Concrete containing attractant and concrete structure

Attractant-containing concrete with cement and calcium aluminate admixture efficiently attracts herbivorous animals, addressing the inefficiencies of manual removal methods and enhancing removal efficiency.

JP7568229B2Active Publication Date: 2024-10-16DENKA CO LTD +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021055297
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-29
Publication Date
2024-10-16
Estimated Expiration
2041-03-29

AI Technical Summary

Technical Problem

Existing methods for reducing feeding damage by herbivorous animals in seaweed beds, such as manual removal by divers, are labor-intensive and inefficient, and existing concrete structures do not effectively utilize calcium aluminate as an admixture.

Method used

Development of attractant-containing concrete comprising cement, calcium aluminate admixture, and food ingredients that attract herbivorous animals, particularly seaweed and vegetables, to gather them in a specific area for efficient removal.

Benefits of technology

The attractant-containing concrete effectively attracts and gathers herbivorous animals, improving their removal efficiency and reducing labor requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568229000001
    Figure 0007568229000001
  • Figure 0007568229000002
    Figure 0007568229000002
Patent Text Reader

Abstract

To provide a concrete containing an attractant that improves the removal efficiency of herbivores and a concrete structure made by hardening the concrete containing an attractant.SOLUTION: A concrete containing an attractant includes cement, a calcium aluminate admixture containing calcium aluminate and gypsum, and an attractant containing food materials that attract herbivores. A concrete structure is made by hardening the concrete containing an attractant of the present invention.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an attractant-containing concrete and a concrete structure obtained by hardening the attractant-containing concrete. [Background technology]

[0002] Coastal waters are home to seaweed beds where seaweed grows luxuriantly, and these beds play an important role as feeding and spawning grounds for marine life. However, in recent years, a phenomenon known as "isoyake" (reef denudation) has been observed in which seaweed beds disappear. There are various causes for this phenomenon, but damage caused by herbivores such as sea urchins and fish is considered to be a particular problem (Non-Patent Document 1).

[0003] Various techniques have been proposed to reduce damage caused by herbivores by removing them (Non-Patent Document 1, Patent Documents 1 and 2).

[0004] However, removal of herbivores is mainly done manually by divers, and due to the large amount of work involved, it is difficult to continue, and has not yet succeeded in improving rocky shore denudation. Patent Documents 3 and 4 describe seaweed reefs. However, these documents only describe concrete blocks as a site for growing seaweed, and do not exemplify calcium aluminate as an admixture. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 3311339 [Patent Document 2] JP 2011-167083 A [Patent Document 3] JP 2000-197426 A [Patent Document 4] Japanese Patent Application Publication No. 11-137117 [Non-patent literature]

[0006] [Non-Patent Document 1] Fisheries Agency, Revised Guidelines for Countermeasures against Rocky Coastal Denudation, 2015 Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made to solve the above-mentioned problems of the prior art, and has an object to provide an attractant-containing concrete that improves the efficiency of removing herbivores. [Means for solving the problem]

[0008] The present inventors have conducted intensive research to achieve the above object and have discovered that the above problems can be solved by using concrete containing an attractant that contains foodstuffs that attract herbivores. The present invention is based on the above findings and has the following gist. [1] An attractant-containing concrete comprising cement, a calcium aluminate admixture containing calcium aluminate and gypsum, and an attractant containing food material that attracts herbivores. [2] The attractant-containing concrete described in [1] above, wherein the food material is at least one of seaweed and vegetables. [3] The attractant-containing concrete described in [2] above, wherein the seaweed is leafy seaweed and the vegetables are leafy vegetables. [4] The attractant-containing concrete according to any one of the above [1] to [3], wherein the amount of the attractant used is 10 to 60 parts by mass per 100 parts by mass of the attractant-containing concrete. [5] The attractant-containing concrete according to any one of the above [1] to [4], further comprising aggregate. [6] The attractant-containing concrete according to any one of the above [1] to [5], further containing water. [7] A concrete structure obtained by hardening the attractant-containing concrete according to any one of [1] to [6] above. Effect of the Invention

[0009] According to the present invention, it is possible to provide an attractant-containing concrete that improves the efficiency of removing herbivores, and a concrete structure obtained by hardening the attractant-containing concrete. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] [Concrete containing attractant] The attractant-containing concrete of the present invention contains cement, a calcium aluminate admixture containing calcium aluminate and gypsum, and an attractant containing food materials that attract herbivores. This allows at least some of the herbivores to gather in a predetermined area, and by capturing the gathered herbivores, the efficiency of removing the herbivores can be improved.

[0011] (cement) In this specification, cement is a general term for cement paste, cement mortar, and concrete. Examples of cements used in the attractant-containing concrete of the present invention include various Portland cements such as ordinary, early strength, super early strength, low heat, and moderate heat, various mixed cements obtained by mixing these Portland cements with blast furnace slag, fly ash, or silica, filler cements obtained by mixing these Portland cements with limestone powder or blast furnace slag powder, and environmentally friendly cements (ecocements) produced using municipal waste incineration ash and sewage sludge incineration ash as raw materials. These cements can be used alone or in combination of two or more. Among these cements, ordinary Portland cement is preferred from the viewpoint of easily incorporating the attractant.

[0012] The Blaine specific surface area of ​​the cement used in the attractant-containing concrete of the present invention is 2500 to 4800 cm from the viewpoint of an appropriate hydration rate of the cement. 2 / g is preferred, and 2800 to 4000 cm 2 / g is more preferable, and 3000 to 3600 cm 2The Blaine specific surface area can be measured in accordance with JIS R 5201-1997 "Physical Testing Methods for Cement."

[0013] The cement used in the attractant-containing concrete of the present invention preferably contains cement clinker and gypsum. This prevents the cement from setting too quickly and increases the strength and chemical resistance of the cement hardened body. From this viewpoint, the mineral composition of the cement clinker calculated using the Bogue formula is preferably 40-70 mass% C3S (tricalcium silicate), 7-40 mass% C2S (dicalcium silicate), 1-15 mass% C3A (tricalcium aluminate), and 5-20 mass% C4AF (tetracalcium aluminate ferroferroate). The content of gypsum in the cement is preferably 0.5-4 mass%, more preferably 1.5-3 mass%, calculated as SO3.

[0014] The content of cement in the attractant-containing concrete of the present invention is preferably 10 to 95 parts by mass relative to 100 parts by mass of the total of cement, calcium aluminate admixture, and attractant, from the viewpoint of maintaining the strength of the concrete at a certain level or higher. Also, from the viewpoint of enhancing the attractant effect on herbivores, the content of cement in the attractant-containing concrete of the present invention is more preferably 20 to 90 parts by mass. Furthermore, from the viewpoint of shape retention in the sea, the content of cement in the attractant-containing concrete of the present invention is even more preferably 30 to 80 parts by mass.

[0015] (Calcium aluminate admixture) The calcium aluminate admixture used in the attractant-containing concrete of the present invention contains calcium aluminate and gypsum. The calcium aluminate admixture may further contain a shrinkage-reducing agent and / or fibers.

[0016] Calcium aluminate is a general term for a substance with hydration activity, mainly composed of CaO and Al2O3, and is a material that has a fast hardening time and high early strength development. Alumina cement is a representative example of calcium aluminate, and commercially available products can be used. Examples of commercially available alumina cement that can be used include Alumina Cement No. 1 and Alumina Cement No. 2. However, amorphous calcium aluminate that is quenched after melting is preferred because it hardens in a shorter time than alumina cement and has a higher initial strength development thereafter.

[0017] From the viewpoint of early strength development, the molar ratio of CaO to Al2O3 (CaO / Al2O3 molar ratio) in calcium aluminate is preferably 1.0 to 3.0, more preferably 1.7 to 2.5. Even when the molar ratio of CaO to Al2O3 (CaO / Al2O3 molar ratio) in calcium aluminate is 1.0 to 1.7, it is possible to further shorten the hardening time and improve the early strength development by blending cement, slaked lime, and quicklime.

[0018] The Blaine specific surface area of ​​calcium aluminate is 3000 cm 2 / g or more. The Blaine specific surface area of ​​calcium aluminate is preferably 3000 cm 2 When the Blaine specific surface area is 1 / g or more, the rapid setting power of calcium aluminate can be prevented from decreasing. The Blaine specific surface area can be measured in accordance with JIS R 5201-1997 "Physical Testing Methods for Cement".

[0019] From the viewpoint of reaction activity, the vitrification rate of calcium aluminate is preferably 70% or more, more preferably 90% or more. When the vitrification rate of calcium aluminate is 70% or more, the initial strength development can be improved. The vitrification rate of calcium aluminate is measured by measuring the main peak area S of the crystalline mineral by powder X-ray diffraction method before heating a sample, heating it at 1000°C for 2 hours, and then slowly cooling it at a cooling rate of 1 to 10°C / min, and determining the main peak area S0 of the crystalline mineral after heating by powder X-ray diffraction method, and calculating the vitrification rate χ using the values ​​of S0 and S according to the following formula. Vitrification rate χ(%)=100×(1-S / S0)

[0020] As the gypsum of the calcium aluminate admixture, for example, hemihydrate gypsum and anhydrous gypsum can be used, and from the viewpoint of strength development, anhydrous gypsum is preferred. As the anhydrous gypsum, for example, hydrofluoric acid by-product anhydrous gypsum and natural anhydrous gypsum can be used.

[0021] The pH of the water when the gypsum is immersed in the water is preferably 8 or less. That is, the water when the gypsum is immersed in the water is preferably weakly alkaline to acidic. If the pH of the water when the gypsum is immersed in the water is 8 or less, the solubility of the gypsum component can be suppressed from increasing, and the inhibition of the initial strength development due to the dissolution of the gypsum component can be suppressed. The pH of the water when the gypsum is immersed in the water is the pH of a diluted slurry at 20°C where gypsum / ion-exchanged water=1 g / 100 g, measured using an ion-exchange electrode or the like.

[0022] The Blaine specific surface area of ​​gypsum is 3000 cm 2 / g or more, and from the viewpoint of early strength development and obtaining an appropriate working time, it is preferable that the hardness be 5000 cm 2 The Blaine specific surface area can be measured in accordance with JIS R 5201-1997 "Physical Testing Methods for Cement."

[0023] The amount of gypsum used in the calcium aluminate admixture is not particularly limited, but is preferably 50 to 250 parts by mass relative to 100 parts by mass of calcium aluminate. When the amount of gypsum used is 50 parts by mass or more, sufficient working time can be secured and strength development can be improved. When the amount of gypsum used is 250 parts by mass or less, sufficient working time and sufficient initial strength can be obtained.

[0024] The content of the calcium aluminate admixture in the attractant-containing concrete of the present invention is preferably 3 to 50 parts by mass per 100 parts by mass of the total of the cement, the calcium aluminate admixture and the attractant, from the viewpoint of maintaining the strength of the concrete at a certain level or higher. Also, from the viewpoint of enhancing the attractant effect on herbivores, the content of the calcium aluminate admixture is more preferably 5 to 40 parts by mass. Furthermore, from the viewpoint of shape retention in the sea, the content of the calcium aluminate admixture is even more preferably 10 to 30 parts by mass.

[0025] (Attractant) The attractant used in the attractant-containing concrete of the present invention contains foodstuffs that attract herbivorous animals. Here, the foodstuffs are the ingredients of human food. The foodstuffs used as the attractant may be waste. This allows for the effective use of discarded foodstuffs, and also makes it easier to obtain the attractant. Examples of discarded foodstuffs include foodstuffs that do not meet commercial standards, foodstuffs that are discarded to prevent foodstuff prices from dropping due to an overabundance of harvests, and food waste generated when harvesting or processing foodstuffs. Also, the herbivorous animals are animals that mainly eat seaweed. Examples of herbivorous animals include sea urchins, turban shells, sea hares, small snail shells, and predatory fish (rabbitfish, parrotfish, sea lions, sea bream, etc.). The attractant-containing concrete of the present invention is particularly suitable for removing sea urchins.

[0026] From the viewpoint of easy availability, the food material used as the attractant is preferably at least one of seaweed and vegetables. The seaweed used as the attractant may be any commonly available seaweed, and may be, for example, the leaves or stems of leaf-like seaweed such as kombu, wakame, arame, and kajime. The shape of the seaweed is not particularly limited as long as it can be mixed with the concrete and calcium aluminate admixture and hardened. The vegetables used as attractants may be any commonly available vegetable, such as cabbage, lettuce, Chinese cabbage, etc. The shape of the vegetables is not particularly limited as long as they can be mixed with the concrete and calcium aluminate admixture and hardened.

[0027] The attractant may contain materials other than the above-mentioned food ingredients, as long as the effects of the present invention are not impaired. Examples of materials other than food ingredients include soil, sand, stones, and other materials that are mixed into discarded food ingredients. However, from the viewpoint of further enhancing the effect of attracting herbivorous animals in the attractant-containing concrete of the present invention, the content of the above-mentioned food ingredients in the attractant is preferably 80 to 100 mass%, more preferably 90 to 100 mass%, even more preferably 95 to 100 mass%, and particularly preferably 100 mass%.

[0028] The content of the attractant in the attractant-containing concrete of the present invention is preferably 10 to 60 parts by mass relative to 100 parts by mass of the total of cement, calcium aluminate admixture and attractant, from the viewpoint of maintaining the strength of the hardened body of the attractant-containing concrete at a certain level or higher. Also, from the viewpoint of enhancing the attracting effect on herbivores, the content of the attractant is more preferably 20 to 60 parts by mass. Furthermore, from the viewpoint of the shape retention of the hardened body of the attractant-containing concrete in the sea, the content of the attractant is even more preferably 20 to 45 parts by mass.

[0029] (water) The attractant-containing concrete of the present invention preferably further contains water. From the viewpoint of workability of the attractant-containing concrete of the present invention, the amount of water used in the attractant-containing concrete of the present invention is preferably 10 to 200 parts by mass, more preferably 40 to 150 parts by mass, even more preferably 60 to 130 parts by mass, and even more preferably 80 to 110 parts by mass, relative to 100 parts by mass in total of the cement, the calcium aluminate admixture, and the attractant.

[0030] (aggregate) The attractant-containing concrete of the present invention preferably further contains aggregate from the viewpoint of attracting effect and from the viewpoint of improving the strength of the hardened body of the attractant-containing concrete. Examples of the aggregate include fine aggregate, coarse aggregate, river sand, mountain sand, crushed stone, etc. These aggregates can be used alone or in combination of two or more.

[0031] From the viewpoint of the attracting effect and the strength improvement of the hardened body of the attractant-containing concrete, the particle size of the aggregate is preferably 0.1 to 20 mm, and more preferably 5 to 13 mm.

[0032] The amount of aggregate used in the attractant-containing concrete of the present invention is preferably 100 to 1000 parts by mass relative to 100 parts by mass of the total of cement, calcium aluminate admixture, and attractant. When the amount of aggregate used is 100 parts by mass or more, the attractant effect can be sustained for a long period of time, and when the amount of aggregate used is 1000 parts by mass or less, the strength of the hardened body of the attractant-containing concrete increases. From this viewpoint, the amount of aggregate used is more preferably 300 to 750 parts by mass, and even more preferably 400 to 550 parts by mass.

[0033] [Concrete structure] The concrete structure of the present invention is obtained by hardening the attractant-containing concrete of the present invention. The concrete structure of the present invention may be obtained by hardening and further molding. As a result, the concrete structure of the present invention becomes an attractant for herbivorous animals.

[0034] The structure of the concrete structure of the present invention is not particularly limited, but in order to maintain the attraction effect, it is preferable that the structure is a porous structure. The shape of the concrete structure of the present invention is not particularly limited. Examples of the shape of the concrete structure include a cylinder, a rectangular prism, a rectangular parallelepiped, a cone, a sphere, and a tetrapod body. It is desirable to determine the size and shape of the concrete structure according to the conditions of the sea area in which it is installed. For example, in a sea area with a fast tidal current, by combining multiple tetrapod-shaped concrete structures, the concrete structure can be prevented from being washed away and can be kept in the desired location.

[0035] <Action and effect> An example of the effect of the attractant-containing concrete of the present invention will be described below.

[0036] The attractant-containing concrete of the present invention is made by hardening an attractant containing foodstuffs that attract herbivores using cement and calcium aluminate admixture, thereby allowing the attractant's attractive effect to last for a long period of time.

[0037] The attractant-containing concrete of the present invention has an attractant effect on herbivores, particularly sea urchins, which mainly eat seaweed, and thus can sufficiently attract at least a portion of the herbivores, thereby improving the efficiency of removing the herbivores. EXAMPLES

[0038] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.

[0039] [Compressive strength evaluation test] In accordance with JIS R 5201-1997 "Physical Testing Methods for Cement," the compressive strength of the concrete structure was measured 28 days after mixing the cement paste and aggregate. Those that could not maintain their shape after 28 days were deemed unmeasurable. [Evaluation test of Blaine specific surface area] The Blaine specific surface areas of cement, calcium aluminate, and gypsum were measured in accordance with JIS R 5201-1997 "Physical testing methods for cement." [Aggregate particle size evaluation test] Sieving was performed in accordance with JIS A 1102 "Sieving test of aggregates," and the sieve size of the sieve with the highest mass fraction retained on each sieve was taken as the particle size of the aggregate. [Method of evaluating the attraction effect] A concrete structure made of hardened concrete containing the attractant was installed in the actual sea area, and an evaluation test of the attractant effect was carried out. 2 A square area was set up, and a rectangular concrete structure (10cm x 10cm x 9cm) was placed in the center of the area. The change in the number of sea urchins in the area over time was examined, and the attraction effect was evaluated as follows, compared to a control area without a concrete structure: ○: effective (increase in number of sea urchins of 20% or more), △: slightly effective (increase in number of sea urchins of 10% to less than 20%), ×: no effect (increase in number of sea urchins of 0% to less than 10%).

[0040] [Example 1] 80 parts by mass of cement, 10 parts by mass of calcium aluminate admixture, 10 parts by mass of attractant A, and 100 parts by mass of tap water were mixed in a concrete mixer (Omni Mixer, manufactured by Chiyoda Machinery Co., Ltd.) to prepare a cement paste, which was then poured into a 10 cm x 10 cm x 9 cm formwork. After leaving it to cure at room temperature for one week, the molded body was removed and used to evaluate the above-mentioned attractant effect.

[0041] [Example 2] The same procedure as in Example 1 was carried out except that 80 parts by mass of cement, 10 parts by mass of calcium aluminate admixture, 10 parts by mass of attractant B, and 100 parts by mass of tap water were charged into a concrete mixer.

[0042] [Example 3] The same procedure as in Example 1 was carried out except that 60 parts by mass of cement, 30 parts by mass of calcium aluminate admixture, 10 parts by mass of attractant A, and 100 parts by mass of tap water were charged into a concrete mixer.

[0043] [Example 4] The same procedure as in Example 1 was carried out except that 60 parts by mass of cement, 30 parts by mass of calcium aluminate admixture, 10 parts by mass of attractant B, and 100 parts by mass of tap water were charged into a concrete mixer.

[0044] [Example 5] The same procedure as in Example 1 was carried out except that 30 parts by mass of cement, 30 parts by mass of calcium aluminate admixture, 40 parts by mass of attractant A, and 100 parts by mass of tap water were charged into a concrete mixer.

[0045] [Example 6] The same procedure as in Example 1 was carried out, except that 30 parts by mass of cement, 30 parts by mass of calcium aluminate admixture, 40 parts by mass of attractant B, and 100 parts by mass of tap water were charged into a concrete mixer.

[0046] [Example 7] The same procedure as in Example 1 was carried out except that 30 parts by mass of cement, 10 parts by mass of calcium aluminate admixture, 60 parts by mass of attractant A, and 100 parts by mass of tap water were charged into a concrete mixer.

[0047] [Example 8] The same procedure as in Example 1 was carried out except that 30 parts by mass of cement, 10 parts by mass of calcium aluminate admixture, 60 parts by mass of attractant B, and 100 parts by mass of tap water were charged into a concrete mixer.

[0048] [Example 9] 70 parts by mass of cement, 10 parts by mass of calcium aluminate admixture, 20 parts by mass of attractant A, and 100 parts by mass of tap water were put into a concrete mixer and mixed to prepare a cement paste. 470 parts by mass of aggregate was added to the cement paste relative to the total of 100 parts by mass of cement, calcium aluminate admixture, and attractant, and further mixed. The mixture was poured into a 10 cm x 10 cm x 9 cm formwork, and compacted for about 20 seconds using a table vibrator (CF-1033, manufactured by Maruto Seisakusho Co., Ltd.) at a vibration frequency of 2800 rpm, but the same procedure was followed as in Example 1.

[0049] [Example 10] 70 parts by mass of cement, 10 parts by mass of calcium aluminate admixture, 20 parts by mass of attractant B, and 100 parts by mass of tap water were put into a concrete mixer and mixed to prepare a cement paste. 470 parts by mass of aggregate was added to the cement paste relative to the total of 100 parts by mass of cement, calcium aluminate admixture, and attractant, and further mixed. The mixture was poured into a 10 cm x 10 cm x 9 cm formwork, and compacted for about 20 seconds using a table vibrator (CF-1033, manufactured by Maruto Seisakusho Co., Ltd.) at a vibration frequency of 2800 rpm, but the same procedure as in Example 1 was repeated.

[0050] [Comparative Example 1] 100 parts by mass of cement and 17 parts by mass of tap water were mixed in a concrete mixer (Omni Mixer, manufactured by Chiyoda Machinery Co., Ltd.) to prepare a cement paste, which was then poured into a 10 cm x 10 cm x 9 cm formwork. After leaving it to stand at room temperature for one week to cure, the molded body was removed from the form and used to evaluate the above-mentioned attraction effect.

[0051] [Comparative Example 2] 100 parts by mass of calcium aluminate admixture and 17 parts by mass of tap water were mixed in a concrete mixer (Omni Mixer, manufactured by Chiyoda Machinery Co., Ltd.) to prepare a cement paste, which was then poured into a 10 cm x 10 cm x 9 cm formwork. After leaving it to stand at room temperature for one week to cure, the attractant effect was evaluated in the same manner as in Comparative Example 1.

[0052] [Comparative Example 3] 1 kg of the attractant A was placed in a laundry net, and the attractant effect was evaluated in the same manner as in Comparative Example 1.

[0053] [Comparative Example 4] 1 kg of the attractant B was placed in a laundry net, and the attractant effect was evaluated in the same manner as in Comparative Example 1.

[0054] [Comparative Example 5] The same procedure as in Comparative Example 1 was carried out except that 50 parts by mass of cement, 50 parts by mass of calcium aluminate admixture, and 100 parts by mass of tap water were charged into the concrete mixer.

[0055] [Comparative Example 6] The same procedure as in Comparative Example 1 was carried out except that 30 parts by mass of cement, 70 parts by mass of attractant A, and 100 parts by mass of tap water were added to the concrete mixer.

[0056] [Comparative Example 7] The same procedure as in Comparative Example 1 was carried out, except that 30 parts by mass of cement, 70 parts by mass of attractant B, and 100 parts by mass of tap water were added to the concrete mixer.

[0057] [Comparative Example 8] The same procedure as in Comparative Example 1 was carried out except that 30 parts by mass of calcium aluminate admixture, 70 parts by mass of attractant A, and 100 parts by mass of tap water were added to the concrete mixer.

[0058] [Comparative Example 9] The same procedure as in Comparative Example 1 was carried out, except that 30 parts by mass of calcium aluminate admixture, 70 parts by mass of attractant B, and 100 parts by mass of tap water were added to the concrete mixer.

[0059] (Raw materials used) In the above examples and comparative examples, the following raw materials were used. Cement: Ordinary Portland cement, commercially available, Blaine specific surface area 3300 cm 2 / g, and the cement mineral composition in the cement clinker was 56 mass% C3S, 26 mass% C2S, 9 mass% C3A, and 9 mass% C4AF. The gypsum content in the cement was 2.1 mass% converted to SO3. Calcium aluminate admixture: Calcium aluminate (CaO / Al2O3 molar ratio 2.2, vitrification rate 97%, Blaine specific surface area 5000 cm 2 / g) 100 parts by mass and gypsum (natural anhydrous gypsum, Blaine value 6000 cm 2 / g, pH 7.2) 100 parts by weight. Attractant A: Wakame stems discarded at a wakame farm Attractant B: Cabbage Aggregate: No. 6 crushed stone (produced in Itoigawa, Niigata Prefecture, particle size 5 to 13 mm) Water: Tap water

[0060] [Table 1]

[0061] [Table 2]

[0062] In Examples 1 to 10, the effect of attracting sea urchins was observed from 15 minutes to 24 hours later. Therefore, it was found that sufficient time for collecting sea urchins could be secured and the efficiency of removing sea urchins could be sufficiently improved. In Comparative Examples 1, 2 and 5, since the concrete did not contain an attractant, no effect of attracting sea urchins was observed. In Comparative Examples 3, 4, 8 and 9, the attractant effect was observed up to 30 minutes after the treatment. However, since the attractant was not hardened using cement, the attractant effect was not observed after 90 minutes and 24 hours. This resulted in insufficient time to collect sea urchins, and it was found that it was difficult to improve the efficiency of sea urchin removal. In Comparative Examples 6 and 7, the attractant effect was observed up to 90 minutes after the treatment. However, since no calcium aluminate admixture was used, the hardening of the attractant by cement was insufficient, and therefore the attractant effect was not observed after 24 hours. As a result, the time available for collecting sea urchins was insufficient, and it was found that it was difficult to improve the efficiency of removing sea urchins.

[0063] From the above, it was found that the attractant-containing concrete containing cement, calcium aluminate admixture, and attractant has an attractant effect for a long period of time. Furthermore, it was found that in order to obtain the attractant effect, it is preferable to set the content of the attractant in the range of 10 to 60 parts by mass per 100 parts by mass of the total of the cement, calcium aluminate admixture, and attractant. [Industrial Applicability]

[0064] The attractant-containing concrete of the present invention can supply foodstuffs that herbivores like to the coastal sea area, and can gather herbivores in a specific area. This attractant effect can improve the efficiency of herbivorous animal removal and reduce the labor required for herbivorous animal removal.

Claims

1. Cement and A calcium aluminate admixture containing calcium aluminate and gypsum; and an attractant containing food material that attracts herbivorous animals. The food material is at least one of seaweed and vegetables, The amount of the attractant used is 10 to 60 parts by mass per 100 parts by mass of the attractant-containing concrete.

2. 2. The attractant-containing concrete according to claim 1, wherein the seaweed is a leafy seaweed and the vegetable is a leafy vegetable.

3. The attractant-containing concrete according to claim 1 or 2, further comprising aggregate.

4. The attractant-containing concrete according to any one of claims 1 to 3, further comprising water.

5. A concrete structure obtained by hardening the attractant-containing concrete according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Composite of cement

    JP1977139133A

  • Manufacture of cement moldings

    JP1988185873A

  • Concrete block for creating seaweed colony and seaweed reef

    JP1999137117A

  • Seaweed community forming unit and seaweed bank

    JP2000197426A

  • Artificial fish reef

    JP2004298172A