Thermoplastic elastomer composition and molded article thereof

A thermoplastic elastomer composition with a propylene-based polymer, styrene-based block copolymer, and halogen flame retardant addresses the challenge of maintaining flame retardancy and scratch resistance in thin automobile interior materials, ensuring excellent moldability and feel.

JP7567806B2Active Publication Date: 2024-10-16MCPP INNOVATION LLC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021558336
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-11-19
Filing Date
2020-11-12
Publication Date
2024-10-16
Estimated Expiration
2040-11-12

AI Technical Summary

Technical Problem

Existing thermoplastic elastomer compositions used in automobile interior materials face challenges in maintaining flame retardancy, moldability, and scratch resistance when the materials are thinned, as conventional flame retardants like magnesium hydroxide compromise these properties.

Method used

A thermoplastic elastomer composition containing a propylene-based polymer, a styrene-based block copolymer, a hydrocarbon-based rubber softener, and a halogen flame retardant, specifically with a balanced ratio of components to enhance flame retardancy while preserving moldability and scratch resistance.

Benefits of technology

The composition achieves high flame retardancy, excellent tactile feel, and effective scratch resistance, making it suitable for thin automobile interior materials without compromising injection moldability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567806000001
    Figure 0007567806000001
Patent Text Reader

Abstract

Provided are: a thermoplastic elastomer composition that exhibits excellent injection molding properties, texture, scratch resistance and flame retardancy; and a molded body thereof. This thermoplastic elastomer composition contains components (A) to (D) below. The content of component (D) is 0.01-30 parts by mass relative to a total of 100 parts by mass of components (A) to (D). The molded body is obtained by molding this thermoplastic elastomer composition. Component (A): a propylene-based polymer Component (B): a block copolymer having at least two polymer blocks P comprising mainly an aromatic vinyl compound unit and at least one polymer block Q comprising mainly a conjugated diene compound unit, and / or a hydrogenation product of this block copolymer Component (C): a softening agent for a hydrocarbon-based rubber Component (D): a halogen-based flame retardant
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoplastic elastomer composition and a molded article thereof. More specifically, the present invention relates to a thermoplastic elastomer composition having excellent injection moldability, touch, scratch resistance, and flame retardancy, and a molded article made of the thermoplastic elastomer composition. [Background technology]

[0002] Thermoplastic elastomers soften and become fluid when heated, and have rubber elasticity when cooled. Thermoplastic elastomers have moldability similar to that of thermoplastic resins, as well as unique rubber elasticity. They are also recyclable, and therefore are widely used in automobile parts, building parts, medical parts, electric wire coating materials, miscellaneous goods, and other applications.

[0003] Patent Document 1 discloses, as a thermoplastic elastomer composition for injection molding, a so-called styrene-based elastomer including a block copolymer consisting of at least one polymer block A mainly made of an aromatic vinyl compound and at least one polymer block B mainly made of a conjugated diene compound, a hydrogenated block copolymer obtained by hydrogenating the block copolymer, and a propylene-based block copolymer. Patent Document 1 also describes that the styrene-based elastomer can be used for automobile interior materials.

[0004] Styrene-based elastomers are also actively used in insulated electric wires, cables, and cords, optical fiber cores, and optical fiber cords used in the internal and external wiring of electric and electronic devices. In such cases, it is known that it is preferable to use non-halogen flame retardants in order to improve the heat dissipation and flame retardancy of electric and electronic devices, which are heat-generating bodies, and to consider the environmental impact. For example, Patent Documents 2 to 4 disclose that thermoplastic elastomers using magnesium hydroxide as a non-halogen flame retardant are used in thermoplastic elastomers for electronic and electronic devices such as insulated wires, cables, and cords.

[0005] [Patent Document 1] JP 2006-83323 A [Patent Document 2] JP 2012-107212 A [Patent Document 3] JP 2013-072033 A [Patent Document 4] JP 2013-072034 A

[0006] In recent years, there has been an increasing trend for the interior space of an automobile to have a more luxurious feel and be more comfortable as a living space. As a result, automobile interior materials, particularly the surface layers of automobile interior materials such as arm rests and console pads, are required to have good appearance, feel, and scratch resistance. Recently, the ease of molding and the simplification of the interior finishing process have improved, and the thickness of these skins has become thinner.

[0007] When the surface of an automobile interior material is made thinner, its flame retardancy decreases, so it is necessary to compensate for this decrease in flame retardancy by adding flame retardants. However, the flame retardants such as magnesium hydroxide disclosed in Patent Documents 2 to 4 are not sufficient to improve the decrease in flame retardancy that accompanies thinning in the above-mentioned applications. When an attempt is made to improve flame retardancy by blending a large amount of flame retardant, the touch and scratch resistance are deteriorated, and moldability and appearance are also impaired. Summary of the Invention

[0008] An object of the present invention is to provide a thermoplastic elastomer composition which is capable of exhibiting excellent injection moldability, good touch and scratch resistance, and which also has excellent flame retardancy, and a molded article made of this thermoplastic elastomer composition.

[0009] The present inventors have discovered that by blending a halogen-based flame retardant with a thermoplastic elastomer composition containing a propylene-based polymer, a styrene-based (hydrogenated) block copolymer, and a hydrocarbon-based rubber softener, it is possible to obtain a molded article that has high flame retardancy while maintaining good touch, injection moldability, and scratch resistance, and is optimal for the surface of automobile interior materials, etc., and have completed the present invention.

[0010] That is, the gist of the present invention lies in the following [1] to

[10] .

[0011] [1] A thermoplastic elastomer composition comprising the following components (A) to (D), wherein the content of component (D) is 0.01 to 30 parts by mass per 100 parts by mass of the total of components (A) to (D): Component (A) Propylene-based polymer Component (B) A block copolymer having at least two polymer blocks P mainly composed of aromatic vinyl compound units and at least one polymer block Q mainly composed of conjugated diene compound units, and / or a hydrogenated product thereof. Component (C) Hydrocarbon-based rubber softener Component (D) Halogen-based flame retardant

[0012] [2] The thermoplastic elastomer composition according to [1], further comprising silicone.

[0013] [3] The thermoplastic elastomer composition according to [1] or [2], wherein the halogen atom of the halogen-based flame retardant of component (D) is at least one selected from the group consisting of fluorine atoms, chlorine atoms and bromine atoms.

[0014] [4] The thermoplastic elastomer composition according to any one of [1] to [3], wherein the content ratio of the component (D) is 0.9 to 30 parts by mass based on a total of 100 parts by mass of the components (A), (B), (C), and (D).

[0015] [5] The thermoplastic elastomer composition according to [4], containing 1 to 80 parts by mass of component (A), 5 to 80 parts by mass of component (B), 5 to 80 parts by mass of component (C), and 0.9 to 30 parts by mass of component (D) relative to 100 parts by mass in total of components (A) to (D).

[0016] [6] The thermoplastic elastomer composition according to any one of [1] to [5], wherein the content of halogen atoms contained in the halogen-based flame retardant of the component (D) is 70 to 95 mass %.

[0017] [7] A molded article obtained by molding the thermoplastic elastomer composition according to any one of [1] to [6].

[0018] [8] An injection-molded article obtained by injection molding the thermoplastic elastomer composition according to any one of [1] to [6].

[0019] [9] An automobile part using the thermoplastic elastomer composition according to any one of [1] to [6].

[0020]

[10] An automobile part using a thermoplastic elastomer composition containing the following components (A) to (D): Component (A) Propylene-based polymer Component (B) A block copolymer having at least two polymer blocks P mainly composed of aromatic vinyl compound units and at least one polymer block Q mainly composed of conjugated diene compound units, and / or a hydrogenated product thereof. Component (C) Hydrocarbon-based rubber softener Component (D) Halogen-based flame retardant Effect of the Invention

[0021] According to the present invention, it is possible to provide a thermoplastic elastomer composition having excellent injection moldability, tactile feel, scratch resistance and flame retardancy, as well as a molded article made of this thermoplastic elastomer composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described in detail below with reference to the preferred embodiments. The present invention is not limited to the following description, and can be modified in any manner without departing from the spirit and scope of the present invention. In this specification, when "~" is used with a numerical value or a physical property value enclosed therein, the values ​​before and after the "~" are included in the expression.

[0023] [Thermoplastic elastomer composition] The thermoplastic elastomer composition of the present invention is characterized by containing the following components (A) to (D) in given ratios. Component (A) Propylene-based polymer Component (B) at least two polymer blocks P mainly composed of aromatic vinyl compound units; and a polymer block Q mainly composed of at least one conjugated diene compound unit. Copolymer and / or its hydrogenated product Component (C) Hydrocarbon-based rubber softener Component (D) Halogen-based flame retardant

[0024] <Mechanism> The reason why the thermoplastic elastomer composition of the present invention exhibits the effects of excellent injection moldability, good touch and scratch resistance, and excellent flame retardancy is presumed to be as follows. The composition includes a propylene polymer as component (A), a block copolymer having a polymer block P mainly composed of at least two aromatic vinyl compound units and a polymer block Q mainly composed of at least one conjugated diene compound unit as component (B) and / or a hydrogenated product thereof, and a hydrocarbon-based rubber softener as component (C), and thereby provides a rubber composition having excellent injection moldability, good touch, and excellent scratch resistance. By incorporating a halogen-based flame retardant as component (D) as a flame retardant, it is possible to improve flame retardancy while maintaining injection moldability, good tactile feel, and scratch resistance.

[0025] <Component (A)> The propylene polymer of component (A) used in the present invention (hereinafter may be referred to as "propylene polymer (A)") may contain 50% by mass or more of propylene units as a main component in the monomer units constituting the propylene polymer (A). From the viewpoints of heat resistance, rigidity, crystallinity, chemical resistance, etc., the content of propylene units in the propylene polymer (A) is preferably 60% by mass or more, more preferably 75% by mass or more, and even more preferably 90% by mass or more. The upper limit of the content of propylene units in the propylene polymer (A) is not particularly limited, and may be 100% by mass.

[0026] The content of the propylene unit in component (A) and each of the structural units of the other copolymerization components described below can be determined by infrared spectroscopy.

[0027] The type of the propylene polymer (A) is not particularly limited, and specific examples thereof include a propylene homopolymer, a propylene-ethylene random copolymer, a propylene-ethylene block copolymer, etc., and any of these can be used.

[0028] The melt flow rate (JIS K7210, 230°C, 21.2N load) of the propylene polymer (A) is not particularly specified, but is usually 0.05 to 200g / 10min, preferably 0.05 to 100g / 10min, and more preferably 0.1 to 80g / 10min. If the melt flow rate is equal to or higher than the lower limit, the moldability is good, and the appearance of the obtained molded article is good. If the melt flow rate is equal to or lower than the upper limit, the mechanical properties, particularly the tensile breaking strength, tend to be good.

[0029] The catalyst used in producing the propylene polymer (A) is not particularly limited, but a preferred example is a stereoregular catalyst. Examples of the stereoregular catalyst include, but are not limited to, Ziegler catalysts and metallocene catalysts. Among these catalysts, metallocene catalysts are preferred.

[0030] Examples of Ziegler catalysts include, but are not limited to, two-component catalysts consisting of a transition metal component, such as a titanium halide compound such as titanium trichloride, titanium tetrachloride, or trichloroethoxytitanium, or an organometallic component, such as an alkylaluminum compound or its halide, hydride, or alkoxide, and a three-component catalyst obtained by adding an electron-donor compound containing nitrogen, carbon, phosphorus, sulfur, oxygen, silicon, or the like to any of the above components.

[0031] The metallocene catalyst is not limited to the following, but may be, for example, a catalyst consisting of a transition metal compound of Group 4 of the periodic table containing a ligand having a cyclopentadienyl skeleton (so-called metallocene compound), a cocatalyst capable of activating the metallocene compound to a stable ionic state by reacting with the metallocene compound, and, if necessary, an organoaluminum compound, and any known catalyst can be used. The metallocene compound is preferably a bridged metallocene compound capable of stereoregular polymerization of propylene, and more preferably a bridged metallocene compound capable of isoregular polymerization of propylene.

[0032] Examples of the method for producing the propylene-based polymer (A) include a slurry method using an inert solvent in the presence of the catalyst, a solution method, a gas phase method substantially without a solvent, or a bulk polymerization method using a polymerization monomer as a solvent. For example, in the case of a slurry polymerization method, the polymerization can be carried out in an inert hydrocarbon or liquid monomer such as n-butane, isobutane, n-pentane, isopentane, hexane, heptane, octane, cyclohexane, benzene, toluene, or xylene. The polymerization temperature is usually -80 to 150°C, preferably 40 to 120°C. The polymerization pressure is preferably 1 to 60 atm. The molecular weight of the resulting propylene-based polymer (A) can be adjusted with hydrogen or other known molecular weight regulators. The polymerization is carried out by a continuous or batch reaction, and the conditions may be those usually used. The polymerization reaction may be carried out in one stage or multiple stages.

[0033] The propylene polymer (A) may be a commercially available product. Examples of the commercially available propylene polymer (A) include polypropylene block copolymer manufactured by Sunallomer Corporation, and Novatec (registered trademark) PP and WAYMAX (registered trademark) manufactured by Japan Polypropylene Corporation.

[0034] The propylene polymer (A) may be used alone or in combination of two or more different types having different copolymer compositions, physical properties, etc.

[0035] <Ingredient (B)> Component (B) used in the present invention is a block copolymer and / or a hydrogenated product thereof (hereinafter sometimes referred to as a "(hydrogenated) block copolymer") having a polymer block P (hereinafter sometimes referred to as a "block P") mainly composed of at least two aromatic vinyl compound units and a polymer block Q (hereinafter sometimes referred to as a "block Q") mainly composed of at least one conjugated diene compound unit.

[0036] Here, the term "mainly composed of" means that the target monomer unit is contained in the target polymer block in an amount of 50 mol % or more.

[0037] The aromatic vinyl compound constituting the block P is not particularly limited, and examples thereof include aromatic vinyl compounds such as styrene, α-methylstyrene, p-methylstyrene, divinylbenzene, 1,1-diphenylethylene, N,N-dimethyl-p-aminoethylstyrene, and N,N-diethyl-p-aminoethylstyrene. Among these, from the viewpoints of availability and productivity, styrene, α-methylstyrene, and p-methylstyrene are preferably used. Styrene is particularly preferred.

[0038] The block P may be composed of one type of aromatic vinyl compound unit or two or more types of aromatic vinyl compound units. The block P may contain a monomer unit other than the vinyl aromatic compound unit.

[0039] The conjugated diene compound constituting the block Q is a diolefin having a pair of conjugated double bonds. Examples of the conjugated diene compound include, but are not limited to, 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, and 1,3-hexadiene. Among these, 1,3-butadiene and isoprene are preferably used from the viewpoints of availability and productivity. 1,3-butadiene is particularly preferred.

[0040] The block Q may be composed of one type of conjugated diene compound unit or may be composed of two or more types of conjugated diene compound units. The block Q may contain a monomer unit other than the conjugated diene compound unit.

[0041] The (hydrogenated) block copolymer of component (B) is preferably one in which the aromatic vinyl compound units are styrene units and the conjugated diene compound units are butadiene units.

[0042] The block polymer having at least two blocks P and at least one block Q may be linear, branched, radial, or the like, but is preferably a block copolymer represented by the following formula (1) or (2). P-(QP)m (1) (PQ)n (2) (In the formula, P represents a block P, and Q represents a block Q. m represents an integer of 1 to 5. n represents an integer of 2 to 5.) When a plurality of blocks P and a plurality of blocks Q are present, the compound units may be the same or different.

[0043] In formula (1) or (2), the larger the m and n, the better in terms of lowering the order-disorder transition temperature of the rubber-like polymer, but the smaller the m and n, the better in terms of ease of production and cost.

[0044] From the viewpoint of rubber elasticity of the composition, component (B) is preferably a block copolymer represented by formula (1), more preferably a block copolymer represented by formula (1) in which m is 3 or less, even more preferably a block copolymer represented by formula (1) in which m is 2 or less, and most preferably a block copolymer represented by formula (1) in which m is 1.

[0045] Component (B) may be a hydrogenated product of a block copolymer having a block P and a block Q. In this case, it is preferably a hydrogenated product of a block copolymer represented by formula (1), more preferably a hydrogenated product of a block copolymer represented by formula (1) in which m is 3 or less, even more preferably a hydrogenated product of a block copolymer represented by formula (1) in which m is 2 or less, and most preferably a hydrogenated product of a block copolymer represented by formula (1) in which m is 1.

[0046] The proportion of block P in the block copolymer of component (B) is preferably high from the viewpoint of mechanical strength of the thermoplastic elastomer composition, and is preferably low from the viewpoint of flexibility and resistance to bleeding out. Specifically, the content of block P in the block copolymer of component (B) is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, and particularly preferably 20% by mass or more. On the other hand, the content of block P in the block copolymer of component (B) is preferably 70% by mass or less, more preferably 60% by mass or less, even more preferably 50% by mass or less, and particularly preferably 40% by mass or less. The higher the proportion of block P, the better the mechanical strength, and the lower the proportion, the better the flexibility and the more unlikely it is to bleed out.

[0047] The proportion of block Q in the block copolymer of component (B) is preferably high from the viewpoint of flexibility and resistance to bleeding out of the thermoplastic elastomer composition, and is preferably low from the viewpoint of mechanical strength. Specifically, the content of block Q in the block copolymer of component (B) is preferably 30% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, and particularly preferably 60% by mass or more. On the other hand, the content of block Q in the block copolymer of component (B) is preferably 95% by mass or less, more preferably 90% by mass or less, even more preferably 85% by mass or less, and particularly preferably 80% by mass or less. The higher the proportion of block Q, the more excellent the flexibility and the more difficult it is to bleed out, and the lower the proportion, the more excellent the mechanical strength.

[0048] The weight average molecular weight (Mw) of the (hydrogenated) block copolymer of component (B) is preferably large in terms of heat resistance and mechanical strength, but is preferably small in terms of molded appearance, fluidity, and moldability. The weight average molecular weight (Mw) of the (hydrogenated) block copolymer of component (B) is preferably 10,000 or more, more preferably 30,000 or more, and is preferably 800,000 or less, more preferably 650,000 or less, and even more preferably 500,000 or less.

[0049] Here, the weight average molecular weight (Mw) is a polystyrene-equivalent weight average molecular weight measured by gel permeation chromatography (hereinafter sometimes abbreviated as GPC) under the following conditions. (Measurement conditions) Equipment: "150C ALC / GPC" manufactured by Nihon Millipore Column: Showa Denko "AD80M / S" x 3 Detector: FOXBORO infrared spectrophotometer "MIRANIA" Wavelength: 3.42μm Solvent: o-dichlorobenzene Temperature: 140℃ Flow rate: 1cm 3 / min Injection volume: 200 microliters Concentration: 2mg / cm 3 0.2% by mass of 2,6-di-t-butyl-p-phenol was added as an antioxidant.

[0050] Preferred examples of component (B) include styrene-butadiene-styrene block copolymers and hydrogenated products thereof, styrene-isoprene-styrene copolymers and hydrogenated products thereof, and styrene-isoprene-butadiene-styrene block copolymers and hydrogenated products thereof.

[0051] Commercially available products can also be used as component (B). Specific examples of commercially available products of component (C) include "Kraton (registered trademark) G" manufactured by Kraton Polymers, "Septon (registered trademark)" manufactured by Kuraray Co., Ltd., "Tuftec (registered trademark)" and "SOE (registered trademark)" manufactured by Asahi Kasei Corporation, and "TAIPOL (registered trademark)" manufactured by TSRC.

[0052] The (hydrogenated) block copolymer of component (B) may be used alone or in combination of two or more. They may also be used in combination.

[0053] <Ingredient (C)> The hydrocarbon-based rubber softener, component (C), used in the present invention is effective in improving the flexibility and flowability of the thermoplastic elastomer composition of the present invention.

[0054] As the hydrocarbon-based rubber softener, mineral oil-based softeners and synthetic resin-based softeners are preferred because of their high affinity for component (B), and mineral oil-based softeners are more preferred.

[0055] Mineral oil-based softeners are generally mixtures of aromatic hydrocarbons, naphthenic hydrocarbons, and paraffinic hydrocarbons. Oils in which 50% or more of the total carbon atoms are derived from paraffinic hydrocarbons are called paraffinic oils, oils in which approximately 30 to 45% of the total carbon atoms are derived from naphthenic hydrocarbons are called naphthenic oils, and oils in which 35% or more of the total carbon atoms are derived from aromatic hydrocarbons are called aromatic oils. The hydrocarbon-based rubber softener used as component (C) may be any one of the above-mentioned softeners or a mixture of multiple types. Among these, paraffin-based oils are preferred because of their good color.

[0056] Examples of synthetic resin-based softeners include polybutene and low molecular weight polybutadiene.

[0057] The kinetic viscosity of the hydrocarbon-based rubber softener at 40° C. is preferably low in terms of improving the fluidity of the thermoplastic elastomer composition of the present invention, but is preferably high in terms of preventing fogging, etc. The kinetic viscosity of the hydrocarbon-based rubber softener at 40° C. is preferably 20 centistokes (cSt) or more, more preferably 50 centistokes or more, while being preferably 800 centistokes or less, more preferably 600 centistokes or less. The flash point (COC method) of the hydrocarbon-based rubber softener is preferably 200° C. or higher, and more preferably 250° C. or higher. The pour point of the hydrocarbon rubber softener is preferably 20°C or higher and -10°C or lower. The aniline point of the hydrocarbon rubber softener is preferably 110°C or higher and 150°C or lower.

[0058] <Ingredient (D)> The halogen-based flame retardant of component (D) used in the present invention is effective in improving the flame retardancy while maintaining the tactile feel and scratch resistance of the thermoplastic elastomer composition of the present invention.

[0059] The halogen atom contained in the halogen-based flame retardant of component (D) is preferably a fluorine atom, a chlorine atom, or a bromine atom, and more preferably a bromine atom, since an excellent effect of imparting and improving flame retardancy can be obtained by adding a small amount.

[0060] The content of halogen atoms contained in component (D) is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and particularly preferably 70% by mass or more, calculated as halogen atom concentration. The upper limit is preferably 95% by mass or less, and more preferably 90% by mass or less. The higher the content of halogen atoms, the more excellent the flame retardancy tends to be, and the lower the content of halogen atoms, the more the mold contamination and environmental load tend to be reduced.

[0061] Examples of the halogen-based flame retardant of component (D) include hexabromocyclododecane, bis(dibromopropyl)tetrabromo-bisphenol A, bis(dibromopropyl)tetrabromo-bisphenol S, tris(dibromopropyl)isocyanurate, tris(tribromoneopentyl)phosphate, decabromodiphenylene oxide, brominated epoxy resin, 1,2-bis(2,3,4,5,6-pentabromophenyl)ethane, tris(tribromophenoxy)triazine, ethylenebis(tetrabromophthalic)imide, polybromophenylindane, brominated polystyrene, tetrabromobisphenol A polycarbonate, brominated polyphenylene oxide, and polypentabromobenzyl acrylate. Preferably, 1,2-bis(2,3,4,5,6-pentabromophenyl)ethane.

[0062] The halogen-based flame retardant of component (D) may be used alone or in combination of two or more. It's fine.

[0063] The thermoplastic elastomer composition of the present invention may contain flame retardants other than halogen-based flame retardants, but preferably does not substantially contain them. "Substantially does not contain" means that the flame retardant is not added in an amount that functions as a flame retardant, and is usually 0.1 mass% or less based on the resin component. "Flame retardants other than halogen-based flame retardants" refers to flame retardants that do not contain halogens, and examples of such flame retardants include phosphorus-based flame retardants such as phosphate esters, polyphosphates, and red phosphorus, inorganic flame retardants such as aluminum hydroxide and magnesium hydroxide, silicone-based flame retardants, and triazine-based flame retardants. Here, the resin component refers to the total of component (A) and component (B) and other resins and elastomers, which are used as necessary and will be described later.

[0064] <Mixing ratio> In the thermoplastic elastomer composition of the present invention, the content of component (D) is 0.01 to 30 parts by mass relative to 100 parts by mass of the total of components (A), (B), (C) and (D). From the viewpoint of good touch and scratch resistance, the upper limit is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 12 parts by mass or less. From the viewpoint of obtaining the desired flame retardancy, the lower limit is preferably 0.5 parts by mass or more, more preferably 0.9 parts by mass or more, and even more preferably 1 part by mass or more.

[0065] In the thermoplastic elastomer composition of the present invention, the content ratios of component (A), component (B), component (C) and component (D) are preferably 1 to 80 parts by mass of component (A), 5 to 80 parts by mass of component (B), 5 to 80 parts by mass of component (C), and 0.9 to 30 parts by mass of component (D) relative to a total of 100 parts by mass of these. The content ratios are more preferably 5 to 70 parts by mass of component (A), 10 to 70 parts by mass of component (B), 10 to 70 parts by mass of component (C), and 1.0 to 20 parts by mass of component (D), still more preferably 5 to 60 parts by mass of component (A), 10 to 65 parts by mass of component (B), 10 to 65 parts by mass of component (C), and 1.0 to 15 parts by mass of component (D), and particularly preferably 10 to 55 parts by mass of component (A), 15 to 55 parts by mass of component (B), 15 to 55 parts by mass of component (C), and 1.0 to 12 parts by mass of component (D).

[0066] The mass ratio of component (A) to component (B) in the thermoplastic elastomer composition of the present invention [mass of component (A)]:[mass of component (B)] is preferably in the range of 5:95 to 90:10, more preferably in the range of 10:90 to 80:20, and even more preferably in the range of 10:90 to 70:30.

[0067] In addition, the mass ratio of component (B) to component (C) in the thermoplastic elastomer composition of the present invention [mass of component (B)]:[mass of component (C)] is preferably in the range of 20:80 to 80:20, more preferably in the range of 25:75 to 75:25, and even more preferably in the range of 25:75 to 65:35.

[0068] When the thermoplastic elastomer composition of the present invention contains the propylene-based polymer of component (A) within the above range, the effects of improving the heat resistance, injection moldability, and mechanical properties of component (A) can be sufficiently obtained while the blending effects of the other components can be sufficiently obtained.

[0069] By containing the (hydrogenated) block copolymer of component (B) within the above range, the thermoplastic elastomer composition of the present invention can fully obtain the effects of the heat resistance and oil resistance of component (B) and the bleed resistance of the hydrocarbon-based rubber softener of component (C), while fully obtaining the effects of the blending of the other components.

[0070] By containing the hydrocarbon rubber softener of component (C) in the above range, the thermoplastic elastomer composition of the present invention can fully obtain the effect of improving flexibility and flowability provided by component (C) while fully obtaining the compounding effects of the other components.

[0071] By containing the halogen-based flame retardant of component (D) in the above range, the thermoplastic elastomer composition of the present invention can sufficiently obtain the effect of improving flame retardancy while sufficiently maintaining the blending effects of the other components.

[0072] <Other ingredients> The thermoplastic elastomer composition of the present invention may contain other components (sometimes simply referred to as "other components" in this specification) in addition to the components (A) to (D) as necessary, provided that the object of the present invention is not impaired. Examples of other components include resins and elastomers other than the components (A) and (B) (sometimes collectively referred to as "other resins" in this specification) and various additives.

[0073] The content of the other components is preferably 900 parts by mass or less, more preferably 570 parts by mass or less, even more preferably 400 parts by mass or less, and particularly preferably 300 parts by mass or less, when the total of components (A) to (D) is 100 parts by mass.

[0074] Examples of other resins that may be contained in the thermoplastic elastomer composition of the present invention include polyolefin resins (excluding those corresponding to the above-mentioned component (A)), polyester resins, polyamide resins, styrene resins (excluding those corresponding to the above-mentioned component (B)), acrylic resins, polycarbonate resins, polyvinyl chloride resins, and other resins; olefin-based elastomers such as ethylene-propylene copolymer rubber (EPM), ethylene-propylene-non-conjugated diene copolymer rubber (EPDM), ethylene-butene copolymer rubber (EBM), and ethylene-propylene-butene copolymer rubber; polyamide-based elastomers such as polyamide-polyol copolymers; polyvinyl chloride-based elastomers and polybutadiene-based elastomers, hydrogenated products thereof, products modified with acid anhydrides, etc. to introduce polar functional groups, and products obtained by grafting, randomly, and / or block copolymerizing other monomers. The above-mentioned other resins may be contained alone or in combination of two or more types.

[0075] Examples of additives that may be contained in the thermoplastic elastomer composition of the present invention include molding aids such as antioxidants, crystal nucleating agents, lubricants, etc., ultraviolet absorbers, light stabilizers such as hindered amine compounds, hydrolysis resistance improvers, colorants such as pigments and dyes, antistatic agents, conductive agents, reinforcing agents, fillers, plasticizers, release agents, and foaming agents.

[0076] It is effective to blend silicone as a lubricant in the thermoplastic elastomer composition of the present invention. Silicone is a component that imparts abrasion resistance to the thermoplastic elastomer composition and prevents the stickiness that is characteristic of elastomers.

[0077] There are no particular limitations on the type of substituent bonded to the siloxane main chain in the molecular structure of the silicone, but among these, dimethyl silicone (dimethyl polysiloxane), methyl phenyl silicone, or alkyl modified silicone is preferably used. The kinetic viscosity (25°C) of the silicone is usually 1 centistoke or more, preferably 5 centistoke or more, more preferably 10 centistoke or more, with no particular upper limit. The higher the kinetic viscosity of the silicone, the greater the effect of improving abrasion resistance and scratch resistance, and the lower the viscosity, the greater the effect of improving stickiness.

[0078] When the thermoplastic elastomer composition of the present invention contains a lubricant such as silicone oil, the content thereof is preferably 0.1 to 15 parts by mass, more preferably 0.1 to 10 parts by mass, per 100 parts by mass of the total of components (A), (B), (C) and (D). A silicone content of 0.1 part by mass or more is preferable from the viewpoint of improving abrasion resistance, scratch resistance and stickiness resistance, and a silicone content of 15 parts by mass or less is preferable from the viewpoints of mechanical strength, flame retardancy, etc.

[0079] The thermoplastic elastomer composition of the present invention may contain, as an antioxidant (heat stabilizer), a hydroxylamine-based antioxidant, a dithiocarbamate-based antioxidant, a hindered phenol-based antioxidant, a sulfur-based antioxidant, a phosphorus-based antioxidant, or the like.

[0080] As the hydroxylamine-based antioxidant, N,N-dialkylhydroxylamines are preferred, and are represented by the general formula R 1 R 2 NOH (in the formula, R 1 and R 2Each independently represents an alkyl group. 1 or R 2 is dodecyl, tetradecyl, hexadecyl, octadecyl, heptadecyl. Particularly preferred dialkylhydroxylamines are N,N-dioctadecylhydroxylamine and N,N-dihexadecylhydroxylamine or mixtures thereof.

[0081] As the dithiocarbamate-based antioxidant, metal salts of dialkyldithiocarbamic acid are preferred, among which nickel dialkyldithiocarbamate is preferred, and nickel dibutyldithiocarbamate is particularly preferred because of its large effect of improving heat aging resistance.

[0082] Known hindered phenol-based antioxidants can be used, and it is particularly preferable to use those having a molecular weight of 500 or more, such as tetrakis[methylene-3(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane. Commercially available products include "Irganox (registered trademark) 1010" manufactured by BASF.

[0083] The sulfur-based antioxidants are compounds containing sulfur, such as thioethers, dithioacid salts, mercaptobenzimidazoles, thiocarbanilides, and thiodipropionate compounds. However, they do not include compounds equivalent to the dithiocarbamate antioxidants. Among these, thiodipropionate compounds are particularly preferred.

[0084] Examples of phosphorus-based antioxidants include phosphorus-containing compounds such as phosphoric acid, phosphorous acid, hypophosphorous acid derivatives, phenylphosphonic acid, polyphosphonates, dialkyl pentaerythritol diphosphites, and dialkyl bisphenol A diphosphites.

[0085] These antioxidants may be used alone or in combination of two or more kinds.

[0086] When the thermoplastic elastomer composition of the present invention contains an antioxidant, the content of the antioxidant is preferably 0.01 to 5 parts by mass per 100 parts by mass of the total of components (A), (B), (C) and (D). A content of the antioxidant of 0.01 parts by mass or more is preferable from the viewpoint of the effect of improving heat deterioration resistance, and a content of 5 parts by mass or less is preferable from the viewpoint of preventing problems such as bleeding and the mechanical strength of the composition.

[0087] The hindered amine light stabilizer is a compound containing a hindered piperidine structure, and known compounds can be used. Commercially available hindered amine light stabilizers include the "Tinuvin (registered trademark)" series manufactured by BASF. The hindered amine light stabilizers may be used alone or in combination of two or more.

[0088] When the thermoplastic elastomer composition of the present invention contains a hindered amine-based light stabilizer, the content thereof is preferably 0.005 to 2 parts by mass, and more preferably 0.01 to 0.5 parts by mass, per 100 parts by mass of the total of components (A), (B), (C) and (D). When the content of the hindered amine-based light stabilizer is within the above range, weather resistance is sufficient and bleeding to the surface of the molded article is unlikely to occur, which is preferable.

[0089] The total content of the additives such as the antioxidants in the thermoplastic elastomer composition of the present invention is preferably 2 parts by mass or less, and more preferably 1 part by mass or less, per 100 parts by mass of the total of component (A), component (B), component (C), and component (D).

[0090] <Method of producing thermoplastic elastomer composition> The method for producing the thermoplastic elastomer composition of the present invention is not particularly limited. The thermoplastic elastomer composition of the present invention can be produced, for example, by dry blending the components (A), (B), (C) and (D) and other components added as necessary, and then melt-kneading the mixture according to a conventional method.

[0091] The mixing device used in this case is not particularly limited, and examples thereof include kneading devices such as a Banbury mixer, a Labo Plastomill, a single screw extruder, a twin screw extruder, etc. Among these, the melt mixing method using an extruder is preferred from the viewpoints of productivity and good kneading properties. The melting temperature during kneading can be appropriately set, but is usually within the range of 130 to 300°C, and preferably within the range of 150 to 250°C.

[0092] <Physical properties of thermoplastic elastomer composition> From the viewpoint of moldability, the thermoplastic elastomer composition of the present invention preferably has a melt flow rate (MFR) of 2 g / 10 min or more, more preferably 5 g / 10 min or more, and even more preferably 10 g / 10 min or more, as measured by a method conforming to JIS K7210 at a measurement temperature of 230° C. and a measurement load of 21.2 N. From the viewpoint of moldability, the melt flow rate (MFR) of the thermoplastic elastomer composition of the present invention is preferably 200 g / 10 min or less, more preferably 185 g / 10 min or less, and even more preferably 160 g / 10 min or less.

[0093] From the viewpoint of flexibility, the thermoplastic elastomer composition of the present invention preferably has a tensile elongation of 200% or more, more preferably 300% or more, measured according to a procedure in accordance with the measuring method of JIS K6251. From the viewpoint of fluidity, the upper limit of the tensile elongation is preferably 1500% or less, more preferably 1200% or less.

[0094] <Application> The thermoplastic elastomer composition of the present invention may be used in any applications, but is particularly useful as a molding material for automobile parts, building parts, medical parts, electric wire covering materials, miscellaneous goods, and the like.

[0095] [Molded body] The thermoplastic elastomer composition of the present invention can be molded into various molded articles. For molding the thermoplastic elastomer composition of the present invention, various molding methods such as ordinary injection molding and extrusion molding can be used.

[0096] Specific examples of the molded article of the present invention obtained by molding the thermoplastic elastomer composition of the present invention include injection molded articles and extrusion molded articles.

[0097] The molding conditions for injection molding the thermoplastic elastomer composition of the present invention are as follows. The molding temperature is usually 160 to 250°C, and preferably 170 to 220°C. The injection pressure is usually 5 to 100 MPa, and preferably 10 to 80 MPa. The mold temperature is usually 10 to 80°C, and preferably 20 to 60°C.

[0098] The injection molded article obtained by injection molding the thermoplastic elastomer composition of the present invention can also be used as a composite molded article by heat fusing it with an olefin-based hard resin such as a propylene resin.

[0099] The molded article of the present invention is useful as an automobile part, a building part, a medical part, an electric wire coating material, miscellaneous goods, etc. Because of its good appearance and touch, scratch resistance and excellent flame retardancy, the molded article of the present invention is useful as a surface of an automobile interior material, such as an armrest or a console pad. EXAMPLES

[0100] The specific embodiments of the present invention will be described in more detail below using examples. The present invention is not limited to the following examples as long as the gist of the present invention is not exceeded. The values ​​of various manufacturing conditions and evaluation results in the following examples are meant as preferred upper or lower limit values ​​in the embodiments of the present invention, and a preferred range may be a range defined by a combination of the above-mentioned upper or lower limit value and the values ​​of the following examples or values ​​between the examples.

[0101] In the following Examples and Comparative Examples, the raw materials used in the preparation of the thermoplastic elastomer compositions and the methods for evaluating the obtained thermoplastic elastomer compositions are as follows.

[0102] [Raw materials used] <Component (A)> A-1: "Novatec PP (registered trademark) BC06C" manufactured by Japan Polypropylene Corporation Propylene-ethylene copolymer Polypropylene unit content: 91% by mass MFR (JIS K7210, 230℃, 21.2N load): 60g / 10 minutes

[0103] <Ingredient (B)> B-1: “TAIPOL (registered trademark) 6159” manufactured by TSRC Hydrogenated styrene-butadiene-styrene block copolymer Weight average molecular weight: 400,000 Styrene unit content: 30% by mass B-2: Kuraray's "Septon (registered trademark) 4077" Hydrogenated styrene-isoprene-butadiene-styrene block copolymer Weight average molecular weight: 380,000 Styrene unit content: 30% by mass B-3: Asahi Kasei Corporation "SOE-SS (registered trademark) S1605" Hydrogenated styrene-butadiene-styrene block copolymer Weight average molecular weight: 200,000 Styrene unit content: 60% by mass

[0104] <Ingredient (C)> C-1: Idemitsu Kosan's "Diana Process Oil PW90" Paraffin oil Dynamic viscosity (40℃): 90 centistokes

[0105] <Ingredient (D)> D-1: "SAYTEX (registered trademark) 8010" manufactured by Albemarle Corporation 1,2-Bis(2,3,4,5,6-pentabromophenyl)ethane Bromine atom content: 82% by mass

[0106] <Other flame retardants> X-1: "Kisuma (registered trademark) 5" manufactured by Kyowa Chemical Industry Co., Ltd. Magnesium hydroxide (Mg(OH)2) X-2: "ADEKA STAB (registered trademark) FP-2200" manufactured by ADEKA Corporation Phosphorus-based antioxidants

[0107] <Other additives> E-1: BASF "Irganox (registered trademark) 1010" Hindered phenol antioxidants F-1: Toray Dow Corning "BY27-001" Dimethyl silicone containing masterbatch Dimethyl silicone content: 50% by mass

[0108] [Evaluation of Thermoplastic Elastomer Composition] <Flame retardancy: Burning rate FMVSS No.302> Using an FMVSS No. 302 combustion tester, a burner flame of 38 mm was applied to the right end of an injection molded product (350 mm x 100 mm x 1.5 mm) made from pellets of the thermoplastic elastomer composition obtained in the Examples and Comparative Examples for 15 seconds to measure the burning rate over a burning distance of 254 mm between the marked lines. Measurements were performed with a wire on the test jig, and the average value was calculated from five tests. The slower the burning rate, the higher the flame retardancy. The burning rate is preferably 40 mm / min or less, more preferably 35 mm / min or less, and even more preferably 30 mm / min or less.

[0109] <Tactile sensation> The injection-molded articles (350 mm × 100 mm × 1.5 mm) made from the pellets of the thermoplastic elastomer compositions obtained in the Examples and Comparative Examples were examined for tactile sensation when touched by a human hand with three fingers, and evaluated according to the following criteria. The feel of the injection molded article is preferably such that no bleeding occurs on the surface and the article does not stick to the hands, and more preferably has a smooth feel. A: It is smooth and does not feel sticky on the hands. B: It is slightly dry and does not feel sticky on the hands. C: Sticky or dry but feels sticky on hands

[0110] <Scratch resistance: Taber scratch> For injection-molded articles (350 mm × 100 mm × 1.5 mm) made from pellets of the thermoplastic elastomer compositions obtained in the Examples and Comparative Examples, a Taber scratch tester manufactured by Toyo Seiki Seisakusho Co., Ltd. was used. A tungsten carbide cutter with its straight blade was attached to a jig and the test pieces were rotated at a load of 350 g and a rotation speed of 0.5 rpm to observe the condition of the test pieces and evaluate them according to the following criteria. The most preferable scratch resistance of the injection molded article is one in which there are no cuts or penetrations, no changes, or only surface chipping. A: No change, or some surface wear B: The entire surface is scraped and some of the surface is cut. C: Penetration

[0111] <Liquidity: MFR> The thermoplastic elastomer compositions obtained in the examples and comparative examples were measured in accordance with JIS K7210 (1999) at a measurement temperature of 230° C. and a measurement load of 21.2 N.

[0112] <Flexibility: Tensile elongation> For injection molded articles (350 mm×100 mm×1.5 mm) made from pellets of the thermoplastic elastomer compositions obtained in the Examples and Comparative Examples, measurements were made at a test speed of 500 mm / min according to a method in accordance with JIS K6251.

[0113] [Examples 1 to 5, Comparative Examples 1 to 6] The raw materials were mixed according to the composition shown in Table 1, and the resulting mixture was melt-kneaded in a twin-screw kneader (cylinder temperature: 180° C. to 200° C.) to produce pellets of a thermoplastic elastomer composition. The MFR of the resulting thermoplastic elastomer composition was measured, and the results are shown in Table 1. The obtained thermoplastic elastomer composition was injected and filled into a sheet-shaped mold having dimensions of 350 mm length × 100 mm width × 1.5 mm thickness at an injection speed of 40 mm / sec using an electric injection molding machine (manufactured by Sumitomo Heavy Industries, Ltd.) with a clamping force of 180 t, a cylinder temperature of 200°C, and a mold temperature of 40°C. After the filling was completed, the molded article was cooled for 30 seconds and then removed. The molded article was evaluated for flame retardancy, touch, scratch resistance, and tensile elongation. The results are shown in Table 1.

[0114] [Table 1]

[0115] [Evaluation Results] The following can be said from Table 1: In Examples 1 to 5, the compositions contain a propylene-based polymer (A), a hydrogenated block copolymer (B), a hydrocarbon-based rubber softener (C), and a halogen-based flame retardant (D), and thus have a burning rate of 40 mm / min or less, an excellent feel, and excellent scratch resistance with no cuts in the scratch resistance evaluation.The MFR value indicates that the compositions also have excellent moldability, and the tensile elongation value indicates that the compositions also have excellent flexibility.

[0116] Comparative Examples 1 and 2 did not contain a halogen-based flame retardant, and had a high burning rate and poor flame retardancy. In Comparative Examples 3 to 5, magnesium hydroxide was used as a flame retardant. Of these, Comparative Example 3, which contains a relatively small amount of magnesium hydroxide, had a faster burning rate and poorer flame retardancy than Example 2, and the Taber scratch test showed chipping and cutting on the entire surface. Comparative Examples 4 and 5, which contain a large amount of magnesium hydroxide, have a burning rate of 40 mm / min or less, but bleeding was felt on the hand in the tactile evaluation, and the blade penetrated the test piece in the Taber scratch test. In Comparative Example 6, a phosphorus-based flame retardant was blended in place of the halogen-based flame retardant, but the flame retardancy imparting effect was inferior to the case where a halogen-based flame retardant was used.

[0117] Although the present invention has been described in detail with reference to specific embodiments, it will be apparent to those skilled in the art that various modifications can be made without departing from the spirit and scope of the invention. This application is based on Japanese Patent Application No. 2019-208921 filed on November 19, 2019, the entirety of which is incorporated by reference. [Industrial Applicability]

[0118] The molded articles obtained from the thermoplastic elastomer composition of the present invention have excellent flame retardancy, touch, and scratch resistance, and are suitable for use in automobile parts such as automobile interior parts, building parts, medical parts, electric wire coating materials, miscellaneous goods, etc.

Claims

1. An injection-molded article obtained by injection molding a thermoplastic elastomer composition comprising the following components (A) to (D), and containing 1 to 80 parts by mass of component (A), 5 to 80 parts by mass of component (B), 5 to 80 parts by mass of component (C), and 0.01 to 15 parts by mass of component (D) relative to a total of 100 parts by mass of components (A) to (D). Component (A) Propylene-based polymer Component (B) A block copolymer having at least two polymer blocks P mainly composed of aromatic vinyl compound units and at least one polymer block Q mainly composed of conjugated diene compound units, and / or a hydrogenated product thereof. Component (C) Hydrocarbon-based rubber softener Component (D) Halogen-based flame retardant

2. The injection molded article according to claim 1 , wherein the thermoplastic elastomer composition further contains silicone.

3. 3. The injection molded article according to claim 1, wherein the halogen atom of the halogen-based flame retardant of the component (D) is at least one kind selected from the group consisting of a fluorine atom, a chlorine atom and a bromine atom.

4. The injection molded article according to any one of claims 1 to 3, wherein the content of halogen atoms contained in the halogen-based flame retardant of the component (D) is 70 to 95 mass%.

5. The injection molded article according to any one of claims 1 to 4, wherein the thermoplastic elastomer composition has a melt flow rate (MFR) of 10 g / 10 min or more and 200 g / 10 min or less, as measured at a measurement temperature of 230°C and a measurement load of 21.2 N according to a method in accordance with JIS K7210 standard for thermoplastic elastomer compositions.

6. An automobile part using the injection molded article according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Flame-retardant resin composition

    JP1987064852A

  • Flame-retardant resin composition

    JP1987068845A

  • Flame-retardant resin composition

    JP1987068846A

  • Flame-retardant resin composition

    JP1987070439A

  • Flame-retardant polyolefin film and laminate thereof

    JP1995330986A