Acrylic rubber veil with excellent storage stability and water resistance
The production of acrylic rubber veils through controlled emulsion polymerization and extrusion processes addresses storage stability and water resistance issues, achieving high stability and resistance through low ash content and specific gravity, enhancing workability and water resistance.
Patent Information
- Application Number
- JP2021534589
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-19
- Filing Date
- 2020-06-05
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-06-05
AI Technical Summary
Existing methods for producing acrylic rubber veils face issues with storage stability and water resistance, particularly due to high ash content, air entrainment, and inadequate removal of emulsifiers and coagulants, leading to poor workability and insufficient water resistance under harsh conditions.
The production method involves emulsion polymerization of a monomer component containing (meth)acrylic acid ester and reactive group-containing monomers, followed by controlled dehydration and drying using a screw-type extruder, and lamination of sheet-like dry rubber to form a veil, with specific control over ash content, specific gravity, and molecular weight distribution to enhance stability and resistance.
The method produces an acrylic rubber veil with excellent storage stability and water resistance, characterized by low ash content, high specific gravity, and controlled molecular weight distribution, resulting in improved workability and enhanced water resistance.
Smart Images

Figure 0007567793000003 
Figure 0007567793000004 
Figure 0007567793000005
Abstract
Description
[Technical field]
[0001] The present invention relates to an acrylic rubber veil and a method for producing the same, a rubber mixture and a method for producing the same, and a cross-linked rubber product, and more specifically to an acrylic rubber veil having excellent storage stability and water resistance and a method for producing the same, a rubber mixture containing the acrylic rubber veil and a method for producing the same, and a cross-linked rubber product obtained by cross-linking it. [Background technology]
[0002] Acrylic rubber is a polymer mainly composed of acrylic ester, and is generally known as a rubber with excellent heat resistance, oil resistance, and ozone resistance, and is widely used in the field of automobiles, etc. Such acrylic rubber is usually produced by emulsion polymerization of the monomer components constituting the acrylic rubber, contacting the obtained emulsion polymerization liquid with a coagulant, drying the obtained water-containing crumbs, and then baling them to produce a product.
[0003] Regarding acrylic rubber, for example, Patent Document 1 (JP 2006-328239 A) discloses a method for producing a rubber polymer, which comprises a step of obtaining a crumb slurry containing a crumb-like rubber polymer by contacting a polymer latex with a coagulation liquid, a step of crushing the crumb-like rubber polymer contained in the crumb slurry with a mixer equipped with a stirring and crushing function having a stirring power of 1 kW / m3 or more, a dehydration step of removing water from the crumb slurry in which the crumb-like rubber polymer is crushed to obtain a crumb-like rubber polymer, and a step of heating and drying the crumb-like rubber polymer from which the water has been removed, and it is described that the dried crumb is introduced in a baler in a flake form and compressed to form a bale. As the rubber polymer used here, an unsaturated nitrile-conjugated diene copolymer latex obtained by emulsion polymerization is specifically shown, and it is also shown that the method can be applied to copolymers composed only of acrylates, such as ethyl acrylate / n-butyl acrylate copolymer and ethyl acrylate / n-butyl acrylate / 2-methoxyethyl acrylate copolymer. However, such acrylic rubbers composed only of acrylates have the problem of being inferior in crosslinked rubber properties such as heat resistance and compression set resistance.
[0004] As an acrylic rubber having a reactive group with excellent heat resistance and compression set resistance, for example, Patent Document 2 (International Publication No. 2018 / 116828 pamphlet) discloses a method in which a monomer component consisting of ethyl acrylate, n-butyl acrylate, and mono-n-butyl fumarate is emulsified with sodium lauryl sulfate as an emulsifier, polyethylene glycol monostearate, and water, and emulsion-polymerized in the presence of a polymerization initiator until a polymerization conversion rate of 95% is reached, and then the acrylic rubber latex is added to an aqueous solution of magnesium sulfate and a polymer flocculant, dimethylamine-ammonia-epichlorohydrin polycondensate, and then stirred at 85 ° C. to generate a crumb slurry, and then the crumb slurry is washed once with water and then passed through a 100-mesh wire net in its entirety to capture only the solid content and recover the crumb-like acrylic rubber. According to this method, the obtained hydrous crumbs are dehydrated by centrifugation or the like, dried at 50 to 120°C by a band dryer or the like, and then introduced into a baler, compressed, and baled. However, this method has problems such as the generation of a large amount of semi-coagulated hydrous crumbs in the coagulation reaction, which adheres to the coagulation tank in large quantities, and the inability to sufficiently remove the coagulant and emulsifier by washing, and even if bales are produced, there are problems such as poor storage stability and water resistance.
[0005] In addition, Patent Document 3 (International Publication No. 2018 / 079783) discloses a method for producing an acrylic rubber having excellent water resistance (volume change after immersion in distilled water at 80 ° C. for 70 hours) with little residual emulsifier or coagulant by emulsifying monomer components consisting of ethyl acrylate, n-butyl acrylate, and mono-n-butyl fumarate using pure water and an emulsifier consisting of sodium lauryl sulfate and polyoxyethylene dodecyl ether, and emulsion-polymerizing the monomer components to a polymerization conversion rate of 95% by weight in the presence of a polymerization initiator to obtain an emulsion polymerization liquid, and then continuously adding sodium sulfate to produce a water-containing crumb. The water-containing crumb thus produced is then washed four times with industrial water, washed once with an acid of pH 3, and washed once with pure water, and then dried in a hot air dryer at 110 ° C. for 1 hour. However, there is no description of using the rubber in a veil shape, and there is a problem that handling sticky acrylic rubber in a crumb shape is poor in workability and storage stability. Furthermore, there is a demand for high water resistance in harsher environments.
[0006] On the other hand, for example, Patent Document 4 (JP Patent Publication 1-225512 A) discloses a method for producing sheet-shaped acrylic rubber, in which a twin-screw extruder dryer consisting of a feed barrel, a dehydration barrel, a standard barrel, a vent barrel, and a vacuum barrel is used to feed nitrile rubber (NBR) crumbs having a moisture content of about 50% to the feed barrel, and after most of the moisture is removed in the dehydration barrel, the remaining moisture and evaporated vapor are removed by suction in the vacuum barrel, and the crumbs are continuously extruded in a strip shape through a breaker plate and a die, and it is described that acrylic rubber crumbs are used as the rubber crumbs to be applied. However, the same Patent Document does not disclose the use of such acrylic rubber sheets to form bales. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2006-328239 A [Patent Document 2] International Publication No. 2018 / 116828 Brochure [Patent Document 3] International Publication No. 2018 / 079783 Brochure [Patent Document 4] Japanese Patent Application Publication No. 1-225512 Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to provide an acrylic rubber veil having excellent storage stability and water resistance and a production method thereof, a rubber mixture containing the acrylic rubber veil and a production method thereof, and a cross-linked rubber product thereof. [Means for solving the problem]
[0009] The present inventors conducted intensive research in light of the above-mentioned problems and discovered that an acrylic rubber veil made of an acrylic rubber having a reactive group, with an ash content below a specific level, with little air entrapment, and with a high specific gravity, has highly excellent storage stability and water resistance.
[0010] The inventors have also discovered that the storage stability and water resistance of the acrylic rubber veil can be further improved by specifying the content and composition ratio of specific components in the ash, the molecular weight and molecular weight distribution with emphasis on the high molecular weight region, the complex viscosity at 60°C and 100°C, the gel amount of the methyl ethyl ketone insoluble matter, and the water content.
[0011] The present inventors have also discovered that such an acrylic rubber veil can be easily produced by contacting an emulsion polymerization liquid, which is obtained by emulsion polymerizing a monomer component containing a (meth)acrylic acid ester and a reactive group-containing monomer, with a coagulation liquid to produce water-containing crumbs, which are then dehydrated and dried using a specific screw-type extruder, and then extruded into a sheet and laminated.
[0012] The inventors have further discovered that an acrylic rubber bale with excellent storage stability and water resistance can be produced more efficiently by specifying the emulsifier and coagulant, the contacting method and stirring peripheral speed of the emulsion polymerization liquid and the coagulation liquid in the coagulation step, the temperature in the drying barrel of the screw extruder and the resin pressure in the die section, the cutting temperature of the sheet-like dried rubber, and the lamination temperature of the sheet-like dried rubber.
[0013] Based on these findings, the present inventors have completed the present invention.
[0014] Thus, according to the present invention, there is provided an acrylic rubber veil which is made of an acrylic rubber having a reactive group, has an ash content of 0.2% by weight or less, has a total content of at least one element selected from the group consisting of sodium, sulfur, calcium, magnesium and phosphorus of at least 50% by weight relative to the total ash content, and has a specific gravity of 0.9 or more.
[0015] The acrylic rubber veil of the present invention preferably has a specific gravity in the range of 1 to 1.2.
[0016] In the acrylic rubber veil of the present invention, the total amount of sodium and sulfur in the ash is preferably 50% by weight or more relative to the total ash amount.
[0017] In the acrylic rubber veil of the present invention, it is more preferable that the total amount of sodium and sulfur in the ash is 90% by weight or more based on the total ash amount.
[0018] In the acrylic rubber veil of the present invention, the ratio of sodium to sulfur in the ash ([Na] / [S]) is preferably in the range of 0.4 to 2.5 by weight.
[0019] In the acrylic rubber veil of the present invention, the ratio of sodium to sulfur in the ash ([Na] / [S]) is more preferably in the range of 0.7 to 1 by weight.
[0020] In the acrylic rubber veil of the present invention, the weight average molecular weight (Mw) of the acrylic rubber is preferably in the range of 100,000 to 5,000,000. The ratio (Mz / Mw) of the z-average molecular weight (Mz) to the weight average molecular weight (Mw) of the acrylic rubber is preferably 1.3 or more.
[0021] In the acrylic rubber veil of the present invention, the complex viscosity at 60°C ([η]60°C) is preferably 15,000 Pa s or less, and the ratio ([η]100°C / [η]60°C) of the complex viscosity at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) is preferably 0.5 or more.
[0022] In the acrylic rubber veil of the present invention, it is more preferable that the ratio ([η]100°C / [η]60°C) of the complex viscosity at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) is 0.83 or more.
[0023] In the acrylic rubber veil of the present invention, the amount of gel insoluble in methyl ethyl ketone is preferably 50% by weight or less.
[0024] Furthermore, in the acrylic rubber veil of the present invention, the water content is preferably less than 1% by weight.
[0025] The present invention also provides a method for producing an acrylic rubber bale, which includes an emulsion polymerization step of emulsifying a monomer component containing a (meth)acrylic acid ester and a reactive group-containing monomer with water and an emulsifier, and emulsion-polymerizing the resulting emulsion polymerization liquid in the presence of a polymerization catalyst; a coagulation step of contacting the resulting emulsion polymerization liquid with a coagulation liquid consisting of a coagulant-containing aqueous solution to produce wet crumbs; a washing step of washing the produced wet crumbs; a dehydration / drying / molding step of dehydrating the washed wet crumbs in the dehydration barrel using a screw-type extruder having a dehydration slit, a drying barrel under reduced pressure, and a die at the tip, to a water content of 1 to 40% by weight, and then drying in the drying barrel to a water content of less than 1% by weight, and extruding a sheet-like dried rubber from the die; and a baling step of stacking the extruded sheet-like dried rubber to form a bale.
[0026] In the method for producing an acrylic rubber veil of the present invention, it is preferable that the emulsifier is a sulfate ester salt and the coagulant is a sodium salt.
[0027] In the method for producing the acrylic rubber veil of the present invention, the emulsion polymerization liquid is preferably brought into contact with the coagulation liquid by adding the emulsion polymerization liquid to the coagulation liquid while stirring.
[0028] In the method for producing an acrylic rubber veil of the present invention, the peripheral speed of the stirred coagulation liquid is preferably 0.5 m / s or more.
[0029] In the method for producing an acrylic rubber bale of the present invention, the temperature of the water-containing crumb supplied to the screw-type extruder is preferably in the range of 50 to 90°C.
[0030] In the method for producing an acrylic rubber bale of the present invention, the degree of vacuum in the drying barrel of the screw-type extruder is preferably in the range of 1 to 50 kPa.
[0031] In the method for producing an acrylic rubber bale of the present invention, the set temperature of the drying barrel of the screw-type extruder is preferably 100 to 250°C.
[0032] In the method for producing an acrylic rubber veil of the present invention, the resin pressure at the die of the screw-type extruder is preferably in the range of 0.1 to 10 MPa.
[0033] In the method for producing an acrylic rubber veil of the present invention, lamination of the dry rubber sheet is preferably carried out after cutting of the dry rubber sheet.
[0034] In the method for producing an acrylic rubber veil of the present invention, the cutting of the dry rubber sheet is preferably carried out at a temperature of the dry rubber sheet of 60° C. or lower.
[0035] In the method for producing an acrylic rubber veil of the present invention, the lamination of the dry rubber sheet is preferably carried out at a dry rubber sheet temperature of 30° C. or higher.
[0036] According to the present invention, there is also provided a rubber mixture obtained by mixing the acrylic rubber veil with a filler and a crosslinking agent.
[0037] The present invention also provides a method for producing a rubber mixture, which comprises mixing the acrylic rubber veil with a filler and a crosslinking agent in a mixer.
[0038] The present invention also provides a method for producing a rubber mixture, which comprises mixing the acrylic rubber veil with a filler and then mixing a crosslinking agent therein.
[0039] According to the present invention, there is further provided a cross-linked rubber product obtained by cross-linking the above rubber mixture. Effect of the Invention
[0040] According to the present invention, there are provided an acrylic rubber veil having excellent storage stability and water resistance and a method for producing the same, a rubber mixture containing the acrylic rubber veil and a method for producing the same, and a cross-linked rubber product obtained by cross-linking the rubber mixture. [Brief description of the drawings]
[0041] [Figure 1]FIG. 1 is a diagram illustrating an example of an acrylic rubber production system used to produce an acrylic rubber veil according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram showing the configuration of the screw-type extruder in FIG. 1. [Diagram 3] FIG. 2 is a diagram showing the configuration of a transportable cooling device used as the cooling device in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0042] The acrylic rubber veil of the present invention is characterized in that it is made of an acrylic rubber having a reactive group, has an ash content of 0.2% by weight or less, the content of at least one element selected from sodium, sulfur, calcium, magnesium and phosphorus in the ash is at least 50% by weight in total relative to the total ash content, and has a specific gravity of 0.9 or more.
[0043] <Monomer components> The acrylic rubber veil of the present invention is made of an acrylic rubber having a reactive group. The reactive group in the acrylic rubber is appropriately selected depending on the purpose of use, but is preferably at least one functional group selected from a carboxyl group, an epoxy group, and a halogen group, and more preferably at least one functional group selected from the group consisting of a carboxyl group, an epoxy group, and a chlorine atom. The acrylic rubber having such a reactive group may be one in which a reactive group is imparted to the acrylic rubber by a post-reaction, but is preferably one obtained by copolymerizing a reactive group-containing monomer.
[0044] The acrylic rubber constituting the acrylic rubber veil of the present invention preferably contains a (meth)acrylic acid ester, and the amount of the (meth)acrylic acid ester in the acrylic rubber is not particularly limited, but is usually 50% by weight or more, preferably 70% by weight or more, and more preferably 80% by weight or more. In addition, the (meth)acrylic acid ester preferably contains at least one (meth)acrylic acid ester selected from (meth)acrylic acid alkyl esters and (meth)acrylic acid alkoxyalkyl esters. In the present invention, the term "(meth)acrylic acid ester" is a general term for esters of acrylic acid and / or methacrylic acid.
[0045] Specific examples of preferred acrylic rubbers having reactive groups include those composed of at least one (meth)acrylic acid ester selected from (meth)acrylic acid alkyl esters and (meth)acrylic acid alkoxyalkyl esters, a reactive group-containing monomer, and other copolymerizable monomers as necessary.
[0046] The (meth)acrylic acid alkyl ester is not limited, but is usually a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 12 carbon atoms, preferably a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 8 carbon atoms, and more preferably a (meth)acrylic acid alkyl ester having an alkyl group having 2 to 6 carbon atoms.
[0047] Specific examples of (meth)acrylic acid alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate. Ethyl (meth)acrylate and n-butyl (meth)acrylate are preferred, and ethyl acrylate and n-butyl acrylate are more preferred.
[0048] The (meth)acrylic acid alkoxyalkyl ester is not limited, but is usually an (meth)acrylic acid alkoxyalkyl ester having an alkoxyalkyl group of 2 to 12, preferably an (meth)acrylic acid alkoxyalkyl ester having an alkoxyalkyl group of 2 to 8, and more preferably an (meth)acrylic acid alkoxyalkyl ester having an alkoxyalkyl group of 2 to 6 carbon atoms.
[0049] Specific examples of such (meth)acrylic acid alkoxyalkyl esters include methoxymethyl (meth)acrylate, methoxyethyl (meth)acrylate, methoxypropyl (meth)acrylate, methoxybutyl (meth)acrylate, ethoxymethyl (meth)acrylate, ethoxyethyl (meth)acrylate, propoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, etc. Among these, methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, etc. are preferred, and methoxyethyl acrylate, ethoxyethyl acrylate, etc. are more preferred.
[0050] At least one (meth)acrylic acid ester selected from these (meth)acrylic acid alkyl esters and (meth)acrylic acid alkoxyalkyl esters is used alone or in combination of two or more, and the ratio of the (meth)acrylic acid ester in the acrylic rubber is usually 50 to 99.99% by weight, preferably 70 to 99.9% by weight, more preferably 80 to 99.5% by weight, and most preferably 87 to 99% by weight. If the amount of the (meth)acrylic acid ester in the monomer component is excessively small, the weather resistance, heat resistance, and oil resistance of the resulting acrylic rubber may decrease, which is not preferable.
[0051] The type of the reactive group-containing monomer is not limited and may be appropriately selected depending on the intended use, but a monomer having at least one functional group selected from a carboxyl group, an epoxy group, and a halogen group is preferred, and a monomer having at least one functional group selected from the group consisting of a carboxyl group, an epoxy group, and a chlorine atom is preferred.
[0052] The monomer having a carboxyl group is not limited, but an ethylenically unsaturated carboxylic acid can be suitably used. Examples of the ethylenically unsaturated carboxylic acid include ethylenically unsaturated monocarboxylic acid, ethylenically unsaturated dicarboxylic acid, and ethylenically unsaturated dicarboxylic acid monoester, and among these, ethylenically unsaturated dicarboxylic acid monoester is particularly preferred because it can further improve the compression set resistance property when the acrylic rubber is made into a rubber cross-linked product.
[0053] The ethylenically unsaturated monocarboxylic acid is not limited, but is preferably an ethylenically unsaturated monocarboxylic acid having 3 to 12 carbon atoms, and examples thereof include acrylic acid, methacrylic acid, α-ethylacrylic acid, crotonic acid, and cinnamic acid.
[0054] The ethylenically unsaturated dicarboxylic acid is not limited, but is preferably an ethylenically unsaturated dicarboxylic acid having 4 to 12 carbon atoms, and specific examples include butenedioic acids such as fumaric acid and maleic acid, itaconic acid, citraconic acid, etc. The ethylenically unsaturated dicarboxylic acid also includes those that exist as an anhydride.
[0055] The ethylenically unsaturated dicarboxylic acid monoester is not limited, but is usually an ethylenically unsaturated dicarboxylic acid having 4 to 12 carbon atoms and an alkyl monoester having 1 to 12 carbon atoms, preferably an ethylenically unsaturated dicarboxylic acid having 4 to 6 carbon atoms and an alkyl monoester having 2 to 8 carbon atoms, and more preferably an alkyl monoester having 2 to 6 carbon atoms of butenedioic acid having 4 carbon atoms.
[0056] Specific examples of such ethylenically unsaturated dicarboxylic acid monoesters include butenedioic acid monoalkyl esters such as monomethyl fumarate, monoethyl fumarate, mono-n-butyl fumarate, monomethyl maleate, monoethyl maleate, mono-n-butyl maleate, monocyclopentyl fumarate, monocyclohexyl fumarate, monocyclohexenyl fumarate, monocyclopentyl maleate, and monocyclohexyl maleate; and itaconic acid monoalkyl esters such as monomethyl itaconate, monoethyl itaconate, mono-n-butyl itaconate, and monocyclohexyl itaconate. Among these, mono-n-butyl fumarate and mono-n-butyl maleate are preferred, and mono-n-butyl fumarate is particularly preferred.
[0057] Examples of the monomer having an epoxy group include epoxy group-containing (meth)acrylic acid esters such as glycidyl (meth)acrylate; epoxy group-containing vinyl ethers such as allyl glycidyl ether and vinyl glycidyl ether; and the like.
[0058] Examples of monomers having a halogen group include unsaturated alcohol esters of halogen-containing saturated carboxylic acids, (meth)acrylic acid haloalkyl esters, (meth)acrylic acid haloacyloxyalkyl esters, (meth)acrylic acid (haloacetylcarbamoyloxy)alkyl esters, halogen-containing unsaturated ethers, halogen-containing unsaturated ketones, halomethyl group-containing aromatic vinyl compounds, halogen-containing unsaturated amides, and haloacetyl group-containing unsaturated monomers.
[0059] Specific examples of unsaturated alcohol esters of halogen-containing saturated carboxylic acids include vinyl chloroacetate, vinyl 2-chloropropionate, and allyl chloroacetate. Examples of (meth)acrylic acid haloalkyl esters include chloromethyl (meth)acrylate, 1-chloroethyl (meth)acrylate, 2-chloroethyl (meth)acrylate, 1,2-dichloroethyl (meth)acrylate, 2-chloropropyl (meth)acrylate, 3-chloropropyl (meth)acrylate, and 2,3-dichloropropyl (meth)acrylate. Examples of (meth)acrylic acid haloacyloxyalkyl esters include 2-(chloroacetoxy)ethyl (meth)acrylate, 2-(chloroacetoxy)propyl (meth)acrylate, 3-(chloroacetoxy)propyl (meth)acrylate, and 3-(hydroxychloroacetoxy)propyl (meth)acrylate.
[0060] Specific examples of (meth)acrylic acid (haloacetylcarbamoyloxy)alkyl esters include 2-(chloroacetylcarbamoyloxy)ethyl (meth)acrylate and 3-(chloroacetylcarbamoyloxy)propyl (meth)acrylate. Specific examples of halogen-containing unsaturated ethers include chloromethyl vinyl ether, 2-chloroethyl vinyl ether, 3-chloropropyl vinyl ether, 2-chloroethyl allyl ether, and 3-chloropropyl allyl ether. Specific examples of halogen-containing unsaturated ketones include 2-chloroethyl vinyl ketone, 3-chloropropyl vinyl ketone, and 2-chloroethyl allyl ketone. Specific examples of halomethyl group-containing aromatic vinyl compounds include p-chloromethylstyrene, m-chloromethylstyrene, o-chloromethylstyrene, and p-chloromethyl-α-methylstyrene. Specific examples of halogen-containing unsaturated amides include N-chloromethyl(meth)acrylamide, and specific examples of haloacetyl group-containing unsaturated monomers include 3-(hydroxychloroacetoxy)propyl allyl ether and p-vinylbenzyl chloroacetate.
[0061] These reactive group-containing monomers may be used alone or in combination of two or more, and their proportion in the acrylic rubber is usually 0.01 to 20% by weight, preferably 0.1 to 10% by weight, more preferably 0.5 to 5% by weight, and most preferably 1 to 3% by weight.
[0062] The monomers other than the above-mentioned monomers (hereinafter referred to as "other monomers") used as necessary are not particularly limited as long as they are copolymerizable with the above-mentioned monomers, and examples thereof include aromatic vinyl, ethylenically unsaturated nitriles, acrylamide monomers, other olefin monomers, etc. Specific examples of aromatic vinyls used as other monomers include styrene, α-methylstyrene, and divinylbenzene. Specific examples of ethylenically unsaturated nitriles include acrylonitrile and methacrylonitrile. Specific examples of acrylamide monomers include acrylamide and methacrylamide. Specific examples of other olefin monomers include ethylene, propylene, vinyl acetate, ethyl vinyl ether, and butyl vinyl ether.
[0063] These other monomers may be used alone or in combination of two or more, and their proportion in the acrylic rubber is usually in the range of 0 to 30% by weight, preferably 0 to 20% by weight, more preferably 0 to 15% by weight, and most preferably 0 to 10% by weight.
[0064] <Acrylic rubber> The acrylic rubber constituting the acrylic rubber veil of the present invention is characterized by having reactive groups in the polymer. The content of the reactive groups may be appropriately selected depending on the purpose of use, but when the weight ratio of the reactive groups themselves is usually in the range of 0.001 to 5 wt%, preferably 0.01 to 3 wt%, more preferably 0.05 to 1 wt%, and particularly preferably 0.1 to 0.5 wt%, it is suitable because the properties such as the processability, strength properties, compression set resistance, oil resistance, cold resistance, and water resistance of the acrylic rubber veil are highly balanced.
[0065] Specific examples of the acrylic rubber constituting the acrylic rubber veil of the present invention include at least one (meth)acrylic ester selected from (meth)acrylic acid alkyl esters and (meth)acrylic acid alkoxyalkyl esters, a reactive group-containing monomer, and other copolymerizable monomers contained as necessary, and the proportions of each in the acrylic rubber are usually 50 to 99.99% by weight, preferably 70 to 99.9% by weight, more preferably 80 to 99.5% by weight, and particularly preferably 87 to 99% by weight, of the at least one (meth)acrylic ester selected from (meth)acrylic acid alkyl esters and (meth)acrylic acid alkoxyalkyl esters, the reactive group-containing monomer is usually 0.01 to 20% by weight, preferably 0.1 to 10% by weight, more preferably 0.5 to 5% by weight, and particularly preferably 1 to 3% by weight, and the other monomers are usually 0 to 30% by weight, preferably 0 to 20% by weight, more preferably 0 to 15% by weight, and particularly preferably 0 to 10% by weight. By setting the ratio of these monomers in the acrylic rubber within the above ranges, the objects of the present invention can be achieved to a high degree, and the water resistance and compression set resistance properties are significantly improved when the acrylic rubber veil is crosslinked, which is preferable.
[0066] The weight average molecular weight (Mw) of the acrylic rubber constituting the acrylic rubber veil of the present invention is not limited, but when the absolute molecular weight measured by GPC-MALS is usually in the range of 100,000 to 5,000,000, preferably 500,000 to 4,000,000, more preferably 700,000 to 3,000,000, and most preferably 1,000,000 to 2,500,000, the processability during mixing of the acrylic rubber veil, strength properties, and compression set resistance properties are highly balanced and suitable.
[0067] The ratio (Mz / Mw) of the z-average molecular weight (Mz) to the weight-average molecular weight (Mw) of the acrylic rubber constituting the acrylic rubber veil of the present invention is not limited, but when the ratio is usually 1.3 or more, preferably 1.4 to 5, and more preferably 1.5 to 2, in terms of absolute molecular weight distribution measured by GPC-MALS, the processability and strength characteristics of the acrylic rubber veil are highly balanced and changes in physical properties during storage can be mitigated, which is suitable.
[0068] The glass transition temperature (Tg) of the acrylic rubber constituting the acrylic rubber veil of the present invention is not limited, but is usually 20° C. or lower, preferably 10° C. or lower, and more preferably 0° C. or lower. The lower limit of the glass transition temperature (Tg) is also not limited, but is usually −80° C. or higher, preferably −60° C. or higher, and more preferably −40° C. or higher. By setting the glass transition temperature (Tg) of the acrylic rubber veil to the above-mentioned lower limit temperature or higher, it is possible to provide the acrylic rubber veil with superior oil resistance and heat resistance, and by setting it to the above-mentioned upper limit temperature or lower, it is possible to provide the acrylic rubber veil with superior cold resistance and processability.
[0069] The content of the acrylic rubber in the acrylic rubber veil of the present invention is appropriately selected depending on the intended use of the acrylic rubber veil, but is usually 95% by weight or more, preferably 97% by weight or more, and more preferably 98% by weight or more.
[0070] <Acrylic rubber veil> The acrylic rubber veil of the present invention is made of the above-mentioned acrylic rubber and is characterized in that the ash content, ash components and specific gravity are all within specific ranges.
[0071] The ash content in acrylic rubber bales is measured in accordance with JIS K6228 Method A, and the main components are residues of the emulsifier used when emulsifying the monomer components and carrying out emulsion polymerization in the production of acrylic rubber, and the coagulant used to coagulate the emulsion polymerization liquid.
[0072] The acrylic rubber veil of the present invention has an ash content of 0.2% by weight or less, preferably 0.15% by weight or less, more preferably 0.12% by weight or less, particularly preferably 0.11% by weight or less, and most preferably 0.1% by weight or less, which is suitable for excellent storage stability and water resistance. There is no restriction on the lower limit of the ash content, but when it is usually 0.0001% by weight or more, preferably 0.0005% by weight or more, more preferably 0.001% by weight or more, particularly preferably 0.005% by weight or more, and most preferably 0.01% by weight or more, it is suitable for excellent workability, as it suppresses metal adhesion.
[0073] The ash content for achieving a high level of balance between storage stability, water resistance, and metal adhesion of the acrylic veil of the present invention is usually in the range of 0.0001 to 0.2% by weight, preferably 0.0005 to 0.15% by weight, more preferably 0.001 to 0.12% by weight, particularly preferably 0.005 to 0.11% by weight, and most preferably 0.01 to 0.1% by weight.
[0074] The acrylic rubber veil of the present invention is suitable in that when the total content of at least one element selected from sodium, sulfur, calcium, magnesium and phosphorus in the ash is at least 30% by weight, preferably 50% by weight or more, more preferably 70% by weight or more, and particularly preferably 80% by weight or more, the storage stability and water resistance of the acrylic rubber veil are highly excellent.
[0075] In particular, when the total amount of sodium and sulfur in the ash of the acrylic rubber veil of the present invention is usually 30% by weight or more, preferably 50% by weight or more, more preferably 70% by weight or more, particularly preferably 80% by weight or more, and most preferably 90% by weight or more, the storage stability and water resistance are highly excellent and it is suitable.
[0076] The ratio of sodium to sulfur in the ash of the acrylic rubber veil of the present invention ([Na] / [S]) is not particularly limited, but when the ratio by weight is usually in the range of 0.4 to 2.5, preferably 0.6 to 1.5, more preferably 0.7 to 1, particularly preferably 0.75 to 0.95, and most preferably 0.8 to 0.9, water resistance is highly excellent and the ratio is suitable.
[0077] The specific gravity of the acrylic rubber veil of the present invention is at least 0.9 or more, preferably 0.9 to 1.3, more preferably 0.95 to 1.25, and particularly preferably 1.0 to 1.2. An acrylic rubber veil with a high specific gravity is suitable because it has excellent storage stability.
[0078] The water content of the acrylic rubber veil of the present invention is not limited, but when it is generally less than 1% by weight, preferably 0.8% by weight or less, and more preferably 0.6% by weight or less, the vulcanization characteristics are optimized and properties such as heat resistance and water resistance are highly excellent, making it suitable.
[0079] There are no limitations on the gel content of the acrylic rubber veil of the present invention, but processability is highly improved and it is suitable when the gel content, in terms of the content insoluble in methyl ethyl ketone, is usually 50% by weight or less, preferably 40% by weight or less, more preferably 30% by weight or less, particularly preferably 10% by weight or less, and most preferably 5% by weight or less.
[0080] The pH of the acrylic rubber sheet of the present invention is not limited, but is usually 6 or less, preferably 2 to 6, more preferably 2.5 to 5.5, and particularly preferably 3 to 5, and is therefore suitable since storage stability is highly improved.
[0081] The complex viscosity at 60°C of the acrylic rubber veil of the present invention ([η]60°C) is not limited, but is usually 15,000 Pa·s or less, preferably 2,000 to 10,000 Pa·s, more preferably 2,500 to 7,000 Pa·s, and most preferably 2,700 to 5,500 Pa·s, which is suitable for excellent processability, oil resistance, and shape retention. The complex viscosity at 100°C ([η]100°C) is not limited, but is usually 1,500 to 6,000 Pa·s, preferably 2,000 to 5,000 Pa·s, more preferably 2,500 to 4,000 Pa·s, and most preferably 2,500 to 3,500 Pa·s, which is suitable for excellent processability, oil resistance, and shape retention.
[0082] The ratio ([η]100°C / [η]60°C) of the complex viscosity at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) of the acrylic rubber veil of the present invention is not limited, but is usually 0.5 or more, preferably 0.6 or more, more preferably 0.7 or more, particularly preferably 0.8 or more, and most preferably 0.83 or more. In addition, when the ratio ([η]100°C / [η]60°C) of the complex viscosity at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) is usually in the range of 0.5 to 0.99, preferably 0.5 to 0.98, more preferably 0.6 to 0.95, particularly preferably 0.75 to 0.93, and most preferably 0.8 to 0.93, the processability, oil resistance, and shape retention are highly balanced and are suitable.
[0083] The Mooney viscosity (ML1+4, 100°C) of the acrylic rubber veil of the present invention is not limited, but when it is in the range of usually 10 to 150, preferably 20 to 100, and more preferably 25 to 70, the processability and strength properties are highly balanced and it is suitable.
[0084] The size of the acrylic rubber veil of the present invention is not limited, but the width is usually in the range of 100 to 800 mm, preferably 200 to 500 mm, and more preferably 250 to 450 mm, the length is usually in the range of 300 to 1,200 mm, preferably 400 to 1,000 mm, and more preferably 500 to 800 mm, and the height (thickness) is usually in the range of 50 to 500 mm, preferably 100 to 300 mm, and more preferably 150 to 250 mm. The shape of the acrylic rubber veil of the present invention is also not limited and may be appropriately selected depending on the purpose of use of the acrylic rubber veil, but in many cases a rectangular parallelepiped is suitable.
[0085] <Manufacturing method of acrylic rubber veil> The acrylic rubber veil can be suitably produced by the production method of the present invention, which includes the following steps (1) to (5): (1) an emulsion polymerization step of emulsifying a monomer component mainly composed of a (meth)acrylic acid ester with water and an emulsifier, and emulsion-polymerizing the monomer component in the presence of a polymerization catalyst to obtain an emulsion polymerization liquid; (2) a coagulation step in which the obtained emulsion polymerization liquid is contacted with a coagulation liquid to produce water-containing crumbs; (3) A washing step for washing the produced hydrous crumbs; (4) a dehydration, drying and molding process in which the washed wet crumbs are dehydrated in the dehydration barrel using a screw-type extruder having a dehydration slit, a drying barrel under reduced pressure, and a die at the tip, to a moisture content of 1 to 40% by weight, and then dried in the drying barrel to a moisture content of less than 1% by weight, and a sheet-like dried rubber is extruded through the die; (5) a baling process in which the extruded dry rubber sheets are layered and baled; The method of the present invention, which comprises the steps of:
[0086] (Emulsion polymerization process) The emulsion polymerization step (1) in the method for producing the acrylic rubber veil of the present invention is characterized in that the monomer components are emulsified with water and an emulsifier, and then emulsion-polymerized in the presence of a polymerization catalyst to obtain an emulsion polymerization liquid.
[0087] The emulsifier used in the emulsion polymerization step is not limited, but examples thereof include anionic emulsifiers, cationic emulsifiers, nonionic emulsifiers, etc. Among these, anionic emulsifiers and nonionic emulsifiers are preferred, and anionic emulsifiers are particularly preferred.
[0088] Examples of the anionic emulsifier include fatty acid-based emulsifiers, sulfonic acid-based emulsifiers, sulfosuccinic acid-based emulsifiers, sulfuric acid-based emulsifiers, and phosphoric acid-based emulsifiers, and preferably sulfuric acid-based emulsifiers.
[0089] Examples of fatty acid emulsifiers include sodium octanoate, sodium decanoate, sodium laurate, sodium myristate, sodium palmitate, and sodium stearate.
[0090] Examples of sulfonic acid emulsifiers include sodium hexanesulfonate, sodium octane sulfonate, sodium decane sulfonate, sodium toluenesulfonate, sodium cumenesulfonate, sodium octylbenzenesulfonate, sodium dodecylbenzenesulfonate, ammonium dodecylbenzenesulfonate, sodium naphthalenesulfonate, sodium alkylnaphthalenesulfonate, and sodium alkyldiphenyletherdisulfonate.
[0091] Examples of sulfosuccinic acid emulsifiers include sodium dioctyl sulfosuccinate and sodium dihexyl sulfosuccinate.
[0092] As the sulfate-based emulsifier, sulfate ester salts can be suitably used, such as sodium lauryl sulfate, ammonium lauryl sulfate, sodium myristyl sulfate, sodium laureth sulfate, sodium polyoxyethylene alkyl sulfate, and sodium polyoxyethylene alkylaryl sulfate, with sodium lauryl sulfate being particularly preferred.
[0093] Examples of the phosphoric acid-based emulsifier include sodium lauryl phosphate, potassium lauryl phosphate, and sodium polyoxyalkylene alkyl ether phosphate.
[0094] Examples of the cationic emulsifier include alkyltrimethylammonium chloride, dialkylammonium chloride, and benzylammonium chloride.
[0095] Examples of the nonionic emulsifier include polyoxyalkylene fatty acid esters such as polyoxyethylene stearate ester; polyoxyalkylene alkyl ethers such as polyoxyethylene dodecyl ether; polyoxyalkylene alkylphenol ethers such as polyoxyethylene nonylphenyl ether; and polyoxyethylene sorbitan alkyl esters. Of these, polyoxyalkylene alkyl ethers and polyoxyalkylene alkylphenol ethers are preferred, and polyoxyethylene alkyl ethers and polyoxyethylene alkylphenol ethers are more preferred.
[0096] These emulsifiers can be used alone or in combination of two or more. The amount used is usually 0.01 to 10 parts by weight, preferably 0.1 to 5 parts by weight, and more preferably 1 to 3 parts by weight, per 100 parts by weight of the monomer component.
[0097] The monomer component, water, and emulsifier may be mixed in a conventional manner, such as by stirring the monomer, emulsifier, and water with a stirrer such as a homogenizer or a disk turbine. The amount of water used is usually 10 to 750 parts by weight, preferably 50 to 500 parts by weight, and more preferably 100 to 400 parts by weight, based on 100 parts by weight of the monomer component.
[0098] The polymerization catalyst used in the emulsion polymerization step is not limited as long as it is one that is usually used in emulsion polymerization. For example, a redox catalyst consisting of a radical generator and a reducing agent can be used.
[0099] Examples of the radical generator include peroxides and azo compounds, and preferably peroxides. As the peroxide, inorganic peroxides and organic peroxides can be used.
[0100] Examples of the inorganic peroxide include sodium persulfate, potassium persulfate, hydrogen peroxide, and ammonium persulfate. Among these, potassium persulfate, hydrogen peroxide, and ammonium persulfate are preferred, and potassium persulfate is particularly preferred.
[0101] Examples of the organic peroxides include 2,2-di(4,4-di(t-butylperoxy)cyclohexyl)propane, 1-di(t-hexylperoxy)cyclohexane, 1,1-di(t-butylperoxy)cyclohexane, 4,4-di(t-butylperoxy)n-butyl valerate, 2,2-di(t-butylperoxy)butane, t-butyl hydroperoxide, cumene hydroperoxide, diisopropylbenzene hydroperoxide, paramenthane hydroperoxide, benzoyl peroxide, 1,2-di(t-butylperoxy)cyclohexane ... ,1,3,3-tetraethylbutyl hydroperoxide, t-butylcumyl peroxide, di-t-butyl peroxide, di-t-hexyl peroxide, di(2-t-butylperoxyisopropyl)benzene, dicumyl peroxide, diisobutyryl peroxide, di(3,5,5-trimethylhexanoyl) peroxide, dilauroyl peroxide, disuccinic acid peroxide, dibenzoyl peroxide, di(3-methylbenzoyl) peroxide, benzoyl(3-methylbenzoyl) peroxide, Diisobutyryl peroxydicarbonate, di-n-propyl peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, di-sec-butyl peroxydicarbonate, 1,1,3,3-tetramethylbutyl peroxyneodecanate, t-hexyl peroxypivalate, t-butyl peroxyneodecanate, t-hexyl peroxypivalate, t-butyl peroxypivalate, 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane, 1,1,3,3-tetramethylbutyl peroxy Peroxy-2-ethylhexanate, t-hexylperoxy-2-ethylhexanate, t-butylperoxy-3,5,5-trimethylhexanate, t-hexylperoxyisopropylmonocarbonate, t-butylperoxyisopropylmonocarbonate, t-butylperoxy-2-ethylhexylmonocarbonate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-butylperoxyacetate, t-hexylperoxybenzoate, t-butylperoxybenzoate, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, and among these, diisopropylbenzene hydroperoxide, cumene hydroperoxide, paramenthane hydroperoxide, benzoyl peroxide, and the like are preferred.
[0102] Examples of the azo compound include azobisisoptylonitrile, 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis[2-(2-imidazolin-2-yl)propane, 2,2'-azobis(propane-2-carboxamidine), 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropanamide], 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane}, 2,2'-azobis(1-imino-1-pyrrolidino-2-methylpropane), and 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propanamide}.
[0103] These radical generators can be used alone or in combination of two or more kinds. The amount used is usually in the range of 0.0001 to 5 parts by weight, preferably 0.0005 to 1 part by weight, and more preferably 0.001 to 0.5 parts by weight, per 100 parts by weight of the monomer component.
[0104] The reducing agent is not limited as long as it is used in a redox catalyst for emulsion polymerization, but in the present invention, it is particularly preferable to use at least two kinds of reducing agents in combination. As the at least two kinds of reducing agents, for example, a combination of a metal ion compound in a reduced state and another reducing agent is preferable.
[0105] The reduced metal ion compound is not particularly limited, but examples thereof include ferrous sulfate, sodium iron hexamethylenediaminetetraacetate, and cuprous naphthenate, with ferrous sulfate being preferred among these.
[0106] These reduced metal ion compounds can be used alone or in combination of two or more kinds, and the amount used is usually in the range of 0.000001 to 0.01 parts by weight, preferably 0.00001 to 0.001 parts by weight, and more preferably 0.00005 to 0.0005 parts by weight, per 100 parts by weight of the monomer component.
[0107] The reducing agent other than the metal ion compound in a reduced state is not particularly limited, and examples thereof include ascorbic acid or a salt thereof such as ascorbic acid, sodium ascorbate, and potassium ascorbate; erythorbic acid or a salt thereof such as erythorbic acid, sodium erythorbate, and potassium erythorbate; sulfinic acid salts such as sodium hydroxymethanesulfinate; sulfite salts such as sodium sulfite, potassium sulfite, sodium hydrogen sulfite, aldehyde sodium hydrogen sulfite, and potassium hydrogen sulfite; Examples of suitable phosphorous acids include pyrosulfites such as sodium pyrosulfite, potassium pyrosulfite, sodium hydrogen pyrosulfite, and potassium hydrogen pyrosulfite; thiosulfates such as sodium thiosulfate and potassium thiosulfate; phosphorous acid or a salt thereof such as phosphorous acid, sodium phosphite, potassium phosphite, sodium hydrogen phosphite, and potassium hydrogen phosphite; pyrophosphorous acid or a salt thereof such as pyrophosphorous acid, sodium pyrophosphite, potassium pyrophosphite, sodium hydrogen pyrophosphite, and potassium hydrogen pyrophosphite; sodium formaldehyde sulfoxylate, etc. Among these, ascorbic acid or a salt thereof, sodium formaldehyde sulfoxylate, etc. are preferred, and ascorbic acid or a salt thereof is particularly preferred.
[0108] These reducing agents other than metal ion compounds in a reduced state can be used alone or in combination of two or more kinds, and the amount used is usually in the range of 0.001 to 1 part by weight, preferably 0.005 to 0.5 parts by weight, and more preferably 0.01 to 0.3 parts by weight, per 100 parts by weight of the monomer component.
[0109] A preferred combination of a metal ion compound in a reduced state and another reducing agent is a combination of ferrous sulfate and ascorbic acid or a salt thereof and / or sodium formaldehyde sulfoxylate, more preferably a combination of ferrous sulfate and an ascorbate and / or sodium formaldehyde sulfoxylate, and most preferably a combination of ferrous sulfate and an ascorbate. The amount of ferrous sulfate used is usually 0.000001 to 0.01 parts by weight, preferably 0.00001 to 0.001 parts by weight, more preferably 0.00005 to 0.0005 parts by weight, relative to 100 parts by weight of the monomer component, and the amount of ascorbic acid or a salt thereof and / or sodium formaldehyde sulfoxylate used is usually 0.001 to 1 part by weight, preferably 0.005 to 0.5 parts by weight, more preferably 0.01 to 0.3 parts by weight, relative to 100 parts by weight of the monomer component.
[0110] The amount of water used in the emulsion polymerization reaction may be only the amount used during emulsification of the monomer components, but is adjusted to be in the range of usually 10 to 1,000 parts by weight, preferably 50 to 500 parts by weight, more preferably 80 to 400 parts by weight, and most preferably 100 to 300 parts by weight, per 100 parts by weight of the monomer components used in the polymerization.
[0111] The emulsion polymerization reaction may be carried out in a conventional manner, and may be any of batch, semi-batch, and continuous. The polymerization temperature and polymerization time are not particularly limited and may be appropriately selected depending on the type of polymerization initiator used. The polymerization temperature is usually in the range of 0 to 100°C, preferably 5 to 80°C, and more preferably 10 to 50°C, and the polymerization time is usually 0.5 to 100 hours, and preferably 1 to 10 hours.
[0112] The polymerization conversion rate of the emulsion polymerization reaction is not particularly limited, but is usually 80% by weight or more, preferably 90% by weight or more, and more preferably 95% by weight or more, which is suitable since the acrylic rubber veil produced has excellent strength characteristics and is free of monomer odor. A polymerization terminator may be used to terminate the polymerization.
[0113] (solidification process) The coagulation step (2) in the method for producing an acrylic rubber sheet of the present invention is characterized in that the emulsion polymerization liquid obtained in the emulsion polymerization step (1) is brought into contact with a coagulation liquid consisting of an aqueous solution containing a coagulant to produce water-containing crumbs.
[0114] The solids concentration of the emulsion polymerization liquid used in the coagulation step is not limited, but is usually adjusted to within the range of 5 to 50% by weight, preferably 10 to 45% by weight, and more preferably 20 to 40% by weight.
[0115] The coagulant used in the coagulation step is not particularly limited, but a metal salt is usually used. Examples of the metal salt include alkali metals, Group 2 metal salts of the periodic table, and other metal salts, and are preferably alkali metal salts and Group 2 metal salts of the periodic table, and more preferably alkali metal salts.
[0116] Examples of alkali metal salts include sodium salts such as sodium chloride, sodium nitrate, and sodium sulfate; potassium salts such as potassium chloride, potassium nitrate, and potassium sulfate; and lithium salts such as lithium chloride, lithium nitrate, and lithium sulfate. Among these, sodium salts such as sodium chloride and sodium sulfate are preferred, and sodium sulfate is particularly preferred.
[0117] Examples of the salt of a metal of Group 2 of the periodic table include magnesium chloride, calcium chloride, magnesium nitrate, calcium nitrate, magnesium sulfate, and calcium sulfate, and preferably calcium chloride and magnesium sulfate.
[0118] Other metal salts used as coagulants include, for example, zinc chloride, titanium chloride, manganese chloride, iron chloride, cobalt chloride, nickel chloride, aluminum chloride, tin chloride, zinc nitrate, titanium nitrate, manganese nitrate, iron nitrate, cobalt nitrate, nickel nitrate, aluminum nitrate, tin nitrate, zinc sulfate, titanium sulfate, manganese sulfate, iron sulfate, cobalt sulfate, nickel sulfate, aluminum sulfate, and tin sulfate.
[0119] These coagulants can be used alone or in combination of two or more, and the amount used is usually 0.01 to 100 parts by weight, preferably 0.1 to 50 parts by weight, and more preferably 1 to 30 parts by weight, relative to 100 parts by weight of the monomer component. When the amount of the coagulant is within this range, it is preferable because it is possible to sufficiently coagulate the acrylic rubber while highly improving the compression set resistance and water resistance when the acrylic rubber veil is crosslinked.
[0120] The coagulant concentration of the coagulation liquid (aqueous coagulant solution) used is usually in the range of 0.1 to 20% by weight, preferably 0.5 to 15% by weight, more preferably 1 to 10% by weight, and particularly preferably 1.5 to 5% by weight, which is suitable for concentrating the particle size of the generated hydrous crumbs uniformly in a specific region.
[0121] The temperature of the coagulation liquid is not limited, but when it is usually 40°C or higher, preferably 40 to 90°C, more preferably in the range of 50 to 80°C, uniform water-containing crumbs are preferably formed.
[0122] The method for contacting the emulsion polymerization liquid with the coagulation liquid is not limited, and may be, for example, a method of adding the emulsion polymerization liquid to the coagulation liquid being stirred, or a method of adding the coagulation liquid to the emulsion polymerization liquid being stirred. In the production method of the present invention, however, the method of adding the emulsion polymerization liquid to the coagulation liquid being stirred is preferable, because the shape and diameter of the generated water-containing crumbs can be made uniform and the crumbs can be concentrated, and the washing efficiency of the emulsifier and coagulation agent can be significantly improved.
[0123] The rotation speed (agitation speed) of the stirred coagulation liquid is represented by the rotation speed of the stirring blade of the stirring device installed in the coagulation bath, and is usually 100 rpm or more, preferably 200 to 1,000 rpm, more preferably 300 to 900 rpm, and particularly preferably in the range of 400 to 800 rpm.
[0124] The rotation speed of the coagulation liquid is preferably set to a value at which the coagulation liquid is stirred vigorously to some extent, since this allows the generated hydrous crumbs to have a small and uniform particle size. By setting the rotation speed to the above lower limit or higher, it is possible to prevent the generation of crumbs with excessively large or small particle sizes, while by setting the rotation speed to the above upper limit or lower, it becomes easier to control the coagulation reaction.
[0125] The peripheral speed of the stirred coagulation liquid is expressed by the linear speed of the outer circumference of the stirring blade of the stirring device installed in the coagulation bath, and it is preferable that the coagulation liquid is stirred vigorously to a certain extent in order to make the particle size of the water-containing crumbs small and uniform, and is usually 0.5 m / s or more, preferably 1 m / s or more, more preferably 1.5 m / s or more, particularly preferably 2 m / s or more, and most preferably 2.5 m / s or more. On the other hand, the upper limit of the peripheral speed is not limited, but it is usually 50 m / s or less, preferably 30 m / s or less, more preferably 25 m / s or less, and most preferably 20 m / s or less, which is preferable because it makes it easier to control the coagulation reaction.
[0126] By controlling the above-mentioned various conditions of the coagulation reaction in the coagulation step (contact method, solids concentration of the emulsion polymerization liquid, concentration and temperature of the coagulation liquid, rotation speed and peripheral speed during stirring of the coagulation liquid, etc.) within specific ranges, the shape and diameter of the generated water-containing crumbs are made uniform and concentrated, and the removal of the emulsifier and coagulant during the subsequent washing and dehydration is significantly improved, which is preferable.
[0127] The thus-obtained water-containing crumbs are suitable because they satisfy all of the following conditions (a) to (e) when sieved through a JIS classification sieve. The JIS sieve complies with the provisions of the Japanese Industrial Standards (JIS Z 8801-1). (a) The proportion of water-containing crumbs that do not pass through a JIS sieve with a mesh size of 9.5 mm is 10% by weight or less; (b) the proportion of wet crumbs that pass through a JIS sieve with a mesh size of 9.5 mm but do not pass through a JIS sieve with a mesh size of 6.7 mm is 30% by weight or less; (c) the proportion of moist crumbs that pass through a JIS sieve with a mesh size of 6.7 mm but do not pass through a JIS sieve with a mesh size of 710 μm is 20% by weight or more; (d) The proportion of water-containing crumbs that pass through a JIS sieve with a mesh size of 710 μm but do not pass through a JIS sieve with a mesh size of 425 μm is 30% by weight or less; and (e) The proportion of moist crumbs passing through a JIS sieve having an opening of 425 μm is 10% by weight or less.
[0128] When all the generated wet crumbs are sieved, (a) the proportion of relatively large wet crumbs that do not pass through a JIS sieve with a mesh size of 9.5 mm is 10% by weight or less, preferably 5% by weight or less, and more preferably 1% by weight or less, (b) the proportion of wet crumbs that pass through a JIS sieve with a mesh size of 9.5 mm but do not pass through a JIS sieve with a mesh size of 6.7 mm is 30% by weight or less, preferably 20% by weight or less, and more preferably 5% by weight or less, and (c) the proportion of wet crumbs that pass through a JIS sieve with a mesh size of 6.7 mm but do not pass through a JIS sieve with a mesh size of 710 μm is 20% by weight or more, preferably 40% by weight or less. % by weight or more, more preferably 70% by weight or more, and most preferably 80% by weight or more; (d) the proportion of water-containing crumbs that pass through a JIS sieve with a mesh size of 710 μm but not a JIS sieve with a mesh size of 425 μm is 30% by weight or less, preferably 20% by weight or less, and more preferably 15% by weight or less; and further, (e) the proportion of relatively small water-containing crumbs that pass through a JIS sieve with a mesh size of 425 μm is 10% by weight or less, preferably 5% by weight or less, and more preferably 1% by weight or less, which is preferable because the washing efficiency of the emulsifier and coagulant is significantly improved and productivity is also increased.
[0129] In the present invention, the washing efficiency of the emulsifier and coagulant is improved, and it is preferable when the proportion of (f) hydrous crumbs that pass through a JIS sieve with a mesh size of 6.7 mm but do not pass through a JIS sieve with a mesh size of 4.75 mm out of the total hydrous crumbs produced is usually 40% by weight or less, preferably 10% by weight or less, and more preferably 5% by weight or less.
[0130] In the present invention, it is also preferable that the proportion of (g) hydrous crumbs that pass through a JIS sieve with a mesh size of 4.75 mm but do not pass through a JIS sieve with a mesh size of 710 μm out of the total hydrous crumbs produced is usually 40% by weight or more, preferably 60% by weight or more, and more preferably 80% by weight or more, since this significantly improves the removal efficiency of the emulsifier and coagulant during washing and dehydration.
[0131] In the present invention, furthermore, when the proportion of (h) hydrous crumbs that pass through a JIS sieve with a mesh size of 3.35 mm but do not pass through a JIS sieve with a mesh size of 710 μm out of the total hydrous crumbs produced is usually 20% by weight or more, preferably 40% by weight or more, more preferably 50% by weight or more, particularly preferably 60% by weight or more, and most preferably 70% by weight or more, this is preferable because the removal efficiency of the emulsifier and coagulant during washing and dehydration is significantly improved.
[0132] (Cleaning process) The washing step (3) in the method for producing an acrylic rubber veil of the present invention is a step of washing the water-containing crumbs generated in the coagulation step (2) above. The washing method is not limited and may be a conventional method, for example, by mixing the generated water-containing crumbs with a large amount of water.
[0133] The amount of water used in washing is not particularly limited, but when the amount of water used per one water wash is usually at least 50 parts by weight, preferably within the range of 50 to 15,000 parts by weight, more preferably 100 to 10,000 parts by weight, and particularly preferably 150 to 5,000 parts by weight, per 100 parts by weight of the monomer components, the ash content in the acrylic rubber veil can be effectively reduced, and this is suitable.
[0134] The temperature of the water used for washing is not limited, but the washing efficiency is improved when warm water is used as the washing water. The temperature of the warm water is not limited, but is usually 40° C. or higher, preferably 40 to 100° C., more preferably 50 to 90° C., and most preferably 60 to 80° C., since the washing efficiency can be significantly improved. By setting the temperature of the washing water to the above lower limit temperature or higher, the emulsifier and coagulant are released from the water-containing crumbs, and the washing efficiency is further improved.
[0135] The washing time is not limited, but is usually within the range of 1 to 120 minutes, preferably 2 to 60 minutes, and more preferably 3 to 30 minutes.
[0136] The number of times of washing with water is not particularly limited, and is usually 1 to 10 times, preferably multiple times, and more preferably 2 to 3 times. From the viewpoint of reducing the amount of residual coagulant in the finally obtained acrylic rubber veil, it is desirable to wash with water more frequently, but the number of times of washing can be significantly reduced by specifying the shape and diameter of the above-mentioned water-containing crumbs and / or setting the washing temperature within the above-mentioned range.
[0137] (Dehydration, drying, molding process) The above-mentioned (4) dehydrating / drying / molding step in the method for producing an acrylic rubber veil of the present invention is characterized in that the hydrous crumb washed in the above-mentioned (3) washing step is dehydrated in the dehydrating barrel using a dehydrating barrel having a dehydration slit, a drying barrel under reduced pressure, and a screw-type extruder having a die at the tip thereof to a moisture content of 1 to 40% by weight, and then dried in the drying barrel to a moisture content of less than 1% by weight, and a sheet-like dried rubber is extruded through the die.
[0138] In the present invention, the water-containing crumbs to be supplied to the screw-type extruder are preferably those from which free water has been removed (drained) after washing.
[0139] Draining process In the process for producing the acrylic rubber veil of the present invention, it is preferable to provide a draining step in which free water is separated from the washed wet crumbs by a drainer after the washing (water-rinsing) step (3) above and before the dehydration and drying steps described below, in order to increase the dehydration efficiency.
[0140] As the drainer, any known one can be used without any particular limitation, for example, a wire net, a screen, an electric sieve, etc., and preferably a wire net or a screen. The mesh size of the drainer is not limited, but is usually in the range of 0.01 to 5 mm, preferably 0.1 to 1 mm, more preferably 0.2 to 0.6 mm, which is suitable because it reduces the loss of water-containing crumb and allows efficient draining.
[0141] The moisture content of the hydrous crumbs after draining, i.e., the moisture content of the hydrous crumbs fed into the dehydration and drying process, is not limited, but is usually in the range of 50 to 80% by weight, preferably 50 to 70% by weight, and more preferably 50 to 60% by weight.
[0142] The temperature of the hydrous crumbs after draining, i.e., the temperature of the hydrous crumbs fed into the dehydration and drying step, is not limited, but is usually in the range of 40°C or higher, preferably 40 to 100°C, more preferably 50 to 90°C, particularly preferably 55 to 85°C, and most preferably 60 to 80°C, which is suitable because it allows efficient dehydration and drying of hydrous crumbs such as the acrylic rubber of the present invention, which has a high specific heat of 1.5 to 2.5 KJ / kg K and is difficult to raise in temperature, using a screw-type extruder.
[0143] Dehydration of crumbs (dehydration barrel section) The dehydration of the hydrous crumb is carried out in a dehydration barrel having a dehydration slit provided in a screw-type extruder. The opening of the dehydration slit may be appropriately selected depending on the conditions of use, but it is usually in the range of 0.01 to 5 mm, preferably 0.1 to 1 mm, more preferably 0.2 to 0.6 mm, which is suitable for minimizing hydrous crumb loss and efficiently dehydrating the hydrous crumb.
[0144] The number of dehydration barrels in the screw-type extruder is not limited, but it is generally suitable to have multiple barrels, preferably 2 to 10 barrels, and more preferably 3 to 6 barrels, since this allows efficient dehydration of the viscous acrylic rubber.
[0145] Water is removed from the wet crumb in the dewatering barrel in two ways: in liquid form (wastewater) through the dewatering slit, and in vapor form (exhaust steam). In the present invention, the wastewater is defined as dewatering, and the exhaust steam is defined as pre-drying, to distinguish between the two.
[0146] When using a screw-type extruder equipped with multiple dehydration barrels, a combination of drainage and exhaust steam can be used to efficiently dehydrate the viscous acrylic rubber, which is preferable.Whether each barrel of a screw-type extruder equipped with three or more dehydration barrels is a drainage type dehydration barrel or an exhaust steam type dehydration barrel can be selected appropriately depending on the purpose of use, but when the ash content in the acrylic rubber bale to be produced is reduced, the number of drainage type barrels is increased, and when the moisture content is reduced, the number of exhaust steam type barrels is increased.
[0147] The set temperature of the dehydration barrel is appropriately selected depending on the monomer composition of the acrylic rubber, the ash content, the water content of the crumbs, the operating conditions, etc., but is usually in the range of 60 to 150°C, preferably 70 to 140°C, and more preferably 80 to 130°C. The set temperature of the drainage type dehydration barrel in which dehydration is performed in a drainage state is usually in the range of 60 to 120°C, preferably 70 to 110°C, and more preferably 80 to 100°C. The set temperature of the exhaust steam type dehydration barrel in which dehydration is performed in an exhaust steam state is usually in the range of 100 to 150°C, preferably 105 to 140°C, and more preferably 110 to 130°C.
[0148] The moisture content after dehydration in a drainage type dehydration barrel that squeezes out moisture from the wet crumb is not limited, but is usually 1 to 40% by weight, preferably 5 to 40% by weight, more preferably 5 to 35% by weight, particularly preferably 10 to 35% by weight, and most preferably 15 to 35% by weight, which is suitable because it provides a high balance between productivity and efficiency of ash removal.
[0149] When dehydration of adhesive acrylic rubber having reactive groups is performed using a centrifuge, the acrylic rubber adheres to the dehydration slits and is hardly dehydrated, and the water content is reduced only to about 45 to 55% by weight. In contrast, in the present invention, the water content can be reduced to the above range by using, for example, a screw-type extruder having a dehydration slit and forcibly squeezed by a screw.
[0150] In the case where a drainage type dehydration barrel and a steam exhaust type dehydration barrel are provided, the moisture content after dehydration in the drainage type dehydration barrel is usually 5 to 40% by weight, preferably 10 to 35% by weight, and more preferably 15 to 35% by weight, and the moisture content after pre-drying in the steam exhaust type dehydration barrel is usually 1 to 30% by weight, preferably 3 to 20% by weight, and more preferably 5 to 15% by weight.
[0151] In the production method of the present invention, the moisture content of the crumbs after the dehydration step is set to 1 to 40% by weight as described above. By setting the moisture content at this stage to be equal to or above the above-mentioned lower limit, the dehydration time can be shortened and deterioration of the acrylic rubber can be suppressed, and by setting the moisture content to be equal to or below the above-mentioned upper limit, the ash content can be sufficiently reduced.
[0152] Drying of moist crumbs (drying barrel section) The dehydration of the hydrous crumbs is carried out in a drying barrel section under reduced pressure, which is provided downstream (closer to the die) of the dehydration barrel of the screw extruder. The degree of reduced pressure in the drying barrel may be appropriately selected, but is usually 1 to 50 kPa, preferably 2 to 30 kPa, and more preferably 3 to 20 kPa, which is suitable for efficiently drying the hydrous crumbs.
[0153] The set temperature of the drying barrel may be appropriately selected, but a temperature in the range of usually 100 to 250°C, preferably 110 to 200°C, and more preferably 120 to 180°C is suitable because it allows efficient drying without causing scorching or deterioration of the acrylic rubber and also reduces the amount of gel of the acrylic rubber that is insoluble in methyl ethyl ketone.
[0154] The number of drying barrels in the screw extruder is not limited, but is usually more than one, preferably 2 to 10, more preferably 3 to 8. When there are more than one drying barrel, the degree of vacuum may be similar for all drying barrels, or may be different. When there are more than one drying barrel, the set temperature may be similar for all drying barrels, or may be different, but it is preferable to set the temperature of the discharge part (closer to the die) higher than the temperature of the introduction part (closer to the dehydration barrel) of the crumbs, since this can increase the drying efficiency.
[0155] The water content of the dried rubber after drying is usually less than 1% by weight, preferably 0.8% by weight or less, and more preferably 0.6% by weight or less. In the present invention, it is particularly preferable to set the water content of the dried rubber to this value (a state in which almost all water has been removed) in a screw-type extruder before melt extrusion, since this reduces the amount of gel of the methyl ethyl ketone-insoluble portion of the acrylic rubber veil.
[0156] Shape of acrylic rubber (die part) The acrylic rubber dehydrated and dried in the screw section of the dehydrating barrel and the drying barrel is sent to the screw-free straightening die section. A breaker plate or wire mesh may or may not be provided between the screw section and the die section.
[0157] The dried rubber extruded from the die of the screw extruder is preferably produced in a sheet shape with a substantially rectangular die shape, which results in less air entrapment and a dried rubber with a high specific gravity and excellent storage stability. The resin pressure in the die is not particularly limited, but is preferably in the range of usually 0.1 to 10 MPa, preferably 0.5 to 5 MPa, and more preferably 1 to 3 MPa, which results in less air entrapment (high specific gravity) and excellent productivity.
[0158] Screw type extruder and operating conditions The screw length (L) of the screw extruder used may be appropriately selected depending on the intended use, but is usually in the range of 3,000 to 15,000 mm, preferably 4,000 to 10,000 mm, and more preferably 4,500 to 8,000 mm. The screw diameter (D) of the screw extruder may also be appropriately selected depending on the intended use, but is usually in the range of 50 to 250 mm, preferably 100 to 200 mm, and more preferably 120 to 160 mm.
[0159] The ratio (L / D) of the screw length (L) to the screw diameter (D) of the screw extruder is not limited, but is usually in the range of 10 to 100, preferably 20 to 80, more preferably 30 to 60, and particularly preferably 40 to 50, since this allows the moisture content to be reduced to less than 1% by weight without causing a decrease in the molecular weight of the dried rubber or discoloration.
[0160] The rotation speed (N) of the screw-type extruder may be appropriately selected depending on various conditions, but is usually suitable to be 10 to 1,000 rpm, preferably 50 to 750 rpm, more preferably 100 to 500 rpm, and most preferably 120 to 300 rpm, since this allows the water content of the acrylic rubber and the amount of gel of the methyl ethyl ketone-insoluble matter to be efficiently reduced.
[0161] The extrusion rate (Q) of the screw extruder is not limited, but is usually in the range of 100 to 1,500 kg / hr, preferably 300 to 1,200 kg / hr, more preferably 400 to 1,000 kg / hr, and most preferably 500 to 800 kg / hr. The ratio (Q / N) of the extrusion rate (Q) to the rotation speed (N) of the screw extruder is also not limited, but is usually in the range of 2 to 10, preferably 3 to 8, and more preferably 4 to 6, which is suitable since it provides a high balance between the quality, including the strength properties, of the obtained acrylic rubber veil and the production productivity.
[0162] Dry rubber sheet In the production method of the present invention, the dried rubber extruded from the screw extruder is in the form of a sheet, which is preferable because the specific gravity can be increased without entraining air during extrusion and the storage stability is highly improved. The sheet-like dried rubber extruded from the screw extruder in this manner is usually cooled and cut to be used as an acrylic rubber sheet.
[0163] The thickness of the sheet-like dry rubber extruded from the screw extruder is not particularly limited, but is preferably in the range of usually 1 to 40 mm, preferably 2 to 35 mm, more preferably 3 to 30 mm, and most preferably 5 to 25 mm, which is excellent in workability and productivity. In particular, when the thermal conductivity of the sheet-like dry rubber is as low as 0.15 to 0.35 W / mK and the cooling efficiency is increased to significantly improve the productivity, the thickness of the sheet-like dry rubber is usually in the range of 1 to 30 mm, preferably 2 to 25 mm, more preferably 3 to 15 mm, and particularly preferably 4 to 12 mm.
[0164] The width of the sheet-like dry rubber extruded from the screw extruder is appropriately selected depending on the intended use, but is usually in the range of 300 to 1,200 mm, preferably 400 to 1,000 mm, and more preferably 500 to 800 mm.
[0165] The temperature of the dried rubber extruded from the screw extruder is not limited, but is usually in the range of 100 to 200°C, preferably 110 to 180°C, and more preferably 120 to 160°C.
[0166] The water content of the dry rubber extruded from the screw-type extruder is usually less than 1% by weight, preferably 0.8% by weight or less, and more preferably 0.6% by weight or less.
[0167] The complex viscosity at 100°C of the dry rubber sheet extruded from the screw extruder ([η]100°C) is not limited, but is usually in the range of 1,500 to 6,000 Pa·s, preferably 2,000 to 5,000 Pa·s, more preferably 2,500 to 4,000 Pa·s, and most preferably 2,500 to 3,500 Pa·s, which is suitable since it provides a high balance between extrudability as a sheet and shape retention. That is, by setting the complex viscosity ([η]100°C) to be equal to or higher than the above lower limit, the extrudability can be made superior, and by setting it to be equal to or lower than the above upper limit, deformation or breakage of the dry rubber sheet can be suppressed.
[0168] In the present invention, the dry rubber sheet extruded from the screw extruder is preferably cut and then laminated to form a bale, which results in less air being entrained and excellent storage stability. There are no limitations on the method for cutting the dry rubber sheet, but since the acrylic rubber in the acrylic rubber bale of the present invention has strong adhesion, it is preferable to cut the dry rubber sheet after cooling it in order to cut it continuously without entraining air.
[0169] The cutting temperature of the dry rubber sheet is not limited, but a temperature of usually 60° C. or less, preferably 55° C. or less, and more preferably 50° C. or less provides a high balance between cuttability and productivity, and is therefore suitable.
[0170] The complex viscosity of the dry rubber sheet at 60°C ([η]60°C) is not limited, but is usually 15,000 Pa·s or less, preferably 2,000 to 10,000 Pa·s, more preferably 2,500 to 7,000 Pa·s, and most preferably 2,700 to 5,500 Pa·s, which is suitable for enabling continuous cutting without entraining air.
[0171] The ratio ([η]100°C / [η]60°C) of the complex viscosity of the dry rubber sheet at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) is not limited, but is usually 0.5 or more, preferably 0.5 to 0.98, more preferably 0.6 to 0.95, and most preferably 0.75 to 0.93, which is suitable because it reduces air entrapment and provides a high balance between cutting and productivity.
[0172] The cooling method of the dry rubber sheet is not limited, and the sheet may be cooled by leaving it at room temperature. However, since the thermal conductivity of the dry rubber sheet is very low at 0.15 to 0.35 W / mK, forced cooling such as air cooling using blowing air or cooling, water spraying by spraying water, or immersion in water is preferred in order to increase productivity, and air cooling using blowing air or cooling is particularly preferred.
[0173] In the air-cooling method of the sheet-like dry rubber, for example, the sheet-like dry rubber is extruded from a screw-type extruder onto a conveyor such as a belt conveyor, and conveyed and cooled while blowing cold air. The temperature of the cold air is not limited, but is usually in the range of 0 to 25°C, preferably 5 to 25°C, and more preferably 10 to 20°C. The length to be cooled is not particularly limited, but is usually in the range of 5 to 500m, preferably 10 to 200m, and more preferably 20 to 100m. The cooling rate of the sheet-like dry rubber is not limited, but is usually 50°C / hr or more, more preferably 100°C / hr or more, and more preferably 150°C / hr or more, which is particularly easy to cut and is therefore suitable.
[0174] The cutting length of the dry rubber sheet is not limited and may be appropriately selected according to the size of the acrylic rubber bale to be produced, but is usually in the range of 100 to 800 mm, preferably 200 to 500 mm, and more preferably 250 to 450 mm.
[0175] (Baling process) The baling step (5) in the method for producing an acrylic rubber bale of the present invention is, for example, a step of laminating and integrating dry rubber sheets to form a bale.
[0176] The lamination temperature for the dry rubber sheet is not limited, but is usually 30° C. or higher, preferably 35° C. or higher, and more preferably 40° C. or higher, so that air entrapped during lamination can be efficiently released. The number of layers may be appropriately selected depending on the size or weight of the acrylic rubber veil.
[0177] The acrylic rubber veil of the present invention thus obtained is easier to handle and has better storage stability than crumb-like acrylic rubber, and the acrylic rubber veil can be fed directly into a mixer such as a Banbury mixer or roll mixer, or can be cut into the required amount.
[0178] <Rubber mixture> The rubber mixture of the present invention is characterized by being obtained by mixing the above-mentioned acrylic rubber veil with a filler and a crosslinking agent.
[0179] The filler used in the rubber mixture is not limited, but may be, for example, a reinforcing filler or a non-reinforcing filler, with a reinforcing filler being preferred.
[0180] Examples of such reinforcing fillers include carbon blacks such as furnace black, acetylene black, thermal black, channel black, and graphite; silicas such as wet silica, dry silica, and colloidal silica; etc. Examples of the non-reinforcing fillers include quartz powder, diatomaceous earth, zinc oxide, basic magnesium carbonate, activated calcium carbonate, magnesium silicate, aluminum silicate, titanium dioxide, talc, aluminum sulfate, calcium sulfate, barium sulfate, etc.
[0181] These fillers can be used alone or in combination of two or more kinds. The amount of the filler to be blended is not particularly limited, but is usually 1 to 200 parts by weight, preferably 10 to 150 parts by weight, and more preferably 20 to 100 parts by weight, per 100 parts by weight of the acrylic rubber veil.
[0182] The crosslinking agent used in the rubber mixture may be appropriately selected according to the type of reactive group contained in the acrylic rubber constituting the acrylic rubber veil and the purpose, but is not particularly limited as long as it can crosslink the acrylic rubber veil, and for example, conventionally known crosslinking agents such as polyamine compounds such as diamine compounds and carbonates thereof, sulfur compounds, sulfur donors, triazine thiol compounds, polyepoxy compounds, organic ammonium carboxylate salts, organic peroxides, polycarboxylic acids, quaternary onium salts, imidazole compounds, isocyanuric acid compounds, organic peroxides, and triazine compounds can be used. Among these, polyamine compounds, ammonium carboxylate salts, metal dithiocarbamate salts, and triazine thiol compounds are preferred, and hexamethylenediamine carbamate, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, ammonium benzoate, and 2,4,6-trimercapto-1,3,5-triazine are particularly preferred.
[0183] When the acrylic rubber veil used is composed of a carboxyl group-containing acrylic rubber, it is preferable to use a polyamine compound or a carbonate thereof as the crosslinking agent. Examples of the polyvalent amine compound include aliphatic polyvalent amine compounds such as hexamethylenediamine, hexamethylenediamine carbamate, and N,N'-dicinnamylidene-1,6-hexanediamine; and aromatic polyvalent amine compounds such as 4,4'-methylenedianiline, p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-(m-phenylenediisopropylidene)dianiline, 4,4'-(p-phenylenediisopropylidene)dianiline, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-diaminobenzanilide, 4,4'-bis(4-aminophenoxy)biphenyl, m-xylylenediamine, p-xylylenediamine, and 1,3,5-benzenetriamine. Among these, hexamethylenediamine carbamate, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, and the like are preferred.
[0184] When the acrylic rubber veil used is composed of an epoxy group-containing acrylic rubber, examples of the crosslinking agent that can be used include aliphatic polyamine compounds and carbonates thereof, such as hexamethylenediamine and hexamethylenediamine carbamate; aromatic polyamine compounds, such as 4,4'-methylenedianiline; ammonium carboxylates, such as ammonium benzoate and ammonium adipate; metal dithiocarbamate salts, such as zinc dimethyldithiocarbamate; polycarboxylic acids, such as tetradecanedioic acid; quaternary onium salts, such as cetyltrimethylammonium bromide; imidazole compounds, such as 2-methylimidazole; and isocyanuric acid compounds, such as ammonium isocyanurate. Of these, ammonium carboxylates and metal dithiocarbamate salts are preferred, with ammonium benzoate being more preferred.
[0185] When the acrylic rubber veil used is composed of a halogen-containing acrylic rubber, it is preferable to use sulfur, a sulfur donor, or a triazine thiol compound as a crosslinking agent. Examples of sulfur donors include dipentamethylene thiuram hexasulfide and triethyl thiuram disulfide. Examples of triazine compounds include 6-trimercapto-s-triazine, 2-anilino-4,6-dithiol-s-triazine, 1-dibutylamino-3,5-dimercaptotriazine, 2-dibutylamino-4,6-dithiol-s-triazine, 1-phenylamino-3,5-dimercaptotriazine, 2,4,6-trimercapto-1,3,5-triazine, and 1-hexylamino-3,5-dimercaptotriazine, and among these, 2,4,6-trimercapto-1,3,5-triazine is preferred.
[0186] These crosslinking agents can be used alone or in combination of two or more, and the amount of the crosslinking agent is usually 0.001 to 20 parts by weight, preferably 0.1 to 10 parts by weight, and more preferably 0.1 to 5 parts by weight, per 100 parts by weight of the acrylic rubber veil. By setting the amount of the crosslinking agent within this range, it is possible to obtain excellent mechanical strength as a crosslinked rubber product while ensuring sufficient rubber elasticity, which is preferable.
[0187] The rubber mixture of the present invention may contain, as a rubber component, the above-mentioned acrylic rubber veil, as well as other rubber components as required.
[0188] Other rubber components that are blended as necessary are not particularly limited, and examples thereof include natural rubber, polybutadiene rubber, polyisoprene rubber, styrene-butadiene rubber, acrylonitrile-butadiene rubber, silicone rubber, fluororubber, olefin-based elastomer, styrene-based elastomer, vinyl chloride-based elastomer, polyester-based elastomer, polyamide-based elastomer, polyurethane-based elastomer, polysiloxane-based elastomer, etc. The shape of the other rubber components is not limited, and may be, for example, any of powder, crumb, sheet, veil, etc.
[0189] These other rubber components may be used alone or in combination of two or more kinds. The amount of these other rubber components used is appropriately selected within a range that does not impair the effects of the present invention.
[0190] The rubber mixture of the present invention may contain an antioxidant as required. Examples of the antioxidant include, but are not limited to, 2,6-di-t-butyl-4-methylphenol, 2,6-di-t-butylphenol, butylhydroxyanisole, 2,6-di-t-butyl-α-dimethylamino-p-cresol, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, styrenated phenol, 2,2'-methylene-bis(6-α-methyl-benzyl-p-cresol), 4,4'-methylenebis( Other phenols such as 2,6-di-t-butylphenol), 2,2'-methylene-bis(4-methyl-6-t-butylphenol), 2,4-bis[(octylthio)methyl]-6-methylphenol, 2,2'-thiobis-(4-methyl-6-t-butylphenol), 4,4'-thiobis-(6-t-butyl-o-cresol), 2,6-di-t-butyl-4-(4,6-bis(octylthio)-1,3,5-triazin-2-ylamino)phenol, Phenolic antioxidants; phosphorous ester antioxidants such as tris(nonylphenyl)phosphite, diphenylisodecylphosphite, and tetraphenyldipropylene glycol diphosphite; sulfur ester antioxidants such as dilauryl thiodipropionate; phenyl-α-naphthylamine, phenyl-β-naphthylamine, p-(p-toluenesulfonylamido)-diphenylamine, and 4,4'-(α,α-dimethylbenzyl)diphenylamine. Examples of such antioxidants include amine-based antioxidants such as butyl aldehyde, N,N-diphenyl-p-phenylenediamine, N-isopropyl-N'-phenyl-p-phenylenediamine, and butyraldehyde-aniline condensates; imidazole-based antioxidants such as 2-mercaptobenzimidazole; quinoline-based antioxidants such as 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline; and hydroquinone-based antioxidants such as 2,5-di-(t-amyl)hydroquinone. Among these, amine-based antioxidants are particularly preferred.
[0191] These antioxidants can be used alone or in combination of two or more. The amount of the antioxidant to be added is in the range of 0.01 to 15 parts by weight, preferably 0.1 to 10 parts by weight, and more preferably 1 to 5 parts by weight, per 100 parts by weight of the acrylic rubber veil.
[0192] The rubber mixture of the present invention contains the acrylic rubber veil of the present invention, a filler, a crosslinking agent, and if necessary, other rubber components and antiaging agents, and further, if necessary, other additives normally used in the technical field can be arbitrarily blended, such as crosslinking aids, crosslinking accelerators, crosslinking retarders, silane coupling agents, plasticizers, processing aids, lubricants, pigments, colorants, antistatic agents, foaming agents, etc. These other compounding agents can be used alone or in combination of two or more, and the amount of each compounded is appropriately selected within a range that does not impair the effects of the present invention.
[0193] <Method of manufacturing rubber mixture> The method for producing the rubber mixture of the present invention includes a method in which the acrylic rubber veil of the present invention is mixed with a filler, a crosslinking agent, and other compounding ingredients that can be contained as necessary, and any means conventionally used in the field of rubber processing can be used to mix the components, such as an open roll, a Banbury mixer, various kneaders, etc. That is, the acrylic rubber veil can be directly mixed with the filler, the crosslinking agent, etc., using these mixers, and preferably mixed by direct kneading.
[0194] In this case, the acrylic rubber veil of the present invention may be used in the form of a veil obtained, or may be divided (cut, etc.) before use.
[0195] The mixing procedure of each component is not limited, but for example, two-stage mixing is preferred in which components that do not easily react or decompose when heated are thoroughly mixed, and then components that easily react or decompose when heated, such as crosslinking agents, are mixed for a short time at a temperature at which they do not react or decompose. Specifically, it is preferred to mix the acrylic rubber veil and filler in the first stage, and then mix the crosslinking agent in the second stage. Other rubber components and antioxidants are usually mixed in the first stage, the crosslinking accelerator in the second stage, and other compounding agents may be selected as appropriate.
[0196] The Mooney viscosity (ML1+4, 100° C.; compound Mooney) of the rubber mixture of the present invention thus obtained is not limited, but is usually in the range of 10-150, preferably 20-100, more preferably 25-80.
[0197] <Rubber cross-linked products> The cross-linked rubber product of the present invention is obtained by cross-linking the above-mentioned rubber mixture. The cross-linked rubber product of the present invention can be produced by using the rubber mixture of the present invention, molding it into a desired shape using a molding machine such as an extruder, an injection molding machine, a compressor, a roll, etc., and heating it to cause a cross-linking reaction, and fixing the shape as a cross-linked rubber product.
[0198] In this case, crosslinking may be performed after molding in advance, or simultaneously with molding. The molding temperature is usually 10 to 200°C, preferably 25 to 150°C. The crosslinking temperature is usually 100 to 250°C, preferably 130 to 220°C, more preferably 150 to 200°C, and the crosslinking time is usually 0.1 minutes to 10 hours, preferably 1 minute to 5 hours. The heating method may be appropriately selected from methods used for crosslinking rubber, such as press heating, steam heating, oven heating, and hot air heating.
[0199] The cross-linked rubber of the present invention may be further heated to carry out secondary cross-linking depending on the shape, size, etc. of the cross-linked rubber. The secondary cross-linking is preferably carried out for 1 to 48 hours, although it varies depending on the heating method, cross-linking temperature, shape, etc. The heating method and heating temperature may be appropriately selected.
[0200] The cross-linked rubber of the present invention has excellent water resistance while maintaining basic rubber properties such as tensile strength, elongation, and hardness.
[0201] Taking advantage of the above-mentioned excellent properties, the cross-linked rubber product of the present invention can be suitably used for, for example, sealing materials such as O-rings, packings, diaphragms, oil seals, shaft seals, bearing sheaths, mechanical seals, well head seals, seals for electric and electronic devices, and seals for air compressors; various gaskets such as a rocker cover gasket attached to the joint between a cylinder block and a cylinder head, an oil pan gasket attached to the joint between an oil pan and a cylinder head or a transmission case, a gasket for a fuel cell separator attached between a pair of housings sandwiching a unit cell having a positive electrode, an electrolyte plate, and a negative electrode, and a gasket for the top cover of a hard disk drive; cushioning materials, vibration-proofing materials; wire covering materials; industrial belts; tubes and hoses; sheets; and the like.
[0202] The cross-linked rubber product of the present invention can also be suitably used as an extrusion molded product and a mold cross-linked product for automotive applications, for example, various hoses such as fuel oil hoses around fuel tanks, such as fuel hoses, filler neck hoses, vent hoses, paper hoses and oil hoses, air hoses such as turbo air hoses and mission control hoses, radiator hoses, heater hoses, brake hoses and air conditioner hoses.
[0203] <Device configuration used in the production of acrylic rubber veils> Next, the configuration of the equipment used in the production of the acrylic rubber veil according to one embodiment of the present invention will be described. Fig. 1 is a diagram showing a schematic diagram of an example of an acrylic rubber production system having an equipment configuration used in the production of the acrylic rubber veil according to one embodiment of the present invention. For example, the acrylic rubber production system 1 shown in Fig. 1 can be used to produce the acrylic rubber according to the present invention.
[0204] The acrylic rubber production system 1 shown in FIG. 1 is composed of an emulsion polymerization reactor, a coagulation device 3, a washing device 4, a draining machine 43, a screw-type extruder 5, a cooling device 6, and a baling device 7, all of which are not shown.
[0205] The emulsion polymerization reactor is configured to carry out the treatment related to the emulsion polymerization step described above. Although not shown in FIG. 1, this emulsion polymerization reactor has, for example, a polymerization reaction tank, a temperature control unit for controlling the reaction temperature, and a stirring device equipped with a motor and a stirring blade. In the emulsion polymerization reactor, the monomer components for forming the acrylic rubber are mixed with water and an emulsifier, emulsified while being appropriately stirred with a stirrer, and emulsion-polymerized in the presence of a polymerization catalyst to obtain an emulsion polymerization liquid. The emulsion polymerization reactor may be any of a batch type, a semi-batch type, and a continuous type, and may be any of a tank type reactor and a tubular type reactor.
[0206] The solidification device 3 shown in Fig. 1 is configured to perform the above-mentioned solidification process. As shown in Fig. 1, the solidification device 3 has, for example, a stirring tank 30, a heating unit 31 for heating the inside of the stirring tank 30, a temperature control unit (not shown) for controlling the temperature inside the stirring tank 30, a stirring device 34 equipped with a motor 32 and a stirring blade 33, and a drive control unit (not shown) for controlling the number of revolutions and the rotation speed of the stirring blade 33. In the solidification device 3, the emulsion polymerization liquid obtained in the emulsion polymerization reactor is brought into contact with a coagulation liquid as a coagulant and solidified to produce water-containing crumbs.
[0207] In the coagulation device 3, for example, the emulsion polymerization liquid is brought into contact with the coagulation liquid by adding the emulsion polymerization liquid to the coagulation liquid being stirred. That is, the stirring tank 30 of the coagulation device 3 is filled with the coagulation liquid, and the emulsion polymerization liquid is added to and brought into contact with the coagulation liquid to coagulate the emulsion polymerization liquid, thereby generating water-containing crumbs.
[0208] The heating unit 31 of the solidification device 3 is configured to heat the solidification liquid filled in the stirring tank 30. The temperature control unit of the solidification device 3 is configured to control the heating operation by the heating unit 31 while monitoring the temperature in the stirring tank 30 measured by a thermometer, thereby controlling the temperature in the stirring tank 30. The temperature of the solidification liquid in the stirring tank 30 is controlled by the temperature control unit to be usually 40°C or higher, preferably in the range of 40 to 90°C, and more preferably 50 to 80°C.
[0209] The agitator 34 of the solidification device 3 is configured to agitate the solidification liquid filled in the agitation tank 30. Specifically, the agitator 34 includes a motor 32 that generates rotational power, and an agitator blade 33 that spreads in a direction perpendicular to the rotation axis of the motor 32. The agitator blade 33 can cause the solidification liquid filled in the agitation tank 30 to flow by rotating around the rotation axis by the rotational power of the motor 32. The shape, size, and number of the agitator blades 33 to be installed are not particularly limited.
[0210] The drive control unit of the solidification device 3 is configured to control the rotation drive of the motor 32 of the agitation device 34 to set the number of rotations and the rotation speed of the agitation blade 33 of the agitation device 34 to a predetermined value. The rotation of the agitation blade 33 is controlled by the drive control unit so that the agitation speed of the solidification liquid is, for example, usually 100 rpm or more, preferably 200 to 1,000 rpm, more preferably 300 to 900 rpm, and particularly preferably 400 to 800 rpm. The rotation of the agitation blade 33 is controlled by the drive control unit so that the peripheral speed of the solidification liquid is usually 0.5 m / s or more, preferably 1 m / s or more, more preferably 1.5 m / s or more, particularly preferably 2 m / s or more, and most preferably 2.5 m / s or more. Furthermore, the rotation of the agitation blade 33 is controlled by the drive control unit so that the upper limit of the peripheral speed of the solidification liquid is usually 50 m / s or less, preferably 30 m / s or less, more preferably 25 m / s or less, and most preferably 20 m / s or less.
[0211] The washing device 4 shown in Fig. 1 is configured to perform the treatment related to the washing step described above. As shown in Fig. 1, the washing device 4 has, for example, a washing tank 40, a heating unit 41 that heats the inside of the washing tank 40, and a temperature control unit (not shown) that controls the temperature inside the washing tank 40. In the washing device 4, the water-containing crumbs generated in the solidifying device 3 are mixed with a large amount of water and washed, thereby effectively reducing the amount of ash in the finally obtained acrylic rubber veil.
[0212] The heating unit 41 of the cleaning device 4 is configured to heat the inside of the cleaning tank 40. The temperature control unit of the cleaning device 4 is configured to control the heating operation by the heating unit 41 while monitoring the temperature inside the cleaning tank 40 measured by a thermometer, thereby controlling the temperature inside the cleaning tank 40. As described above, the temperature of the cleaning water inside the cleaning tank 40 is controlled to be usually in the range of 40°C or higher, preferably 40 to 100°C, more preferably 50 to 90°C, and most preferably 60 to 80°C.
[0213] The water-containing crumb washed in the washing device 4 is supplied to a screw-type extruder 5 which performs a dehydration step and a drying step. At this time, the water-containing crumb after washing is preferably supplied to the screw-type extruder 5 through a drainer 43 capable of separating free water. For the drainer 43, for example, a wire net, a screen, an electric sieve, or the like can be used.
[0214] In addition, when the washed wet crumbs are supplied to the screw-type extruder 5, the temperature of the wet crumbs is preferably 40° C. or higher, more preferably 60° C. or higher. For example, the temperature of the water used for washing in the washing device 4 may be set to 60° C. or higher (e.g., 70° C.) so that the temperature of the wet crumbs when supplied to the screw-type extruder 5 can be maintained at 60° C. or higher, or the wet crumbs may be heated to a temperature of 40° C. or higher, preferably 60° C. or higher, when conveyed from the washing device 4 to the screw-type extruder 5. This makes it possible to effectively perform the subsequent dehydration and drying steps, and to significantly reduce the moisture content of the finally obtained dried rubber.
[0215] The screw-type extruder 5 shown in Fig. 1 is configured to perform the processes related to the dehydration step and the drying step described above. Although the screw-type extruder 5 is shown in Fig. 1 as a suitable example, a centrifuge or a squeezer may be used as a dehydrator that performs the process related to the dehydration step, and a hot air dryer, a reduced pressure dryer, an expander dryer, a kneader dryer, etc. may be used as a dryer that performs the process related to the drying step.
[0216] The screw-type extruder 5 is configured to mold the dried rubber obtained through the dehydration process and the drying process into a predetermined shape and discharge it. Specifically, the screw-type extruder 5 is equipped with a dehydration barrel section 53 having a function as a dehydrator for dehydrating the wet crumbs washed in the washing device 4, and a drying barrel section 54 having a function as a dryer for drying the wet crumbs, and further equipped with a die 59 downstream of the screw-type extruder 5 having a molding function for molding the wet crumbs.
[0217] Hereinafter, the configuration of the screw-type extruder 5 will be described with reference to Fig. 2. Fig. 2 shows the configuration of a specific example suitable for the screw-type extruder 5 shown in Fig. 1. By using this screw-type extruder 5, the above-mentioned dehydration and drying process can be suitably carried out.
[0218] The screw-type extruder 5 shown in Fig. 2 is a twin-screw type extrusion dryer having a pair of screws (not shown) in a barrel unit 51. The screw-type extruder 5 has a drive unit 50 that rotates and drives the pair of screws in the barrel unit 51. The drive unit 50 is attached to the upstream end (left end in Fig. 2) of the barrel unit 51. The screw-type extruder 5 also has a die 59 at the downstream end (right end in Fig. 2) of the barrel unit 51.
[0219] The barrel unit 51 has, from the upstream side to the downstream side (from the left side to the right side in FIG. 2), a supply barrel section 52, a dewatering barrel section 53, and a drying barrel section .
[0220] The supply barrel section 52 is made up of two supply barrels, that is, a first supply barrel 52a and a second supply barrel 52b.
[0221] The dehydration barrel section 53 is made up of three dehydration barrels, that is, a first dehydration barrel 53a, a second dehydration barrel 53b, and a third dehydration barrel 53c.
[0222] The drying barrel section 54 is composed of eight drying barrels, namely, a first drying barrel 54a, a second drying barrel 54b, a third drying barrel 54c, a fourth drying barrel 54d, a fifth drying barrel 54e, a sixth drying barrel 54f, a seventh drying barrel 54g, and an eighth drying barrel 54h.
[0223] In this manner, the barrel unit 51 is configured by connecting the divided 13 barrels 52a to 52b, 53a to 53c, and 54a to 54h from the upstream side to the downstream side.
[0224] The screw-type extruder 5 also has heating means (not shown) for individually heating each of the barrels 52a to 52b, 53a to 53c, and 54a to 54h to heat the water-containing crumbs in each of the barrels 52a to 52b, 53a to 53c, and 54a to 54h to a predetermined temperature. The number of heating means corresponds to each of the barrels 52a to 52b, 53a to 53c, and 54a to 54h. As such a heating means, for example, a configuration in which high-temperature steam is supplied from a steam supply means to a steam circulation jacket formed in each of the barrels 52a to 52b, 53a to 53c, and 54a to 54h is adopted, but is not limited thereto. The screw-type extruder 5 also has temperature control means (not shown) for controlling the set temperature of each heating means corresponding to each of the barrels 52a to 52b, 53a to 53c, and 54a to 54h.
[0225] The number of supply barrels, dewatering barrels, and drying barrels constituting each of barrel portions 52, 53, and 54 in barrel unit 51 is not limited to the embodiment shown in FIG. 2, and can be set to a number depending on factors such as the moisture content of the moisture-containing acrylic rubber crumbs to be dried.
[0226] For example, the number of supply barrels installed in supply barrel section 52 is, for example, 1 to 3. The number of dehydration barrels installed in dehydration barrel section 53 is, for example, preferably 2 to 10, and more preferably 3 to 6, since this allows efficient dehydration of the water-containing crumbs of sticky acrylic rubber. The number of drying barrels installed in drying barrel section 54 is, for example, preferably 2 to 10, and more preferably 3 to 8.
[0227] The pair of screws in the barrel unit 51 are rotated by a driving means such as a motor housed in the drive unit 50. The pair of screws extend from the upstream side to the downstream side in the barrel unit 51, and are rotated to convey the wet crumb supplied to the supply barrel section 52 to the downstream side while mixing them. The pair of screws is preferably a twin-shaft intermeshing type in which the peaks and valleys are intermeshed with each other, which can increase the dewatering and drying efficiency of the wet crumb.
[0228] The rotation directions of the pair of screws may be the same or different, but from the viewpoint of self-cleaning performance, it is preferable that the screws rotate in the same direction. The screw shape of the pair of screws is not particularly limited as long as it is a shape required for each of the barrel portions 52, 53, and 54.
[0229] The supply barrel section 52 is a region for supplying the wet crumbs into the barrel unit 51. The first supply barrel 52a of the supply barrel section 52 has a feed port 55 for supplying the wet crumbs into the barrel unit 51.
[0230] The dewatering barrel section 53 is a region where liquid (serum water) containing a coagulant and the like is separated from the water-containing crumbs and discharged.
[0231] The first to third dewatering barrels 53a to 53c constituting the dewatering barrel section 53 each have a dewatering slit 56a, 56b, 56c for discharging moisture from the wet crumb to the outside. A plurality of dewatering slits 56a, 56b, 56c are formed in each of the dewatering barrels 53a to 53c.
[0232] The slit width, i.e., mesh size, of each dewatering slit 56a, 56b, 56c may be appropriately selected depending on the conditions of use, and is typically 0.01 to 5 mm. From the viewpoints of minimizing loss of moist crumb and enabling efficient dewatering of the moist crumb, the width is preferably 0.1 to 1 mm, and more preferably 0.2 to 0.6 mm.
[0233] The removal of moisture from the wet crumb in each of the dehydration barrels 53a to 53c of the dehydration barrel section 53 can be done in two ways: in liquid form through the dehydration slits 56a, 56b, and 56c, and in vapor form. In the dehydration barrel section 53 of this embodiment, the removal of moisture in liquid form is defined as drainage, and the removal of moisture in vapor form is defined as exhaust steam, and are distinguished between these.
[0234] In the dehydration barrel section 53, the combination of drainage and exhaust steam is suitable because it can efficiently reduce the moisture content of the viscous acrylic rubber. In the dehydration barrel section 53, which of the first to third dehydration barrels 53a to 53c is used for drainage or steam exhaust may be appropriately set according to the purpose of use, but when the amount of ash in the acrylic rubber to be produced is usually reduced, it is preferable to increase the number of dehydration barrels for drainage. In that case, for example, as shown in FIG. 2, drainage is performed in the first and second dehydration barrels 53a and 53b on the upstream side, and steam exhaust is performed in the third dehydration barrel 53c on the downstream side. In addition, for example, when the dehydration barrel section 53 has four dehydration barrels, it is possible to consider an embodiment in which drainage is performed in three dehydration barrels on the upstream side and steam exhaust is performed in one dehydration barrel on the downstream side. On the other hand, when the moisture content is reduced, it is preferable to increase the number of dehydration barrels for steam exhaust.
[0235] As described above in the dehydrating / drying process, the set temperature of the dehydrating barrel section 53 is usually in the range of 60 to 150°C, preferably 70 to 140°C, and more preferably 80 to 130°C. The set temperature of the dehydrating barrel for dehydrating in a drainage state is usually in the range of 60 to 120°C, preferably 70 to 110°C, and more preferably 80 to 100°C. The set temperature of the dehydrating barrel for dehydrating in an exhaust steam state is usually in the range of 100 to 150°C, preferably 105 to 140°C, and more preferably 110 to 130°C.
[0236] The drying barrel section 54 is a region where the dehydrated water-containing crumbs are dried under reduced pressure. Among the first to eighth drying barrels 54a to 54h constituting the drying barrel section 54, the second drying barrel 54b, the fourth drying barrel 54d, the sixth drying barrel 54f and the eighth drying barrel 54h each have a vent port 58a, 58b, 58c, 58d for degassing. The vent ports 58a, 58b, 58c, 58d are each connected to a vent pipe (not shown).
[0237] A vacuum pump (not shown) is connected to the end of each vent pipe, and the pressure inside the drying barrel portion 54 is reduced to a predetermined level by operation of the vacuum pumps. The screw-type extruder 5 has a pressure control means (not shown) that controls the operation of the vacuum pumps to control the degree of reduced pressure inside the drying barrel portion 54.
[0238] The degree of reduced pressure in the drying barrel section 54 may be appropriately selected, but as described above, it is usually set to 1 to 50 kPa, preferably 2 to 30 kPa, and more preferably 3 to 20 kPa.
[0239] The temperature set within the drying barrel section 54 may be appropriately selected, but as described above, it is usually set to 100 to 250°C, preferably 110 to 200°C, and more preferably 120 to 180°C.
[0240] In each of the drying barrels 54a to 54h that make up the drying barrel section 54, the set temperatures in all of the drying barrels 54a to 54h may be similar or different, but it is preferable to set the temperature on the downstream side (die 59 side) higher than the temperature on the upstream side (dehydration barrel section 53 side), as this improves drying efficiency.
[0241] The die 59 is a metal mold disposed at the downstream end of the barrel unit 51, and has an outlet of a predetermined nozzle shape. The acrylic rubber dried in the drying barrel section 54 passes through the outlet of the die 59, and is extruded into a shape corresponding to the predetermined nozzle shape. The acrylic rubber passing through the die 59 is molded into various shapes, such as granular, columnar, round rod, and sheet, depending on the nozzle shape of the die 59. For example, the acrylic rubber can be extruded into a sheet by forming the outlet of the die 59 into a substantially rectangular shape. A breaker plate or a wire mesh may or may not be provided between the screw and the die 59.
[0242] According to the screw-type extruder 5 of this embodiment, the water-containing crumbs of the raw acrylic rubber are extruded into a sheet-like dry rubber in the following manner.
[0243] The hydrous crumbs of the acrylic rubber obtained through the washing process are supplied to the supply barrel section 52 from the feed port 55. The hydrous crumbs supplied to the supply barrel section 52 are transferred from the supply barrel section 52 to the dehydration barrel section 53 by the rotation of the pair of screws in the barrel unit 51. In the dehydration barrel section 53, the hydrous crumbs are dehydrated by draining water contained in the hydrous crumbs and discharging steam from the dehydration slits 56a, 56b, and 56c provided in the first to third dehydration barrels 53a to 53c, respectively, as described above.
[0244] The water-containing crumbs dewatered in the dewatering barrel section 53 are sent to the drying barrel section 54 by the rotation of a pair of screws in the barrel unit 51. The water-containing crumbs sent to the drying barrel section 54 are plasticized and mixed to become a melt, and are transported downstream while generating heat and increasing in temperature. Then, the water contained in the acrylic rubber melt vaporizes, and the water (steam) is discharged to the outside through vent pipes (not shown) connected to each of the vent ports 58a, 58b, 58c, and 58d.
[0245] As described above, by passing through the drying barrel section 54, the water-containing crumb is dried and becomes a molten acrylic rubber. The acrylic rubber is supplied to the die 59 by the rotation of the pair of screws in the barrel unit 51 and is extruded from the die 59 as a sheet-like dried rubber.
[0246] Here, an example of operating conditions for the screw-type extruder 5 according to this embodiment will be given.
[0247] The rotation speed (N) of the pair of screws in barrel unit 51 may be appropriately selected depending on various conditions, and is usually set to 10 to 1,000 rpm. From the viewpoint of efficiently reducing the water content and gel amount in the acrylic rubber veil, it is preferably 50 to 750 rpm, more preferably 100 to 500 rpm, and most preferably 120 to 300 rpm.
[0248] The extrusion rate (Q) of the acrylic rubber is not particularly limited, but is usually 100 to 1,500 kg / hr, preferably 300 to 1,200 kg / hr, more preferably 400 to 1,000 kg / hr, and most preferably 500 to 800 kg / hr.
[0249] In addition, the ratio (Q / N) of the extrusion amount (Q) of the acrylic rubber to the screw rotation speed (N) is not particularly limited, but is usually 1 to 20, preferably 2 to 10, more preferably 3 to 8, and particularly preferably 4 to 6.
[0250] The cooling device 6 shown in Fig. 1 is configured to cool the dried rubber obtained through the dehydration process using a dehydrator and the drying process using a dryer. As a cooling method using the cooling device 6, various methods can be adopted, including an air-cooling method using blowing air or air conditioning, a water-spraying method in which water is sprayed, and an immersion method in which the rubber is immersed in water. The dried rubber may also be cooled by leaving it at room temperature.
[0251] As described above, the dry rubber discharged from the screw-type extruder 5 is extruded and molded into various shapes such as granules, columns, round rods, sheets, etc., depending on the nozzle shape of the die 59. Hereinafter, a conveying type cooling device 60 that cools the sheet-shaped dry rubber 10 molded into a sheet will be described as an example of the cooling device 6 with reference to Fig. 3.
[0252] Fig. 3 shows the configuration of a conveyor-type cooling device 60 suitable for use as the cooling device 6 shown in Fig. 1. The conveyor-type cooling device 60 shown in Fig. 3 is configured to cool the sheet-like dry rubber 10 discharged from the discharge port of the die 59 of the screw-type extruder 5 by air cooling while conveying the sheet-like dry rubber 10. By using this conveyor-type cooling device 60, the sheet-like dry rubber discharged from the screw-type extruder 5 can be suitably cooled.
[0253] The conveying cooling device 60 shown in FIG. 3 is used by being directly connected to the die 59 of the screw-type extruder 5 shown in FIG.
[0254] The conveying type cooling device 60 has a conveyor 61 that conveys the sheet-like dried rubber 10 discharged from the die 59 of the screw-type extruder 5 in the direction of arrow A in Figure 3, and a cooling means 65 that blows cold air onto the sheet-like dried rubber 10 on the conveyor 61.
[0255] The conveyor 61 has rollers 62, 63, and a conveyor belt 64 that is wound around the rollers 62, 63 and on which the sheet-like dry rubber 10 is placed. The conveyor 61 is configured to continuously transport the sheet-like dry rubber 10 discharged from the die 59 of the screw-type extruder 5 onto the conveyor belt 64 downstream (to the right in FIG. 3).
[0256] The cooling means 65 is not particularly limited, but may be, for example, a means configured to blow cooling air sent from a cooling air generating means (not shown) onto the surface of the sheet-like dried rubber 10 on the conveyor belt 64.
[0257] The length L1 of the conveyor 61 and the cooling means 65 of the transport-type cooling device 60 (the length of the part where cooling air can be blown) is not particularly limited, but is, for example, 10 to 100 m, and preferably 20 to 50 m. The transport speed of the sheet-like dry rubber 10 in the transport-type cooling device 60 may be appropriately adjusted depending on the length L1 of the conveyor 61 and the cooling means 65, the discharge speed of the sheet-like dry rubber 10 discharged from the die 59 of the screw-type extruder 5, the target cooling speed and cooling time, and is, for example, 10 to 100 m / hr, and more preferably 15 to 70 m / hr.
[0258] According to the conveying type cooling device 60 shown in Figure 3, the sheet-like dry rubber 10 discharged from the die 59 of the screw-type extruder 5 is conveyed by a conveyor 61 while cooling air is blown from a cooling means 65 onto the sheet-like dry rubber 10, thereby cooling the sheet-like dry rubber 10.
[0259] 3, the transportable cooling device 60 is not particularly limited to a configuration including one conveyor 61 and one cooling means 65, but may be configured to include two or more conveyors 61 and two or more corresponding cooling means 65. In that case, the total length of each of the two or more conveyors 61 and the cooling means 65 may be within the above range.
[0260] The baling device 7 shown in Fig. 1 is configured to process the dry rubber extruded from the screw-type extruder 5 and cooled in the cooling device 6 to produce a bale, which is a block. As described above, the screw-type extruder 5 is capable of extruding the dry rubber into various shapes such as granules, columns, round bars, and sheets, and the baling device 7 is configured to bales the dry rubber thus formed into various shapes. The weight and shape of the acrylic rubber bales produced by the baling device 7 are not particularly limited, but for example, an approximately rectangular parallelepiped acrylic rubber bale weighing about 20 kg is produced.
[0261] The baling device 7 may include, for example, a baler, and the cooled, dried rubber may be compressed by the baler to produce an acrylic rubber bale.
[0262] Furthermore, when the sheet-like dry rubber 10 is produced by the screw-type extruder 5, an acrylic rubber bale in which the sheet-like dry rubber 10 is laminated may be produced. For example, a cutting mechanism for cutting the sheet-like dry rubber 10 may be provided in the baling device 7 arranged downstream of the conveying cooling device 60 shown in FIG. 3. Specifically, the cutting mechanism of the baling device 7 is configured, for example, to continuously cut the cooled sheet-like dry rubber 10 at predetermined intervals and process it into cut sheet-like dry rubber 16 of a predetermined size. By laminating a plurality of cut sheet-like dry rubber 16 cut to a predetermined size by the cutting mechanism, an acrylic rubber bale in which the cut sheet-like dry rubber 16 is laminated can be produced.
[0263] When manufacturing an acrylic rubber veil in which cut sheet-like dry rubber 16 is laminated, it is preferable to laminate cut sheet-like dry rubber 16 at, for example, 40° C. or higher. By laminating cut sheet-like dry rubber 16 at 40° C. or higher, good air release is achieved by further cooling and compression due to its own weight. EXAMPLES
[0264] The present invention will be described in more detail below with reference to Examples, Comparative Examples and Reference Examples. In each example, "parts", "%" and "ratio" are by weight unless otherwise specified. Various physical properties were evaluated according to the following methods.
[0265] [Monomer composition] Regarding the monomer composition of the acrylic rubber, the monomer composition of each monomer unit in the acrylic rubber was confirmed by H-NMR, and the remaining activity of reactive groups in the acrylic rubber and the content of each reactive group were confirmed by the following test methods. The content ratio of each monomer unit in the acrylic rubber was calculated from the amount of each monomer used in the polymerization reaction and the polymerization conversion rate. Specifically, the polymerization reaction was an emulsion polymerization reaction, and the polymerization conversion rate was approximately 100%, with no unreacted monomers being confirmed, so the content ratio of each monomer unit was set to be the same as the amount of each monomer used.
[0266] [Reactive group content] The reactive group content in the acrylic rubber veil was measured as the content in the acrylic rubber veil by the following method. (1) The amount of carboxyl groups was calculated by dissolving the acrylic rubber veil in acetone and performing potentiometric titration with potassium hydroxide solution. (2) The amount of epoxy groups was calculated by dissolving the acrylic rubber base in methyl ethyl ketone, adding a specified amount of hydrochloric acid to react with the epoxy groups, and titrating the amount of residual hydrochloric acid with potassium hydroxide. (3) The amount of chlorine was calculated by completely burning an acrylic rubber veil in a combustion flask, absorbing the chlorine generated in water, and titrating it with silver nitrate.
[0267] [Ash content] The ash content (%) in the acrylic rubber veil was measured in accordance with JIS K6228 Method A.
[0268] [Ash content] The amount (ppm) of each component in the acrylic rubber veil ash was measured by pressing the ash sampled during the above-mentioned ash content measurement onto a titration filter paper of Φ20 mm and subjecting it to XRF measurement using ZSX Primus (manufactured by Rigaku Co., Ltd.).
[0269] [specific gravity] The specific gravity of the acrylic rubber veil was measured in accordance with JIS K6268 crosslinked rubber - density measurement method A.
[0270] [Gel amount] The gel content (%) of the acrylic rubber veil is the amount of insoluble matter in methyl ethyl ketone, and was determined by the following method. Approximately 0.2 g of acrylic rubber bale was weighed out (Xg), immersed in 100 ml of methyl ethyl ketone and left to stand at room temperature for 24 hours, after which the insoluble matter in methyl ethyl ketone was filtered off using an 80 mesh wire screen. The filtrate, i.e., the filtrate containing only the rubber components soluble in methyl ethyl ketone, was evaporated, dried and solidified, and the dried solid content (Yg) was weighed and calculated using the following formula. Gel volume (%) = 100 × (XY) / X
[0271] [Glass transition temperature (Tg)] The glass transition temperature (Tg) of the acrylic rubber was measured using a differential scanning calorimeter (DSC, product name "X-DSC7000", manufactured by Hitachi High-Tech Science Corporation).
[0272] [pH] The pH of the acrylic rubber veil was measured with a pH electrode after dissolving 6 g (±0.05 g) of acrylic rubber veil in 100 g of tetrahydrofuran, adding 2.0 ml of distilled water, and confirming complete dissolution.
[0273] [Water content] The water content (%) of the acrylic rubber veil was measured in accordance with JIS K6238-1: Oven A (volatile matter measurement) method.
[0274] [Molecular weight and molecular weight distribution] The weight average molecular weight (Mw) and molecular weight distribution (Mz / Mw) of the acrylic rubber that constitutes the acrylic rubber veil are absolute molecular weight and absolute molecular weight distribution measured by the GPC-MALS method using a solution in which dimethylformamide was added with 0.05 mol / L lithium chloride and 0.01% concentrated 37% hydrochloric acid as the solvent. Specifically, a multi-angle laser light scattering photometer (MALS) and a differential refractometer (RI) were incorporated into a GPC (Gel Permeation Chromatography) device, and the light scattering intensity and refractive index difference of the molecular chain solution size-fractionated by the GPC device were measured over the elution time, and the molecular weight of the solute and its content were calculated sequentially. The measurement conditions and method using the GPC device are as follows. Column: 2 TSKgel α-M (φ7.8mm×30cm, Tosoh Corporation) Column temperature: 40℃ Flow rate: 0.8ml / mm Sample preparation: 5 ml of solvent was added to 10 mg of sample, and the mixture was gently stirred at room temperature (dissolution was visually confirmed).Then, the mixture was filtered using a 0.5 μm filter.
[0275] [Complex viscosity] The complex viscosity η of the acrylic rubber veil was measured at 473% strain and 1 Hz using a dynamic viscoelasticity measuring device "Rubber Process Analyzer RPA-2000" (manufactured by Alpha Technology Co., Ltd.) to measure the temperature dispersion (40 to 120°C) and obtain the complex viscosity η at each temperature. Here, the dynamic viscoelasticity at 60°C of the above-mentioned dynamic viscoelasticity was taken as the complex viscosity η(60°C), and the dynamic viscoelasticity at 100°C was taken as the complex viscosity η(100°C), and the values of η(100°C) / η(60°C) and η(60°C) / η(100°C) were calculated.
[0276] [Mooney viscosity (ML1+4, 100℃)] The Mooney viscosity (ML1+4,100°C) of the acrylic rubber veil was measured in accordance with the physical testing method for uncrosslinked rubber of JIS K6300.
[0277] [Processability evaluation] The processability of the rubber samples was evaluated by putting the rubber samples into a Banbury mixer heated to 50°C and masticating for 1 minute, then adding compounding ingredient A of the rubber mixture formulation shown in Table 1, and measuring the time until the rubber mixture in the first stage was integrated and showed the maximum torque value, i.e., the Black Incorporation Time (BIT), and evaluating it with an index of 100 for Comparative Example 1 (the smaller the index, the better the processability).
[0278] [Storage stability evaluation] The storage stability of the rubber samples was evaluated by placing the rubber samples in a thermo-hygrostat (SH-222, manufactured by ESPEC) at 45°C x 80% RH for 7 days, measuring the workability (BIT) of the rubber samples before and after placing in the thermo-hygrostat, calculating the rate of change in BIT before and after placing in the thermo-hygrostat, and using an index with Comparative Example 1 set to 100 (the smaller the index, the better the storage stability).
[0279] [Water resistance evaluation] The water resistance of the rubber samples was evaluated by an immersion test in accordance with JIS K6258, in which the crosslinked rubber samples were immersed in distilled water at 85°C for 100 hours, and the volume change rate before and after immersion was calculated according to the following formula, with Comparative Example 1 being set at 100 (the smaller the index, the better the water resistance). Volume change rate before and after immersion (%) = (volume of test piece after immersion - volume of test piece before immersion) / volume of test piece before immersion) x 100
[0280] [Example 1] A mixing vessel equipped with a homomixer was charged with 46 parts of pure water, 48.5 parts of ethyl acrylate, 29 parts of n-butyl acrylate, 21 parts of methoxyethyl acrylate, 1.5 parts of vinyl chloroacetate, and, as emulsifiers, 0.709 parts of sodium lauryl sulfate and 1.82 parts of polyoxyethylene dodecyl ether (molecular weight 1500), and the mixture was stirred to obtain a monomer emulsion.
[0281] Next, 170 parts of pure water and 3 parts of the monomer emulsion obtained by emulsion polymerization were added to a polymerization reaction tank equipped with a thermometer and a stirrer, and cooled to 12°C under a nitrogen stream. Then, the remainder of the monomer emulsion, 0.00033 parts of ferrous sulfate, 0.264 parts of sodium ascorbate, and 0.22 parts of potassium persulfate were continuously dropped into the polymerization reaction tank over 3 hours. Thereafter, the reaction was continued while maintaining the temperature in the polymerization reaction tank at 23°C, and it was confirmed that the polymerization conversion rate reached approximately 100%, and hydroquinone was added as a polymerization terminator to terminate the polymerization reaction, thereby obtaining an emulsion polymerization liquid.
[0282] In a coagulation bath equipped with a thermometer and a stirrer, the obtained emulsion polymerization liquid was heated to 80°C and continuously added to a 2% aqueous sodium sulfate solution (coagulation liquid) that was heated to 80°C and vigorously stirred (rotation speed 600 rpm: peripheral speed 3.1 m / s), to coagulate the polymer, which was then filtered off to obtain hydrous crumbs.
[0283] Next, 194 parts of hot water (70°C) was added to the coagulation bath and stirred for 15 minutes, after which the water was removed, and 194 parts of hot water (70°C) was added again and stirred for 15 minutes to wash the wet crumbs. The washed wet crumbs (wet crumb temperature 65°C) were fed to a screw extruder, dehydrated and dried, and extruded into a sheet-like dry rubber having a width of 300 mm and a thickness of 10 mm. Next, the sheet-like dry rubber was cooled at a cooling rate of 200°C / hr using a conveying cooling device directly connected to the screw extruder 15.
[0284] The screw extruder used in this Example 1 is composed of one supply barrel, three dehydration barrels (first to third dehydration barrels), and five drying barrels (first to fifth drying barrels). The first and second dehydration barrels discharge water, and the third dehydration barrel discharges steam. The operating conditions of the screw extruder were as follows.
[0285] Water content: Moisture content of wet crumbs after draining in the second dewatering barrel: 20% Moisture content of wet crumb after steaming in the third dewatering barrel: 10% Moisture content of wet crumb after drying in the fifth drying barrel: 0.4% Rubber Temperature: Temperature of wet crumbs fed into the first feed barrel: 65℃ -Temperature of rubber discharged from screw extruder: 140℃ Set temperature for each barrel: First dehydration barrel: 90℃ Second dehydration barrel: 100℃ ·Third dehydration barrel: 120℃ ·First drying barrel: 120℃ Second drying barrel: 130℃ ·Third drying barrel: 140℃ ·Fourth drying barrel: 160℃ · Fifth drying barrel: 180℃ Operating conditions: Diameter of the screw in the barrel unit (D): 132mm Total length of the screw in the barrel unit (L): 4620mm Length / Depth:35 - Rotation speed of the screw in the barrel unit: 135 rpm -Rubber extrusion rate from die: 700kg / hr Die resin pressure: 2MPa
[0286] The sheet-like dried rubber extruded from the screw-type extruder was cooled to 50°C, cut with a cutter, and laminated to 20 parts (20 kg) before the temperature dropped below 40°C to obtain an acrylic rubber veil (A). The reactive group content, ash content, ash component content, specific gravity, gel content, glass transition temperature (Tg), pH, water content, molecular weight, molecular weight distribution, complex viscosity, and Mooney viscosity (ML1+4,100°C) of the obtained acrylic rubber veil (A) were measured and shown in Table 2. The value of "water content after dehydration (drainage) (%)" shown in the dehydration process column in Table 2 is the water content of the water-containing crumb immediately after drainage in the drainage type dehydration barrel (immediately before the exhaust steam type dehydration barrel).
[0287] Next, 100 parts of the acrylic rubber veil (A) and compounding agent A of "Compound 1" shown in Table 1 were added using a Banbury mixer and mixed for 5 minutes at 50°C. At this time, the processability of the acrylic rubber veil was evaluated, and further, the storage stability was evaluated, and the results are shown in Table 2. Furthermore, the obtained mixture was transferred to a roll at 50°C, and compounding agent B of "Compound 1" was compounded and mixed to obtain a rubber mixture.
[0288] [Table 1]
[0289] The obtained rubber mixture was placed in a mold 15 cm long, 15 cm wide, and 0.2 cm deep, and pressed at 180°C for 10 minutes while applying a pressure of 10 MPa to cause primary crosslinking, and then the obtained primary crosslinked product was further heated in a gear oven at 180°C for 2 hours to cause secondary crosslinking, thereby obtaining a sheet-like crosslinked rubber product. A test piece measuring 3 cm x 2 cm x 0.2 cm was cut from the obtained sheet-like crosslinked rubber product and subjected to a water resistance test, and the results are shown in Table 2.
[0290] [Example 2] The monomer components were changed to 98.5 parts of ethyl acrylate and 1.5 parts of vinyl chloroacetate, the temperature of the first dehydration barrel of the screw extruder was changed to 100°C, the temperature of the second dehydration barrel was changed to 120°C, and only the first dehydration barrel was used for drainage. In addition, the moisture content of the water-containing crumb after drainage in the first dehydration barrel was changed to 30%. The same procedure as in Example 1 was carried out, and an acrylic rubber veil (B) was obtained and its properties were evaluated. The results are shown in Table 2.
[0291] [Example 3] The same procedure as in Example 2 was carried out except that the monomer components were changed to 43 parts of ethyl acrylate, 25 parts of n-butyl acrylate, 26 parts of methoxyethyl acrylate, 2 parts of acrylonitrile, and 4 parts of allyl glycidyl ether, and an acrylic rubber veil (C) was obtained and its properties were evaluated (the compounding agent was replaced with "Compound 2"). The results are shown in Table 2.
[0292] [Example 4] The same procedure as in Example 2 was carried out except that the monomer components were changed to 4.5 parts of ethyl acrylate, 64.5 parts of n-butyl acrylate, 39.5 parts of methoxyethyl acrylate, and 1.5 parts of mono n-butyl fumarate, and an acrylic rubber veil (D) was obtained and its properties were evaluated (the compounding agent was changed to "Compound 3"). The results are shown in Table 2.
[0293] [Example 5] The same procedure as in Example 2 was carried out except that the monomer components were changed to 42.2 parts of ethyl acrylate, 35 parts of n-butyl acrylate, 20 parts of methoxyethyl acrylate, 1.5 parts of acrylonitrile, and 1.3 parts of vinyl chloroacetate, to obtain an acrylic rubber veil (E), and the properties thereof were evaluated. The results are shown in Table 2.
[0294] [Comparative Example 1] The emulsion polymerization liquid (rotation speed 100 rpm, peripheral speed 0.5 m / s) was subjected to emulsion polymerization in the same manner as in Example 5, and a 0.7% aqueous sodium sulfate solution was added to generate hydrous crumbs. 194 parts of industrial water was added to 100 parts of the generated hydrous crumbs, and the mixture was stirred in a coagulation tank at 25°C for 5 minutes, after which the hydrous crumbs were washed 4 times by draining the water from the coagulation tank, and then 194 parts of an aqueous sulfuric acid solution of pH 3 was added and stirred at 25°C for 5 minutes, after which the water was drained from the coagulation tank and acid washed once, and then 194 parts of pure water was added and pure water washed once, and the washed hydrous crumbs were dried in a hot air dryer at 160°C to obtain an acrylic rubber (F) with a water content of 0.4% by weight. The properties of the obtained crumb-like acrylic rubber (F) were evaluated and shown in Table 2.
[0295] [Reference example 1] The washing process was carried out in the same manner as in Example 5, and the washed water-containing crumbs were dried in a hot air dryer at 160° C. to obtain an acrylic rubber (G) with a water content of 0.4% by weight. The properties of the obtained crumb-like acrylic rubber (G) were evaluated and are shown in Table 2.
[0296] [Table 2]
[0297] From Table 2, it can be seen that the acrylic rubber veils (A) to (E) made of the acrylic rubber having reactive groups of the present invention, having an ash content of 0.2% by weight or less, a total content of at least one element selected from sodium, sulfur, calcium, magnesium and phosphorus in the ash of at least 50% by weight, and a specific gravity of 0.9 or more, are excellent in storage stability and water resistance, and also in processability (Examples 1 to 5).
[0298] Also, from Table 2, it can be seen that when a coagulation liquid is added to an emulsion polymerization liquid in a coagulation reaction to generate hydrous crumbs, the ash content does not decrease and water resistance is insufficient even if washing with water four times, washing with acid once, and washing with pure water once in the washing process (Comparative Example 1).On the other hand, it can be seen that when a coagulation liquid is added to a high-concentration coagulation liquid that is being stirred vigorously to some extent in a coagulation reaction to generate hydrous crumbs, the ash content decreases to some extent and water resistance is improved by washing with warm water only twice (Reference Example 1).
[0299] In addition, looking at the relationship between the amount of sodium (Na) and the amount of sulfur (S) in the ash in Table 2, it can be seen that by carrying out the coagulation method and washing method in Reference Example 1, the total amount of sodium (Na) and sulfur (S) (Na+S) remains the same as in Comparative Example 1, but the amount of sodium (Na) is reduced and the Na / S ratio is smaller. This is because by carrying out the coagulation and washing method in Reference Example 1, most of the coagulant (sodium sulfate: Na2SO4: high Na ratio) used is removed, but the emulsifier (sodium lauryl sulfate: NaC 12 H 25 This is presumably because sodium (Na) and sulfur (S) derived from sulfur dioxide (SO4) are inherent in the hydrous crumbs and cannot be fully removed by washing.
[0300] Furthermore, from Table 2, it can be seen that the method of Reference Example 1 improves water resistance and storage stability to a certain extent, but further improvement is desired, and the processability needs to be greatly improved.
[0301] In contrast, by carrying out a coagulation reaction in the same manner as in Reference Example 1, washing twice with warm water, and then dehydrating and drying in a screw-type extruder until the moisture content is less than 1% by weight, the ash content in the acrylic rubber bale is greatly reduced, and it is clear that all of the properties of water resistance, storage stability, and processability are significantly improved (Examples 1 to 5). Here, it can be seen that the water resistance is due to the effect of significantly reducing the ash content by dehydrating and drying in the screw-type extruder (the prerequisite being that the above-mentioned Na / S ratio is within a specific ratio), but as for the storage stability and processability, it can be seen that changes occur within the screw-type extruder that cannot be explained by the ash content and ash component ratio alone.
[0302] Table 2 also shows that the crumb-like acrylic rubber obtained by drying the washed water-containing crumbs with hot air is sticky and in a loose mass, has a low specific gravity of the 0.7 range, and contains air (Comparative Example 1 and Reference Example 1).In contrast, the acrylic rubber veils obtained by drying the crumbs with a screw-type extruder, forming them into sheets, and laminating them all have a high specific gravity of the 1.0 range, contain almost no air, and have significantly superior storage stability (Examples 1 to 5). This is believed to be because the conditions of the screw-type extruder used in the examples, for example, the temperature of the water-containing crumbs fed in, the moisture content in the dehydration barrel section, the set temperature and vacuum level in the drying barrel section, enabled reliable drying and melt-kneading to a state in the drying barrel section that was substantially free of moisture, and because the die section resin pressure, the temperature of the extruded sheet-like dried rubber, and the temperature of the sheet-like dried rubber at the time of cutting, among other things, enabled the production of an acrylic rubber sheet with little air entrapment (high specific gravity), and because the acrylic rubber sheet with little air entrapment could be used to produce the acrylic rubber veil using a lamination method that allows air to easily escape.
[0303] From Table 2, it can be seen that the gel amount of the methyl ethyl ketone insoluble matter in the crumb-like acrylic rubber obtained by drying the washed water-containing crumbs with hot air is large (Comparative Example 1 and Reference Example 1), but the gel amount of all the methyl ethyl ketone insoluble matter in the acrylic rubber veil dried in a screw-type extruder, formed into a sheet, and laminated is reduced to 5% or less, and the processability is significantly improved (Examples 1 to 5). This is presumably because the polymerization reaction was carried out up to a polymerization conversion rate of approximately 100% in the emulsion polymerization, so the gel amount of the methyl ethyl ketone insoluble matter in the acrylic rubber increased rapidly, and the crumb-like acrylic rubber dried with hot air had a high gel amount as it was, but by controlling the temperature of the water-containing crumbs fed, the water content in the dehydration barrel section, the set temperature and vacuum level of the drying barrel section, etc. in the screw-type extruder, it was possible to dry the acrylic rubber to a state where it was substantially free of moisture in the drying barrel section and melt-knead it, and the gel of the methyl ethyl ketone insoluble matter that had rapidly increased during the polymerization reaction disappeared.
[0304] Furthermore, from Table 2, it can be seen that the weight average molecular weight (Mw) of the acrylic rubber veil of the present invention exceeds 1 million, and the ratio (Mz / Mw) of the z-average molecular weight (Mz), which places emphasis on the high molecular weight region, to the weight average molecular weight (Mw) is far greater than 1.3, thereby maintaining the strength characteristics of the acrylic rubber veil and ensuring workability. [Explanation of symbols]
[0305] 1 Acrylic rubber manufacturing system 3 Coagulation device 4. Cleaning equipment 5 Screw Extruder 6 Cooling device 7 Baling Equipment
Claims
1. An acrylic rubber veil comprising an acrylic rubber having a reactive group, having an ash content of 0.2% by weight or less, a content of at least one element selected from the group consisting of sodium, sulfur, calcium, magnesium and phosphorus in the ash being at least 50% by weight in total relative to the total ash content, a specific gravity of 0.9 or more, and a complex viscosity at 60°C ([η]60°C) of 15,000 Pa s or less.
2. 2. The acrylic rubber veil according to claim 1, which has a specific gravity in the range of 1 to 1.
2.
3. 3. The acrylic rubber veil according to claim 1, wherein the total amount of sodium and sulfur in the ash is 50% by weight or more based on the total amount of ash.
4. 4. The acrylic rubber veil according to claim 1, wherein the total amount of sodium and sulfur in the ash is 90% by weight or more based on the total ash amount.
5. 5. The acrylic rubber veil according to claim 1, wherein the ratio of sodium to sulfur in the ash ([Na] / [S]) is in the range of 0.4 to 2.5 by weight.
6. 6. The acrylic rubber veil according to any one of claims 1 to 5, wherein the ratio of sodium to sulfur in the ash ([Na] / [S]) is in the range of 0.7 to 1 by weight.
7. The acrylic rubber veil according to any one of claims 1 to 6, wherein the weight average molecular weight (Mw) of the acrylic rubber is in the range of 100,000 to 5,000,000.
8. The acrylic rubber veil according to any one of claims 1 to 7, wherein the ratio (Mz / Mw) of the z-average molecular weight (Mz) to the weight-average molecular weight (Mw) of the acrylic rubber is 1.3 or more.
9. The acrylic rubber veil according to any one of claims 1 to 8, wherein the ratio ([η]100°C / [η]60°C) of the complex viscosity at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) is 0.5 or more.
10. The acrylic rubber veil according to any one of claims 1 to 9, wherein the ratio ([η]100°C / [η]60°C) of the complex viscosity at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) is 0.83 or more.
11. The acrylic rubber veil according to any one of claims 1 to 10, wherein the amount of gel insoluble in methyl ethyl ketone is 50% by weight or less.
12. The acrylic rubber veil according to any one of claims 1 to 11, having a water content of less than 1% by weight.
13. an emulsion polymerization step of emulsifying a monomer component containing a (meth)acrylic acid ester and a reactive group-containing monomer with water and an emulsifier, and emulsion-polymerizing the resulting emulsion in the presence of a polymerization catalyst to obtain an emulsion polymerization liquid; a coagulation step in which the obtained emulsion polymerization liquid is contacted with a coagulation liquid consisting of a coagulant-containing aqueous solution to produce water-containing crumbs; A washing step of washing the produced hydrous crumbs; a dehydration, drying and molding process in which the washed wet crumbs are dehydrated in the dehydration barrel using a screw-type extruder having a dehydration slit, a drying barrel under reduced pressure, and a die at the tip thereof to a moisture content of 1 to 40% by weight, and then dried in the drying barrel to a moisture content of less than 1% by weight, and a sheet-like dried rubber is extruded through a die; a baling process in which the extruded sheet-like dry rubber is layered to form bales; A method for producing an acrylic rubber veil comprising the steps of:
14. 14. The method for producing an acrylic rubber veil according to claim 13, wherein the emulsifier is a sulfate ester salt and the coagulant is a sodium salt.
15. 15. The method for producing an acrylic rubber veil according to claim 13 or 14, wherein the contact between the emulsion polymerization liquid and the coagulation liquid is carried out by adding the emulsion polymerization liquid to the coagulation liquid while stirring.
16. 16. The method for producing an acrylic rubber veil according to claim 15, wherein the peripheral speed of the stirred coagulation liquid is 0.5 m / s or more.
17. The method for producing an acrylic rubber veil according to any one of claims 13 to 16, wherein the temperature of the water-containing crumbs supplied to the screw-type extruder is in the range of 50 to 90°C.
18. The method for producing an acrylic rubber veil according to any one of claims 13 to 17, wherein the degree of vacuum in the drying barrel of the screw-type extruder is in the range of 1 to 50 kPa.
19. The method for producing an acrylic rubber veil according to any one of claims 13 to 18, wherein the set temperature of the drying barrel of the screw-type extruder is 100 to 250°C.
20. The method for producing an acrylic rubber veil according to any one of claims 13 to 19, wherein the resin pressure at the die portion of the screw-type extruder is in the range of 0.1 to 10 MPa.
21. The method for producing an acrylic rubber veil according to any one of claims 13 to 20, wherein the lamination of the sheet-like dry rubber is carried out after the sheet-like dry rubber is cut.
22. 22. The method for producing an acrylic rubber veil according to claim 21, wherein the cutting of the sheet-like dry rubber is carried out at a temperature of the sheet-like dry rubber of 60° C. or less.
23. The method for producing an acrylic rubber veil according to any one of claims 13 to 22, wherein the lamination of the sheet-like dry rubber is carried out at a sheet-like dry rubber temperature of 30°C or higher.
24. A rubber mixture obtained by mixing the acrylic rubber veil according to any one of claims 1 to 12 with a filler and a crosslinking agent.
25. A method for producing a rubber mixture, comprising mixing the acrylic rubber veil according to any one of claims 1 to 12 with a filler and a crosslinking agent in a mixer.
26. A method for producing a rubber mixture, comprising mixing the acrylic rubber veil according to any one of claims 1 to 12 with a filler, and then mixing a crosslinking agent therewith.
27. A cross-linked rubber product obtained by cross-linking the rubber mixture according to claim 24.
Citation Information
Patent Citations
Driving method for rubber-like polymer
JP1989225512A
Manufacturing method of rubbery polymer
JP2006328239A
Acrylic rubber and crosslinked rubber
WO2018079783A1
Method for producing acrylic rubber
WO2018116828A1
Method for producing acrylic rubber
WO2018139466A1