Porous polyimide film and method for producing same

A method using pyromellitic dianhydride and 4,4'-diaminodiphenyl ether in a controlled solvent system produces a thin, highly porous polyimide film with enhanced properties for flexible printed circuits, addressing the limitations of existing technologies.

JP7568332B2Active Publication Date: 2024-10-16I S T CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023569473
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-12-23
Filing Date
2022-12-21
Publication Date
2024-10-16
Estimated Expiration
2042-12-21

AI Technical Summary

Technical Problem

Existing methods struggle to produce a relatively thin porous polyimide film with high porosity, limiting its suitability for applications such as electrical insulating and frequency selective films in flexible printed circuits.

Method used

A method involving the polymerization of pyromellitic dianhydride and 4,4'-diaminodiphenyl ether in a specific solvent system, followed by drying and firing to create a porous polyimide film with controlled solvent properties, ensuring high porosity and thinness.

Benefits of technology

The resulting porous polyimide film exhibits high porosity, suitable for electrical insulation and frequency selectivity, with improved thermal conductivity, dielectric properties, and mechanical strength, making it suitable for flexible printed circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568332000001
    Figure 0007568332000001
  • Figure 0007568332000002
    Figure 0007568332000002
Patent Text Reader

Abstract

The present invention addresses the problem of providing a porous polyimide film which can be suitably used as an electrical insulating film, a frequency-selective film, or the like in a flexible substrate (FPC) or the like. In a method for producing a porous polyimide film according to the present invention, a polyamic acid solution is dried and then sintered to obtain the porous polyimide film, the polyamic acid solution comprising: (a) a polyamic acid which is obtained by polymerization reaction between an aromatic tetracarboxylic dianhydride containing at least a pyromellitic dianhydride and an aromatic diamine containing at least 4,4'-diaminodiphenyl ether; (b) an organic polar solvent which is a good solvent for the polyamic acid; and (c) a hydrophobic solvent which is a poor solvent for the polyamic acid, is dissolved in the organic polar solvent, is less likely to evaporate than the organic polar solvent at the same temperature and pressure, and has logP ranging from 4.00 to 6.00.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a porous polyimide film that can be suitably used as an electrical insulating film or a frequency selective film in a flexible printed circuit (FPC) or the like, and a method for producing the same. [Background technology]

[0002] Porous bodies of polyimide resins, which have excellent physical properties such as mechanical strength, chemical properties such as heat resistance and chemical resistance, and electrical properties such as low dielectric constant and low dielectric tangent, are used as useful materials that take advantage of these properties in a variety of industrial applications.

[0003] For example, Japanese Patent Laid-Open Publication No. 49-45152 discloses a method for producing a porous polyimide film by casting a solution of a polyamic acid obtained by a polymerization reaction between an aromatic tetracarboxylic dianhydride and an aromatic diamine onto a liquid thin film, and precipitating the thin film while imidizing it in a poor solvent.

[0004] Furthermore, Japanese Patent Application Laid-Open No. 9-100363 discloses a heat-resistant low-dielectric plastic insulating film used for printed wiring boards for electronic devices and the like, slot insulation for rotating machines, etc., which contains a porous plastic with a porosity of 10 vol% or more, has a heat-resistant temperature of 100°C or more, and a dielectric constant of 2.5 or less.

[0005] In addition, known methods for producing porous polyimide include a method in which a polymer solution in which a polyimide resin is dissolved in a good aprotic solvent is brought into contact with a poor solvent such as water that is compatible with the good aprotic solvent to form a porous membrane, usually by a method called dry-wet spinning (e.g., JP-A-11-537), and a thermally induced phase separation method in which a polymer solution is made porous by applying a temperature change (e.g., JP-A-6-166116). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Publication No. 49-45152 [Patent Document 2] Japanese Patent Application Publication No. 9-100363 [Patent Document 3] Japanese Patent Application Publication No. 11-537 [Patent Document 4] Japanese Patent Application Publication No. 6-166116 Summary of the Invention [Problem to be solved by the invention]

[0007] However, when a relatively thin porous polyimide film is produced by the above-mentioned method for producing a porous polyimide film, it is difficult to increase the porosity of the film. For this reason, the industrial world has been waiting for the emergence of a relatively thin porous polyimide film having a high porosity.

[0008] An object of the present invention is to provide a porous polyimide film which is relatively thin but has a high porosity, and which can be suitably used as an electrical insulating film or a frequency selective film in a flexible printed circuit (FPC) or the like. [Means for solving the problem]

[0009] In a method for producing a porous polyimide film according to a first aspect of the present invention, (a) a polyamic acid obtained by polymerizing an aromatic tetracarboxylic dianhydride containing at least pyromellitic dianhydride with an aromatic diamine containing at least 4,4'-diaminodiphenyl ether; (b) an organic polar solvent that is a good solvent for the polyamic acid; (c) a solvent that is a poor solvent for the polyamic acid and dissolves in the organic polar solvent; The boiling point at the same pressure minus the boiling point of the organic polar solvent is within the range of 15°C to 260°C. and a hydrophobic solvent having a logP in the range of 4.00 to 6.00. The polyamic acid solution is dried and then baked to obtain a porous polyimide film.

[0010] In the method for producing a porous polyimide film according to the first aspect of the present invention, the hydrophobic solvent preferably has a boiling point at 1 atmospheric pressure in the range of 280° C. or more and 350° C. or less.

[0011] In the method for producing a porous polyimide film according to the first aspect of the present invention, the polyamic acid solution preferably contains 60% by mass or more of polyamic acid obtained by polymerization reaction of pyromellitic dianhydride and 4,4'-diaminodiphenyl ether.

[0012] The porous polyimide film according to the second aspect of the present invention contains at least a polyimide resin obtained from a polyamic acid obtained by polymerization reaction of pyromellitic dianhydride and 4,4'-diaminodiphenyl ether. The porous polyimide film contains at least The boiling point at 1 atmosphere is within the range of 280℃ to 350℃. A hydrophobic poor solvent having a logP value in the range of 4.00 to 6.00 remains. Effect of the Invention

[0013] The porous polyimide film according to the present invention is relatively thin but has a high porosity, and can be suitably used as an electrical insulating film or a frequency selective film in a flexible printed circuit (FPC), etc. Moreover, the method for producing a porous polyimide film according to the present invention can produce such a porous polyimide film. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 shows measurement charts obtained when the porous polyimide films obtained in Examples 1, 3, and 4 and Comparative Example 8 were heated from room temperature to 500° C. at a heating rate of 5° C. / min using a simultaneous differential thermal / thermogravimetric (TG / DTA) measurement device. [Diagram 2] 1 is a digital microscope photograph of the porous polyimide film obtained in Example 1 after hole drilling. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] In the method for producing a porous polyimide film according to the embodiment of the present invention, a polyamic acid solution containing a polyamic acid, an organic polar solvent, and a hydrophobic solvent is dried and then baked to obtain a porous polyimide film. The polyamic acid is a polyamic acid obtained by polymerizing an aromatic tetracarboxylic dianhydride containing at least pyromellitic dianhydride and an aromatic diamine containing at least 4,4'-diaminodiphenyl ether. The organic polar solvent is a good solvent for the polyamic acid. The hydrophobic solvent is a poor solvent for the polyamic acid and dissolves in the organic polar solvent. The hydrophobic solvent is less likely to evaporate than the organic polar solvent at the same temperature and pressure. The logP of the hydrophobic solvent is in the range of 4.00 to 6.00.

[0016] In the method for producing a porous polyimide film according to the embodiment of the present invention, the boiling point of the hydrophobic solvent is preferably higher than that of the organic polar solvent. The boiling point of the hydrophobic solvent at 1 atmospheric pressure is preferably in the range of 280°C to 350°C, more preferably in the range of 300°C to 350°C. The boiling point of the organic polar solvent at 1 atmospheric pressure is preferably in the range of 60°C to 270°C. The value obtained by subtracting the boiling point of the organic polar solvent from the boiling point of the hydrophobic solvent is preferably in the range of 15°C to 260°C, more preferably in the range of 50°C to 180°C, and even more preferably in the range of 70°C to 160°C.

[0017] In an embodiment of the present invention, the polyamic acid may be synthesized by polymerizing an aromatic tetracarboxylic dianhydride and an aromatic diamine in a mixed solvent of an organic polar solvent and a hydrophobic poor solvent, or may be synthesized by polymerizing an aromatic tetracarboxylic dianhydride and an aromatic diamine in an organic polar solvent, in which case the hydrophobic poor solvent is added to the resulting polyamic acid solution.

[0018] In the synthesis of the polyamic acid according to the embodiment of the present invention, an aromatic tetracarboxylic dianhydride other than pyromellitic dianhydride may be used within the scope of the present invention. Examples of such aromatic tetracarboxylic dianhydrides include 1,2,5,6-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 2,3,3'4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 2,3,3',4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), bis(3,4-dicarboxyphenyl)sulfone dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)methane dianhydride, 1,1-bis Examples of suitable dianhydrides include (2,3-dicarboxyphenyl)ethane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, 2,2-bis[3,4-(dicarboxyphenoxy)phenyl]propane dianhydride (BPADA), 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, oxydiphthalic anhydride (ODPA), bis(3,4-dicarboxyphenyl)sulfone dianhydride, bis(3,4-dicarboxyphenyl)sulfoxide dianhydride, thiodiphthalic dianhydride, 3,4,9,10-perylene tetracarboxylic dianhydride, 2,3,6,7-anthracene tetracarboxylic dianhydride, 1,2,7,8-phenanthrene tetracarboxylic dianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, and 9,9-bis[4-(3,4'-dicarboxyphenoxy)phenyl]fluorene dianhydride. However, from the viewpoint of solubility in hydrophobic solvents and from the viewpoint of obtaining a porous polyimide film with high porosity, it is preferable that the aromatic tetracarboxylic dianhydride is mostly pyromellitic dianhydride.

[0019] In the synthesis of the polyamic acid according to the embodiment of the present invention, aromatic diamines other than 4,4'-diaminodiphenyl ether may be used within the scope of the present invention. Examples of such aromatic diamines include paraphenylenediamine (PPD), metaphenylenediamine (MPDA), 2,5-diaminotoluene, 2,6-diaminotoluene, 4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dimethoxy-4,4'-diaminobiphenyl, 2,2-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 3,3'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane (MDA), 2,2-bis-(4-aminophenyl)propane, 3,3'-diaminodiphenylsulfone (33DDS), 4,4'-diaminodiphenylsulfone (44DDS), 3,3'-diaminodiphenylsulfide, 4,4'-diaminodiphenylsulfide, 3,3'-diaminodiphenylether, and 3,4'-diaminodiphenylether (34ODA). 1,5-Diaminonaphthalene, 4,4'-Diaminodiphenyldiethylsilane, 4,4'-Diaminodiphenylsilane, 4,4'-Diaminodiphenylethylphosphine oxide, 1,3-Bis(3-aminophenoxy)benzene (133APB), 1,3-Bis(4-aminophenoxy)benzene (134APB), 1,4-Bis(4-aminophenoxy)benzene, Bis[4-(3-aminophenoxy)phenyl]sulfonate Examples of aromatic diamines include bis[4-(4-aminophenoxy)phenyl]sulfone (BAPSM), bis[4-(4-aminophenoxy)phenyl]sulfone (BAPS), 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), 2,2-bis(3-aminophenyl)1,1,1,3,3,3-hexafluoropropane, 2,2-bis(4-aminophenyl)1,1,1,3,3,3-hexafluoropropane, and 9,9-bis(4-aminophenyl)fluorene. However, from the viewpoint of solubility in hydrophobic solvents and from the viewpoint of obtaining a porous polyimide film with a high porosity, it is preferable that most of the aromatic diamines are 4,4'-diaminodiphenyl ether.

[0020] The polyamic acid obtained from the aromatic tetracarboxylic dianhydride and aromatic diamine preferably contains 60% by mass or more of polyamic acid obtained by polymerization reaction of pyromellitic dianhydride and 4,4'-diaminodiphenyl ether, because the polyamic acid does not gel and the porous polyimide film can maintain its shape well in the method for producing the porous polyimide film according to the embodiment of the present invention.

[0021] The solids concentration of the polyamic acid solution according to the embodiment of the present invention is not particularly limited as long as it is a solids concentration that results in a viscosity range suitable for producing a porous polyimide film, but for example, it is preferably within the range of 5 mass % or more and 30 mass % or less, more preferably within the range of 5 mass % or more and 27 mass % or less, and even more preferably within the range of 5 mass % or more and 25 mass % or less.

[0022] In addition, examples of hydrophobic solvents used in the method for producing a porous polyimide film according to an embodiment of the present invention include (1,7,7-trimethylbicyclo[2.2.1]hept-2-yl)cyclohexane-1-ol (boiling point 308°C, logP 4.96), 4-(5,5,6-trimethylbicyclo[2.2.1]heptan-2-yl)cyclohexanol (boiling point 324.5°C, logP 4.48), 3-[2,3,3-trimethylbicyclo[2,2,1]hept-5-yl]cyclohexanol (boiling point 312°C, logP 4.47), and 1,2,3,4,4a,5,6,7-octahydro-2,5,5-trimethyl-2-naphthol (boiling point 280.1°C, logP 4.07).

[0023] In addition, hydrophobic solvents such as 1-hydroxycyclohexyl phenyl ketone (boiling point 339°C, log P 2.04), 4-(4-hydroxy-4-methylpentyl)-3-cyclohexenecarbaldehyde (boiling point 290°C, log P 2.78), and 4,4'-bicyclohexanol (boiling point 324°C, log P 2.49) can also be used in combination with the above-mentioned hydrophobic solvents within the scope of the present invention.

[0024] As described above, the logP of the hydrophobic solvent is in the range of 4.00 to 6.00. This logP is calculated by a known calculation method. Specifically, the logP is calculated by a commercially available software using a quantitative structure-activity relationship algorithm. An example of such commercially available software is ChemdrawPro12.0. The logP can also be calculated using the online site http: / / www.vcclab.org / lab / alogps / start.html.

[0025] Examples of organic polar solvents used in the method for producing a porous polyimide film according to an embodiment of the present invention include amide solvents such as N,N-dimethylformamide (boiling point 153° C.), N,N-dimethylacetamide (boiling point 165° C.), 3-methoxy-N,N-dimethylpropanamide (boiling point 215° C.), dimethylisobutyric acid amide (boiling point 175° C.), N-methyl-2-pyrrolidone (boiling point 202° C.), and hexamethylphosphoric triamide (boiling point 233° C.), gamma butyrolactone (boiling point 204° C.), etc. Examples of the organic polar solvent include ester solvents such as 1,2-dimethoxyethane (boiling point 85°C), diglyme (boiling point 162°C), triglyme (boiling point 216°C), tetrahydrofuran (boiling point 66°C), 1,3-dioxolane (boiling point 74°C), and 1,4-dioxane (boiling point 101°C), ketone solvents such as cyclopentanone (boiling point 131°C), and urea solvents such as tetramethylurea (boiling point 176.5°C), N,N-dimethylethylurea (boiling point 262°C), and 1,3-dimethyl-2-imidazolidinone (boiling point 225°C). In addition, the organic polar solvent is preferably a urea solvent or an amide solvent, and more preferably an amide solvent, because it maintains good solubility in polyamic acid and good reactivity between aromatic tetracarboxylic dianhydride and aromatic diamine. As the amide-based solvent, N,N-dimethylformamide, N,N-dimethylacetamide (DMAC), and N-methyl-2-pyrrolidone (NMP) are particularly preferred. These organic polar solvents may be used alone or in combination. In addition, aromatic hydrocarbons such as toluene and xylene may be mixed with the organic polar solvent.

[0026] The obtained polyamic acid solution can be used as it is for producing a porous polyimide film, but if necessary, the polyamic acid solution may be used for producing a porous polyimide film after removing or adding a solvent thereto.

[0027] Furthermore, an imidization catalyst, an organic phosphorus-containing compound, inorganic fine particles, etc. may be added to the polyamic acid solution according to the embodiment of the present invention, if necessary.

[0028] Examples of the imidization catalyst include substituted or unsubstituted nitrogen-containing heterocyclic compounds, N-oxide compounds of the nitrogen-containing heterocyclic compounds, substituted or unsubstituted amino acid compounds, aromatic hydrocarbon compounds having a hydroxyl group, or aromatic heterocyclic compounds. In particular, lower alkyl imidazoles such as 1,2-dimethylimidazole, N-methylimidazole, N-benzyl-2-methylimidazole, 2-methylimidazole, 2-ethyl-4-methylimidazole, and 5-methylbenzimidazole, benzimidazoles such as N-benzyl-2-methylimidazole, isoquinoline, and substituted pyridines such as 3,5-dimethylpyridine, 3,4-dimethylpyridine, 2,5-dimethylpyridine, 2,4-dimethylpyridine, and 4-n-propylpyridine can be suitably used. The imidization catalyst is preferably added in an amount of 0.01 to 2 times the equivalent of the amic acid unit of the polyamic acid, and more preferably added in an amount of 0.02 to 1 times the equivalent. The physical properties of the resulting porous polyimide film, particularly the elongation and edge tear resistance, may be improved by adding an imidization catalyst to the polyamic acid solution.

[0029] Examples of the organic phosphorus-containing compound include phosphates such as monocaproyl phosphate, monooctyl phosphate, monolauryl phosphate, monomyristyl phosphate, monocetyl phosphate, monostearyl phosphate, monophosphate of triethylene glycol monotridecyl ether, monophosphate of tetraethylene glycol monolauryl ether, monophosphate of diethylene glycol monostearyl ether, dicaproyl phosphate, dioctyl phosphate, dicapryl phosphate, dilauryl phosphate, dimyristyl phosphate, dicetyl phosphate, distearyl phosphate, diphosphate of tetraethylene glycol mononeopentyl ether, diphosphate of triethylene glycol monotridecyl ether, diphosphate of tetraethylene glycol monolauryl ether, and diphosphate of diethylene glycol monostearyl ether, as well as amine salts of these phosphates. Examples of the amine in the amine salt include ammonia, monomethylamine, monoethylamine, monopropylamine, monobutylamine, dimethylamine, diethylamine, dipropylamine, dibutylamine, trimethylamine, triethylamine, tripropylamine, tributylamine, monoethanolamine, diethanolamine, and triethanolamine.

[0030] Examples of inorganic fine particles include inorganic oxide powders such as titanium dioxide powder, silicon dioxide (silica) powder, magnesium oxide powder, aluminum oxide (alumina) powder, and zinc oxide powder, inorganic nitride powders such as silicon nitride powder and titanium nitride powder, inorganic carbide powders such as silicon carbide powder, and inorganic salt powders such as calcium carbonate powder, calcium sulfate powder, and barium sulfate powder. These inorganic fine particles may be used alone or in combination. In addition, known methods can be used to uniformly disperse these inorganic fine particles in the polyamic acid solution.

[0031] Next, the porous polyimide film according to the embodiment of the present invention contains at least a polyimide resin obtained from a polyamic acid obtained by polymerizing pyromellitic dianhydride and 4,4'-diaminodiphenyl ether. At least a hydrophobic solvent remains in this porous polyimide film. In this porous polyimide film, the hydrophobic solvent often remains in the pores. Therefore, the water absorption of the porous polyimide film is suppressed, and the dimensional change due to the expansion of the porous polyimide film can be suppressed.

[0032] The porous polyimide film according to the embodiment of the present invention contains at least a polyimide resin obtained from a polyamic acid obtained by polymerization reaction of pyromellitic dianhydride and 4,4'-diaminodiphenyl ether. This porous polyimide film has an exothermic peak in the temperature range of 350°C to 450°C when measured by differential thermal / thermogravimetry (TG / DTA) at a heating rate of 5°C / min. In addition, the weight loss rate of the porous polyimide film in the same temperature range is preferably in the range of 0.5% to 3.0%, more preferably in the range of 0.5% to 2.5%.

[0033] The porous polyimide film according to the embodiment of the present invention preferably has a thermal conductivity of 0.2 or less, more preferably 0.17 or less. The lower limit of the thermal conductivity is not particularly limited, but is greater than the thermal conductivity of air. The lower the thermal conductivity, the higher the heat insulating property of the porous polyimide film, which is preferable.

[0034] The porous polyimide film according to the embodiment of the present invention preferably has a dielectric constant (10 GHz) in the range of 1.00 to 2.5, more preferably in the range of 1.4 to 2.0. Also, the dielectric loss tangent (10 GHz) is preferably in the range of 0.0001 to 0.02, more preferably in the range of 0.005 to 0.015. The lower the dielectric properties (dielectric constant, dielectric loss tangent), the higher the communication properties at high frequencies, which is preferable.

[0035] The porous polyimide film according to the embodiment of the present invention preferably has a porosity in the range of 50% or more and less than 80%, more preferably in the range of 50% or more and less than 70%, and even more preferably in the range of 60% or more and less than 70%. When the porosity is within the above range, a good balance between the thermal conductivity, dielectric properties, etc., and the mechanical strength is maintained.

[0036] In the porous polyimide film according to the embodiment of the present invention, it is preferable that the independent pores are formed so that the pore size gradually increases from the surface side in contact with the atmosphere toward the surface side in contact with the substrate, but continuous pores may be present in some parts.

[0037] In particular, the porous polyimide film according to the embodiment of the present invention can be suitably used at least as a base film (base film for forming a metal layer). A porous polyimide film may be laminated in order to improve the rigidity and electrical insulation of the porous polyimide film. The method of laminating the porous polyimide film is not particularly limited, and the porous polyimide film may be directly laminated, or a porous polyimide film and a porous polyimide film may be laminated (attached) via an adhesive layer (adhesive layer).

[0038] The adhesive component constituting the adhesive layer is not particularly limited, and may be, for example, either a thermosetting resin or a thermoplastic resin.

[0039] The metal forming the above-mentioned metal layer (metal foil) is not particularly limited, and examples thereof include copper and its alloys, stainless steel and its alloys, nickel and its alloys, and aluminum and its alloys. Among the above-mentioned metals, copper and its alloys are particularly preferred. Examples of copper alloys include copper alloys containing at least one metal selected from nickel, zinc, iron, chromium, cobalt, molybdenum, tungsten, vanadium, beryllium, titanium, tin, manganese, aluminum, phosphorus, silicon, and the like, and copper. Copper and its alloys can be used preferably in circuit processing. Examples of circuit processing methods for copper and its alloys include rolling, electrolytic plating, and sputtering.

[0040] By laminating the above-mentioned metal layer and the porous polyimide film, a metal foil laminate is obtained. That is, the porous polyimide film according to the embodiment of the present invention can be suitably used as a base film of the metal foil laminate. In addition, a rust-proof layer, a heat-resistant layer (for example, plating treatment of chromium, zinc, etc.), a silane coupling agent layer, etc. may be formed on the surface of the metal foil.

[0041] The thickness of the metal layer is not particularly limited, but is, for example, about 1 to 150 μm (eg, 3 to 50 μm).

[0042] The metal foil laminate is not particularly limited in the form of lamination, as long as it has the porous polyimide film according to the embodiment of the present invention and a metal layer.Depending on the purpose of use of the porous polyimide film according to the embodiment of the present invention (whether it is used as a base film or as a coverlay, etc.), for example, the porous polyimide film according to the embodiment of the present invention and the metal layer may be directly laminated, or the porous polyimide film according to the embodiment of the present invention and the metal foil may be laminated (attached) via an adhesive layer (adhesive layer).

[0043] The adhesive component constituting the adhesive layer is not particularly limited, and may be, for example, either a thermosetting resin or a thermoplastic resin.

[0044] Incidentally, the metal foil-clad laminate can be through-hole processed because the pores in the porous polyimide film are relatively small. By etching the metal layer of the metal foil-clad laminate to form a desired pattern wiring, various miniaturized and highly dense parts can be mounted on the pattern wiring. Of course, the metal foil-clad laminate according to the embodiment of the present invention can be used not only for the above-mentioned applications but also for various other applications. In addition, since the metal foil-clad laminate has excellent dielectric properties due to the presence of the porous polyimide film, it is effective as a part for mobile information communication devices such as multi-function mobile phones and tablet terminals. More specifically, it is expected to be used as a part for 5G terminals that can meet the requirements of ultra-high speed, large capacity, low latency, and multiple simultaneous connections, and to be applied to parts such as high-speed switching power supplies for automobiles, collision prevention millimeter wave radar devices, advanced driving assistance systems, and artificial intelligence.

[0045] The porous polyimide film according to the embodiment of the present invention preferably has an air permeability of more than 1500s. When the air permeability is more than 1500s, it is possible to confirm that closed cells, not open cells, are formed.

[0046] <Preparation of polyamic acid solution> As described above, in the embodiment of the present invention, the polyamic acid may be synthesized by polymerizing an aromatic tetracarboxylic dianhydride and an aromatic diamine in a mixed solvent of an organic polar solvent and a hydrophobic poor solvent, or may be synthesized by polymerizing an aromatic tetracarboxylic dianhydride and an aromatic diamine in an organic polar solvent. In the latter case, the hydrophobic poor solvent is added to the obtained polyamic acid solution.

[0047] Here, as the organic polar solvent and the hydrophobic solvent, those described above are used.

[0048] It is preferable that the aromatic tetracarboxylic dianhydride and the aromatic diamine are polymerized in approximately equimolar amounts. The polymerization temperature is preferably about 100° C. or less, more preferably 80° C. or less, further preferably 0 to 60° C., and particularly preferably 20 to 60° C. The polymerization time is preferably about 0.2 hours or more, more preferably 0.3 to 60 hours.

[0049] The viscosity of the polyamic acid solution may be appropriately adjusted depending on the object of molding of the porous polyimide film, the molding method (coating, casting, etc.), and the purpose of production. From the viewpoint of workability, the polyamic acid solution (polyimide precursor solution) preferably exhibits a rotational viscosity measured at 30°C of about 0.1 to 5000 poise, more preferably 0.5 to 2000 poise, and even more preferably 1 to 2000 poise. Therefore, it is preferable to carry out the above-mentioned polymerization reaction to such an extent that the obtained polyamic acid solution exhibits the above-mentioned viscosity, or to adjust the viscosity by diluting or concentrating the obtained polyamic acid solution.

[0050] <Formation of porous polyimide film from polyamic acid solution> The method for forming a porous polyimide film from a polyamic acid solution is not particularly limited, and a known method can be used. More specifically, a porous polyimide film is produced by casting a polyamic acid solution or a polyamic acid solution composition onto a support, heating it, and forming it to such an extent that it can be peeled off from the support. The heating temperature and heating time during the formation of the porous polyimide film can be appropriately determined. A preferred example of a combination of heating temperature and heating time is a temperature of 100 to 180°C for 1 to 60 minutes.

[0051] The support is not particularly limited as long as the polyamic acid solution can be cast onto it, but it is preferable to use a smooth substrate, such as a drum or belt made of a metal such as stainless steel.

[0052] In this method, the solvent may be removed to such an extent that the film can be peeled off from the support. The imidization may be performed before or after the film is peeled off from the support. In the latter case, the imidization may be performed, for example, by conveying the obtained film while holding both ends in the width direction with a tenter device and heating the film. In such a case, the heating temperature is preferably equal to or higher than the boiling point of the hydrophobic solvent from the viewpoint of promoting the toughening and porosity of the polyimide film and removing as much of the hydrophobic solvent as possible. The heating time can be appropriately determined, but is preferably within the range of 0.5 hours to 5 hours from the viewpoint of promoting the toughening and porosity of the polyimide film and removing as much of the hydrophobic solvent as possible.

[0053] An example of producing a porous polyimide film is shown below. First, a polyamic acid solution is cast on the surface of a suitable support to form a liquid film of the polyamic acid solution with a uniform thickness of about 10 to 2000 μm (more preferably about 20 to 1000 μm). Next, the liquid film of the polyamic acid solution is dried at 80° C. to 150° C. for 10 minutes to 1 hour using a heat source such as hot air or infrared rays, and then the film formed on the support is peeled off from the support and the film is fixed to a tenter or the like, and the film is heated from 150° C. to 300° C. for 30 minutes to 3 hours, and the film is further baked at 300° C. to 400° C. for 20 minutes to 1 hour to form a porous polyimide film. In this case, imidization proceeds during the final baking.

[0054] <Examples and Comparative Examples> The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to these examples. EXAMPLES

[0055] 1. Preparation of Polyamic Acid Solution 7.46 g of 4,4'-diaminodiphenyl ether (ODA) as an aromatic diamine and 7.96 g of pyromellitic dianhydride (PMDA) as an aromatic tetracarboxylic dianhydride were added to 91 g of N-methyl-2-pyrrolidone and stirred to obtain a polyamic acid solution (composition PMDA / ODA, solid content 14.5 parts by mass). Next, 30.4 g of (1,7,7-trimethylbicyclo[2.2.1]hept-2-yl)cyclohexane-1-ol (boiling point 308°C, logP 4.96) was added to the polyamic acid solution as a hydrophobic poor solvent and stirred to obtain the target polyamic acid solution (composition PMDA / ODA, solid content 11.2 parts by mass).

[0056] 2. Formation of porous polyimide film The polyamic acid solution was cast on a glass substrate to form a coating film of the polyamic acid solution, and the glass substrate on which the coating film was formed was placed in an oven at 130°C to dry the coating film for 30 minutes. The glass substrate was then removed from the oven, and the film formed on the glass substrate was peeled off from the glass substrate and fixed to a tenter, and the film was placed in an oven and heated from 150°C to 350°C over 2 hours. After the oven temperature reached 350°C, the temperature was maintained for 20 minutes to bake the film, and the desired porous polyimide film was obtained. The thickness of the porous polyimide film was 105.5 μm.

[0057] 3. Physical property evaluation (1) Measurement of thermal conductivity The thermal conductivity of the porous polyimide film was measured with reference to JIS R2616. Specifically, the porous polyimide film was cut into a 2 cm x 2 cm piece, and a transistor was attached to one side of the film piece via thermal conductive grease, and a heat sink (made of aluminum) was attached to the other side via thermal conductive grease. Next, a current was applied to the transistor to raise its temperature until it reached 60°C, and the porous polyimide film was heated for 3 minutes with the transistor that had reached 60°C. The surface temperature A of the porous polyimide film on the transistor side and the surface temperature B of the porous polyimide film on the heat sink side were measured using a thermocouple. In addition, the power consumption of the transistor was measured, and the thermal resistance was calculated from the following formula using the temperatures A and B of each surface and the power consumption of the transistor.

[0058] Thermal resistance = (Surface temperature A (℃) - Surface temperature B (℃)) / Power consumption (W)

[0059] In addition, when the thermal conductivity was calculated from the thermal resistance calculated by the above formula according to the formula shown below, the thermal conductivity was 0.14 W / mK.

[0060] Thermal conductivity = thickness of porous polyimide film / (cross-sectional area of ​​transistor × thermal resistance)

[0061] (2) Measurement of dielectric constant (10 GHz) The dielectric constant (ε) and dielectric dissipation factor of the porous polyimide film at a frequency of 10 GHz were measured using a vector network analyzer (manufactured by Agilent, product name: Vector Network Analyzer E8363C) and a split post dielectric resonator (SPDR). The dielectric constant was 1.68 and the dielectric dissipation factor was 0.0083.

[0062] (3) Porosity measurement The thickness and mass of the porous polyimide film cut to a predetermined size were measured, and the porosity of the porous polyimide film was calculated from the basis weight using the formula shown below, and the porosity was found to be 53.7%.

[0063] Porosity=(1-w / (S×d) / D)×100 In the above formula, S is the area of ​​the porous polyimide film piece, d is the thickness of the porous polyimide film piece, w is the measured mass of the porous polyimide film piece, and D is the density of the polyimide. The density of polyimide is 1.43 g / cm 3 It was decided.

[0064] (4) Thermogravimetric analysis Using a Shimadzu Corporation DTG-60 differential thermal / thermogravimetry (TG / DTA) simultaneous measurement device, a porous polyimide film was heated in an air atmosphere from room temperature to 500°C at a heating rate of 5°C / min to perform thermogravimetry of the porous polyimide film. A heat generation peak was confirmed at 370°C (see Figure 1), and the weight loss rate from 350°C to 450°C was 0.9%.

[0065] The above-mentioned weight reduction rate is calculated by (weight (g) at 350°C - weight (g) at 450°C) / weight (g) at 350°C x 100.

[0066] (5) Liquid chromatograph (HPLC) mass spectrometry After the porous polyimide film was immersed in methanol, the methanol was analyzed using a Hitachi high-performance liquid chromatograph Chromaster, and (1,7,7-trimethylbicyclo[2.2.1]hept-2-yl)cyclohexan-1-ol was detected. In the above-mentioned high-performance liquid chromatograph Chromaster, a Daicel CHIRALPAK IB (particle size 5 μm, inner diameter 4.6 mm, length 150 mm) was used as the column, THF was used as the mobile phase, and a photodiode array detector was used as the detector. The photodiode array detector detects the ultraviolet-visible spectrum. The flow rate of the mobile phase was 1 mL / min.

[0067] (6) Measurement of air permeability When the air permeability of the porous polyimide film was measured based on JIS P8117 (Gurley test method), it was confirmed that the porous polyimide film exhibited an air permeability higher than 1500s.

[0068] (7) Hole drilling When holes were drilled in the porous polyimide film using a 0.3 mm diameter drill, the holes could be drilled without any problems. Figure 2 shows a photograph of the porous polyimide film that had been drilled using a Hirox KH-1300 digital microscope at a magnification of 50x. EXAMPLES

[0069] A porous polyimide film was obtained in the same manner as in Example 1, except that the amount of (1,7,7-trimethylbicyclo[2,2,1]hept-2-yl)cyclohexane-1-ol added was changed to 36.5 g. The solid content of the polyamic acid solution was 10.1 parts by mass. The thickness of the obtained porous polyimide film was 107.9 μm.

[0070] The physical properties of the obtained porous polyimide film were measured in the same manner as in Example 1, and the thermal conductivity was 0.13 W / mK, the dielectric constant (10 GHz) was 1.58, the dielectric loss tangent (10 GHz) was 0.0075, and the porosity was 66.8%. In addition, as a result of thermogravimetric analysis, a heat generation peak was confirmed at 370°C in this porous polyimide film, and the weight loss rate of the porous polyimide film was 1.0%. In addition, (1,7,7-trimethylbicyclo[2.2.1]hept-2-yl)cyclohexane-1-ol was detected from the porous polyimide film by HPLC mass spectrometry. In addition, it was confirmed that the air permeability of this porous polyimide film was higher than 1500s. In addition, when a hole was drilled in the porous polyimide film using a drill with a diameter of 0.3 mm, the hole drilling could be performed without any problems. EXAMPLES

[0071] A porous polyimide film was obtained in the same manner as in Example 1, except that 30.4 g of (1,7,7-trimethylbicyclo[2.2.1]hept-2-yl)cyclohexan-1-ol was replaced with 30.4 g of 4-(5,5,6-trimethylbicyclo[2.2.1]heptan-2-yl)cyclohexanol (boiling point 324.5°C, logP 4.48). At this time, the solid content of the polyamic acid solution was 11.2 parts by mass. The thickness of the obtained porous polyimide film was 48.7 μm.

[0072] The physical properties of the obtained porous polyimide film were measured in the same manner as in Example 1, and the thermal conductivity was 0.13 W / mK, the dielectric constant (10 GHz) was 1.92, the dielectric loss tangent (10 GHz) was 0.0118, and the porosity was 50.0%. In addition, as a result of thermogravimetric analysis, a heat generation peak was confirmed at 380°C in this porous polyimide film (see FIG. 1), and the weight loss rate of the porous polyimide film was 0.8%. In addition, 4-(5,5,6-trimethylbicyclo[2.2.1]heptan-2-yl)cyclohexanol was detected from the porous polyimide film by HPLC mass spectrometry. In addition, it was confirmed that the air permeability of this porous polyimide film was higher than 1500s. In addition, when a hole was drilled in the porous polyimide film using a drill with a diameter of 0.3 mm, the hole drilling could be performed without any problems. EXAMPLES

[0073] A porous polyimide film was obtained in the same manner as in Example 1, except that 30.4 g of (1,7,7-trimethylbicyclo[2.2.1]hept-2-yl)cyclohexane-1-ol was replaced with 30.4 g of 1,2,3,4,4a,5,6,7-octahydro-2,5,5-trimethyl-2-naphthol (boiling point 280.1°C, logP 4.07). At this time, the solid content of the polyamic acid solution was 11.2 parts by mass. The thickness of the obtained porous polyimide film was 86.1 μm.

[0074] The physical properties of the obtained porous polyimide film were measured in the same manner as in Example 1, and the thermal conductivity was 0.15 W / mK, the dielectric constant (10 GHz) was 1.84, the dielectric loss tangent (10 GHz) was 0.0116, and the porosity was 55.1%. In addition, as a result of thermogravimetric analysis, a heat generation peak was confirmed at 375°C in this porous polyimide film (see FIG. 1), and the weight loss rate of the porous polyimide film was 2.1%. In addition, 1,2,3,4,4a,5,6,7-octahydro-2,5,5-trimethyl-2-naphthol was detected from the porous polyimide film by HPLC mass spectrometry. In addition, it was confirmed that the air permeability of this porous polyimide film was higher than 1500s. In addition, when a hole was drilled in the porous polyimide film using a drill with a diameter of 0.3 mm, the hole drilling could be performed without any problems. EXAMPLES

[0075] 4.22 g of paraphenylenediamine (PPD) as an aromatic diamine and 11.26 g of 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA) as an aromatic tetracarboxylic dianhydride were added to 91 g of N-methyl-2-pyrrolidone and stirred to obtain a polyamic acid solution (composition BPDA / PPD, solid content 14.5 parts by mass). Next, 63.6 g of the polyamic acid solution (composition PMDA / ODA, solid content 14.5 parts by mass) obtained in Example 1, 42.4 g of the above-mentioned polyamic acid solution (composition BPDA / PPD, solid content 14.5 parts by mass), and 30.4 g of (1,7,7-trimethylbicyclo[2.2.1]hept-2-yl)cyclohexane-1-ol (boiling point 308 ° C., log P 4.96) as a hydrophobic poor solvent were mixed and stirred to obtain the target polyamic acid solution (composition PMDA / ODA: BPDA / PPD = 6: 4 (mass ratio), solid content 11.2 parts by mass). Then, a porous polyimide film was obtained in the same manner as in Example 1. The thickness of the porous polyimide film was 118.2 μm.

[0076] The physical properties of the obtained porous polyimide film were measured in the same manner as in Example 1, and the thermal conductivity was 0.17 W / mK, the dielectric constant (10 GHz) was 1.87, the dielectric loss tangent (10 GHz) was 0.0101, and the porosity was 65.6%. In addition, as a result of thermogravimetric analysis, a heat generation peak was confirmed at 370°C in this porous polyimide film, and the weight loss rate of the porous polyimide film was 1.0%. In addition, (1,7,7-trimethylbicyclo[2.2.1]hept-2-yl)cyclohexane-1-ol was detected from the porous polyimide film by HPLC mass spectrometry. In addition, it was confirmed that the air permeability of this porous polyimide film was higher than 1500s. In addition, when a hole was drilled in the porous polyimide film using a drill with a diameter of 0.3 mm, the hole drilling could be performed without any problems. EXAMPLES

[0077] 6.36 g of 4,4'-diaminodiphenyl ether (ODA) as an aromatic diamine and 9.07 g of 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA) as an aromatic tetracarboxylic dianhydride were added to 91 g of N-methyl-2-pyrrolidone and stirred to obtain a polyamic acid solution (composition BPDA / ODA, solid content 14.5 parts by mass). Next, 63.6 g of the polyamic acid solution (composition PMDA / ODA, solid content 14.5 parts by mass) obtained in Example 1, 42.4 g of the above-mentioned polyamic acid solution (composition BPDA / ODA, solid content 14.5 parts by mass), and 30.4 g of (1,7,7-trimethylbicyclo[2.2.1]hept-2-yl)cyclohexane-1-ol (boiling point 308°C, logP 4.96) as a hydrophobic poor solvent were mixed and stirred to obtain the target polyamic acid solution (composition: PMDA / ODA:BPDA / ODA = 6:4 (mass ratio), solid content 11.2 parts by mass). Then, a porous polyimide film was obtained in the same manner as in Example 1. The thickness of the porous polyimide film was 115.3 μm.

[0078] The physical properties of the obtained porous polyimide film were measured in the same manner as in Example 1, and the thermal conductivity was 0.16 W / mK, the dielectric constant (10 GHz) was 1.77, the dielectric loss tangent (10 GHz) was 0.0069, and the porosity was 54.2%. In addition, as a result of thermogravimetric analysis, a heat generation peak was confirmed at 370°C in this porous polyimide film, and the weight loss rate of the porous polyimide film was 1.0%. In addition, (1,7,7-trimethylbicyclo[2.2.1]hept-2-yl)cyclohexane-1-ol was detected from the porous polyimide film by HPLC mass spectrometry. In addition, it was confirmed that the air permeability of this porous polyimide film was higher than 1500s. In addition, when a hole was drilled in the porous polyimide film using a drill with a diameter of 0.3 mm, the hole drilling could be performed without any problems. EXAMPLES

[0079] A porous polyimide film was obtained in the same manner as in Example 2, except that a porous polyimide film having a thickness of 253.7 μm was obtained.

[0080] The physical properties of the obtained porous polyimide film were measured in the same manner as in Example 1, and the thermal conductivity was 0.13 W / mK, the dielectric constant (10 GHz) was 1.59, the dielectric loss tangent (10 GHz) was 0.0070, and the porosity was 63.8%. In addition, as a result of thermogravimetric analysis, a heat generation peak was confirmed at 370°C in this porous polyimide film, and the weight loss rate of the porous polyimide film was 1.0%. In addition, (1,7,7-trimethylbicyclo[2.2.1]hept-2-yl)cyclohexane-1-ol was detected from the porous polyimide film by HPLC mass spectrometry. In addition, it was confirmed that the air permeability of this porous polyimide film was higher than 1500s. In addition, when a hole was drilled in the porous polyimide film using a drill with a diameter of 0.3 mm, the hole drilling could be performed without any problems. EXAMPLES

[0081] A porous polyimide film was obtained in the same manner as in Example 1, except that N-methyl-2-pyrrolidone was replaced with N,N-dimethylacetamide. The solid content of the polyamic acid solution was 11.2 parts by mass. The thickness of the obtained porous polyimide film was 48 μm.

[0082] The physical properties of the obtained porous polyimide film were measured in the same manner as in Example 1, and the thermal conductivity was 0.13 W / mK, the dielectric constant (10 GHz) was 1.70, the dielectric loss tangent (10 GHz) was 0.0078, and the porosity was 58.7%. In addition, as a result of thermogravimetric analysis, a heat generation peak was confirmed at 370°C in this porous polyimide film, and the weight loss rate of the porous polyimide film was 1.0%. In addition, (1,7,7-trimethylbicyclo[2.2.1]hept-2-yl)cyclohexane-1-ol was detected from the porous polyimide film by HPLC mass spectrometry. In addition, it was confirmed that the air permeability of this porous polyimide film was higher than 1500s. In addition, when a hole was drilled in the porous polyimide film using a drill with a diameter of 0.3 mm, the hole drilling could be performed without any problems.

[0083] Comparative Example 1 1. Preparation of Polyamic Acid Solution 7.46 g of 4,4'-diaminodiphenyl ether (ODA) as an aromatic diamine and 7.96 g of pyromellitic dianhydride (PMDA) as an aromatic tetracarboxylic dianhydride were added to 91 g of N-methyl-2-pyrrolidone and stirred to obtain a polyamic acid solution (composition PMDA / ODA, solid content 14.5 parts by mass). Next, 13.1 g of glycerin (boiling point 290°C, logP-1.96) was added to the polyamic acid solution as a poor solvent and stirred to obtain the target polyamic acid solution (composition PMDA / ODA, solid content 12.7 parts by mass).

[0084] 2. Formation of porous polyimide film The polyamic acid solution was cast onto a glass substrate to form a coating film of the polyamic acid solution, and the glass substrate on which the coating film was formed was placed in an oven at 130°C to dry the coating film for 30 minutes. The glass substrate was then removed from the oven, and the film formed on the glass substrate was peeled off from the glass substrate and fixed to a tenter. The film was then placed in an oven and heated from 150°C to 350°C over 2 hours. After the oven temperature reached 350°C, the temperature was maintained for 20 minutes to bake the film, but it was not possible to form it into a film.

[0085] Comparative Example 2 Except for changing glycerin to cyclohexanol (boiling point 161° C., logP 1.35) and adding cyclohexanol to the polyamic acid solution so that the solid content of the polyamic acid solution was 11.5 parts by mass, the target polyamic acid solution and a polyimide film were obtained in the same manner as in Comparative Example 1. The thickness of the obtained porous polyimide film was 39.0 μm.

[0086] The porosity of the resulting polyimide film was measured in the same manner as in Example 1, and was found to be 0%, meaning that the polyimide film was not porous.

[0087] Comparative Example 3 The target polyamic acid solution was obtained in the same manner as in Comparative Example 1, except that glycerin was changed to ethylene glycol (boiling point 198°C, logP -1.53) and ethylene glycol was added to the polyamic acid solution so that the solid content of the polyamic acid solution was 9.8 parts by mass, and an attempt was made to mold a polyimide film from the obtained solution, but it was not possible to mold it into a film.

[0088] Comparative Example 4 The target polyamic acid solution was obtained in the same manner as in Comparative Example 3, except that ethylene glycol was added to the polyamic acid solution so that the solid content of the polyamic acid solution was 11.2 parts by mass, and an attempt was made to mold a polyimide film from the obtained solution, but it was not possible to mold it into a film.

[0089] Comparative Example 5 Except for changing glycerin to tetraglyme (boiling point 275°C, logP-0.12) and adding tetraglyme to the polyamic acid solution so that the solid content of the polyamic acid solution was 11.5 parts by mass, the target polyamic acid solution and a polyimide film were obtained in the same manner as in Comparative Example 1. The thickness of the obtained porous polyimide film was 45.0 µm.

[0090] The porosity of the resulting polyimide film was measured in the same manner as in Example 1, and was found to be 0%, meaning that the polyimide film was not porous.

[0091] Comparative Example 6 A polyamic acid solution (composition BPDA / PPD, solid content 20.9 parts by mass) was obtained in the same manner as in Comparative Example 1, except that glycerin was changed to (1,7,7-trimethylbicyclo[2.2.1]hept-2-yl)cyclohexane-1-ol (boiling point 308°C, logP 4.96), 4,4'-diaminodiphenyl ether (ODA) was replaced with paraphenylenediamine (PPD) and the amount added was changed to 4.24g, and pyromellitic dianhydride (PMDA) was replaced with 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA) and the amount added was changed to 11.20g. In addition, a polyimide film was formed in the same manner as in Comparative Example 1, but it could not be formed into a film.

[0092] Comparative Example 7 Except for changing the amount of 4,4'-diaminodiphenyl ether (ODA) to 6.36 g, and changing pyromellitic dianhydride (PMDA) to 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA) and changing the amount of BPDA to 9.07 g, a polyamic acid solution (composition BPDA / ODA, solid content 11.2 parts by mass) was obtained in the same manner as in Comparative Example 1. Furthermore, a polyimide film was formed using the polyamic acid solution in the same manner as in Comparative Example 1, but it could not be formed into a film.

[0093] Comparative Example 8 7.44 g of 4,4'-diaminodiphenyl ether (ODA) as an aromatic diamine and 7.98 g of pyromellitic dianhydride (PMDA) as an aromatic tetracarboxylic dianhydride were added to 84.7 g of N-methyl-2-pyrrolidone and stirred to obtain a polyamic acid solution (composition PMDA / ODA, solid content 15.3 parts by mass).

[0094] The porosity of the obtained polyimide film was measured in the same manner as in Example 1, and was found to be 0%, meaning that the polyimide film was not porous. In addition, the obtained polyimide film was subjected to thermogravimetric analysis in the same manner as in Example 1, and no exothermic peak was confirmed between 350°C and 450°C (see FIG. 1). In addition, the weight loss rate of the polyimide film was 0.3%. [Industrial Applicability]

[0095] The method for producing a porous polyimide film according to the present invention can provide a porous polyimide film that is inexpensive and has a high porosity of 50% or more even when it is relatively thin. The porous polyimide film can be suitably used as an electrical insulating film or a frequency selective film in a flexible printed circuit (FPC) or the like.

Claims

1. (a) a polyamic acid obtained by polymerizing an aromatic tetracarboxylic dianhydride containing at least pyromellitic dianhydride and an aromatic diamine containing at least 4,4'-diaminodiphenyl ether; (b) an organic polar solvent that is a good solvent for the polyamic acid; (c) a hydrophobic solvent which is a poor solvent for the polyamic acid, dissolves in the organic polar solvent, and has a boiling point at the same pressure minus the boiling point of the organic polar solvent in the range of 15° C. to 260° C. and a log P value in the range of 4.00 to 6.

00. The polyamic acid solution is dried and then baked to obtain a porous polyimide film. A method for producing a porous polyimide film.

2. The hydrophobic solvent has a boiling point at 1 atmosphere in the range of 280° C. or more and 350° C. or less. The method for producing the porous polyimide film according to claim 1 .

3. The polyamic acid solution contains 60% by mass or more of polyamic acid obtained by polymerization reaction of the pyromellitic dianhydride and the 4,4'-diaminodiphenyl ether. The method for producing the porous polyimide film according to claim 1 or 2.

4. The porous polyimide film according to any one of claims 1 to 3, which has a porosity in the range of more than 70% and less than 80%, At least a hydrophobic poor solvent remains, which has a boiling point at 1 atmospheric pressure in the range of 280° C. or more and 350° C. or less and a log P value in the range of 4.00 or more and 6.00 or less. Porous polyimide film.

5. The dielectric constant (10 GHz) is in the range of 1.0 or more and less than 1.

5. The porous polyimide film according to claim 4.

6. The composition contains at least a polyimide resin obtained from a polyamic acid obtained by polymerizing pyromellitic dianhydride and 4,4'-diaminodiphenyl ether, At least a hydrophobic poor solvent remains, the hydrophobic poor solvent having a boiling point at 1 atmospheric pressure in the range of 280° C. or more and 350° C. or less and a log P value in the range of 4.00 or more and 6.00 or less, The porosity is in the range of more than 70% and less than 80%. Porous polyimide film.

7. The dielectric constant (10 GHz) is in the range of 1.0 or more and less than 1.

5. The porous polyimide film according to claim 6.

Citation Information

Patent Citations

  • [hitaishiyouseiporiimidomakutosonoseihou[hitaishiyouseiporiimidomakutosonoseihou]

    JP1974045152A

  • Porous polymer structure and production of said structure by thermally-induced phase separation

    JP1994166116A

  • Low-permittivity insulating plastic film and its production

    JP1997100363A

  • Porous polymer dehumidifying membrane

    JP1999000537A

  • Porous polyimide film and its production method

    JP2001294704A