Polyamide resin composition for injection molding and sliding part made of the same
The polyamide resin composition with crystalline polyamide and liquid crystal polyester fibers addresses moldability and abrasion issues, providing enhanced sliding stability and wear resistance for complex and lightweight parts.
Patent Information
- Application Number
- JP2021520746
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-05-20
- Filing Date
- 2020-05-14
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-05-14
Smart Images

Figure 0007567784000001 
Figure 0007567784000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyamide resin composition for injection molding, and more particularly to a polyamide resin composition for injection molding suitable for sliding parts. [Background technology]
[0002] Polyamide resin is a molding material with excellent sliding properties due to its crystallinity, but in order to obtain even better sliding properties, it is known to compound it with solid lubricants such as molybdenum disulfide, graphite, and fluororesin, various lubricating oils, and liquid lubricants such as silicone oil.
[0003] Of these sliding improvers, solid lubricants have the disadvantage that they require the blending of large amounts of solid lubricants, which significantly reduces the toughness of the base polyamide resin. Liquid lubricants can impart highly effective sliding properties with relatively small amounts of the solid lubricants, but in many cases they are poorly compatible with the base resin, and the surface of the molded article is often contaminated by these liquid lubricants, which limits their uses.
[0004] As methods for improving the drawbacks of blending various lubricants, a method of blending carbon fiber or aramid fiber (Patent Document 1) and a method of blending modified polyethylene (Patent Document 2) have been proposed. Such polyamide resin compositions have made it possible to provide molded products with excellent sliding properties without the above-mentioned drawbacks. However, in recent years, due to trends such as weight reduction and more complex shapes of molded products, higher levels of properties such as improved sliding properties are being required. In addition, due to the complexity of products, the abrasion properties of not only metals but also resin compositions themselves are becoming important. Therefore, the methods proposed so far have not necessarily been able to provide satisfactory properties. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. WO2017 / 110323 [Patent Document 2] International Publication No. WO2008 / 075699 Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention provides a polyamide resin composition for injection molding which is suitable for use in sliding parts which are required to have excellent moldability and heat stability as well as excellent abrasion resistance and sliding stability. [Means for solving the problem]
[0007] As a result of extensive investigations aimed at achieving the above object, the present inventors have found that organic fibers having a liquid crystal skeleton, particularly polyester fibers, affect the sliding properties, and have arrived at the present invention.
[0008] That is, the present invention has the following configuration. [1] A polyamide-based resin composition for injection molding, comprising: a crystalline polyamide resin (A); and polyester fibers (B) having a liquid crystal skeleton. [2] The polyamide resin composition for injection molding according to [1], wherein the crystalline polyamide resin (A) has a melting point of 170°C or higher. [3] The polyamide-based resin composition for injection molding according to [1] or [2], characterized in that it contains 0.1 to 40 mass % of polyester fibers (B) having a liquid crystal skeleton based on the total mass of the polyamide-based resin composition. [4] A sliding part comprising the polyamide resin composition according to any one of [1] to [3]. Effect of the Invention
[0009] The polyamide resin composition of the present invention not only has excellent moldability and heat resistance stability, but also has improved abrasion resistance and further improved sliding properties such as a reduced dynamic friction coefficient. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be specifically described below. The crystalline polyamide resin (A) in the present invention is not particularly limited as long as it is a polymer having an amide bond (-NHCO-) in the main chain and is crystalline. Examples of the crystalline polyamide resin (A) include polyamide 6 (PA6), polyamide 66 (PA66), polyamide 46 (PA46), polyamide 11 (PA11), polyamide 12 (PA12), polyamide 610 (PA610), polyamide 612 (PA612), polymetaxylylene adipamide (PAMXD6), hexamethylenediamine-terephthalic acid polymer (PA6T), hexamethylenediamine-terephthalic acid and adipic acid copolymer (PA6T / 66), hexamethylenediamine-terephthalic acid and adipic acid copolymer (PA6T / 66), and the like. Examples of the polyamide resin include, but are not limited to, crystalline polyamide resins such as trimethylhexamethylenediamine-terephthalic acid and ε-caprolactam copolymer (PA6T / 6), trimethylhexamethylenediamine-terephthalic acid polymer (PATMD-T), metaxylylenediamine, adipic acid and isophthalic acid copolymer (PAMXD-6 / I), trihexamethylenediamine, terephthalic acid and ε-caprolactam copolymer (PATMD-T / 6), diaminodicyclohexylenemethane (CA), isophthalic acid and lauryllactam copolymer, and blends thereof.
[0011] The crystalline polyamide resin (A) is preferably a polyamide having a melting point of 170°C or higher. In the case of crystalline polyamides having a melting point lower than the above, the glass transition temperature is often 40°C or lower, and there is a concern that the surface may soften due to heat generated during sliding. The melting point of the crystalline polyamide resin (A) is more preferably 200°C or higher, and even more preferably 220°C or higher. The upper limit of the melting point of the crystalline polyamide resin (A) is preferably 350°C or lower from the viewpoint of suppressing decomposition of the polyester fiber having a liquid crystal skeleton. In the present invention, polyamide 6 and polyamide 66 are particularly preferred as the crystalline polyamide resin (A).
[0012] The relative viscosity of the crystalline polyamide resin (A) in the present invention is not particularly limited, but can be in the range of 2.0 to 5.0 as measured in a 96% sulfuric acid solution (polyamide resin concentration 1 g / dl, temperature 25° C.) The relative viscosity of the crystalline polyamide resin (A) is preferably 2.0 to 3.5, more preferably 2.1 to 3.4. The amount (content) of the crystalline polyamide resin (A) is preferably 35 mass% or more, more preferably 60 to 99.9 mass%, still more preferably 70 to 99 mass%, and particularly preferably 75 to 98 mass%, based on the total mass of the polyamide resin composition.
[0013] The organic fiber (B) in the present invention is preferably a polyester fiber (B) having a liquid crystal skeleton (hereinafter, also referred to as liquid crystal polyester fiber (B)). Examples of polyesters constituting the liquid crystal polyester fiber (B) include, but are not limited to, a polycondensate of ethylene terephthalate and parahydroxybenzoic acid, a polycondensate of dihydric phenol, phthalic acid and parahydroxybenzoic acid, and a polycondensate of 2,6-hydroxynaphthoic acid and parahydroxybenzoic acid, and the like, and may be any synthetic resin that exhibits liquid crystal properties in which linear chains of molecules are regularly arranged and is defined as a thermoplastic resin.
[0014] Other examples of polyesters constituting the liquid crystal polyester fiber (B) include those made of aromatic dicarboxylic acids, aromatic diols and / or aromatic hydroxycarboxylic acids or their derivatives, and in some cases, copolymers of these with alicyclic dicarboxylic acids, alicyclic diols, aliphatic diols or their derivatives. Examples of aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, 4,4'-dicarboxydiphenyl, 2,6-dicarboxynaphthalene, 1,2-bis(4-carboxyphenoxy)ethane, etc., and their nucleus-substituted products with alkyl, aryl, alkoxy, and halogen groups. Examples of aromatic diols include hydroquinone, resorcin, 4,4'-dihydroxydiphenyl, 4,4'-dihydroxybenzophenone, 4,4'-dihydroxydiphenylmethane, 4,4'-dihydroxydiphenylethane, 2,2-bis(4-hydroxyphenyl)propane, 4,4'-dihydroxydiphenylether, 4,4'-dihydroxydiphenylsulfone, 4,4'-dihydroxydiphenylsulfide, 2,6-dihydroxynaphthalene, 1,5-dihydroxynaphthalene, etc., and their nucleus-substituted alkyl, aryl, alkoxy, and halogen groups. Examples of aromatic hydroxycarboxylic acids include p-hydroxybenzoic acid, m-hydroxybenzoic acid, 2-hydroxynaphthalene-6-carboxylic acid, 1-hydroxynaphthalene-5-carboxylic acid, etc., and their nucleus-substituted alkyl, aryl, alkoxy, and halogen groups. Examples of alicyclic dicarboxylic acids include trans-1,4-dicarboxycyclohexane, cis-1,4-dicarboxycyclohexane, etc., and their alkyl, aryl, and halogen nucleus-substituted derivatives. Examples of alicyclic and aliphatic diols include trans-1,4-dihydroxycyclohexane, cis-1,4-dihydroxycyclohexane, ethylene glycol, 1,4-butanediol, and xylylenediol.
[0015] The liquid crystal polyester fiber (B) may contain other polymers or additives, and may be coated with a sizing agent, within the range not impairing the object of the present invention.
[0016] The fiber length and fiber diameter of the liquid crystal polyester fiber (B) are not particularly limited, but the fiber diameter is preferably 0.1 to 50 μm and the fiber length is preferably 0.05 to 10 mm. The fiber diameter is more preferably 1 to 30 μm, further preferably 8 to 25 μm, and particularly preferably 10 to 22 μm. The fiber length is more preferably 0.3 to 5 mm, and chopped strand type fibers are preferably used.
[0017] As the liquid crystal polyester fiber (B), "Zxion (registered trademark)" manufactured by KB Seiren Co., Ltd. and "Vectran (registered trademark)" manufactured by Kuraray Co., Ltd. can be used.
[0018] The blending amount (content) of the liquid crystal polyester fiber (B) is preferably 0.1 to 40 mass% based on the total mass of the polyamide resin composition, more preferably 1 to 30 mass%, and further preferably 2 to 25 mass%. If it is less than 0.1 mass%, the effect of improving the sliding properties is insufficient, while if it exceeds 40 mass%, the effect reaches saturation, which is undesirable, and the liquid crystal polyester fiber may float in the appearance of the molded product.
[0019] In the present invention, the reason why the sliding properties are improved by using the liquid crystal polyester fiber (B), especially the sliding properties through dust, are improved is thought to be that the good friction properties of the liquid crystal polyester fiber impart lubricity to the surface properties of the polyamide resin composition. In addition, when the polyamide resin composition is damaged, the liquid crystal polyester fiber present in the composition is detached and precipitates on the surface. It is also suggested that the fiber is sheared and torn in the fiber direction to be abraded and powdered, and an intermediate layer having lubricity is formed between the abraded body and the abraded body, thereby preventing direct contact with dust. Abrasion through dust is caused by contact with gravel or other inorganic matter, so severe damage occurs on the outermost surface. Therefore, it is not sufficient to simply impart lubricity or improve the elastic modulus of the resin composition surface. Therefore, the formation of an intermediate protective layer having lubricity is extremely effective in suppressing dust abrasion. Although aramid fibers are an example of organic fibers having a liquid crystal skeleton, unlike liquid crystal polyester fibers, they do not shear and split in the fiber direction, but rather shear at the intermolecular wall interface, so the same mechanism does not occur, and dust abrasion progresses without forming an intermediate layer. In carbon fibers, the fibers that precipitate at the same time as damage act as intermediates that can wear away the resin composition, which may promote abrasion and is not suitable. In addition, if the opposing abrasive is a resin, it may also wear away the opposing abrasive.
[0020] In the present invention, strength and rigidity can be significantly improved by further adding a filler, such as glass fiber, carbon fiber, metal fiber, aramid fiber, asbestos, potassium titanate whisker, wollastonite, glass flakes, glass beads, talc, mica, clay, calcium carbonate, barium sulfate, titanium oxide, and aluminum oxide. These are blended when strength and rigidity are prioritized, and the blending amount (content) is preferably 5 to 60 mass % and particularly preferably 5 to 40 mass % based on the total mass of the polyamide resin composition. When sliding properties are prioritized, the blending amount (content) is preferably 5 mass % or less based on the total mass of the polyamide resin composition.
[0021] In the present invention, toughness can be significantly improved by further adding a polyolefin resin or a thermoplastic elastomer. Examples of polyolefin resins include olefin-based resins such as high-density polyethylene, low-density polyethylene, ultra-high molecular weight polyethylene, linear low-density polyethylene, polypropylene, poly(1-butene), and poly(4-methylpentene). Examples of thermoplastic elastomers include styrene-based thermoplastic elastomers, olefin-based thermoplastic elastomers, polyamide-based thermoplastic elastomers, polyester-based thermoplastic elastomers, and polyurethane-based thermoplastic elastomers. When these are blended, the blending amount (content) is preferably from 0.5 to 10 mass %, more preferably from 1 to 8 mass %, based on the total mass of the polyamide resin composition.
[0022] In the polyamide resin composition of the present invention, in addition to (A), (B), the above-mentioned filler, polyolefin resin, and thermoplastic elastomer, weather resistance improvers such as carbon black, copper oxide and / or alkali metal halide, light or heat stabilizer, release agent, crystal nucleating agent, lubricant, antistatic agent, pigment, dye, coupling agent, etc., which are used in ordinary polyamide resin compositions, may be blended without any problem, so long as the blending properties and moldability are not impaired. When these are blended, the total blending amount (content) is preferably 0.1 to 5 mass %, more preferably 0.2 to 3 mass %, based on the total mass of the polyamide resin composition.
[0023] The method for producing the polyamide resin composition of the present invention is not particularly limited, and a general single-screw extruder, twin-screw extruder, pressure kneader, etc. can be used as a kneading device, but in the present invention, a twin-screw extruder is particularly preferred. In one embodiment, the (A) and (B) and, depending on the application, a pigment or the like are mixed and fed into a twin-screw extruder. By uniformly kneading the mixture with the twin-screw extruder, a polyamide-based resin composition with excellent sliding properties can be produced. The kneading temperature of the twin-screw extruder is preferably 220 to 300°C, and the kneading time is preferably about 2 to 15 minutes.
[0024] The polyamide resin composition of the present invention is suitable for injection molding, and can be widely used in a variety of applications requiring sliding properties, such as electric and electronic parts, automobile parts, building materials, industrial parts, etc. Specific applications include bearings, gears, door checkers, chain guides, and retainer plate parts. EXAMPLES
[0025] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way. The raw materials used in the examples and comparative examples of the present invention are as follows.
[0026] Crystalline polyamide resin (A) A1: Polyamide 66 (RV=2.8), Vydyne 21FSR (manufactured by Ascend), melting point 265°C A2: Polyamide 6 (RV=2.6), ZISAMIDE TP4208 (manufactured by Shuseisha), melting point 225°C A3: Polyamide 12 (RV=2.4), Rilsamid (Arkema), melting point 175°C
[0027] Liquid crystal polyester fiber (B) B1: Zxion-VS chopped fiber, fiber diameter 14 μm, fiber length 3 mm (KB Seiren) B2: Zxion-TS chopped fiber, fiber diameter 20 μm, fiber length 3 mm (KB Seiren) B3: Zxion-VS chopped milled fiber, fiber diameter 14 μm, fiber length 0.3 mm (KB Seiren)
[0028] Inorganic Fiber (C) C1: Glass fiber, chopped fiber, T-275H, fiber diameter 11 μm, fiber length 3 mm (manufactured by Nippon Electric Glass Co., Ltd.) C2: Carbon fiber CFUW, chopped fiber, fiber diameter 10 μm, fiber length 3 mm (manufactured by Japan Polymer Industries Co., Ltd.)
[0029] Other organic fibers (D) D: Para-aramid fiber, chopped strand, Technora T322UR 3-12, fiber diameter 12 μm, fiber length 3 mm (Teijin Limited)
[0030] [Examples 1 to 11, Comparative Examples 1 to 7] The evaluation samples were produced by weighing out the raw materials in the blending ratios of the polyamide resin compositions shown in Tables 1 and 2, mixing them in a tumbler, and then feeding them into a twin-screw extruder. The temperature of the twin-screw extruder was set to 250°C to 300°C, and the kneading time was 5 to 10 minutes. The pellets obtained were molded into various evaluation samples using an injection molding machine. The cylinder temperature of the injection molding machine was set to 250°C to 290°C, and the mold temperature was set to 80°C.
[0031] The various evaluation methods are as follows. The evaluation results are shown in Tables 1 and 2. 1. Relative Viscosity (RV) of Polyamide Resin (96% Sulfuric Acid Solution Method) The viscosity was measured using an Ubbelohde viscosity tube at 25° C. in a 96% by weight sulfuric acid solution with a polyamide resin concentration of 1 g / dL.
[0032] 2. Melting point of polyamide resin The measurement was performed using a differential scanning calorimeter EXSTAR 6000 manufactured by Seiko Instruments Inc. at a temperature increase rate of 20° C. / min to determine the endothermic peak temperature.
[0033] 3. Wear characteristics Using a thrust type abrasion tester, a flat plate (size: 50 mm x 50 mm) of a polyamide resin composition obtained by injection molding was brought into contact with a circular SUS jig having a protrusion of 8 mm in length and 1.3 mm in width, and subjected to a load of 48.9 kgf / cm for 20 minutes. 2 The plates were then subjected to continuous sliding at a speed of 15 cm / sec. The amount of wear per unit distance (mg / km) was calculated from the difference in mass between the plate and the cylindrical molded product before and after abrasion and the total abrasion distance, and the dynamic friction coefficient was calculated from the converged load value during the abrasion test.
[0034] 4.Abrasion characteristics caused by dust Using a thrust type abrasion tester, 1 mg of grease containing molybdenum disulfide is uniformly spread on a flat plate (size: 50 mm x 50 mm) of a polyamide resin composition, and then 2 mg of dust made by mixing silica sand and volcanic ash in a mass ratio of 1:1 is spread on the plate to introduce inorganic substances with different particle sizes and hardness. A cylindrical molded product made of polyoxymethylene (POM) is brought into contact with the surface and subjected to a load of 30 kgf / cm for 30 minutes. 2 The plates were then subjected to continuous sliding at a speed of 40 mm / sec. The amount of wear per unit distance (mg / km) was calculated from the difference in mass between the plate and the cylindrical molded product before and after wear, and the total wear distance, and the dynamic friction coefficient was calculated from the converged load value during the wear test.
[0035] 5.Moldability Molding was carried out under the above molding temperature conditions using a mold equipped with a mold release force measuring device, and the mold release force was measured from the 31st shot to the 35th shot to determine the mold release resistance value.
[0036] 6.Heat resistance stability The specimens were heat treated in a recirculating air oven (Nagano Scientific Machinery Works NH-401S hot air circulation dryer) according to the procedure detailed in ISO 2578. At the designated test time (250 hours) in a 120°C environment, the specimens were removed from the oven, cooled to room temperature, and sealed in an aluminum-lined bag until ready for testing. Tensile strength was then measured according to ISO 527-1,2, and the retention rate before and after treatment was calculated from the average value obtained from three specimens.
[0037] [Table 1]
[0038] [Table 2]
[0039] In the abrasion test using a SUS circular jig and the abrasion test using dust, Examples 1 to 11 have physical properties equal to or better than those of Comparative Examples 1 to 7, and have realized good abrasion characteristics. This effect is particularly remarkable in the abrasion test using dust. In addition, the mold release resistance is 1.0 MPa or less, which satisfies the moldability requirements for continuous injection molding, and the heat resistance stability is also at a satisfactory level. Comparative Example 1 is polyamide 66 that has not been modified, and the amount of wear is large. Comparative Examples 2 and 3 contribute to wear resistance in the wear test in which a SUS circular jig is contacted, but the effect is not as great as that of Examples 1 to 11. In addition, the amount of wear after the wear test through dust is not reduced, resulting in increased wear of the cylindrical molded product made of POM, which is the mating material. The tendency to increase the wear of the cylindrical molded product made of POM, which is the mating material, in the wear test through dust is also seen in Comparative Examples 4 and 5, so it can be seen that inorganic fiber reinforcement materials are not suitable when the mating material in contact is a polymer. Comparative Examples 6 and 7 certainly contribute to wear resistance as in Patent Document 1, but their contribution is low compared to the composition of the present invention.
[0040] As the main modification mechanism of Examples 1 to 11, it is suggested that when the composition is damaged, the polyester fiber having a liquid crystal skeleton present in the composition is sheared and broken in the fiber direction, and is abraded into powder, forming an intermediate layer having lubricity between the abrasive and the abraded body, thereby preventing direct contact.It is also suggested that the effect of reducing the dynamic friction coefficient due to the contribution of the low friction of the liquid crystal polyester fiber itself is expressed on the surface. [Industrial Applicability]
[0041] The polyamide resin composition of the present invention is a molding material having excellent sliding properties. It is particularly suitable for sliding parts that are subjected to high contact pressure and require high abrasion resistance, and is expected to make a great contribution to the industrial world as an engineering plastic that can be used in a wide range of fields.
Claims
1. A sliding part made of a polyamide-based resin composition, The polyamide-based resin composition is a polyamide-based resin composition for injection molding, which contains a crystalline polyamide resin (A) and a polyester fiber (B) having a liquid crystal skeleton, The crystalline polyamide resin (A) is polyamide 6 (PA6), polyamide 66 (PA66), polyamide 46 (PA46), polyamide 11 (PA11), polyamide 12 (PA12), polyamide 610 (PA610), or polyamide 612 (PA612), The polyester constituting the polyester fiber (B) having a liquid crystal skeleton is a polycondensate of ethylene terephthalate and parahydroxybenzoic acid, a polycondensate of a dihydric phenol, phthalic acid and parahydroxybenzoic acid, or a polycondensate of 2,6-hydroxynaphthoic acid and parahydroxybenzoic acid, The polyester fiber (B) having a liquid crystal skeleton is contained in an amount of 2 to 25 mass% based on the total mass of the polyamide-based resin composition, The polyester fiber (B) having a liquid crystal skeleton is present as a fiber in a polyamide resin composition.
2. 2. The sliding part according to claim 1, wherein the melting point of the crystalline polyamide resin (A) is 170° C. or higher.
3. 3. The sliding part according to claim 1, wherein the blending amount (content) of the crystalline polyamide resin (A) is 35 mass % or more based on the total mass of the polyamide resin composition.
4. A sliding part according to any one of claims 1 to 3, characterized in that the liquid crystal polyester fiber (B) has a fiber diameter in the range of 0.1 to 50 μm and a fiber length in the range of 0.05 to 10 mm.
Citation Information
Patent Citations
Thermoplastic resin composition
JP1995041665A
Speaker cabinet and its manufacture
JP1997084168A
Polyamide resin composition and molded product
JP2000034404A
Flame-retardant resin composition and molded item thereof
JP2000109687A
Flame-retardant resin composition and its molding product
JP2000154314A