Sintered body
A sintered body with a rare earth oxyfluoride phase, produced via Spark Plasma Sintering, addresses the issue of inadequate corrosion resistance in conventional sintered bodies, enhancing resistance to halogen plasma and minimizing particle formation for improved semiconductor manufacturing.
Patent Information
- Application Number
- JP2021503463
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-07
- Filing Date
- 2020-01-30
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-01-30
AI Technical Summary
Conventional sintered bodies containing rare earth elements and fluorine exhibit inadequate corrosion resistance against halogen plasma, leading to reduced semiconductor yields due to particle formation from deteriorated components.
A sintered body with a phase of a compound containing rare earth elements and fluorine, characterized by a high L* value in the L*a*b* chromaticity system, is produced using a Spark Plasma Sintering (SPS) method at low temperatures to maintain a white color and minimize grain growth, ensuring a dense structure with a main phase of rare earth oxyfluoride.
The sintered body demonstrates enhanced corrosion resistance against halogen plasma, reducing particle formation and maintaining semiconductor device integrity.
Smart Images

Figure 0007568293000003 
Figure 0007568293000004 
Figure 0007568293000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a sintered body having a phase of a compound containing a rare earth element and fluorine. [Background technology]
[0002] In semiconductor manufacturing, components used in environments containing halogen-based gases, such as dry etching equipment, deteriorate when in contact with the halogen-based gas, and the deteriorated materials scatter and adhere to the semiconductor as particles, reducing the semiconductor yield. As a material having a certain degree of corrosion resistance to halogen-based gases, compounds containing rare earth elements and fluorine are used as materials to be sprayed onto the surfaces of semiconductor device components (Patent Document 1) or as sintered bodies that constitute semiconductor devices (Patent Document 2). Patent Document 2 describes that a sintered body of a compound containing rare earth elements and fluorine is denser than a sprayed film of a compound containing rare earth elements and fluorine, and is suitable as a component of semiconductor manufacturing equipment. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] US2015 / 0096462A1 [Patent Document 2] US2017 / 0305796A1 Summary of the Invention
[0004] However, there is still room for improvement in the corrosion resistance of sintered bodies of compounds containing rare earth elements and fluorine to halogen-based plasma.
[0005] Therefore, an object of the present invention is to provide a sintered body of a compound containing a rare earth element and fluorine, which has superior corrosion resistance to halogen-based plasma compared to conventional sintered bodies.
[0006] The present inventors have intensively studied the composition of a sintered body of a compound containing a rare earth element and fluorine in order to improve the corrosion resistance against halogen-based plasma. As a result, they have found that the corrosion resistance against halogen-based plasma can be effectively improved by increasing the whiteness of the sintered body of the compound.
[0007] The present invention provides a sintered body having a phase of a compound containing at least a rare earth element and fluorine, and having an L* value of 70 or more in the L*a*b* chromaticity scale. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a scanning electron microscope image of the sintered body obtained in Example 1. [Diagram 2] FIG. 2 is a scanning electron microscope image of the sintered body obtained in Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention will now be described based on its preferred embodiments. (1) Composition of the sintered body of the present invention One of the characteristics of the sintered body of the present invention is that it has a phase of a compound containing a rare earth element and fluorine (hereinafter, also simply referred to as a "compound containing Ln and F").
[0010] The rare earth elements (Ln) include 16 elements: scandium (Sc), yttrium (Y), lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu). Compounds containing Ln and F contain at least one of these 16 rare earth elements. From the viewpoint of further improving the heat resistance, wear resistance, corrosion resistance, and the like of the sintered body, it is preferable to use at least one element selected from among these elements: yttrium (Y), cerium (Ce), samarium (Sm), gadolinium (Gd), dysprosium (Dy), erbium (Er), and ytterbium (Yb), and it is particularly preferable to use yttrium (Y).
[0011] Preferred examples of the compound containing Ln and F include a fluoride of a rare earth element and / or an oxyfluoride of a rare earth element. From the viewpoint of increasing the corrosion resistance of the sintered body against halogen-based plasma, the compound containing Ln and F preferably includes a compound containing Ln, F and O, and is particularly preferably an oxyfluoride of a rare earth element, or an oxyfluoride of a rare earth element and a fluoride of a rare earth element.
[0012] The rare earth fluoride is preferably represented as LnF3.
[0013] Oxyfluorides of rare earth elements (hereinafter also referred to as "Ln-OF") are compounds consisting of rare earth elements (Ln), oxygen (O), and fluorine (F). Ln-OF may be a compound (LnOF) in which the molar ratio of rare earth elements (Ln), oxygen (O), and fluorine (F) is Ln:O:F=1:1:1, or may be other forms of oxyfluorides of rare earth elements (Ln5O4F7, Ln7O6F9, Ln4O3F6, etc.). From the viewpoint of more effectively achieving the effects of the present invention, such as the ease of production of oxyfluorides and high corrosion resistance, Ln-OF is preferably LnO x F yIt is preferable that the formula is expressed as (0.3≦x≦1.7, 0.1≦y≦1.9). From the above viewpoint, it is more preferable that the formula is 0.35≦x≦1.65, and even more preferable that the formula is 0.4≦x≦1.6. It is also more preferable that the formula is 0.2≦y≦1.8, and even more preferable that the formula is 0.5≦y≦1.5. It is also preferable that the formula is 2.3≦2x+y≦5.3, and especially 2.35≦2x+y≦5.1, and it is particularly preferable that the formula is 2x+y=3.
[0014] The sintered body of the present invention preferably contains a phase of a compound containing Ln and F, and more preferably contains a phase of a compound containing Ln, F and O. It can be confirmed by X-ray diffraction measurement that the sintered body contains a phase of a compound containing Ln and F, and a phase of a compound containing Ln, F and O (for example, a Ln-OF phase).
[0015] From the viewpoint of enhancing corrosion resistance against halogen-based plasma, the sintered body of the present invention preferably has a phase of a compound containing Ln and F as the main phase. The main phase means a phase derived from a substance having the highest peak height among all peaks observed in 2θ=10 to 90 degrees in X-ray diffraction measurement using Cu-Kα radiation or Cu-Kα1 radiation. Therefore, it can be confirmed that the sintered body of the present invention has a phase of a compound containing Ln and F as the main phase by the fact that the peak having the highest peak height among all peaks observed in the range of 2θ=10 to 90 degrees in X-ray diffraction measurement using Cu-Kα radiation or Cu-Kα1 radiation is that of a compound containing Ln and F. For example, the fact that the sintered body of the present invention has a phase of a compound containing Ln, F and O (for example, a Ln-OF phase) as the main phase can be confirmed by the fact that the peak with the highest peak height among all peaks observed in the range of 2θ=10 to 90 degrees in an X-ray diffraction measurement using Cu-Kα radiation or Cu-Kα1 radiation is that of a compound containing Ln, F and O (for example, a Ln-OF phase). It is particularly preferable that the sintered body of the present invention has a phase of a compound containing Ln, F and O as the main phase, and it is most preferable that the phase of Ln-OF is the main phase. When the phase of a compound containing Ln, F and O is the main phase, it may or may not have other crystal phases, but if it has them, it is preferable that the phase of LnF3 is the subphase.
[0016] From the viewpoint of further enhancing the corrosion resistance, in X-ray diffraction measurement at 2θ=10 to 90 degrees using Cu-Kα radiation or Cu-Kα1 radiation, the sintered body of the present invention has a peak height of the maximum height of a peak originating from a component other than the compound containing Ln and F of preferably 10% or less, more preferably 5% or less, and even more preferably 3% or less, relative to the main peak originating from a compound containing Ln and F, and most preferably no peak originating from a component other than the compound containing Ln and F is observed. The unit of peak height is cps.
[0017] The above items only need to be applicable to X-ray diffraction measurements using either Cu-Kα radiation or Cu-Kα1 radiation, and do not necessarily apply to X-ray diffraction measurements using both Cu-Kα radiation and Cu-Kα1 radiation. The X-ray diffraction measurement used in the present invention is a powder X-ray diffraction measurement method.
[0018] The sintered body of the present invention preferably has one or both of a rare earth element fluoride phase and a rare earth element oxyfluoride phase. When the sintered body of the present invention has a rare earth element fluoride phase and a rare earth element oxyfluoride phase, either of them may be the main phase, but it is preferable to have the rare earth element oxyfluoride as the main phase from the viewpoint of corrosion resistance to halogen plasma.
[0019] For example, when the sintered body of the present invention has a rare earth element fluoride phase and a rare earth element oxyfluoride phase, in an X-ray diffraction measurement at 2θ=10 to 90 degrees using Cu-Kα radiation or Cu-Kα1 radiation, the peak height of the peak derived from the (020) plane of the rare earth element fluoride is preferably 5% to 70%, more preferably 10% to 40%, of the main peak of the rare earth element oxyfluoride phase. For example, in an X-ray diffraction measurement using Cu-Kα radiation or Cu-Kα1 radiation, the peak derived from the (020) plane of yttrium fluoride is usually observed around 26.0, specifically in the range of 25.9 to 26.1 degrees. For example, when the rare earth element is yttrium, the main peak positions of yttrium fluoride and yttrium oxyfluoride may overlap, and for convenience, the presence of the rare earth element fluoride was confirmed here by the peak derived from the (020) plane. Among the yttrium oxyfluorides, the main peak of YOF is observed at 28.0 to 29.0 degrees, and the main peak of Y5O4F7 is usually observed at 27.5 to 28.5 degrees.
[0020] (2) L value The sintered body of the present invention has high corrosion resistance against halogen plasma because the L*a*b* chromaticity display, i.e., the L* value of the L*a*b* color coordinate system color coordinate system is 70 or more. This is believed to be due to the following reasons. Compounds containing Ln and F are white powders before sintering. However, when using them to produce a sintered body, in order to produce a sintered body of a certain strength in a general sintering method such as a hot press method, it is usually necessary to sinter at 1200°C or higher. When sintered at 1200°C, the movement and reaction of fluorine in the powder becomes active, and composition changes such as fluorine desorption defects are likely to occur, and when the powder contains oxygen, oxygen desorption defects are likely to occur. In particular, when sintered at 1200°C or higher in a low-oxygen state, fluorine and oxygen desorption defects are likely to occur. These defects are likely to lead to gray or black coloring. On the other hand, when sintering is performed at less than 1200°C, it is easy to obtain a sintered body with almost the same composition as the raw powder, even if it is fired in air or in a low-oxygen environment. In particular, when rare earth oxyfluorides or rare earth fluorides are sintered using plasma discharge sintering (SPS) or a pulse current sintering method other than SPS, it is possible to sinter them at low temperatures and in a relatively short time, and to obtain a sintered body that has few defects and maintains its white color. Such white sintered bodies have few fluorine and oxygen defects, so they are thought to have high corrosion resistance to halogen plasma. Whiteness can be measured with a color difference meter and can be determined by the L* value measured on the surface of the sintered body.
[0021] From the above viewpoint, in order to further enhance the halogen plasma corrosion resistance, the sintered body of the present invention preferably has an L* value of 75 or more, more preferably 80 or more, in the L*a*b* color coordinate system. From the viewpoint of ease of production of the sintered body, the upper limit of the L* value in the L*a*b* color coordinate system is preferably 95 or less, and more preferably 90 or less.
[0022] (3) a* value, b* value In a sintered body having a phase of a compound containing Ln and F, the a* value of the L*a*b* color coordinate system is generally -1 or more and 3 or less, and preferably 0 or more and 1 or less. In a sintered body having a phase of a compound containing Ln and F, the b* value of the L*a*b* color coordinate system is generally -1 or more and 3 or less, and preferably 0 or more and 1 or less. Sintered bodies having a* and b* values within the above ranges are preferred because coloring due to composition changes during production is suppressed. A sintered body having the a* and b* values within the above ranges can be obtained by a suitable method for producing a sintered body, which will be described later.
[0023] (4) Average grain size The sintered body of the present invention is dense and has a small average crystal grain size, which is preferable from the viewpoint of halogen-based plasma corrosion resistance. The average crystal grain size is preferably 10 μm or less. A sintered body having an average grain size of the crystal grains equal to or less than the upper limit can be obtained by the SPS (Spark Plasma Sintering) method. In the SPS method, powder raw material is usually filled into a sintering mold, and a DC pulse current is applied to sinter the mold, to which electric energy is directly applied, using the self-heating of the mold as a driving force for sintering together with pressure application. The SPS method generally enables sintering at a lower temperature and in a shorter time than other methods. By sintering at a lower temperature and in a shorter time, the SPS method can suppress grain growth. In particular, the SPS method reduces the heat capacity because the heated parts are only around and inside the sintering mold, making it possible to heat the material quickly. Grain growth can be further suppressed by applying pressure and rapidly raising the temperature at a low temperature. In contrast, as shown in Comparative Examples 1 to 3 described later, the hot pressing method requires high-temperature and long-term sintering, and since it takes a long time to raise the temperature, grain growth is large and the average grain size cannot be suppressed to 10 μm or less. In addition, when sintering at a high temperature of 1200° C. or more, grain growth is generally easy, and the average grain size cannot be suppressed to 10 μm or less.
[0024] In order to further improve the corrosion resistance of the sintered body of the present invention, the average grain size is preferably 10 μm or less, more preferably 5 μm or less, and particularly preferably 3 μm or less. The average grain size of the sintered body is preferably 0.1 μm or more, since sintering proceeds and the strength of the sintered body is obtained. The average grain size of the sintered body can be measured by the method described in the examples below.
[0025] (5) Strength The strength of the sintered body of the present invention is preferably higher than a certain level. This allows the sintered body to have high thermal stress, thermal shock, wear resistance, and processability. Specifically, the sintered body of the present invention preferably has a three-point bending strength of 100 MPa or more, more preferably 110 MPa or more. The higher the three-point bending strength of the sintered body, the more preferable it is, but the upper limit is preferably 500 MPa or less from the viewpoint of ease of manufacturing the sintered body. The sintered body having the above strength can be realized by adopting the SPS method in a vacuum atmosphere. The sintered body having the above strength can be obtained by manufacturing the sintered body of the present invention by a preferred manufacturing method described later. The three-point bending strength is measured by the method described in the examples described later.
[0026] (6) Oxygen content The sintered body of the present invention may contain oxygen in addition to rare earth elements and fluorine, and in that case, the content is preferably 13 mass% or less in terms of high corrosion resistance against halogen-based plasma and halogen-containing gas. From this viewpoint, the sintered body of the present invention more preferably has an oxygen content of 10 mass% or less, and even more preferably has an oxygen content of 9 mass% or less. The oxygen content of the sintered body may be zero, but when the sintered body contains oxygen in addition to rare earth elements and fluorine, it is preferably 0.3 mass% or more, and more preferably 1 mass% or more in terms of high corrosion resistance against oxygen-based plasma and oxygen-containing gas. The oxygen content in the sintered body can be measured, for example, by EMGA-920, an oxygen / nitrogen measuring device manufactured by Horiba, Ltd. The above oxygen content can be achieved by adjusting the oxygen content in the raw material powder to the preferred oxygen content range of the sintered body in a suitable manufacturing method for the sintered body described below.
[0027] (7) Relative density It is also preferable that the sintered body has a relative density of 95% or more. The relative density is the value obtained by dividing the measured density of the sintered body by the theoretical density (also called the calculated density) and multiplying the result by 100. The measured density of the sintered body is measured by the Archimedes method. The theoretical density of the sintered body varies depending on the composition. The theoretical density of Y5O4F7 is 5.15 g / cm 3 , the theoretical density of YOF is 5.23 g / cm 3 The relative density of the sintered body is preferably 95% or more, more preferably 97% or more, and particularly preferably 98% or more, so that a sintered body having high corrosion resistance and high strength can be obtained. From the same viewpoint, a sintered body having Y5O4F7 as the main phase has a measured density of 4.80 g / cm 3 It is preferable that the content is 4.90 g / cm or more. 3 The sintered body having YOF as the main phase has a measured density of 4.85 g / cm 3 It is preferable that the content is 4.95 g / cm or more. 3 More preferably, it is equal to or greater than this.
[0028] (8) Thickness The shape of the sintered body of the present invention is not limited, but the thickness is preferably about 0.1 to 500 mm, more preferably about 0.5 to 100 mm, and even more preferably about 1 to 30 mm, in that it can be suitably used for the various applications mentioned above. The thickness here does not necessarily require the sintered body to be in the form of a plate or film, and means the height when the sintered body is placed on a horizontal surface in a state where its horizontal projection area is maximized, regardless of the shape of the sintered body.
[0029] (9) Suitable manufacturing method Next, a preferred method for producing the sintered body of the present invention will be described. In this method, a raw material powder containing a compound containing Ln and F is preferably sintered at a temperature of less than 1200°C by the SPS method, more preferably the raw material powder is sintered in a vacuum atmosphere at 800°C or higher and lower than 1200°C by the SPS method, and particularly the raw material powder is sintered in a vacuum atmosphere at 800°C or higher and lower than 1200°C and a pressure of 20 MPa or higher and 100 MPa or lower by the SPS method.
[0030] The compound containing Ln and F used as the raw material of the sintered body is usually in powder form. The powder form here includes granular form. It is preferable to use a compound containing Ln and F used as the raw material of the sintered body that has a composition corresponding to the composition of the target sintered body. Therefore, it is preferable to use a fluoride of a rare earth element and / or an oxyfluoride of a rare earth element as the compound containing Ln and F used as the raw material of the sintered body. For example, when a sintered body having only a fluoride phase of a rare earth element is to be obtained, a raw material powder consisting of a fluoride of a rare earth element may be used. When a sintered body having an oxyfluoride phase of a rare earth element is to be obtained, it is preferable to use a raw material powder of an oxyfluoride of a rare earth element that constitutes the phase of the target sintered body from the viewpoint of obtaining a sintered body of uniform composition. Therefore, when a sintered body having only an LnOF phase is to be obtained, it is preferable to use a raw material powder consisting of LnOF, and when a sintered body having only an Ln5O4F7 phase is to be obtained, it is preferable to use a raw material powder consisting of Ln5O4F7. Similarly, when a sintered body having a rare earth element fluoride phase and a rare earth element oxyfluoride phase is to be obtained, it is preferable to use a raw material powder containing a rare earth element fluoride and a rare earth element oxyfluoride from the viewpoint of obtaining a sintered body of uniform composition. The raw material powders may be granular. For example, when a sintered body having a rare earth element fluoride phase and a rare earth element oxyfluoride phase is to be obtained, it is preferable to use 10 parts by mass or more and 1020 parts by mass or less of a rare earth element fluoride per 100 parts by mass of a rare earth element oxyfluoride from the viewpoint of obtaining a sintered body having particularly excellent corrosion resistance against halogen plasma, and it is even more preferable to use 20 parts by mass or more and 250 parts by mass or less of a rare earth element fluoride per 100 parts by mass of a rare earth element oxyfluoride. In addition, when obtaining a sintered body having a rare earth element oxyfluoride phase, a raw material powder in which rare earth element oxide Ln2O3 and rare earth element fluoride LnF3 are mixed may be used. The mixing ratio of Ln2O3 powder and LnF3 powder is preferably adjusted so that the oxygen content of the mixture of the two is 0.3 mass% or more and 10 mass% or less, more preferably 1 mass% or more and 9 mass% or less.The preferred oxygen content of the sintered body, Ln2O3 and LnF3 may be mixed and then fired to produce a powder containing an oxyfluoride of a rare earth element. The firing temperature is preferably 600°C to 1100°C, more preferably 800°C to 1000°C, in order to successfully produce an oxyfluoride of a rare earth element. The firing atmosphere may be an inert atmosphere such as argon or an oxidizing atmosphere such as air.
[0031] From the viewpoint of obtaining a sintered body having desirable physical properties such as denseness and corrosion resistance, the powder of the compound containing Ln and F contained in the raw material powder is preferably 10 μm or less in average particle size if it is not granulated granules. The lower limit of the average particle size of the powder of the compound containing Ln and F as the raw material is preferably 0.1 μm or more in terms of ease of obtaining the raw material, packing property, moldability, and composition stability. Also, from the viewpoint of obtaining a sintered body having desirable physical properties such as denseness and corrosion resistance, the average particle size of the powder of the compound containing Ln and F contained in the raw material powder is preferably 0.5 μm or more and 8 μm or less, more preferably 0.7 μm or more and 5 μm or less. On the other hand, when the powder of the compound containing Ln and F is granulated granules, the average particle size is preferably 10 μm or more and 50 μm or less, more preferably 20 μm or more and 48 μm or less, from the viewpoint of obtaining a sintered body having desirable physical properties such as denseness and corrosion resistance. The average particle size of the raw powder containing the compound containing Ln and F is preferably within the preferred range of the average particle size of the powder of the compound containing Ln and F. The average particle size of the powder of the compound containing Ln and F and the raw powder is the 50% diameter (hereinafter, simply referred to as "D50") in the cumulative fraction based on volume, and is measured by a laser diffraction / scattering particle size distribution measurement method. The specific measurement method is as follows. In the measurement of the average particle size by the method below, ultrasonic treatment is not performed as a pretreatment for granulated granules, but ultrasonic treatment at 300 W for 5 minutes is performed as a pretreatment for powders other than granulated granules.
[0032] (Method of measuring average particle size) Measurements are performed using a Microtrac HRA manufactured by Nikkiso Co., Ltd. During the measurements, a 2% by mass aqueous solution of sodium hexametaphosphate is used as the dispersion medium, and the sample is added to the chamber of the Microtrac HRA sample circulator until the device determines that the sample is at the appropriate concentration.
[0033] In this manufacturing method, the raw material powder is filled into a sintered mold, and then compression molding is performed. Compression molding can be performed, for example, by uniaxial pressing, but is not limited thereto. The DC pulse current may be applied to the sintered mold simultaneously with compression molding, or may be applied after compression molding. The pressures of compression molding and pressing during current application are preferably 20 MPa or more, more preferably 25 MPa or more, in that the average grain size of the crystal grains is easily made equal to or less than the upper limit described above. In addition, the pressures of compression molding and pressing during current application are preferably 100 MPa or less, in that damage to the press mold is suppressed, and more preferably 60 MPa or less.
[0034] Pulse current sintering can more effectively suppress grain growth by performing the sintering in a vacuum atmosphere. The absolute pressure in the vacuum atmosphere is preferably 10 Pa or less, and more preferably 8 Pa or less.
[0035] The sintering temperature is preferably less than 1200°C in that the L* value of the crystal grains is easily adjusted to the above upper limit or less and the average grain size of the crystal grains is adjusted to the above upper limit or less, more preferably 1100°C or less, and particularly preferably 1000°C or less. The sintering temperature is preferably 800°C or more in that a dense sintered body can be obtained, and more preferably 900°C or more. The sintering temperature here refers to the maximum sintering temperature.
[0036] The sintering time at the above-mentioned maximum sintering temperature is preferably 60 minutes or less in terms of suppressing grain growth and preventing coloration, more preferably 30 minutes or less, and particularly preferably 10 minutes or less.
[0037] The heating rate during pulse current application is preferably 2° C. / min or more in terms of shortening the heating time and effectively preventing grain growth, more preferably 4° C. / min or more, and particularly preferably 10° C. / min or more. The heating rate referred to here refers to the average heating rate during all heating periods when the heating rate from room temperature to the maximum sintering temperature is not constant.
[0038] In addition, during the temperature rise, it is preferable to apply pressure at the above pressure until the maximum sintering temperature is reached from room temperature in order to suppress grain growth. In particular, when the maximum sintering temperature is reached from room temperature and a certain holding time is set at the maximum sintering temperature, it is preferable to apply pressure at the above pressure until the end of the holding time in order to suppress grain growth.
[0039] The duration of one pulse is preferably 10 milliseconds or more and 100 milliseconds or less, from the viewpoint of obtaining a uniform sintered body, and more preferably 20 milliseconds or more and 50 milliseconds or less.
[0040] The sintered body thus obtained is preferably used in a halogen-containing dry etching gas atmosphere, since it can exhibit corrosion resistance against halogen. The applications of the sintered body used in a halogen-containing dry etching gas atmosphere include the vacuum chamber in the etching device, as well as various components in the semiconductor manufacturing device, such as the sample stage, chuck, shower head, wafer holder, focus ring, etching gas supply port, and exposure device in the chamber. Specific examples of halogen-containing dry etching gas include CHF3, CF4, C2F6, CF6, CCl4, BCl3, Cl2, HCl, H2, Ar, etc., and these gases are used in combination as necessary. In addition to being used as a component of a semiconductor manufacturing device, the sintered body of the present invention can also be used as a component of various plasma processing devices and chemical plants. The uses of the sintered body may be other than those of a film forming material such as a sputtering target. EXAMPLES
[0041] The present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to such examples. Unless otherwise specified, "%" means "mass %". The average particle size of the powder in the following examples and comparative examples refers to the above-mentioned D50.
[0042] [Example 1] (Production of sintered body containing Y5O4F7 and YF3 by SPS sintering) A powder of a mixed phase consisting of Y5O4F7 and YF3 was prepared by mixing Y2O3 powder (average particle size 3 μm) and YF3 powder (average particle size 6 μm) in a mass ratio of 4:9 and calcining the powder at 1000 °C for 5 hours in air. The obtained mixed phase powder was slurried, pulverized, granulated in a spray dryer and dried, and further calcined at 600 °C for 6 hours in air to obtain granules with an average particle size of 45 μm. When the powder X-ray diffraction measurement was performed on the granules, Y5O4F7 was observed as the main phase of the crystal phase, and YF3 was observed as the subphase. In the X-ray diffraction measurement, the peak height ratio derived from the (020) plane of YF3 observed around 2θ = 26.0 degrees was 16% with respect to the main peak of Y5O4F7 observed at 2θ = 27.5 to 28.5 degrees. No peaks attributable to components other than Y5O4F7 and YF3 were observed (the method for the X-ray diffraction measurement was the same as the XRD measurement method for the sintered powder described below). 2500g of the mixed phase granules were placed in a cylindrical mold with a diameter of 260mm and pressure-sintered using a pulse current pressure sintering device LABOX-650F (maximum pulse current output 5000A, maximum load 60kN). The chamber was kept in a vacuum atmosphere of 6Pa or less from the start of pressure application. The current application time of one pulse was 40 milliseconds. The pressure condition was 30MPa. Pressure application and current application started simultaneously. The temperature was raised from room temperature to 980°C at a temperature increase rate of 20°C / min, and then the temperature was maintained for 5 minutes. Then, current application and pressure application were stopped simultaneously, and the sintered body was cooled to 100°C, and a sintered body with a thickness of about 10mm was taken out. The results of powder X-ray diffraction measurement of the sintered body under the following conditions are shown in Table 1. In the X-ray diffraction measurement, the peak height ratio of the peak due to the (020) plane of YF3 observed at about 2θ=26.0 degrees to the main peak of Y5O4F7 observed at 2θ=27.5 to 28.5 degrees was 17%. No peaks due to components other than Y5O4F7 and YF3 were observed.
[0043] <XRD measurement of sintered powder> A portion of the sintered body was ground for 10 minutes using a magnetic mortar and pestle with ethanol added dropwise so that the material was completely immersed in it, to obtain a powder. This powder was then classified using a 150 μm sieve, and the undersieve fraction was subjected to X-ray diffraction measurement under the following conditions. Equipment: UltimaIV (Rigaku Corporation) ·Radiation source: CuKα radiation Tube voltage: 40kV ·Tube current: 40mA Scan speed: 2 degrees / min Step: 0.02 degrees Scan range: 2θ=10 degrees to 90 degrees
[0044] [Example 2] (Production of sintered body containing YOF by SPS sintering) Instead of the granules of the mixed phase of Y5O4F7 and YF3, YOF powder (average particle size 0.8 μm) was used. 6 g of this YOF powder was placed in a cylindrical mold with a diameter of 20 mm and pressure sintered using the same device as in Example 1. The inside of the chamber was kept in a vacuum atmosphere of 6 Pa or less from the start of pressure application. The current application time of one pulse was 40 milliseconds. The pressure condition was 30 MPa. Pressurization and current application started simultaneously. The temperature was raised from room temperature to 1000°C at a temperature increase rate of 10°C / min, and then the temperature was maintained for 5 minutes. Then, current application and pressurization were stopped simultaneously, and the mixture was cooled to 100°C, and a sintered body with a thickness of about 4 mm was obtained. When the sintered body was subjected to X-ray diffraction measurement under the above conditions, no peaks derived from components other than YOF were observed.
[0045] [Example 3] (Production of sintered body containing Y5O4F7 by SPS sintering) Instead of the granules of the mixed phase of Y5O4F7 and YF3, Y5O4F7 powder (average particle size 1.1 μm) was used. The temperature was increased by 4°C / min to 900°C, then increased by 2°C / min from 900°C to 950°C, and then held at that temperature for 5 minutes. Except for this, a sintered body with a thickness of about 10 mm was obtained in the same manner as in Example 1. When the sintered body was subjected to X-ray diffraction measurement under the above conditions, no peaks derived from components other than Y5O4F7 were observed.
[0046] [Comparative Example 1] (Production of sintered body containing Y5O4F7 and YF3 by HP sintering) About 200 g of the granules of the mixed phase of Y5O4F7 and YF3 used in Example 1 was placed in a cylindrical mold with a diameter of 76.2 mm, and then placed in a carbon hot press mold of the same size as the mold, and sintered by hot pressing. Under Ar flow (flow rate 2 liters / min), the temperature was raised to 900°C at a rate of 30°C / min, and further raised to 1200°C at a rate of 10°C / min, and then uniaxially pressed at a pressure of 2.94 MPa while maintaining at 1200°C for 2 hours. As a result, a sintered body was obtained.
[0047] [Comparative Example 2] (Production of YOF-containing sintered body by HP sintering) A sintered body was produced in the same manner as in Example 2 of Patent Document 2. That is, about 20 g of YOF powder (average particle size 0.8 μm) was placed in a rectangular mold 35 mm long and 35 mm wide, and primary molding was performed at a pressure of 18.4 MPa using a hydraulic press. This was placed in a carbon hot press mold of the same size as the rectangular mold, and sintered by hot pressing. In an Ar flow (flow rate 2 liters / min), the temperature was raised to 1200°C at 30°C / min, further raised to 1600°C at 10°C / min, held at 1600°C for 1 hour, then lowered to 1200°C at 10°C / min, and then lowered at 30°C / min. While held at 1600°C for 1 hour, uniaxial pressure was applied at a pressure of 36.7 MPa. A sintered body was thus obtained.
[0048] [Comparative Example 3] (Production of sintered body containing Y5O4F7 by HP sintering) A sintered body was manufactured in the same manner as in Example 4 of Patent Document 2. That is, about 20 g of Y5O4F7 powder (average particle size 1.1 μm) was placed in a rectangular mold 35 mm long and 35 mm wide, and primary molding was performed at a pressure of 18.4 MPa using a hydraulic press. This was placed in a carbon hot press mold of the same size as the rectangular mold, and sintered by hot pressing. In an Ar flow (flow rate 2 liters / min), the temperature was raised to 1200°C at 30°C / min, and then further raised to 1400°C at 10°C / min, and then cooled to 1200°C at 10°C / min, and then cooled at 30°C / min. The holding time at 1400°C was 0 hours. While the temperature was 1200°C or higher, uniaxial pressure was applied at 36.7 MPa. As a result, a sintered body was obtained.
[0049] The relative density and oxygen content of the sintered bodies obtained in the examples and comparative examples were measured by the above-mentioned methods. The average grain size, L* value, a* value, b* value, and three-point bending strength were also measured by the following methods. The results are shown in Table 1. Table 1 also shows the results of X-ray diffraction measurement. The measured density of the sintered body of Example 1 was 4.96 g / cm. 3 It was.
[0050] <Average grain size (grain size)> The average grain size of crystal grains was measured using the intercept method. In the intercept method, a straight line is drawn on a scanning electron microscope (SEM) image, the length of one line crossing one grain is taken as the grain size, and the average value is taken as the average grain size of the crystal grains. Five straight lines are drawn parallel to each other in the diagonal direction on the SEM image (photograph). The five straight lines are drawn at positions that divide the distance between two corners facing each other in the diagonal direction of the rectangular SEM image (photograph) into six equal parts. The straight lines are drawn from the grain boundary closest to one end of the image to the grain boundary closest to the other end of the image. This is done for two different fields of view. The total length of the 10 straight lines in the two fields of view is calculated using the following formula 1 from the number of intersections with the grain boundaries. However, the number of intersections does not include both ends of the lines. (Formula 1) Average grain size of crystal grains = total length of 10 straight lines in 2 fields of view / (total number of straight lines in 2 fields of view + total number of intersections with grain boundaries of 10 straight lines in 2 fields of view) The magnification of the SEM image is set so that the number of crystal grains observed in the image is between 10 and 30 (however, the crystal grains counted here include only those crystal grains that are observed in their entirety in the image, and do not include those that are partially cut off and cannot be seen). The samples were broken and cut out to obtain cross sections, which were then mirror-polished, sintered in an argon atmosphere, and thermally etched. The sintering temperatures were based on the melting points of the sintered bodies, and were 830°C for Example 1 and Comparative Example 1, 1400°C for Example 2 and Comparative Example 2, and 900°C for Example 3 and Comparative Example 3. The holding time was 1 hour. The etched surfaces were then photographed with a SEM to obtain images. 1 and 2 show SEM images used in measuring the average grain size of crystal grains in Example 1 and Comparative Example 1. Comparing Fig. 1 and Fig. 2, the sintered body of Example 1 clearly has fewer defects than the sintered body of Comparative Example 1.
[0051] <Method of measuring 3-point bending strength> The sintered body is cut, and the cross-section is mirror-polished to produce strip-shaped test pieces with a thickness of 1.5 to 3.0 mm, a width of about 4 mm, and a length of about 35 mm. These are placed on a jig made of SiC, and a three-point bending test is performed using a universal material testing machine (Model 1185, manufactured by INSTRON). The conditions are a support distance of 30 mm and a crosshead speed of 0.5 mm / min, and the number of test pieces is 5. Based on JIS R1601, the three-point bending strength [MPa] is calculated using the following formula. Three-point bending strength = (3 × P f × L) / (2 × w × t 2 ) (MPa) Here, P f is the load [N] at the time of fracture of the test piece, L is the span distance [mm], w is the width of the test piece [mm], and t is the thickness of the test piece [mm].
[0052] <L* value, a* value, b* value> Measurement was carried out using a spectrocolorimeter CR100 manufactured by Konica Minolta.
[0053]
Table 1
[0054] <Evaluation method for the number of generated particles> Plasma etching was performed on the sintered body. When performing plasma etching, a 3-inch silicon wafer was placed in the chamber. The number of particles with a particle size of about 0.2 μm or more among the particles scattered and adhered to the surface of the silicon wafer due to the etching action was measured using a magnifying glass. The plasma etching conditions were as follows, using fluorine-based plasma. · Atmosphere gas CHF3:Ar:O2 = 80:160:100 mL / min · High-frequency power: 1300 W · Pressure: 4 Pa · Temperature: 60 °C · Etching time: 100 hours Also, the same measurement was carried out when CHF3 of the atmosphere gas was changed to HCl to make chlorine-based plasma. The results are shown in Table 2.
[0055] [Table 2]
[0056] As described above, in the sintered body of Example 1, the number of particles generated was half or less under both fluorine-based and chlorine-based plasma conditions compared to the sintered body of Comparative Example 1, which has a main phase of Y5O4F7 and a subphase of YF3 as in Example 1. Similarly, the number of particles generated was significantly reduced in the sintered body of Example 2, which is a YOF sintered body, compared to Comparative Example 2, and in the sintered body of Example 3, which is a Y5O4F7 sintered body, compared to Comparative Example 3. From the above, it is clear that the sintered body of the present invention, whose L* value is a specific value or less, has excellent halogen-based plasma corrosion resistance. [Industrial Applicability]
[0057] According to the present invention, it is possible to provide a sintered body having a phase of a compound containing a rare earth element and fluorine, and having superior corrosion resistance to halogen-based plasma compared to conventional sintered bodies.
Claims
1. A sintered body for use as a component of semiconductor manufacturing equipment, the sintered body having a rare earth element oxyfluoride phase as the main phase, wherein in the L*a*b* chromaticity display, the L* value is 70 or more and less than 90, the a* value is -1 or more and 3 or less, and the b* value is -1 or more and 3 or less.
2. 2. The sintered body according to claim 1, wherein the average grain size of the crystal grains is 10 μm or less.
3. 3. The sintered body according to claim 1, having a relative density of 95% or more.
4. The sintered body according to any one of claims 1 to 3, having a three-point bending strength of 100 MPa or more.
5. A sintered body described in any one of claims 1 to 4, having an oxygen content of 13 mass% or less.
6. The sintered body according to any one of claims 1 to 5, which is used in a halogen-containing dry etching gas atmosphere.
7. A method for producing a sintered body as described in claim 1, in which a raw material powder containing a rare earth element and a compound containing fluorine is SPS sintered at a temperature of less than 1200°C.
Citation Information
Patent Citations
Sintered body
JP2016098143A
Material for spray coating, spray coating film, and member with spray coating film
JP2016211072A
Manufacturing method of YOF based powder
KR1020190017333A
Thermal spray material and process for preparing same
US20150096462A1
Sintered body
US20170305796A1