby forming the inner-resin component (B1) 3 bonded to the plate material (A) 2 and the resin outer component (C1) 4.

[0063] Here, the resin injection gate port (GB) 22 for forming the resin inner member (B1) 3 is provided on the upper and lower sides of the resin inner member (B1) 3. 1 Each one on the left and right side 2 By arranging them one by one, the molten resin joining line (B2) 16 is formed on the upper and lower sides of the resin inner part (B1) 3. 2 Each one on the left and right side 1 They are formed one by one.

[0064] After that, the resin inner member (B1) 3 is cooled, On molding The mold 32 is removed, and the integrally molded body 1 can be obtained as shown in FIG.

[0065] In order to shift the position of the molten resin merging line (B2) 16 from the position of the molten resin merging line (C2) 17, it is important to adjust the injection conditions of the precursor of the inner resin member (B1) 3 or the precursor of the outer resin member (C1) 4. By adjusting the injection conditions in this way so that the position of the molten resin merging line (B2) 16 and the position of the molten resin merging line (C2) 17 are shifted from each other, it is possible to suppress a decrease in the strength of the molded body.

[0066] As a method of adjusting the injection conditions so that the position of the molten resin merging line (B2) 16 and the position of the molten resin merging line (C2) 17 are shifted in this way, it is preferable to set the position of one of the multiple resin injection gate openings (GB) 22 for injecting the precursor of the resin internal member (B1) 3 and the position of the resin injection gate opening (GC) 21 for injecting the precursor of the resin external member (C1) 4 provided at the position closest to the position of the resin injection gate opening (GB) 22 at positions shifted in a direction parallel to the outer periphery of the integrally molded body 1, as shown in Fig. 13. By using such a positional configuration, the molten resin merging lines formed in the resin internal member (B1) 3 and the resin external member (C1) 4 are shifted from each other, and the lack of strength of the weld line is complementarily compensated for by other resin members, thereby preventing a decrease in strength of the entire molded body.

[0067] Another method for adjusting the injection conditions is to adjust the position of the resin injection gate opening, as described above, when it is not possible to shift the position due to the configuration of the device.

[0068] Even in such a case, as a method for shifting the molten resin joining lines, it is preferable to provide a difference in injection pressure when injecting the resin member from one of the adjacent resin injection gate ports (GB) 22 for injecting and injecting the precursor of the resin internal member (B1) 3. This allows the position where the molten resin joining line is formed to join at a position shifted to either side from the center between the adjacent resin injection gate ports.

[0069] It is also preferable to adopt a method of providing a difference in injection pressure between adjacent resin injection gate ports (GB) 22, and also between adjacent resin injection gate ports (GC) 21 which inject and inject the precursor of the resin outer member (C1) 4. In this case, it is more preferable to adjust both injection pressures so that the molten resin joining line is shifted.

[0070] Figure 13 of Resin inner member (B1) 3, resin outer member (C1) 4, and molten resin joining line formed therebetween Sectional view including is shown in Figure 19. In order to make the molding device compact, the resin injection gate port (GB) 22 and the resin injection gate port (GC) 21 are arranged on the same line without any misalignment. When the resin internal component (B1) is injected from the adjacent resin injection gate ports 22a and 22b of the resin injection gate port (GB) 22, the injection pressure is made higher for the resin injection gate port 22b, so that the molten resin merging line 16 is formed closer to the resin injection gate port 22a.

[0071] Furthermore, when the resin outer member (C1) is injected from adjacent resin injection gate openings 21a and 21b of the resin injection gate opening (GC) 21 on the side of the resin outer member (C1) 4, the injection pressure is made higher at the resin injection gate opening 21a, so that the molten resin merging line 17 is formed closer to the resin injection gate opening 21b. As a result, the molten resin merging line 16 and the molten resin merging line 17 can be formed at positions separated from each other.

[0072] As another method, a difference in resin temperature during injection is provided between adjacent resin injection gate openings. thing This is also a preferred method.

[0073] As another preferred method, in a flow path through which the precursor of the resin internal component (B1) 3 flows, which connects adjacent resin injection gate openings for injecting the precursor of the resin internal component (B1) 3, at least one portion having a different cross-sectional area in a plane perpendicular to the direction in which the precursor of the resin internal component (B1) 3 flows is provided. EXAMPLES

[0074] The integrally molded body 1 of the present invention and a method for producing the same will be described in detail below with reference to examples, but the present invention is not limited to the following examples.

[0075] The measurement methods used in the examples are described below.

[0076] (1) Weld strength measurement of integrally molded products With the design side of the integrally molded body facing up, two cubic blocks made of SUS304, measuring 10 mm in length, 10 mm in width, and 10 mm in height, were placed on a 50 mm Keep your distance A molten resin merging line (B2) formed in the internal resin component (B1) was then placed on top of it so that it was in the center of the span, and a φ10 mm push-pull gauge was pressed against the molten resin merging line (B2) formed in the internal resin component (B1) to measure the value when the internal resin component (B1) was destroyed. Measurements were taken at a total of six points, four points on the long side and two points on the short side. Next, the molten resin merging line (C2) formed in the external resin component (C1) was placed so that it was in the center of the span, and a φ10 mm push-pull gauge was pressed against the molten resin merging line (C2) formed in the external resin component (C1) to measure the value when the external resin component (C2) was destroyed. Measurements were taken at four points on the long side and two points on the short side. 4 A total of eight points were measured. Furthermore, the weld strength values ​​obtained were evaluated according to the following criteria, with A being pass and B being fail. A: The weld strength at each measurement point is 98N (10 kg·f) or more. B: The weld strength at any one measurement point is below 98 N (10 kg·f).

[0077] (Material composition example 1) Preparation of PAN-based carbon fiber bundles Manufacturing A polymer mainly composed of polyacrylonitrile was spun and sintered to obtain a continuous carbon fiber bundle with a total of 12,000 filaments. A sizing agent was applied to this continuous carbon fiber bundle by the immersion method, and the bundle was dried in heated air to obtain a PAN-based carbon fiber bundle. The properties of this PAN-based carbon fiber bundle were as follows: Single fiber diameter: 7μm Mass per unit length: 0.83g / m Density: 1.8g / cm 3 Tensile strength: 4.0GPa Tensile modulus: 235GPa

[0078] (Material composition example 2) Preparation of epoxy resin film Manufacturing An epoxy resin (base resin: dicyandiamide / dichlorophenylmethylurea curing type epoxy resin) was applied onto release paper using a knife coater to obtain an epoxy resin film.

[0079] (Material composition example 3) Preparation of unidirectional prepreg Manufacturing The PAN-based carbon fiber bundles obtained in Material Composition Example 1 were arranged in one direction in the form of a sheet, and two sheets of the epoxy resin film produced in Material Composition Example 2 were placed on both sides of the carbon fiber. The resin was then impregnated by heating and pressurizing to produce a unidirectional prepreg with a carbon fiber weight content of 70% and a thickness of 0.15 mm.

[0080] (Material composition example 4) Preparation of thermoplastic adhesive film (D) Manufacturing Polyester resin (Hytrel® 4057, manufactured by DuPont-Toray Co., Ltd.) was fed from the hopper of a twin-screw extruder, melt-kneaded in the extruder, and then extruded from a T-die. The resin was then taken up on a chill roll at 60°C to cool and solidify, yielding a polyester resin film with a thickness of 0.05 mm. This was used as thermoplastic adhesive film (D).

[0081] (Material composition example 5) Glass fiber reinforced polycarbonate resin Glass fiber reinforced polycarbonate resin GSH2030KR (manufactured by Mitsubishi Engineering Plastics Corporation, polycarbonate resin matrix, fiber weight content 30 wt%) was used.

[0082] (Material composition example 6) Long carbon fiber reinforced nylon resin Long carbon fiber pellets TLP-1146S (manufactured by Toray Industries, Inc., nylon 6 resin matrix, fiber weight content 20 wt%) and nylon 6 resin CM1007 (manufactured by Toray Industries, Inc., nylon 6 resin matrix, non-reinforced) were dry blended to obtain a long carbon fiber reinforced nylon resin with a fiber weight content of 15 wt%.

[0083] Example 1 The unidirectional prepreg obtained in Material Composition Example 3 and the thermoplastic adhesive film (D) obtained in Material Composition Example 4 were adjusted to a size of 400 mm square, and then laminated in the order of [unidirectional prepreg 0° / unidirectional prepreg 90° / unidirectional prepreg 0° / unidirectional prepreg 90° / unidirectional prepreg 90° / unidirectional prepreg 0° / unidirectional prepreg 90° / unidirectional prepreg 0° / adhesive film]. This laminate was sandwiched between release films and further sandwiched between tool plates. Here, a spacer with a thickness of 1.25 mm was inserted between the tool plates to adjust the thickness. After placing the tool plate on a plate surface with a plate surface temperature of 150°C, the plate surface was closed and hot pressed at 3 MPa. After 5 minutes had passed since the pressurization, the plate surface was opened to obtain a thermosetting CFRP plate with a thermoplastic adhesive film (D) in a flat plate shape with a thickness of 1.25 mm. This was used as plate material (A) 2 with a thermoplastic adhesive film (D) attached.

[0084] Next, the glass fiber reinforced polycarbonate resin of Material Composition Example 5 was injection molded in the mold shown in Fig. 8 at 150 MPa, a cylinder temperature of 320°C, a mold temperature of 120°C, and a resin discharge port diameter of φ3 mm to obtain a frame member having a rectangular frame shape with a width of 2.0 mm and a thickness of 3.0 mm as shown in Fig. 2. This was designated as the resin outer member (C1).

[0085] Next, Figure 17 As shown in FIG. 1, the design side of a CFRP plate (plate material (A) 2) with a thermoplastic adhesive film processed to a size of 300 mm x 200 mm is placed on the inside of a resin outer member (C1) while being separated from the resin outer member (C1). molding Lower mold 30 The plates were placed side by side and aligned. molding Upper mold 32 After setting, the glass fiber reinforced polycarbonate resin was injection molded in the mold shown in Fig. 13 at 150 MPa, cylinder temperature 320 ° C, mold temperature 120 ° C, and resin outlet diameter φ3 mm, and after the mold was closed, the GF reinforced polycarbonate resin (resin inner member (B1)) of Material Composition Example 5 was injection molded to produce an integrally molded body 1 composed of a top plate (plate material (A) 2) shown in the schematic diagram of Fig. 3. The properties of the integrally molded body of Example 1 are summarized (Table 1).

[0086] Example 2 An integrally molded body was produced in the same manner as in Example 1, except that the position of the resin injection gate opening (GC) of the outer resin member (C1) was changed to the position shown in Figure 14. The properties of the integrally molded body 1 are summarized in Table 1.

[0087] Example 3 Resin injection gate port (GC) of resin outer component (C1) of An integrally molded body was produced in the same manner as in Example 1, except that the position was changed to that shown in Figure 15. The properties of the integrally molded body 1 are shown in Table 1.

[0088] Example 4 Except for changing the material of the outer resin member (C1) and the material of the inner resin member (B1), an integrally molded body was produced in the same manner as in Example 1. The properties of the integrally molded body 1 are summarized in Table 1.

[0089] Example 5 Except for changing the material of the outer resin member (C1) and the material of the inner resin member (B1), an integrally molded body was produced in the same manner as in Example 3. The properties of the integrally molded body 1 are summarized in Table 1.

[0090] Comparative Example 1 An integrally molded body 1 was produced in the same manner as in Example 1, except that the position of the resin injection gate opening (GC) of the outer resin member (C1) was changed to the position shown in Figure 16. The properties of the integrally molded body 1 are summarized in Table 1.

[0091] [Table 1] [Industrial Applicability]

[0092] The integrally molded article of the present invention can be effectively used for automobile interiors and exteriors, electrical and electronic equipment housings, bicycles, structural materials for sporting goods, aircraft interior materials, transport boxes, and the like. [Explanation of symbols]

[0093] 1 Integrated molded body 2 Plate material (A) 3 Resin internal material (B1) 4 Resin outer material (C1) 5 First Joint 6 Second Joint 7 Area where plate material (A), inner resin material (B1) and outer resin material (C1) are exposed 10. Mold cavity surface 11 Molten resin parts 12 Direction of travel of resin material in molding die 13 Resin parts near the surface 14 Internal molten resin material 15 Resin collision area 16 Molten resin merging line (B2) 17 Molten resin merging line (C2) 18 Outer perimeter length M1 of integrally molded body 19 Distance M2 between the molten resin confluence line (B2) and the nearest molten resin confluence line (C2) 21 Resin injection gate port (GC) 22 Resin injection gate port (GB) 23 Distance L2 between the resin injection gate port (GB) and the nearest resin injection gate port (GC) 24 Narrow section of resin inner part (B1) 25 Narrow section of the resin outer part (C1) 30 Lower mold 31 Upper mold 32 Upper mold

Claims

1. A resin inner member (B1) containing a thermoplastic resin is interposed between a plate material (A) having a design surface on one side thereof and a resin outer member (C1) containing a thermoplastic resin, An integrally molded body which is a rectangular planar structure having a first joint portion where at least a partial area of ​​an outer peripheral side portion and / or an outer peripheral edge portion of the plate material (A) is joined to the resin internal member (B1), and a second joint portion where at least a partial area of ​​an outer peripheral side portion and / or an outer peripheral edge portion of the resin internal member (B1) is joined to the resin external member (C1), On the opposite side (non-design side) of the design surface of the plate material (A), one or more molten resin merging lines are formed in each of the resin inner member (B1) and the resin outer member (C1), and the position of one of the molten resin merging lines (B2) formed in the resin inner member (B1) specified along a direction parallel to the outer periphery of the integrally molded body and the position of the molten resin merging line (C2) formed in the resin outer member (C1) that is closest to the position of the molten resin merging line (B2) are in a position that is shifted from each other, and the ratio M2 / M1 of the distance M2 (mm) between the molten resin merging line (B2) and the molten resin merging line (C2) closest to the molten resin merging line (B2) to the outer periphery length M1 (mm) of the integrally molded body is 0.04 to 0.

4.

2. 2. The integrally molded body according to claim 1, wherein the molten resin joining line (B2) is formed in a narrow portion (B1') provided in a part of the internal resin member (B1).

3. 3. The integrally molded body according to claim 1, wherein the molten resin joining line (C2) is formed in a narrow portion (C1') provided in a part of the outer resin member (C1).

4. The integrally molded body according to any one of claims 1 to 3, wherein the first joint portion is formed around the entire outer periphery of the side surface portion and / or the outer periphery of the plate material (A).

5. The integrally molded body according to any one of claims 1 to 4, wherein the second joint portion is formed over the entire circumference of the outer circumferential side portion and / or the outer circumferential edge portion of the inner resin member (B1).

6. The resin inner member (B1) or the resin outer member (C1) contains reinforcing fibers, the reinforcing fibers are discontinuous fibers, and the weight average fiber length of the discontinuous fibers is 0.3 to 3 mm. An integrally molded body according to any one of claims 1 to 5.

7. A first step of injecting a precursor of a resin outer member (C1) from a plurality of resin injection gate ports (GC) into a molding die to form the resin outer member (C1) in advance; A second step of disposing a plate material (A) inside the resin outer member (C1) at a position spaced apart from at least a portion of the resin outer member (C1); and a third step of injecting a precursor of a resin internal member (B1) from a plurality of resin injection gate ports (GB) into a gap between the plate material (A) and the resin external member (C1) to form a first joint portion that joins at least a portion of an outer peripheral side portion and / or an outer peripheral edge portion of the plate material (A) to the resin internal member (B1) and a second joint portion that joins at least a portion of an outer peripheral side portion and / or an outer peripheral edge portion of the resin internal member (B1) to the resin external member (C1); A method for producing an integrated molded body having a rectangular planar structure, comprising the steps of: A method for manufacturing an integrally molded body, characterized in that, when viewed from the opposite side to the design surface (non-design surface side) of the plate material (A), the position of a molten resin merging line (B2) formed in the internal resin material (B1) specified along a direction parallel to the outer periphery of the integrally molded body and the position of a molten resin merging line (C2) formed in the external resin material (C1) and located closest to the molten resin merging line (B2) are shifted in at least one location or more by adjusting the injection conditions of the precursor of the internal resin material (B1) and the precursor of the external resin material (C1).

8. The method for manufacturing an integrally molded body described in claim 7, wherein the injection conditions are such that the position of one of the multiple resin injection gate openings (GB) for injecting the precursor of the resin inner member (B1) and the position of the resin injection gate opening (GC) for injecting the precursor of the resin outer member (C1) provided at the position closest to the position of the resin injection gate opening (GB) are set at positions shifted from a direction parallel to the outer periphery of the integrally molded body.

Citation Information

Patent Citations

  • Injection molding method and device

    JP1994210669A

  • Resin forming mold and weld line reinforcing method

    JP1994285911A

  • Injection molding method