Inorganic reinforced semi-aromatic polyamide resin composition

The inorganic-reinforced semi-aromatic polyamide resin composition addresses mold staining and fluidity issues, ensuring color stability and heat resistance for electronic and automotive applications.

JP7567798B2Active Publication Date: 2024-10-16TOYOBO MC CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2021548734
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-27
Filing Date
2020-09-01
Publication Date
2024-10-16
Estimated Expiration
2040-09-01

Smart Images

  • Figure 0007567798000001
    Figure 0007567798000001
  • Figure 0007567798000002
    Figure 0007567798000002
  • Figure 0007567798000003
    Figure 0007567798000003
Patent Text Reader

Abstract

[Problem] To provide an inorganic reinforced semi-aromatic polyamide resin composition that has excellent heat resistance and thermal discoloration resistance, is capable of suppressing mold contamination due to outgassing during melt molding, and has excellent melt fluidity and gelling properties. [Solution] The present invention is an inorganic reinforced semi-aromatic polyamide resin composition containing 30-75 mass% of a semi-aromatic polyamide (A) and 25-65 mass% of an inorganic reinforcing material (B). The semi-aromatic polyamide (A) is at least one semi-aromatic polyamide that includes a repeating unit obtained by condensation of at least one aliphatic diamine including two or more carbon atoms and terephthalic acid, and the end groups of the semi-aromatic polyamide (A) in the resin composition satisfy a specific relationship.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a semi-aromatic polyamide resin composition that has excellent heat resistance and resistance to thermal discoloration, and further can suppress mold contamination due to outgassing during melt molding. It also has excellent melt fluidity and gelling properties, and is suitable for molding automobile parts, bicycle parts, electric / electronic parts, etc. [Background technology]

[0002] Among thermoplastic resins, polyamide resins have been used for clothing, industrial fiber, engineering plastics, etc., taking advantage of their excellent properties and ease of melt molding. As an engineering plastic in particular, they are used in a wide range of applications, including not only automobile parts and industrial machinery parts, but also various industrial parts, housing parts, and electrical and electronic parts.

[0003] In recent years, in the mounting of electric and electronic components, surface mounting methods (flow method, reflow method) have been rapidly spreading due to the miniaturization of components accompanying the miniaturization of product size, the high density of mounting, the simplification of processes, and the reduction in costs. In the surface mounting method, the process atmosphere temperature is higher than the solder melting temperature (240 to 260°C), so the resin used is necessarily required to have heat resistance at the above atmosphere temperature. In addition, in the surface mounting process, swelling and deformation of mounted components due to water absorption by the resin can be a problem, so the resin used is required to have low water absorption. Resins that satisfy these characteristics include 6T polyamide and 9T polyamide, and Patent Document 1 and Patent Document 2 show that these aromatic polyamides can be used for surface-mounted electric and electronic components. However, there is a problem that the color tone of the resin is easily changed during the manufacturing process or under the usage environment, and there is room for improvement in terms of the color tone stability of the resin due to external factors. Furthermore, the various semi-aromatic polyamide resins described above have disadvantages in that they have a higher melting point and poorer melt fluidity than aliphatic polyamide resins, and are prone to thickening and gelling during molten retention, and there is room for improvement in terms of processing stability and high fluidity (see, for example, Patent Document 3).

[0004] On the other hand, in order to solve the problems of resin color stability and gelation caused by such external factors, an invention has been made to provide a semi-aromatic polyamide resin that has a high melting point of 290°C or higher, low water absorption, as well as excellent melt fluidity and color stability by adjusting a specific resin composition, melt viscosity, relative viscosity, and end group concentration, and is suitable for resin compositions for molded products such as automobile parts, electric / electronic parts, etc. (see, for example, Patent Document 4).

[0005] Also, in order to solve the problems of color stability and gelation of resins, an invention has been made that provides a polyamide and a polyamide composition comprising the same, which have good thermal stability during drying and molding, do not deteriorate in color even when mixed with recycled materials, produce little foreign matter such as gel-like matter, and have excellent productivity during molding, by leaving a reducing phosphorus compound species in the resin (see, for example, Patent Document 5).

[0006] Although this invention achieved improvements in terms of color stability and gelation, it had the problem that the gas generated during melt molding contaminates the mold, resulting in reduced productivity. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 3-88846 [Patent Document 2] Patent No. 3474246 [Patent Document 3] International Publication No. WO2011 / 052464 [Patent Document 4] International Publication No. WO2017 / 077901 [Patent Document 5] JP 2007-92053 A Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention has been made against the background of the problems of the conventional technology. That is, an object of the present invention is to provide an inorganic reinforced semi-aromatic polyamide resin composition which has solder heat resistance, low water absorption, and mechanical properties required for use in surface mount type electric / electronic components, and is also excellent in heat resistance and resistance to thermal discoloration, and furthermore can suppress mold contamination due to outgassing during melt molding, and has excellent melt fluidity and gelling properties. [Means for solving the problem]

[0009] As a result of extensive investigations, the present inventors have found that the above problems can be solved by the means described below, and have arrived at the present invention. That is, the present invention comprises the following configuration.

[0010] [1] An inorganic reinforced semi-aromatic polyamide resin composition containing 30 to 75 mass% of a semi-aromatic polyamide (A) and 25 to 65 mass% of an inorganic reinforcing material (B), The semi-aromatic polyamide (A) is at least one semi-aromatic polyamide containing a repeating unit formed by condensation of at least one aliphatic diamine containing two or more carbon atoms with terephthalic acid, Further, the inorganic reinforced semi-aromatic polyamide resin composition has a relationship among the amino end concentration (AEG), the carboxy end concentration (CEG), and the end concentration (EC) of the amino end blocked with monocarboxylic acid of the semi-aromatic polyamide (A) in the inorganic reinforced semi-aromatic polyamide resin composition, which satisfies the formulas (1) and (2). 0eq / t≦AEG+CEG≦130eq / t ··· (1) (AEG+CEG) / (AEG+CEG+EC)≦0.60 ··· (2)

[0011] [2] The inorganic reinforced semi-aromatic polyamide resin composition according to [1], characterized in that the semi-aromatic polyamide (A) satisfies the following requirements (i) and (ii): (i) 7.5 or less [number of carbon atoms in polyamide / number of amide bonds in polyamide] (ii) [Number of carbon atoms on aromatic rings in polyamide / Total number of carbon atoms in polyamide]≦0.35

[0012] [3] The inorganic reinforced semi-aromatic polyamide resin composition according to [1], characterized in that the semi-aromatic polyamide (A) is a copolymer containing a structural unit formed by condensation of an aliphatic diamine having 2 to 12 carbon atoms with terephthalic acid, and at least one structural unit selected from aliphatic aminocarboxylic acids and lactams having 11 to 18 carbon atoms.

[0013] [4] The inorganic reinforced semi-aromatic polyamide resin composition according to [1], wherein the semi-aromatic polyamide (A) is a copolymer containing 55 to 75 mol % of structural units formed by condensation of hexamethylenediamine and terephthalic acid, and 45 to 25 mol % of structural units formed by 11-aminoundecanoic acid or undecane lactam.

[0014] [5] The inorganic reinforced semi-aromatic polyamide resin composition according to any one of [1] to [4], characterized in that the sum (P3) of the phosphorus atom content derived from phosphorus compounds detected in the structures of structural formulas (P1) and (P2) in the semi-aromatic polyamide (A) is 30 ppm or more, and P3 is 10% or more of the total amount of phosphorus atoms remaining in the semi-aromatic polyamide.

[0015] [ka]

[0016] [ka]

[0017] (wherein R1 and R2 are hydrogen, an alkyl group, an aryl group, a cycloalkyl group, or an arylalkyl group; X1 to X3 are hydrogen, an alkyl group, an aryl group, a cycloalkyl group, an arylalkyl group, an alkali metal, or an alkaline earth metal; and one of X1 to X3 and one of R1 to R2 in each formula may be bonded to each other to form a ring structure.)

[0018] [6] The inorganic reinforced semi-aromatic polyamide resin composition according to any one of [1] to [5], characterized in that the amount of gas generated (outgassing) when pyrolyzed at 350° C. for 10 minutes is 300 ppm or less.

[0019] [7] The inorganic reinforced semi-aromatic polyamide resin composition according to any one of [1] to [6], characterized in that a reduction rate of bending strength calculated from bending strength before and after treatment for 500 hours in a high temperature and high humidity environment of 80°C and 95% RH is less than 15%.

[0020] [8] The inorganic reinforced semi-aromatic polyamide resin composition according to any one of [1] to [7], characterized in that the flow length at a thickness of 0.2 mm is 3 mm or more.

[0021] [9] The inorganic reinforced semi-aromatic polyamide resin composition according to any one of [1] to [8], characterized in that the tensile breaking strain is 0.3 to 3.4%. Effect of the Invention

[0022] The present invention can provide an inorganic reinforced semi-aromatic polyamide resin composition that is excellent in heat resistance and resistance to thermal discoloration, can further suppress mold contamination due to outgassing during melt molding, and has excellent melt fluidity and gelling properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] The present invention will be described in detail below.

[0024] The semi-aromatic polyamide (A) in the present invention means a polyamide which contains a dicarboxylic acid or diamine having an aromatic skeleton in the repeating unit of the polyamide.

[0025] The semi-aromatic polyamide (A) in the present invention is at least one type of semi-aromatic polyamide containing repeating units formed by condensation of at least one aliphatic diamine having two or more carbon atoms with terephthalic acid, and preferably contains 50 mol% or more of structural units formed by condensation of an aliphatic diamine having two or more carbon atoms with terephthalic acid. The structural units are preferably 55 mol% or more, more preferably 55 to 75 mol%, and even more preferably 60 to 70 mol%. If the structural units formed by condensation of a diamine with terephthalic acid are less than 50 mol%, the crystallinity and mechanical properties are reduced. The aliphatic diamine having two or more carbon atoms is preferably an aliphatic diamine having 2 to 12 carbon atoms.

[0026] Examples of the aliphatic diamine component having 2 to 12 carbon atoms include 1,2-ethylenediamine, 1,3-trimethylenediamine, 1,4-tetramethylenediamine, 1,5-pentamethylenediamine, 2-methyl-1,5-pentamethylenediamine, 1,6-hexamethylenediamine, 1,7-heptamethylenediamine, 1,8-octamethylenediamine, 1,9-nonamethylenediamine, 2-methyl-1,8-octamethylenediamine, 1,10-decamethylenediamine, 1,11-undecamethylenediamine, 1,12-dodecamethylenediamine, and 2,2,4 (or 2,4,4)-trimethylhexamethylenediamine, and these can be used alone or in combination. However, in the case of a semi-aromatic polyamide consisting of a structural unit formed by condensation of an aliphatic diamine having 9 or more carbon atoms with terephthalic acid, it may have a melting point below 290°C, so a semi-aromatic polyamide containing 50 mol% or more of a structural unit formed by condensation of an aliphatic diamine having 2 to 8 carbon atoms with terephthalic acid and having a melting point of 290°C or higher is preferred. The structural unit formed by condensation of an aliphatic diamine having 2 to 8 carbon atoms with terephthalic acid is more preferably 55 mol% or more, even more preferably 55 to 75 mol%, and particularly preferably 60 to 70 mol%. Other than the aliphatic diamine having 2 to 12 carbon atoms, there are 1,13-tridecamethylenediamine, 1,16-hexadecamethylenediamine, 1,18-octadecamethylenediamine, etc., which can also be used as a copolymerization component as long as the amount is within a small range that does not impair the effects of the present invention.

[0027] Examples of the copolymerizable dicarboxylic acid component include aromatic dicarboxylic acids such as isophthalic acid, orthophthalic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 2,2'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 5-sodium sulfonate isophthalic acid, and 5-hydroxyisophthalic acid; and aliphatic or alicyclic dicarboxylic acids such as fumaric acid, maleic acid, succinic acid, itaconic acid, adipic acid, azelaic acid, sebacic acid, 1,11-undecanedioic acid, 1,12-dodecanedioic acid, 1,14-tetradecanedioic acid, 1,18-octadecanedioic acid, 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, 4-methyl-1,2-cyclohexanedicarboxylic acid, and dimer acid. Further examples include lactams such as ε-caprolactam, 12-aminododecanoic acid, and 12-lauryllactam, and aminocarboxylic acids having ring-opened structures of these.

[0028] Among them, it is preferable that the copolymerization component is one or more of aliphatic aminocarboxylic acids having 11 to 18 carbon atoms or aliphatic lactams having 11 to 18 carbon atoms.

[0029] The semi-aromatic polyamide (A) in the present invention preferably satisfies (i) 7.5≦[number of carbon atoms in polyamide / number of amide bonds in polyamide].Furthermore, the semi-aromatic polyamide in the present invention preferably satisfies 7.5≦[number of carbon atoms in polyamide / number of amide bonds in polyamide]≦8.2.

[0030] If the ratio of [number of carbon atoms in polyamide / number of amide bonds in polyamide] is less than 7.5, the concentration of amide groups in the polyamide will be high, making it more likely for discoloration to occur due to resin deterioration caused by heat or light. On the other hand, if the ratio of [number of carbon atoms in polyamide / number of amide bonds in polyamide] is more than 8.2, the concentration of amide groups in the polyamide will be low, and the melting point may fall below 290°C, resulting in insufficient heat resistance.

[0031] The semi-aromatic polyamide (A) in the present invention preferably satisfies (ii) [number of carbon atoms on aromatic rings in polyamide / total number of carbon atoms in polyamide]≦0.35.Furthermore, the semi-aromatic polyamide in the present invention preferably satisfies 0.28≦[number of carbon atoms on aromatic rings in polyamide / total number of carbon atoms in polyamide]≦0.35.

[0032] In LED lighting parts and automotive interior and exterior parts, materials are required to have high UV resistance because they are exposed to ultraviolet rays when used outdoors. If the ratio of [the number of carbon atoms on aromatic rings in polyamide / the total number of carbon atoms in polyamide] exceeds 0.35, the absorption of light, especially in the ultraviolet region, becomes large, and the deterioration of the resin due to the light becomes noticeable. In addition, if aromatic rings are present, the resin is likely to form a conjugated structure that causes discoloration due to deterioration, and shows significant discoloration. Therefore, it is preferable that the concentration of aromatic rings in the resin is low. On the other hand, in order to achieve heat resistance and a high melting point, it is preferable that the ratio of [the number of carbon atoms on aromatic rings in polyamide / the total number of carbon atoms in polyamide] is 0.28 or more.

[0033] As the semi-aromatic polyamide in the present invention, hexamethylenediamine / terephthalic acid / aminoundecanoic acid (or undecalactam), hexamethylenediamine / terephthalic acid / aminododecanoic acid (or 12-lauryl lactam), decamethylenediamine / terephthalic acid / aminoundecanoic acid (or undecalactam), and decamethylenediamine / terephthalic acid / aminododecanoic acid (or 12-lauryl lactam) are particularly preferred. Among these, in terms of a high melting point, when the polyamide has a structural unit (also called a 6T unit) formed by the condensation of hexamethylenediamine and terephthalic acid, in order to realize high heat resistance, fluidity, low water absorbency, and excellent color stability, it is preferred that the polyamide is a copolymer consisting of 55 to 75 mol % of 6T units and 45 to 25 mol % of structural units (also called 11 units) formed by 11-aminoundecanoic acid or undecane lactam. It is more preferable that the polyamide is a copolymer consisting of 60 to 70 mol % of 6T units and 40 to 30 mol % of 11 units.

[0034] The melting point (Tm) of the semi-aromatic polyamide in the present invention is preferably 290 to 350° C., more preferably 290 to 340° C., and even more preferably 300 to 330° C. If Tm exceeds the upper limit, the processing temperature required when molding the semi-aromatic polyamide resin composition by injection molding or the like becomes extremely high, and the composition may decompose during processing, making it difficult to obtain the desired physical properties and appearance. Conversely, if Tm is less than the lower limit, the crystallization rate becomes slow, making molding difficult.

[0035] Generally, the total number of terminals, which is the sum of the amino terminal concentration (AEG), carboxyl terminal concentration (CEG), and terminal concentration blocked with monocarboxylic acid and / or monoamine (EC) of a polyamide resin, is correlated with the relative viscosity (RV). As a result of various studies, it was found that the semi-aromatic polyamide in the semi-aromatic polyamide resin composition of the present invention satisfies the above formulas (1) and (2), and thus a semi-aromatic polyamide resin composition having excellent heat resistance and heat discoloration resistance, as well as suppressing mold contamination due to outgassing during melt molding, and excellent melt fluidity and gelling properties can be obtained. In the present invention, EC refers to the terminal concentration of amino terminals blocked with monocarboxylic acid. For convenience, the amino terminal, the carboxyl terminal, and the terminal blocked with a monocarboxylic acid and / or a monoamine are sometimes referred to as AEG, CEG, and EC, respectively.

[0036] In order for the semi-aromatic polyamide (A) in the semi-aromatic polyamide resin composition to satisfy the above formulas (1) and (2), the (AEG+CEG) of the semi-aromatic polyamide (A) used as the raw material is preferably 10 to 140 eq / t, more preferably 20 to 130 eq / t, and even more preferably 30 to 100 eq / t. If (AEG+CEG) is less than 10 eq / t, there are no remaining reactive terminal groups, and the viscosity cannot be increased to a relative viscosity (RV) that ensures the mechanical strength of the molded product. If (AEG+CEG) exceeds 140 eq / t, the amount of terminal blocking is small and the remaining amount of AEG and CEG is large, resulting in viscosity increase and gelation during melt molding.

[0037] In addition, in order for the semi-aromatic polyamide in the semi-aromatic polyamide resin composition to satisfy the above formulas (1) and (2), the (AEG+CEG) / (AEG+CEG+EC) of the semi-aromatic polyamide (A) used as the raw material is preferably 0.70 or less, more preferably 0.55 or less, even more preferably 0.50 or less, particularly preferably 0.45 or less, and most preferably 0.40 or less. When (AEG+CEG) / (AEG+CEG+EC) exceeds 0.70, the content of the terminal blocking agent is low and the amount of remaining AEG and CEG is large, so that the resin thickens and gels during melt molding. In addition, in general, the thickening of polyamide resins progresses as the amino group terminal reacts with the carboxyl group terminal. However, the thickening may progress as the CEG reacts with EC. When the AEG disappears (becomes 0) during the amidation reaction, the terminals of the semi-aromatic polyamide become CEG and EC. Since there is no AEG, the acid catalytic effect of CEG causes CEG to attack the amide bond formed by the end-capping agent, resulting in an amide exchange reaction. During this process, the thickening reaction proceeds while the end-capping agent is distilled out of the reaction system. This results in an increase in outgassing components derived from the end-capping agent. In addition, the acid component of CEG causes a coloring reaction, resulting in a resin with poor color stability and prone to gelation. In order to avoid such phenomena, it is important that the semi-aromatic polyamide (A) satisfies the above-mentioned end group relationship.

[0038] The AEG, CEG and EC of the semi-aromatic polyamide (A) as the raw material may satisfy the above-mentioned relationship, and the preferred ranges of each are as follows. The AEG is preferably 5 to 70 eq / t, more preferably 10 to 40 eq / t, and even more preferably 15 to 40 eq / t. The CEG is preferably 5 to 100 eq / t, more preferably 5 to 70 eq / t, and even more preferably 15 to 50 eq / t. The EC is preferably 60 to 240 eq / t, more preferably 80 to 200 eq / t, and even more preferably 80 to 170 eq / t.

[0039] The relative viscosity (RV) of the semi-aromatic polyamide (A) in the present invention is preferably 1.3 to 3.5, more preferably 1.5 to 3.0, further preferably 1.8 to 2.8, and even more preferably 1.9 to 2.5. If the RV is less than 1.3, the molded product will not have sufficient mechanical strength. If the RV is more than 3.5, the flowability during melt molding will be low, which is undesirable in terms of melt processability.

[0040] In the semi-aromatic polyamide (A) of the present invention, the sum (P3) of the phosphorus atom content derived from the phosphorus compound detected in the structures of the structural formulas (P1) and (P2) in the semi-aromatic polyamide is preferably 30 ppm or more, and P3 is preferably 10% or more relative to the total phosphorus atom amount remaining in the semi-aromatic polyamide. The phosphorus atom is derived from the phosphorus compound used as a catalyst. P3 is more preferably 40 ppm or more, and further preferably 50 ppm or more. If P3 is less than 30 ppm, the peroxide generated by thermo-oxidative degradation cannot be suppressed, and the resin is likely to yellow in a high-temperature atmosphere. In addition, the resin is likely to gel due to the peroxide generated by thermo-oxidative degradation. If P3 is less than 10% of the total remaining phosphorus atom weight, it means that the resin has been thermally damaged by the thermal history during polymerization or has reacted with oxygen remaining in the polymerization system and is undergoing oxidative deterioration, resulting in a resin that is prone to coloration and gelation. There is no particular upper limit for the ratio of P3 to the total remaining phosphorus atom weight, but in the present invention, it is about 50%. In order to make P3 30 ppm or more and P3 10% or more of the total remaining phosphorus atom weight, the oxygen concentration in the storage tank is set to 10 ppm or less, a low-order condensation product is obtained by polymerizing at a low temperature in the polycondensation process, and then the viscosity is adjusted to the specified level by solid-phase polymerization with little thermal history. In order to make P3 30 ppm or more relative to the total amount of remaining phosphorus atoms, the total amount of phosphorus atoms remaining in the semi-aromatic polyamide is preferably 200 to 400 ppm.

[0041] [ka]

[0042] [ka]

[0043] (wherein R1 and R2 are hydrogen, an alkyl group, an aryl group, a cycloalkyl group, or an arylalkyl group; X1 to X3 are hydrogen, an alkyl group, an aryl group, a cycloalkyl group, an arylalkyl group, an alkali metal, or an alkaline earth metal; and one of X1 to X3 and one of R1 to R2 in each formula may be bonded to each other to form a ring structure).

[0044] The phosphorus compound used as the catalyst will be described later, but when sodium hypophosphite is used as the catalyst, R1 and R2 are hydrogen, and X1 to X3 are each hydrogen or sodium.

[0045] By setting the amount of P3 contained in the semi-aromatic polyamide (A) within the above range, the ΔCo-b before and after the semi-aromatic polyamide resin composition of the present invention is heat-treated at 260°C for 10 minutes in air can be set to 12 or less. In addition, a semi-aromatic polyamide resin composition can be obtained that has a gelation time of 4 hours or more when heat-treated at 330°C in a nitrogen stream. ΔCo-b and gelation time are measured by the method described in the Examples section below.

[0046] The method for producing the semi-aromatic polyamide (A) in the present invention includes a step of preparing an aqueous raw material solution constituting the semi-aromatic polyamide, a raw material introduction step of continuously introducing the aqueous raw material solution into a tubular reactor, an amidation step of passing the introduced raw material through the tubular reactor to perform amidation to obtain a reaction mixture containing an amidated product and condensed water, a step of introducing the reaction mixture into a continuous reactor capable of separating and removing water to perform melt polymerization, and a step of performing solid-state polymerization under vacuum or under a nitrogen gas flow.

[0047] (1) Mixing process A predetermined amount of diamine and dicarboxylic acid are added to a pressure-resistant reactor. At the same time, water is added so that the raw material concentration becomes 30 to 90% by weight, and a phosphorus compound as a polymerization catalyst and a monocarboxylic acid as an end-capping agent are added. In addition, a foam inhibitor is added to those that will foam in the subsequent process.

[0048] The catalyst used in producing the semi-aromatic polyamide (A) of the present invention includes dimethylphosphinic acid, phenylmethylphosphinic acid, hypophosphorous acid, ethyl hypophosphite, compounds of phosphorous acid, their hydrolysates, and condensates. Or, their metal salts, ammonium salts, and esters can be mentioned. Specific examples of the metal species of the metal salt include potassium, sodium, magnesium, vanadium, calcium, zinc, cobalt, manganese, tin, tungsten, germanium, titanium, and antimony. As the ester, ethyl ester, isopropyl ester, butyl ester, hexyl ester, isodecyl ester, octadecyl ester, decyl ester, stearyl ester, and phenyl ester can be added. In the present invention, sodium hypophosphite is preferred as the catalyst. In addition, from the viewpoint of improving the melt retention stability, it is preferred to add sodium hydroxide.

[0049] The timing of adding the terminal blocking agent is preferably when the raw materials are charged, but it may be at the start of polymerization, in the later stage of polymerization, or at the end of polymerization. The terminal blocking agent is not particularly limited as long as it is a monofunctional compound that is reactive with the amino group or carboxyl group at the polyamide terminal, and examples of the terminal blocking agent that can be used include monocarboxylic acids or monoamines, acid anhydrides such as phthalic anhydride, monoisocyanates, monoacid halides, monoesters, and monoalcohols. Examples of the end-capping agent include aliphatic monocarboxylic acids such as acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, pivalic acid, and isobutyric acid; alicyclic monocarboxylic acids such as cyclohexanecarboxylic acid; aromatic monocarboxylic acids such as benzoic acid, toluic acid, α-naphthalenecarboxylic acid, β-naphthalenecarboxylic acid, methylnaphthalenecarboxylic acid, and phenylacetic acid; acid anhydrides such as maleic anhydride, phthalic anhydride, and hexahydrophthalic anhydride; aliphatic monoamines such as methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, decylamine, stearylamine, dimethylamine, diethylamine, dipropylamine, and dibutylamine; alicyclic monoamines such as cyclohexylamine and dicyclohexylamine; and aromatic monoamines such as aniline, toluidine, diphenylamine, and naphthylamine. In the present invention, the end-capping agent is preferably a monocarboxylic acid, and among the above examples, acetic acid and benzoic acid are preferred.

[0050] The salt concentration of the raw material aqueous solution varies depending on the type of polyamide and is not particularly limited, but is generally desirably 30 to 90% by mass. If the salt concentration exceeds 90% by mass, the salt may precipitate due to a slight change in temperature and clog the piping, and since it is necessary to increase the solubility of the salt, the equipment must be high-temperature and high-pressure resistant, which is cost-inefficient. On the other hand, if the salt concentration is less than 30% by mass, the amount of water evaporated after the initial polymerization step increases, which is not only energy-inefficient but also causes an increase in costs due to reduced productivity. The desirable salt concentration is 35 to 85% by mass.

[0051] Although it varies depending on the type of polyamide and salt concentration, the salt solution is generally prepared at a temperature of 60 to 180°C and a pressure of 0 to 1 MPa. If the temperature exceeds 180°C or the pressure exceeds 1 MPa, the equipment must be high-temperature and high-pressure resistant, which increases the equipment cost and is disadvantageous. Conversely, if the temperature is less than 60°C or the pressure is less than 0 MPa, not only will it cause problems such as clogging of pipes due to salt precipitation, but it will also be difficult to increase the salt concentration, resulting in a decrease in productivity. The desirable conditions are a temperature of 70 to 170°C and a pressure of 0.05 to 0.8 MPa, more desirably 75 to 165°C and 0.1 to 0.6 MPa.

[0052] Basically, there is no problem with the storage tank for the aqueous salt solution as long as there is no precipitation of salt, and the conditions for the salt formation step can be applied as is.

[0053] The salt solution thus prepared is continuously fed to the amidation step by a feed pump in the raw material introduction step. The feed pump used here must have excellent quantitative performance. Fluctuations in the feed rate will lead to process fluctuations in the amidation step, resulting in polyamides with large deviations in relative viscosity (RV) and unstable quality. For this reason, it is recommended to use a plunger pump with excellent quantitative performance as the feed pump.

[0054] The oxygen concentration of the atmosphere during raw material mixing has a large effect on the color tone of the resulting polyamide. If the oxygen concentration of the atmosphere during raw material mixing is 10 ppm or less, there is no problem, but if the oxygen concentration exceeds 10 ppm, the resulting polyamide tends to have a strong yellow tinge and the quality of the product tends to deteriorate. On the other hand, the lower limit of the oxygen concentration is not particularly determined, but is, for example, 0.05 ppm or more. In the production of polyamide, there is no problem if the oxygen concentration is less than 0.05 ppm, but in order to achieve less than 0.05 ppm, the oxygen removal process becomes unnecessarily complicated, and there is almost no effect on the color tone and other physical properties. The preferable range of the oxygen concentration is 0.05 ppm or more and 9 ppm or less, and more preferably 0.05 ppm or more and 8 ppm or less.

[0055] In the present invention, it is preferable to supply raw materials to a blending tank (melting tank or raw material salt formation tank) from which oxygen has been removed in advance to an oxygen concentration of 10 ppm or less, or to remove oxygen after the raw materials are charged into the blending tank (melting tank or raw material salt formation tank) to adjust the atmosphere in the blending tank to an oxygen concentration of 10 ppm or less, or to use both. This can be selected from the viewpoint of facilities or operation. It is also preferable to adjust the atmosphere in a storage tank to an oxygen concentration of 10 ppm or less.

[0056] The method for removing oxygen includes a vacuum replacement method, a pressure replacement method, or a combination of the two. The degree of vacuum or pressure applied to the replacement and the number of replacements can be selected based on the most efficient conditions for achieving the desired oxygen concentration.

[0057] (2) Raw material introduction process The salt solution prepared in the raw material preparation step is continuously introduced through a pipeline by a feed pump into the inlet of the tubular reactor of the amidation step.

[0058] (3) Amidation step In the amidation step, an aqueous salt solution continuously introduced into the inlet of the tubular reactor is passed through the tubular reactor to carry out amidation, thereby obtaining a reaction mixture containing an amidation product with a low degree of polymerization and condensation water. Water is not separated and removed in the tubular reactor.

[0059] The tubular reactor preferably has an L / D of 50 or more, where D (mm) is the inner diameter of the tube and L (mm) is the length of the tube. The tubular reactor has the advantages of not requiring liquid level control due to its structure, high plug flow properties, excellent pressure resistance, and low equipment costs. When L / D is less than 50, if L is small, the residence time of the reaction mixture flow is short and the degree of increase in relative viscosity (RV) is small, while if D is large, the plug flow properties are small, a residence time distribution is formed, and the desired function is not achieved. There is no particular upper limit for L / D, but it is about 3000 considering the residence time and the degree of increase in relative viscosity (RV). The lower limit of L / D is more preferably 60 or more, more preferably 80 or more, and the upper limit is more preferably 2000 or less, even more preferably 1000 or less. Moreover, the lower limit of L is preferably 3 m or more, and more preferably 5 m or more, and the upper limit of L is preferably 50 m or less, and more preferably 30 m or less.

[0060] The reaction conditions vary depending on the structure of the polyamide and the desired degree of polymerization, but for example, the internal temperature is 110 to 310°C, the internal pressure is 0 to 5 MPa, and the average residence time of the reaction mixture in the tube is 10 to 120 minutes. The degree of polymerization of the amidation product can be controlled by the internal temperature, internal pressure, and average residence time.

[0061] If the average residence time is shorter than 10 minutes, the degree of polymerization of the low-polymerization amidation product will be low, and as a result, the diamine component will be easily scattered during the polycondensation process, making it difficult to adjust the end group. On the other hand, if the average residence time is longer than 120 minutes, the amidation will reach equilibrium, the increase in RV will plateau, and thermal degradation will progress, which is not preferable. The desirable average residence time is 12 to 110 minutes, and more desirably 15 to 100 minutes. The average residence time can be controlled by adjusting the inner diameter D and length L of the tube of the tubular reactor, or by changing the amount of raw material supplied.

[0062] It is preferable that the relative viscosity (RV) of the reaction mixture is increased by 0.05 to 0.6 at the inlet and outlet of the tubular reactor by the polycondensation reaction in the amidation step. If the increase in RV is less than 0.05, the diamine component is likely to scatter during the polycondensation step, making it difficult to adjust the end groups. On the other hand, if the increase in RV is more than 0.6, thermal degradation is likely to progress due to the influence of the coexisting condensation water (in the case of the salt formation method, the water used for salt formation and the condensation water). In addition, a reaction mixture with an excessively increased viscosity may cause pipe clogging, which may adversely affect operation. The desirable range of increase in RV in the amidation step is 0.15 to 0.5, more preferably 0.2 to 0.4.

[0063] (4) Polycondensation process The reaction conditions in the initial polymerization step are an internal pressure of 0 to 5 MPa, an average residence time of 10 to 150 minutes, and an internal temperature determined according to Flory's melting point depression formula based on the residual moisture content in the can. Desirable reaction conditions are an internal temperature of 230 to 285°C, an internal pressure of 0.5 to 4.5 MPa, and an average residence time of 15 to 140 minutes, and more desirably an internal temperature of 235 to 280°C, an internal pressure of 1.0 to 4.0 MPa, and an average residence time of 20 to 130 minutes. If the reaction conditions are outside the lower limit of the above range, the degree of polymerization achieved is too low, or the resin solidifies in the can, which is undesirable. If the reaction conditions are outside the upper limit of the above range, decomposition of the P3 component and side reactions occur simultaneously, resulting in a P3 content of less than 30 ppm, which is disadvantageous in terms of heat yellowing resistance and gelling properties.

[0064] (5) Solid phase polymerization process The solid-state polymerization in the present invention refers to a process in which a polymerization reaction is carried out under vacuum or nitrogen gas flow at any temperature within a range in which the semi-aromatic polyamide does not melt. The equipment for carrying out the solid-state polymerization is not particularly limited, but examples thereof include a blender and a vacuum dryer. The preferable reaction conditions are an internal temperature of 200 to 260°C and an internal pressure of 0.7 KPa or less, and the more preferable reaction conditions are an internal temperature of 210 to 250°C and an internal pressure of 0.4 KPa or less.

[0065] Although it is possible to melt-polymerize the polyamide prepolymer obtained in the polycondensation process in a twin-screw extruder and thicken it to a specified RV, the thermal history during melting causes decomposition of the P3 component and side reactions, which are disadvantageous in terms of heat yellowing resistance and gelation properties.In addition, low molecular weight substances such as oligomers remain in the semi-aromatic polyamide, making it unsuitable from the perspective of outgassing during the subsequent melt molding process.

[0066] The amount of the semi-aromatic polyamide (A) is 30 to 75 mass%, preferably 35 to 70 mass%, more preferably 40 to 67 mass%, and further preferably 45 to 65 mass%, based on 100 mass% of the inorganic reinforced semi-aromatic polyamide resin composition. In the inorganic reinforced semi-aromatic polyamide resin composition of the present invention, the amount is directly the content in the inorganic reinforced semi-aromatic polyamide resin composition.

[0067] The inorganic reinforcing material (B) in the present invention is one that most effectively improves physical properties such as strength, rigidity, and heat resistance, and specifically includes fibrous materials such as glass fibers, carbon fibers, alumina fibers, silicon carbide fibers, and zirconia fibers, whiskers such as aluminum borate and potassium titanate, acicular wollastonite, milled fibers, etc. In addition to these, glass beads, glass flakes, glass balloons, silica, talc, kaolin, wollastonite, mica, alumina, hydrotalcite, montmorillonite, graphite, carbon nanotubes, fullerenes, zinc oxide, indium oxide, tin oxide, iron oxide, titanium oxide, magnesium oxide, aluminum hydroxide, magnesium hydroxide, red phosphorus, calcium carbonate, potassium titanate, lead zirconate titanate, barium titanate, aluminum nitride, boron nitride, zinc borate, aluminum borate, barium sulfate, magnesium sulfate, layered silicate that has been subjected to organic treatment for the purpose of delamination, and other fillers can also be used as the inorganic reinforcing material (B). Among these, glass fiber, carbon fiber, etc. are particularly preferably used. These inorganic reinforcing materials (B) may be used alone or in combination of two or more kinds.

[0068] When a fibrous reinforcing material is used as the inorganic reinforcing material (B), among the above, glass fiber, carbon fiber, etc. are particularly preferably used. These fibrous reinforcing materials are preferably pretreated with a coupling agent such as an organic silane compound, an organic titanium compound, an organic borane compound, and an epoxy compound, and are particularly preferably those that react easily with a carboxylic acid group or / and a carboxylic anhydride group. Polyamide resin compositions containing glass fibers treated with a coupling agent are preferred because they can provide molded products with excellent mechanical properties and appearance properties. In addition, other fibrous reinforcing materials can also be used by adding a coupling agent after the untreated one.

[0069] When the inorganic reinforcing material (B) is glass fiber, it is preferable to use a chopped strand cut to a fiber length of about 1 to 20 mm. As the cross-sectional shape of the glass fiber, glass fibers having a circular cross section and a noncircular cross section can be used. As the cross-sectional shape of the glass fiber, glass fibers having a noncircular cross section are preferable from the viewpoint of physical properties. Glass fibers having a noncircular cross section include those having a substantially elliptical, substantially oval, or substantially cocoon-shaped cross section perpendicular to the longitudinal direction of the fiber, and the flatness is preferably 1.5 to 8. Here, the flatness is the ratio of the major axis / minor axis when a rectangle having the minimum area circumscribing the cross section perpendicular to the longitudinal direction of the glass fiber is assumed, and the length of the long side of this rectangle is the major axis and the length of the short side is the minor axis. The thickness of the glass fiber is not particularly limited, but the minor axis is about 1 to 20 μm and the major axis is about 2 to 100 μm.

[0070] The amount of inorganic reinforcing material (B) is 25-65% by mass, preferably 30-60% by mass, more preferably 33-55% by mass, and even more preferably 35-50% by mass, based on 100% by mass of the inorganic reinforced semi-aromatic polyamide resin composition. If the amount exceeds 65% by mass, the productivity is deteriorated. If the amount is less than 25% by mass, the effect of the reinforcing material may not be fully exhibited, and the shear force during kneading with the semi-aromatic polyamide (A) component may be insufficient, and the thickening reaction of the (A) component may not proceed sufficiently. In the inorganic reinforced semi-aromatic polyamide resin composition of the present invention, the amount of the inorganic reinforced semi-aromatic polyamide resin composition is the content in the inorganic reinforced semi-aromatic polyamide resin composition.

[0071] As fillers other than the inorganic reinforcing material (B), conductive fillers, magnetic fillers, flame-retardant fillers, and thermally conductive fillers can be used for different purposes other than reinforcing fillers. Specific examples include glass beads, glass flakes, glass balloons, silica, talc, kaolin, wollastonite, mica, alumina, hydrotalcite, montmorillonite, hydroxyapatite, graphite, carbon nanotubes, fullerenes, zinc oxide, indium oxide, tin oxide, iron oxide, titanium oxide, magnesium oxide, aluminum hydroxide, magnesium hydroxide, red phosphorus, calcium carbonate, potassium titanate, lead zirconate titanate, barium titanate, aluminum nitride, boron nitride, zinc borate, aluminum borate, barium sulfate, magnesium sulfate, zinc sulfide, iron, aluminum, copper, and silver. These fillers may be used alone or in combination of several types. The shape is not particularly limited, but needle-shaped, spherical, plate-shaped, and amorphous shapes can be used. be.

[0072] The inorganic reinforced semi-aromatic polyamide resin composition of the present invention can contain various additives for conventional polyamides, such as stabilizers, impact modifiers, flame retardants, release agents, sliding properties modifiers, colorants, plasticizers, crystal nucleating agents, polyamide resins different from the semi-aromatic polyamide (A) of the present invention, and thermoplastic resins other than polyamide resins.

[0073] Examples of the stabilizer include organic antioxidants such as hindered phenol antioxidants, sulfur antioxidants, and phosphorus antioxidants, heat stabilizers, light stabilizers such as hindered amines, benzophenones, and imidazoles, ultraviolet absorbers, metal deactivators, and copper compounds. Examples of the copper compound include copper salts of organic carboxylic acids such as cuprous chloride, cuprous bromide, cuprous iodide, cupric chloride, cupric bromide, cupric iodide, cupric phosphate, cupric pyrophosphate, copper sulfide, copper nitrate, and copper acetate. In addition, it is preferable to contain an alkali metal halide compound as a component other than the copper compound, and examples of the alkali metal halide compound include lithium chloride, lithium bromide, lithium iodide, sodium fluoride, sodium chloride, sodium bromide, sodium iodide, potassium fluoride, potassium chloride, potassium bromide, and potassium iodide. These additives may be used alone or in combination of several types.

[0074] In addition, the inorganic reinforced semi-aromatic polyamide resin composition of the present invention may be polymer blended with a polyamide resin having a composition different from that of the semi-aromatic polyamide (A).

[0075] The inorganic reinforced semi-aromatic polyamide resin composition of the present invention may contain a thermoplastic resin other than the polyamide resin. These thermoplastic resins may be blended in a molten state by melt kneading, but the thermoplastic resin may be made fibrous or granular and dispersed in the composition of the present invention.

[0076] Examples of impact improvers include polyolefin resins such as ethylene-propylene rubber (EPM), ethylene-propylene-diene rubber (EPDM), ethylene-acrylic acid copolymer, ethylene-acrylic acid ester copolymer, ethylene-methacrylic acid copolymer, ethylene-methacrylic acid ester copolymer, and ethylene-vinyl acetate copolymer; vinyl polymer resins such as styrene-butadiene-styrene block copolymer (SBS), styrene-ethylene-butylene-styrene block copolymer (SEBS), styrene-isoprene-styrene copolymer (SIS), and acrylic acid ester copolymer; polyester block copolymers having polybutylene terephthalate or polybutylene naphthalate as a hard segment and polytetramethylene glycol, polycaprolactone, or polycarbonate diol as a soft segment; nylon elastomers, urethane elastomers, silicone rubber, fluorine-based rubber, and polymer particles having a core-shell structure composed of two different polymers.

[0077] The flame retardant may be a halogen-based flame retardant, a non-halogen-based flame retardant, or a flame retardant auxiliary, which may be used alone or in combination.

[0078] Examples of halogen-based flame retardants include brominated polystyrene, brominated polyphenylene ether, brominated bisphenol type epoxy polymers, brominated styrene-maleic anhydride polymers, brominated epoxy resins, brominated phenoxy resins, decabromodiphenyl ether, decabromo biphenyl, brominated polycarbonate, perchlorocyclopentadecane, and brominated crosslinked aromatic polymers.

[0079] Examples of non-halogen flame retardants include melamine cyanurate, red phosphorus, metal salts of phosphinic acid, and nitrogen-containing phosphoric acid compounds.

[0080] Examples of the flame retardant auxiliary include antimony compounds such as antimony trioxide, antimony pentoxide, and sodium antimonate, zinc stannate, zinc borate, zinc sulfide, molybdenum compounds, iron oxide, aluminum hydroxide, magnesium hydroxide, silicone resins, fluororesins, montmorillonite, silica, and metal carbonates.

[0081] Examples of the release agent include long-chain fatty acids or their esters or metal salts, amide compounds, polyethylene wax, silicone, and polyethylene oxide.

[0082] Examples of the sliding property improver include high molecular weight polyethylene, acid-modified high molecular weight polyethylene, fluororesin powder, molybdenum disulfide, silicone resin, silicone oil, zinc, graphite, and mineral oil.

[0083] In the inorganically reinforced semi-aromatic polyamide resin composition of the present invention, the total of the semi-aromatic polyamide (A) and the inorganic reinforcing material (B) preferably accounts for 80 mass% or more, more preferably 90 mass% or more, and even more preferably 95 mass% or more.

[0084] The method for producing the inorganic reinforced semi-aromatic polyamide resin composition of the present invention is not particularly limited, and for example, each component can be melt-kneaded by a conventionally known kneading method. There is also no limitation on the specific kneading device, and examples include single-screw or twin-screw extruders, kneaders, kneaders, etc., but twin-screw extruders are particularly preferred in terms of productivity. There is also no particular limitation on the screw arrangement, but it is preferable to provide a kneading zone in order to disperse each component more uniformly. A specific method includes pre-blending the semi-aromatic polyamide (A) and other additive components in a blender, feeding them from a hopper into a single-screw or twin-screw extruder, and then feeding the inorganic reinforcement (B) into the molten mixture with a feeder into a single-screw or twin-screw extruder while at least a part of (A) is in a molten state, and discharging the mixture in the form of a strand after melt kneading, cooling, and cutting.

[0085] When the inorganic reinforcing material (B) in the molded product obtained from the inorganic reinforced semi-aromatic polyamide resin composition of the present invention is a fibrous reinforcing material, the weight average of the remaining fiber length is preferably 200 to 500 μm. The measurement of the remaining fiber length is performed as follows. In a highly filled material, there is a lot of interference between fibers, and the fibrous reinforcing material is easily damaged during measurement, making it difficult to obtain an accurate fiber length. In order to accurately measure the fiber length in the present invention, the pellets obtained by melt kneading are ignited at 650° C. for 2 hours, and the fibrous reinforcing material is taken out as ash without being damaged, and the obtained fibrous reinforcing material is immersed in water and dispersed in a commonly used ultrasonic cleaner. The dispersed fibrous reinforcing material is taken out on a preparation and observed with a digital microscope (KH-7700 manufactured by Hirox Co., Ltd.) at 80 times to obtain the weight average fiber length, This is the remaining fiber length. The shape of the pellets is not particularly limited as long as it is a commonly obtained shape. For example, the cross section is either circular, elliptical, or oblong, the diameter (including the minor and major axes) is 2.0 mm to 4.0 mm, and the length of the pellets is about 2.5 to 6.0 mm. The conditions for pelletization are not particularly limited as long as they are commonly used conditions. For example, the method in the examples described later can be mentioned.

[0086] The AEG and CEG of the semi-aromatic polyamide (A) in the inorganic reinforced semi-aromatic polyamide resin composition of the present invention are usually smaller than those of the semi-aromatic polyamide (A). This is because some of the end groups react due to melt kneading under high temperature conditions during production, causing a slight increase in viscosity. In a composition containing 25 mass % or more of inorganic reinforcement (B), a higher shear is applied to the semi-aromatic polyamide, so the thickening reaction proceeds further, and the AEG and CEG become smaller. The amount of decrease in AEG and CEG cannot be generalized because it is affected by production conditions such as resin temperature, rotation speed, and kneading time, but as a guideline, the AEG and CEG decrease by 10 to 50 eq / t in one kneading, and approximately the same amount. Hereinafter, when referring to "the end group of the semi-aromatic polyamide (A) in the inorganic reinforced semi-aromatic polyamide resin composition", it may be simply abbreviated to "the end group of the inorganic reinforced semi-aromatic polyamide resin composition".

[0087] Therefore, (AEG+CEG) of the inorganic reinforced semi-aromatic polyamide resin composition is 0 to 130 eq / t, preferably 0 to 120 eq / t, and more preferably 0 to 110 eq / t. If (AEG+CEG) exceeds 130 eq / t, the amount of endblocking is small and the amount of remaining AEG and CEG is large, so that the composition thickens and gels when melted during molding.

[0088] The inorganic reinforced semi-aromatic polyamide resin composition of the present invention has a ratio (AEG+CEG) / (AEG+CEG+EC) of 0.60 or less, preferably 0.55 or less, more preferably 0.50 or less, further preferably 0.45 or less, and particularly preferably 0.40 or less. If the ratio (AEG+CEG) / (AEG+CEG+EC) exceeds 0.60, the content of the end-capping agent is low and the amount of remaining AEG and CEG is large, resulting in thickening and gelation during melt molding.

[0089] The AEG, CEG, and EC of the inorganic reinforced semi-aromatic polyamide resin composition may satisfy the above-mentioned relationship, and the preferred ranges of each are as follows. The AEG is preferably 0 to 70 eq / t, more preferably 0 to 40 eq / t, even more preferably 0 to 30 eq / t, and particularly preferably 0 to 20 eq / t. The CEG is preferably 0 to 130 eq / t, more preferably 0 to 100 eq / t, even more preferably 0 to 70 eq / t, and particularly preferably 0 to 50 eq / t. The EC is preferably 60 to 240 eq / t, more preferably 80 to 200 eq / t, and even more preferably 80 to 170 eq / t.

[0090] In addition, in general, polyamide resins thicken as a result of the reaction between the amino end and the carboxyl end. However, thickening can also occur when CEG reacts with EC. If AEG is lost (reduced to 0) during the amidation reaction, the ends of the semi-aromatic polyamide become CEG and EC. In the absence of AEG, the acid catalyst effect of CEG causes CEG to attack the amide bond formed by the end-capping agent, resulting in an amide exchange reaction. At this time, the thickening reaction proceeds while the end-capping agent is distilled out of the reaction system. This results in an increase in outgassing components derived from the end-capping agent. In addition, the acid component of CEG causes a coloring reaction to occur at the same time, resulting in a resin with poor color stability and prone to gelation. In order to avoid such phenomena, it is important to satisfy the above formulas (1) and (2).

[0091] In addition, the rate of decrease in bending strength calculated from the bending strength before and after treatment of the inorganic reinforced semi-aromatic polyamide resin composition of the present invention in a high temperature and high humidity environment of 80°C and 95% RH for 500 hours is preferably less than 15%, more preferably less than 10%, and even more preferably less than 8%. If it is 15% or more, the rigidity varies depending on the humidity, which is undesirable because it adversely affects the properties of precision electronic parts. The rate of decrease in bending strength can be measured by the method described in the Examples section below.

[0092] In order to mold micro-precise electronic components, it is preferable that the flow length of the inorganic reinforced semi-aromatic polyamide resin composition of the present invention at a thickness of 0.2 mm is 3 mm or more. The flow length can be measured by the method described in the Examples section below.

[0093] The inorganic reinforced semi-aromatic polyamide resin composition of the present invention preferably generates 300 ppm or less gas (outgas) when thermally decomposed at 350°C for 10 minutes. When the semi-aromatic polyamide (A) is further mixed with a fibrous reinforcing material (B) or the like, thermal decomposition proceeds, and the gas amount of the composition increases compared to the gas amount of the (A) component alone. However, by satisfying the above range, a molded product with good appearance can be obtained. The gas amount (outgas) can be measured by the method described in the Examples section below.

[0094] The inorganic reinforced semi-aromatic polyamide resin composition of the present invention preferably has a tensile fracture strain of 0.3 to 3.4%. The inorganic reinforced semi-aromatic polyamide resin composition of the present invention can have a tensile fracture strain in this range by satisfying the above-mentioned configuration. Having a tensile fracture strain in this range is advantageous in that cracking during assembly or use as a part can be suppressed, and loosening of fixed parts can be suppressed, thereby obtaining sufficient fixing force. The tensile fracture strain can be measured by the method described in the Examples section below.

[0095] The inorganic reinforced semi-aromatic polyamide resin composition of the present invention preferably has a tensile strength of 100 MPa or more. More preferably, it is 150 MPa or more, and even more preferably, it is 180 MPa or more. The inorganic reinforced semi-aromatic polyamide resin composition of the present invention can have a tensile strength within this range by satisfying the above-mentioned configuration. Having a tensile strength within this range is advantageous in that the occurrence of cracks during assembly or use as a part can be suppressed. The tensile strength can be measured by the method described in the Examples section below.

[0096] Molded articles obtained from the inorganically reinforced semi-aromatic polyamide resin composition of the present invention have excellent heat resistance and excellent color stability under actual usage environments, and therefore can be suitably used as electrical and electronic components such as connectors, switches, relays, and printed wiring boards that require heat resistance, as well as parts that have a light-reflecting function, such as LEDs and reflectors for lighting fixtures.

[0097] In addition, since the inorganically reinforced semi-aromatic polyamide resin composition of the present invention has excellent heat resistance and excellent melt processability, it can be highly filled with reinforcing materials, fillers, etc., and can be used for automobile parts such as engine peripheral parts, cooling parts, and fuel parts that require high rigidity, as well as industrial parts such as gears, screws, and other sliding parts. EXAMPLES

[0098] The present invention will be specifically described below by showing examples, but the present invention is not limited to these examples.

[0099] (1) Outgassing 3 mg of inorganic reinforced semi-aromatic polyamide resin composition pellets were weighed, and the amount of gas generated under He at 350°C for 10 minutes was measured using a pyrolysis GC / MS (Shimadzu PY-2020iD). The quantitative value was converted using dimethylsiloxane cyclic tetramer as the standard substance. Column: Rxi-5ms, injection port pressure: 80KPa, split ratio: 30, column oven temperature: 40°C (2 minutes) - 300°C (15 minutes), heating rate: 10 minutes / °C, mass measurement range: m / z 30-550.

[0100] (2)RV 0.25 g of the semi-aromatic polyamide (A) was dissolved in 25 ml of 96% sulfuric acid, and 10 ml of this solution was placed in an Ostwald viscosity tube and measured at 20° C. to obtain the viscosity from the following formula. RV=t / t0 (where t0 is the number of seconds the solvent falls, and t is the number of seconds the sample solution falls)

[0101] (3)AEG, CEG, EC, composition 20 mg of semi-aromatic polyamide was dissolved in 0.6 ml of a mixed solvent of deuterated chloroform (CDCl3) / hexafluoroisopropanol (HFIP) = 1 / 1 (vol ratio), and diformic acid was added dropwise. Then, the reaction mixture was analyzed using a 500 MHz Fourier transform nuclear magnetic resonance apparatus (AVANCE500 manufactured by BRUKER). 1 H-NMR analysis was performed, and the AEG, CEG, and EC of the semi-aromatic polyamide were determined from the integral ratio. The inorganic reinforced semi-aromatic polyamide resin compositions AEG, CEG and EC were dissolved in a mixed solvent, centrifuged, the supernatant was taken out, polyformic acid was added dropwise and the measurement was performed in the same manner.

[0102] (4) Melting point 5 mg of the semi-aromatic polyamide was placed in an aluminum sample pan and sealed. The polyamide was measured using a differential scanning calorimeter (DSC) DSC-Q100 (TA Instruments Japan, Inc.) at a heating rate of 20°C / min up to 350°C, and the maximum peak temperature of the heat of fusion was determined as the crystalline melting point.

[0103] (5) Quantification of P compounds The sample was dissolved by the yttrium nitrate method and analyzed by ICP (SPECTROBLUUE, Hitachi High-Tech Science). 0.1 g of sample was weighed into a platinum crucible, and 5 mL of a 5% ethanol solution of yttrium nitrate was added to perform nitrate ashing. 20 mL of 1.2 N hydrochloric acid was added to the ashing residue and it was soaked overnight. After confirming that the resin components were completely dissolved, the solution was centrifuged to remove the supernatant, and the solution was subjected to an ICP emission spectrometer to measure the phosphorus emission intensity at a wavelength of 214 nm. The phosphorus concentration in the solution was quantified and then converted to the phosphorus content in the sample.

[0104] (6) Structural analysis of P compounds 340-350 mg of sample was dissolved in 2.5 ml of a mixed solvent of deuterated chloroform (CDCl3) / hexafluoroisopropanol (HFIP) = 1 / 1 (vol ratio) at room temperature, centrifuged, and the supernatant was removed. Tri(t-butylphenyl)phosphoric acid (hereafter abbreviated as TBPPA) was added as P to the polyamide resin at 100 ppm, and 0.1 ml of trifluoroacetic acid was added at room temperature. After 30 minutes, the sample was analyzed by a Fourier transform nuclear magnetic resonance apparatus (BRUKER AVANCE500). 31 P-NMR analysis was performed. 31 The analysis was performed under the conditions of P resonance frequency of 202.5 MHz, detection pulse flip angle of 45°, data acquisition time of 1.5 seconds, delay time of 1.0 seconds, number of integrations of 1,000 to 20,000, measurement temperature of room temperature, and complete proton decoupling, and the molar ratio of the phosphorus compound represented by structural formula (P1) and the phosphorus compound represented by structural formula (P2) was calculated from the integral ratio.

[0105] (7) Calculation of P3 The amount of P compounds determined by ICP above and 31 The amounts of P1 and P2 were calculated from the molar ratios of P1 and P2 determined by P-NMR, and their sum was determined as P3.

[0106] (8)ΔCo-b 10 g of the inorganic reinforced semi-aromatic polyamide resin composition was frozen with liquid nitrogen, then pulverized in a pulverizer (Osaka Chemical Co., Ltd., ABLOLUTE 3) at 15,000 rpm for 3 minutes to obtain a powder. The Co-b of the pulverized inorganic reinforced semi-aromatic polyamide resin composition was measured using a color meter (Nippon Denshoku Co., Ltd., ZE 2000). The polyamide resin composition powder was thinly spread on a petri dish and placed in a gear oven (TABAI Co., Ltd., GEER OVEN GHPS-222) heated to 260°C, and the Co-b value of the resin composition was measured after heat treatment for 10 minutes under air, and the difference before and after heat treatment was taken as ΔCo-b.

[0107] (9) Gel time 3 g of the inorganic reinforced semi-aromatic polyamide resin composition was placed in an ampoule and heat-treated for a predetermined time in an inert oven (TAMATO DN4101) heated to 330° C. under a nitrogen gas flow of 10 l / min. 0.25 g of the heat-treated resin composition was dissolved in 25 ml of 96% sulfuric acid, and the heat treatment time at which insoluble matter appeared was defined as the gelation time.

[0108] (10) Flow length Using a Toshiba Machine EC-100 injection molding machine, the cylinder temperature was set at 330°C, the mold temperature at 140°C, the injection pressure set at 40%, the injection speed set at 40%, the measurement at 35mm, the injection time at 6 seconds, and the cooling time at 10 seconds, the mold for measuring flow length was injection molded with a width of 1mm and a thickness of 0.2mm to prepare a test piece for evaluation. The flow length (mm) of this test piece was measured to evaluate the flowability.

[0109] (11) Tensile strength and tensile breaking strain Measurements were performed according to the ISO527-2 standard.

[0110] (12) Bending strength before and after high temperature and humidity treatment (water absorption), and rate of decrease due to water absorption The bending strength of ISO tensile test pieces (A-type dumbbell) was measured in accordance with ISO178 before and after 500 hours of treatment in a high-temperature, high-humidity environment of 80°C, 95% RH, and the following reduction rates (%) were calculated. Reduction rate (%) = {(bending strength before treatment - bending strength after treatment) / bending strength before treatment} x 100

[0111] (13) Solder heat resistance Using a Toshiba Machine injection molding machine EC-100, the cylinder temperature was set to the melting point of the resin + 20℃, the mold temperature was set to 140℃, and a UL combustion test piece with a length of 127 mm, width of 12.6 mm, and thickness of 0.8 mmt was injection molded to prepare a test piece. The test piece was left in an atmosphere of 85℃ and 85%RH (relative humidity) for 72 hours. The test piece was preheated in an air reflow furnace (Atec AIS-20-82C) by raising the temperature from room temperature to 150℃ over 60 seconds, and then preheated to 190℃ at a heating rate of 0.5℃ / min. The temperature was then raised to a specified set temperature at a rate of 100℃ / min, held at the specified temperature for 10 seconds, and then cooled. The set temperature was increased in 5℃ increments from 240℃, and the highest set temperature at which no swelling or deformation of the surface occurred was used as an index of solder heat resistance as the reflow heat resistance temperature. ◎: Reflow heat resistance temperature is 280℃ or higher ○: Reflow heat resistance temperature is 260℃ or higher and less than 280℃ ×: Reflow heat resistance temperature is less than 260℃

[0112] (14) Continuous formability Using a Toshiba Machine EC-100 injection molding machine, molding was performed with a cylinder temperature of 330°C, a mold temperature of 140°C, injection for 6 seconds, cooling for 10 seconds, and a 100 x 100 x 2 mmt mold (material: STVAX), and the results were evaluated using the following criteria. XX: Gas components adhere to the molded product in less than 30 shots. Gas components that adhere to the mold gel and take a long time to wipe off. ×: Gas components adhere to the molded product within 30 to 300 shots. △: Gas components adhere to the molded product within 300 to 500 shots. ○: No gas components adhere to the molded product even after 500 shots or more.

[0113] (15) Weld strength Using a Toshiba Machine EC-100 injection molding machine, the molten resin composition was poured into both ends at a cylinder temperature of 330°C and a mold temperature of 140°C to mold test pieces with a size of 125 mm x 13 mm x 0.8 mmt, with a weld formed in the center, and measurements were then performed in accordance with ISO527-1.

[0114] (16) Weld Appearance The appearance of the welds in the molded products produced in (15) was evaluated using the following criteria. ×: Both weld lines and gas burns were observed. △: Almost no weld lines were observed, but some gas burns were observed. ○: Almost no weld lines observed, no gas burns

[0115] Synthesis Example 1 9.13 kg (78.6 mol) of 1,6-hexamethylenediamine, 12.24 kg (73.7 mol) of terephthalic acid, 7.99 kg (39.7 mol) of 11-aminoundecanoic acid, 30.4 g of sodium hypophosphite as a catalyst, 354 g (5.9 mol) of acetic acid as an end-capping agent, and 16.20 kg of ion-exchanged water adjusted to 0.5 ppm or less by nitrogen bubbling were charged into a 50-liter autoclave, pressurized from normal pressure to 0.05 MPa with N2, released, and returned to normal pressure. This operation was repeated 10 times, and after N2 replacement, the mixture was uniformly dissolved at 135°C and 0.3 MPa under stirring. Thereafter, the solution was continuously supplied by a liquid delivery pump, heated to 260°C with a heating pipe, and heated for 0.5 hours. The reaction mixture was then fed into a pressurized reactor and heated to 270°C. Part of the water was distilled off so as to maintain the internal pressure of the reactor at 3 MPa, yielding a low-order condensate. The low-order condensate was then taken out into a vessel at room temperature and pressure in the atmosphere, and dried at 70°C and at a vacuum of 0.07 KPa or less using a vacuum dryer. After drying, the low-order condensate was transferred to a blender (capacity 0.1 m) and mixed with water to obtain a low-order condensate. 3 ) was reacted for 8 hours in an environment of 225°C and a vacuum degree of 0.07 KPa to obtain semi-aromatic polyamide A-1. The properties of the obtained semi-aromatic polyamide are shown in Table 1.

[0116] Synthesis Example 2 The amount of 1,6-hexamethylenediamine was changed to 9.10 kg (78.3 mol), and the amount of acetic acid used as the end blocking agent was changed to 301 g (5.0 mol). The procedure was carried out in the same manner as in Synthesis Example 1 up to vacuum drying to obtain a low-order condensation product. 3 ) was reacted for 8 hours in an environment of 240°C and a vacuum degree of 0.07 KPa to obtain semi-aromatic polyamide A-2.

[0117] Synthesis Example 3 The amount of 1,6-hexamethylenediamine was changed to 8.84 kg (76.1 mol), and the amount of acetic acid used as the end blocking agent was changed to 286 g (4.8 mol). The mixture was subjected to vacuum drying in the same manner as in Synthesis Example 1 to obtain a low-order condensation product. 3 ) was reacted for 8 hours at 230°C under a vacuum of 0.07 KPa to obtain semi-aromatic polyamide A-3.

[0118] Synthesis Example 4 The amount of 1,6-hexamethylenediamine was changed to 9.21 kg (79.3 mol), and the amount of acetic acid used as the end blocking agent was changed to 315 g (5.2 mol), and the mixture was subjected to vacuum drying in the same manner as in Synthesis Example 1 to obtain a low-order condensation product. 3 ) was reacted for 8 hours at 240°C under a vacuum of 0.07 KPa to obtain semi-aromatic polyamide A-4.

[0119] Synthesis Example 5 The amount of 1,6-hexamethylenediamine was changed to 9.11 kg (78.4 mol), and the amount of benzoic acid used as the end blocking agent was changed to 612 g (5.0 mol), and the mixture was subjected to vacuum drying in the same manner as in Synthesis Example 1 to obtain a low-order condensation product. 3 ) was reacted for 8 hours at 240°C under a vacuum of 0.07 KPa to obtain semi-aromatic polyamide A-5.

[0120] Synthesis Example 6 9.00 kg (77.4 mol) of 1,6-hexamethylenediamine, 12.24 kg (73.7 mol) of terephthalic acid, 7.99 kg (39.7 mol) of 11-aminoundecanoic acid, 30.4 g of sodium hypophosphite as a catalyst, 226 g (3.8 mol) of acetic acid as an end-capping agent, and 16.20 kg of ion-exchanged water adjusted to 0.5 ppm or less by nitrogen bubbling were charged into a 50-liter autoclave, pressurized from normal pressure to 0.05 MPa with N2, released, and returned to normal pressure. This operation was repeated 10 times, and after N2 replacement, the mixture was uniformly dissolved at 135°C and 0.3 MPa under stirring. Thereafter, the solution was continuously supplied by a liquid delivery pump, heated to 260°C with a heating pipe, and heated for 0.5 hours. The reaction mixture was then fed into a pressurized reactor and heated to 290°C. Part of the water was distilled off so as to maintain the internal pressure of the reactor at 3 MPa, yielding a low-order condensate. The low-order condensate was then taken out into a vessel at room temperature and pressure in the atmosphere, and dried at 70°C and at a vacuum of 0.07 KPa or less using a vacuum dryer. After drying, the low-order condensate was transferred to a blender (capacity 0.1 m) and mixed with water to obtain a low-order condensate. 3 ) was reacted for 6 hours at 230°C under a vacuum of 0.07 KPa to obtain semi-aromatic polyamide A-6.

[0121] Synthesis Example 7 The amount of 1,6-hexamethylenediamine was changed to 8.89 kg (76.5 mol) and the amount of acetic acid as a terminal blocking agent was changed to 174 g (2.9 mol), and the process was carried out up to vacuum drying in the same manner as in Production Example 1 to obtain a low-order condensate. Next, the mixture was reacted for 8 hours in an environment of 245°C and a vacuum degree of 0.07 KPa using a blender (volume 0.1 m3), to obtain semi-aromatic polyamide A-7.

[0122] Synthesis Example 8 The amount of 1,6-hexamethylenediamine was changed to 8.93 kg (76.9 mol), and the amount of acetic acid as a terminal blocking agent was changed to 197 g (3.3 mol), and the process was carried out up to vacuum drying in the same manner as in Production Example 1 to obtain a low-order condensate. Next, the mixture was reacted for 15 hours in an environment of 245°C and a vacuum degree of 0.07 KPa using a blender (volume 0.1 m3), to obtain semi-aromatic polyamide A-8.

[0123] Synthesis Example 9 3.32 kg (20.0 mol) of terephthalic acid, 2.53 kg (16.0 mol) of 1,9-nonanediamine, 0.63 kg (4.0 mol) of 2-methyl-1,8-octanediamine, 6.5 g of sodium hypophosphite monohydrate as a catalyst, 103 g (0.80 mol) of octylamine as an end-capping agent, and 6 liters of ion-exchanged water adjusted to 0.5 ppm or less by nitrogen bubbling were charged into a 20-liter autoclave, pressurized from normal pressure to 0.05 MPa with N2, released, and returned to normal pressure. This operation was repeated 10 times, and after N2 replacement, the mixture was uniformly dissolved at 100°C and 0.3 MPa under stirring. Thereafter, the solution was continuously supplied by a liquid delivery pump, heated to 230°C with a heating pipe, and heated for 1.5 hours. The reaction mixture was then fed into a pressurized reactor and heated to 290°C. Part of the water was distilled off so as to maintain the internal pressure of the reactor at 3 MPa, yielding a low-order condensate. The low-order condensate was then taken out into a vessel at room temperature and pressure in the atmosphere, and dried at 100°C and at a vacuum of 0.07 KPa or less using a vacuum dryer. After drying, the low-order condensate was transferred to a blender (capacity 0.1 m) and mixed with water to obtain a low-order condensate. 3 ) was reacted for 6 hours at 230°C under a vacuum of 0.07KPa to obtain semi-aromatic polyamide A-9. The properties of the obtained semi-aromatic polyamide are shown in Table 1.

[0124] Synthesis Example 10 The amount of 1,6-hexamethylenediamine was changed to 8.72 kg (75.0 mol), and the amount of acetic acid used as the end blocking agent was changed to 32 g (0.5 mol). The procedure was carried out in the same manner as in Production Example 1 up to vacuum drying to obtain a low-order condensation product. 3 ) was reacted for 5 hours at 180°C under a vacuum of 0.07 KPa to obtain semi-aromatic polyamide A-10.

[0125] Synthesis Example 11 The amount of 1,6-hexamethylenediamine was changed to 8.57 kg (73.8 mol), acetic acid was changed to 140 g (2.3 mol) as an end-capping agent, and sodium hypophosphite was changed to 9 g as a catalyst, and the process was carried out up to vacuum drying in the same manner as in Production Example 1 to obtain a low-order condensation product. 3) was reacted for 4 hours at 220°C under a vacuum of 0.07 KPa to obtain semi-aromatic polyamide A-11.

[0126] Synthesis Example 12 7.54 kg (65.0 mol) of 1,6-hexamethylenediamine, 10.79 kg (65.0 mol) of terephthalic acid, 7.04 kg (35.0 mol) of 11-aminoundecanoic acid, 9 g of sodium hypophosphite as a catalyst, and 17.52 kg of ion-exchanged water were charged into a 50-liter autoclave, pressurized from normal pressure to 0.05 MPa with N2, released, and returned to normal pressure. This operation was repeated three times, and after N2 replacement, the mixture was uniformly dissolved at 135°C and 0.3 MPa under stirring. Thereafter, the solution was continuously supplied by a liquid delivery pump, heated to 240°C by a heating pipe, and heated for 1 hour. The reaction mixture was then supplied to a pressurized reaction vessel, heated to 290°C, and a portion of the water was distilled off so as to maintain the internal pressure of the vessel at 3 MPa, to obtain a low-order condensate (end-blocking rate 0%). Then, this low-order condensate was directly fed to a twin-screw extruder (screw diameter 37 mm, L / D=60) while maintaining the molten state, and polycondensation was carried out in the molten state while adding 107 g (1.8 mol) of acetic acid as an end-capping agent, maintaining the resin temperature at 335°C, and removing water from three vents, to obtain semi-aromatic polyamide A-12. The properties of the semi-aromatic polyamides obtained in each synthesis example are shown in Table 1.

[0127] [Table 1]

[0128] In the table, AcOH stands for acetic acid, BA for benzoic acid, and TOA for octylamine. Also, 9T stands for a unit consisting of 1,9-nonanediamine:2-methyl-1,8-octanediamine (4:1 molar ratio) and terephthalic acid.

[0129] Examples and Comparative Examples (Examples 3, 4, 7, and 9 are reference examples.) The semi-aromatic polyamide resin compositions of the Examples and Comparative Examples were obtained by melt-kneading at 330°C using a twin-screw extruder STS-35 manufactured by Coperion Co., Ltd., so that the content of the inorganic reinforcing material described below was 35 parts by mass for 63.8 parts by mass of each semi-aromatic polyamide of the Synthesis Examples, and the contents of the release agent and stabilizer were each 0.6 parts by mass. The evaluation results are shown in Table 2.

[0130] Inorganic reinforcement material (B): Glass fiber (Nippon Electric Glass Co., Ltd., ECS03T-275H) Release agent: Magnesium stearate Stabilizer: Potassium iodide

[0131] [Table 2]

[0132] In Comparative Example 1, AEG+CEG>130eq / t indicates that the amount of residual AEG and CEG is large, the resin composition is prone to gelation, and the moldability and appearance of the molded product are poor. In addition, (AEG+CEG) / (AEG+CEG+EC)>0.60 indicates that the amount of terminal blocking agent is small, and the resin composition is prone to gelation. In Comparative Example 2, (AEG+CEG) / (AEG+CEG+EC)>0.60, which indicates that the excess acid component at the carboxyl end promotes an amide exchange reaction, increasing the outgas component derived from the end blocking. In addition, a coloring reaction occurs at the same time, resulting in a resin composition that is poor in color stability and prone to gelation. In Comparative Example 3, since the melt polymerization was carried out using a twin-screw extruder and the viscosity was increased to a predetermined RV, no P3 component remained, and it is understood that the outgassing, ΔCo-b, and gelation time were deteriorated. [Industrial Applicability]

[0133] It is possible to provide an inorganically reinforced semi-aromatic polyamide resin composition that has excellent heat resistance and resistance to thermal discoloration, and furthermore can suppress mold contamination due to outgassing during melt molding, and has excellent melt fluidity and gelling properties, making it suitable for molded products such as automobile parts, bicycle parts, and electric / electronic parts. It is expected that this composition will make a significant contribution to the industrial world.

Claims

1. An inorganic reinforced semi-aromatic polyamide resin composition comprising 30 to 75 mass% of a semi-aromatic polyamide (A) and 25 to 65 mass% of an inorganic reinforcing material (B), The semi-aromatic polyamide (A) is at least one semi-aromatic polyamide containing a repeating unit formed by condensation of at least one aliphatic diamine containing two or more carbon atoms with terephthalic acid, and The semi-aromatic polyamide (A) is an inorganic reinforced semi-aromatic polyamide resin composition characterized in that it satisfies the following requirements (i) and (ii): (i) 7.5≦[number of carbon atoms in polyamide / number of amide bonds in polyamide] (ii) [number of carbon atoms on aromatic rings in polyamide / total number of carbon atoms in polyamide]≦0.35 The raw material semi-aromatic polyamide (A) has an amino end group concentration (AEG) of 5 to 33 eq / t and a carboxy end group concentration (CEG) of 11 to 50 eq / t, Further, the inorganic reinforced semi-aromatic polyamide resin composition has a relationship among the amino end group concentration (AEG), the carboxy end group concentration (CEG), and the end concentration (EC) of the amino end blocked with carboxylic acid of the semi-aromatic polyamide (A) in the inorganic reinforced semi-aromatic polyamide resin composition, which satisfies the formulas (1) and (2). 0eq / t≦AEG+CEG≦130eq / t... (1) (AEG+CEG) / (AEG+CEG+EC)≦0.50... (2)

2. The inorganic reinforced semi-aromatic polyamide resin composition according to claim 1, characterized in that the semi-aromatic polyamide (A) is a copolymer containing a structural unit formed by condensation of an aliphatic diamine having 2 to 12 carbon atoms with terephthalic acid, and at least one structural unit selected from aliphatic aminocarboxylic acids and lactams having 11 to 18 carbon atoms.

3. The inorganic reinforced semi-aromatic polyamide resin composition according to claim 1, wherein the semi-aromatic polyamide (A) is a copolymer containing 55 to 75 mol% of a structural unit formed by condensation of hexamethylenediamine and terephthalic acid, and 45 to 25 mol% of a structural unit formed by 11-aminoundecanoic acid or undecane lactam.

4. The inorganic reinforced semi-aromatic polyamide resin composition according to any one of claims 1 to 3, characterized in that the sum (P3) of the phosphorus atom contents derived from phosphorus compounds detected in the structures of structural formulas (P1) and (P2) in the semi-aromatic polyamide (A) is 30 ppm or more, and P3 is 10% or more relative to the total amount of phosphorus atoms remaining in the semi-aromatic polyamide. 【Chemistry 1】 【Chemistry 2】 (wherein R1 and R2 are hydrogen, an alkyl group, an aryl group, a cycloalkyl group, or an arylalkyl group; X1 to X3 are hydrogen, an alkyl group, an aryl group, a cycloalkyl group, an arylalkyl group, an alkali metal, or an alkaline earth metal; and in each formula, one of X1 to X3 and one of R1 to R2 may be bonded to each other to form a ring structure.)

5. 5. The inorganic reinforced semi-aromatic polyamide resin composition according to claim 1, wherein the amount of gas generated (outgassing) when pyrolyzed at 350° C. for 10 minutes is 300 ppm or less.

6. The inorganic reinforced semi-aromatic polyamide resin composition according to any one of claims 1 to 5, characterized in that the reduction rate of bending strength calculated from bending strength before and after treatment for 500 hours in a high temperature and high humidity environment of 80°C and 95% RH is less than 15%.

7. 7. The inorganic reinforced semi-aromatic polyamide resin composition according to claim 1, wherein the flow length at a thickness of 0.2 mm is 3 mm or more.

8. 8. The inorganic reinforced semi-aromatic polyamide resin composition according to claim 1, characterized in that the tensile breaking strain is 0.3 to 3.4%.

Citation Information

Patent Citations

  • Composition for infrared reflow and electronic part

    JP1991088846A

  • Polyamide and composition containing the polyamide

    JP2007092053A

  • Heat-resistant resin composition

    JP2007182550A

  • Polyamide resin composition and molded article comprising the same

    JP2008179753A

  • Method for producing polyamide composition, polyamide composition, and molded article composed of polyamide composition

    JP2010209247A