Water-absorbing composition and method for producing same
By combining cellulose nanofibers with water-soluble polymers and optimizing the composition's properties, the formulation addresses the aggregation issue, resulting in a water-absorbing material with enhanced liquid retention for absorbent applications.
Patent Information
- Application Number
- JP2020149374
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-06
- Filing Date
- 2020-09-04
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-09-04
AI Technical Summary
Cellulose nanofibers in a dry state tend to aggregate easily and have low dispersibility in water, resulting in poor liquid absorption and retention properties, which affects their performance as absorbent materials in articles like diapers.
A water-absorbing composition is formulated by mixing cellulose nanofibers with water-soluble polymers and freeze-drying the mixture, ensuring a specific surface area of 1.0 m²/g or more, with preferred ratios and properties of the cellulose nanofibers and polymers to enhance dispersibility and liquid retention.
The resulting composition exhibits excellent liquid retention properties, capable of absorbing and retaining significant amounts of liquid, making it suitable for use in absorbent articles such as diapers.
Smart Images

Figure 0007568451000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a water-absorbing composition and a method for producing the same. [Background technology]
[0002] As an absorbent material used in absorbent articles such as diapers, cellulose nanofibers are fine fibers obtained from pulp, etc., and are known as a material that puts little strain on the environment during production or disposal. Cellulose nanofibers are highly hydrophilic and have excellent thickening properties, and are expected to be used in a wide range of fields such as food, medical products, and paints. However, cellulose nanofibers in a dry state have high cohesive force and therefore low dispersibility in water. As a technology to solve such problems, Patent Document 1 describes a cellulose porous body that is composed of fine cellulose fibers having a predetermined average fiber diameter and has a predetermined apparent density. Patent Document 2 describes a method for producing a cellulose porous body, which includes a process of freeze-drying a mixture containing cellulose nanofibers with a predetermined solid content concentration and a mixed dispersion medium of water and a water-soluble organic solvent with a predetermined concentration. Patent Document 3 describes a dry solid containing a predetermined amount of water-soluble polymer in anion-modified cellulose nanofibers. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2010-215872 A [Patent Document 2] JP 2013-253137 A [Patent Document 3] International Publication No. 2015 / 107995 Brochure Summary of the Invention [Problem to be solved by the invention]
[0004] Cellulose nanofibers are expected to function as absorbent materials used in absorbent articles such as diapers. However, as described above, cellulose nanofibers in a dry state tend to aggregate and have low dispersibility in water, so that they have low liquid absorption properties and liquid retention properties for retaining liquid after absorption, resulting in insufficient absorption performance. Patent Documents 1 to 3 do not disclose a cellulose nanofiber-containing composition that has sufficient liquid retention properties as the absorbent material.
[0005] Therefore, an object of the present invention is to provide a water-absorbing composition and a method for producing the same that can overcome the above-mentioned drawbacks of the prior art. [Means for solving the problem]
[0006] The present invention relates to a cellulose nanofiber-based fiber sintered body having a specific surface area of 1.0 m2 and a water-soluble polymer. 2 / g or more.
[0007] The present invention also provides a method for producing the water-absorbing composition, which comprises mixing the cellulose nanofibers and the water-soluble polymer in a liquid, and freeze-drying the resulting mixed solution. Effect of the Invention
[0008] The water-absorbing composition of the present invention has excellent liquid retention properties. According to the method for producing a water-absorbing composition of the present invention, a water-absorbing composition having excellent liquid retention properties can be produced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention will be described below based on its preferred embodiments. The water-absorbing composition of the present invention contains cellulose nanofibers and a water-soluble polymer. Hereinafter, the water-absorbing composition of the present invention will be simply referred to as the "water-absorbing composition," and the cellulose nanofiber will be referred to as the "CNF." CNF is a fine cellulose fiber having a fiber diameter of 3 nm to 500 nm and a fiber length of 500 nm to 1000 nm.
[0010] CNF can be produced by known methods such as a method of subjecting raw cellulose fibers to a micronization treatment, a method of synthesizing using bacteria such as acetic acid bacteria, etc. Examples of the micronization treatment include a physical treatment using a defibration device such as a high-pressure homogenizer, and a chemical treatment that loosens cellulose fibers by an oxidation reaction using an enzyme such as cellulase or a catalyst, and these treatments can be used in combination. Examples of the raw cellulose fibers include natural cellulose fibers such as wood pulp, such as coniferous pulp and broadleaf pulp; cotton pulp, such as cotton linter and cotton lint; and non-wood pulp, such as straw pulp and bagasse pulp. These may be used alone or in combination of two or more.
[0011] The CNF may be one in which the hydroxyl groups of cellulose in the cellulose molecular chain are modified. Examples of such CNF include those in which the hydroxyl groups of cellulose are oxidized to carboxyl groups, esterified, etherified, or other functional groups are introduced into the cellulose fibers. From the viewpoint of improving the dispersibility of the CNF, the CNF is preferably an anion-modified CNF in which an anionic group is introduced. Examples of the anionic group contained in the anion-modified CNF include an aldehyde group, a carboxyl group, a sulfate group, and a phosphate group, and from the viewpoint of obtaining finer CNF, the carboxyl group and the phosphate group are preferable.
[0012] Anion-modified CNF can be obtained by known methods such as a method of converting hydroxyl groups of cellulose into anionic groups by oxidation, or a method of reacting at least one selected from the group consisting of a compound having an anionic group, its acid anhydride, or a derivative thereof with the hydroxyl groups of cellulose. For example, there is a method of oxidizing the hydroxyl groups of cellulose by reacting an oxidizing agent such as sodium hypochlorite and a bromide such as sodium bromide with 2,2,6,6-tetramethyl-1-piperidine-N-oxyl (TEMPO) as a catalyst (JP Patent Publication No. 2011-140632).
[0013] A water-soluble polymer is a polymer that can dissolve in water, and has a solubility of 0.5 g or more in 100 g of water at 25°C. The solubility is measured as follows. A predetermined amount of the target is added to 50 mL of ion-exchanged water at 25°C in a 100 mL glass beaker (5 mmΦ), mixed, and a stirrer tip with a length of 20 mm and a width of 7 mm is placed in the beaker, and the mixture is stirred at 600 rpm using a magnetic stirrer HPS-100 manufactured by AS ONE Corporation. Then, it is confirmed whether the total amount of the added target is dissolved in water within 24 hours. This series of operations is performed for multiple samples with different total weights of the target (amount put into the beaker), and the solubility is determined as twice the total weight of the target in the sample with the largest amount of dissolution among the multiple samples in which the total amount of the target is dissolved. The solubility is preferably 1 g or more, more preferably 5 g or more, and even more preferably 10 g or more.
[0014] From the viewpoint of improving the liquid retention of the water-absorbing composition, the water-soluble polymer has a viscosity of a 1% by mass aqueous solution at 25° C. of preferably 5000 mPa·s or more, more preferably 6000 mPa·s or more, even more preferably 7500 mPa·s or more, and also preferably 30000 mPa·s or less, more preferably 20000 mPa·s or less, even more preferably 15000 mPa·s. belowand preferably from 5000 mPa·s to 30000 mPa·s, more preferably from 6000 mPa·s to 20000 mPa·s, and even more preferably from 7500 mPa·s to 15000 mPa·s. The viscosity of a 1 mass % aqueous solution of a water-soluble polymer at 25°C is measured using a B-type viscometer (TVB-10, manufactured by Toki Sangyo Co., Ltd.) under the measurement conditions of rotor No. 4, rotation speed of 30 rpm, and time of 60 seconds.
[0015] Examples of water-soluble polymers include cellulose derivatives, polyvinylpyrrolidone, polyvinyl alcohol, polyvinyl butyral, dextrin, polyethylene oxide, water-soluble nylon, and natural polysaccharides. Examples of natural polysaccharides include sodium alginate, Tragacanth gum , guar gum, xanthan gum, gum arabic, carrageenan, galactomannan, gelatin, casein, albumin, pulpuran, etc. The water-absorbing composition may contain one selected from these components alone or two or more selected from these components in combination. From the viewpoint of increasing the dispersibility of CNF in water, which will be described later, the water-soluble polymer is preferably a cellulose derivative or a salt thereof. The cellulose derivative and its salt are partially modified cellulose, and examples thereof include carboxymethyl cellulose, carboxyethyl cellulose, methyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl cellulose, and salts thereof. As the salt, a water-soluble salt is preferably used, and examples thereof include one or more metal salts selected from alkali metal salts such as sodium salts and potassium salts, and alkaline earth metal salts such as calcium salts and magnesium salts. The water-absorbing composition may use one selected from these components alone or in combination of two or more. From the viewpoint of effectively suppressing the aggregation of CNF, the cellulose derivative is preferably at least one selected from the group consisting of carboxymethyl cellulose, carboxyethyl cellulose, carboxymethyl cellulose salts, and carboxyethyl cellulose salts.
[0016] From the viewpoint of improving the liquid retention of the water-absorbing composition, the cellulose derivative has a degree of etherification of preferably 1.0 or less, more preferably 0.9 or less, even more preferably 0.8 or less, and also preferably 0.4 or more, more preferably 0.5 or more, even more preferably 0.6 or more, and also preferably 0.4 to 1.0, more preferably 0.4 to 0.9, even more preferably 0.6 to 0.8. From the same viewpoint as above, the degree of etherification of the cellulose derivative salt is also preferably within the above range. The degree of etherification is measured by the following measurement method.
[0017] [Method for measuring degree of etherification] The degree of etherification is measured using the ashing measurement method. Approximately 0.7 g of the sample (cellulose derivative or its salt) is precisely weighed, wrapped in filter paper, and placed in a magnetic crucible, and thoroughly ashed at 600°C. After cooling, it is transferred to a 500 mL beaker, and approximately 250 mL of water and 35 mL of 0.05 mol / L sulfuric acid are added, boiled for 30 minutes, and then cooled. Phenolphthalein indicator is added to this, and the excess acid is back-titrated with 0.1 mol / L potassium hydroxide, and the degree of etherification is calculated using the following formula. Degree of etherification = 162 x A / (10000-80 x A) In the formula, A is the number of mL of 0.05 mol / L sulfuric acid consumed by the combined alkali in 1 g of sample.
[0018] The CNF and the water-soluble polymer can be separated from the water-absorbing composition by a filtration process. The filtration process is as follows. A water-absorbing composition consisting of CNF and a water-soluble polymer is diluted with ion-exchanged water so that the concentration of the water-absorbing composition is 0.1% by mass, to prepare a diluted aqueous solution. The diluted aqueous solution is centrifuged at a centrifugal acceleration of 12000×g for 10 minutes using a polytetrafluoroethylene filter with a pore size of 0.5 μm. When centrifugal filtration is performed, the CNF remains on the filter, and the water-soluble polymer passes through the filter. This allows the CNF and the water-soluble polymer to be separated. Various properties such as the viscosity of the water-soluble polymer used in the water-absorbing composition and the degree of etherification of the cellulose derivative can be measured using the water-soluble polymer or cellulose derivative separated from the water-absorbing composition.
[0019] The water-absorbing composition of the present invention has a specific surface area of 1.0 m 2 / g or more, preferably 5.0m 2 / g or more, more preferably 10.0m 2 / g or more, more preferably 15.0m 2 From the viewpoint of manufacturing, the specific surface area is 200 m 2 / g or less is preferable, and 150m 2 / g or less, more preferably 100m 2 / g or less, and more preferably 50m 2 The specific surface area can be determined by obtaining an adsorption isotherm using a nitrogen gas adsorption apparatus (for example, Belsorp II manufactured by Bel Japan Co., Ltd.).
[0020] As a result of extensive research into the liquid retention of CNF, the present inventors have found that a water-absorbing composition containing CNF and a water-soluble polymer, preferably a cellulose derivative, and having the above-mentioned specific surface area has excellent liquid retention properties. Such a water-absorbing composition can be preferably used as an absorbent material for absorbent articles such as diapers.
[0021] From the viewpoint of further improving the liquid retention, when the content of cellulose nanofiber in the water absorbent composition is C1 and the content of the water-soluble polymer in the water absorbent composition is C2, the ratio of C1 to C2, C1:C2, is preferably 1:0.5 to 1:20, more preferably 1:0.8 to 1:15, and even more preferably 1:1 to 1:10. Unless otherwise specified, the content in this specification is based on mass. When the water absorbent composition contains multiple types of water-soluble polymers, C2 is the total content of the multiple types of water-soluble polymers. The C1:C2 ratio can be adjusted to the above range by adjusting the contents of CNF and water-soluble polymer in the mixed solution described below.
[0022] From the viewpoint of further improving the dispersibility of CNF in water, the cellulose derivative preferably has a mass average molecular weight (Mw) of 5,000 to 1,000,000, more preferably 10,000 to 800,000, and even more preferably 100,000 to 600,000.) The mass average molecular weight can be measured using a general gel permeation chromatography (e.g., HLC-8020 manufactured by Tosoh Corporation). The column used in the measurement is appropriately selected in consideration of the expected mass average molecular weight and ionicity.
[0023] From the viewpoint of increasing the water absorption rate and improving the liquid retention, it is preferable that the CNF has the following properties. The average fiber length of the CNF is preferably 500 nm or more, more preferably 5000 nm or more, and also preferably 1000 nm or less, more preferably 3000 nm or less, and also preferably 500 nm or more and 5000 nm or less, more preferably 1000 nm or more and 3000 nm or less. The average fiber diameter of the CNF is preferably 3 nm or more, more preferably 5 nm or more, and is preferably 300 nm or less, more preferably 100 nm or less, and is preferably 3 nm or more and 300 nm or less, more preferably 5 nm or more and 100 nm or less.
[0024] The average fiber length and average fiber diameter are measured, for example, by the following method. Sucking Add water or ethanol to the aqueous composition. Solid concentration 0.0001% by mass A dispersion liquid is prepared, and the dispersion liquid is dropped onto mica and dried to prepare an observation sample. The observation sample is observed using an atomic force microscope (AFM, Nanoscope III Tapping mode AFM, manufactured by Digital Instrument, Inc., and the probe used is Point Probe (NCH) manufactured by Nanosensors, Inc.), and five or more CNFs are selected from the observation sample to measure the average fiber length and average fiber diameter.
[0025] From the viewpoint of improving liquid retention, the average aspect ratio of CNF, i.e., the value of fiber length / fiber diameter, is preferably 50 or more and 2,500 or less, more preferably 75 or more and 2,000 or less, and even more preferably 100 or more and 1,500 or less.
[0026] The water-absorbing composition may contain other components in addition to the CNF and water-soluble polymer. For example, fillers, pigments, dyes, etc. , prevention It may contain preservatives, antioxidants, fragrances, deodorants, antibacterial agents, etc. When other components are contained, the content of the other components in the water-absorbing composition is preferably 10% by mass or less, more preferably 5% by mass or less. When a plurality of types of other components are contained, it is preferable that the total content of these components is within the above range.
[0027] The water-absorbing composition is a solid formed by drying. For example, the water-absorbing composition is used as a particulate, powdery, flaky, fibrous or porous dry solid. The specific surface area of the water-absorbing composition can be controlled by a processing method such as granulation or pulverization. From the viewpoint of increasing the specific surface area, the water-absorbing composition is preferably a particulate, flaky or porous dry solid. From the viewpoint of easy handling as an absorbent material, the water content contained in the water-absorbing composition is preferably 15% by mass or less, more preferably 10% by mass or less.
[0028] When the water-absorbing composition is a flaky dry solid, the thickness of the water-absorbing composition is preferably 0.1 μm to 100 μm, more preferably 1 μm to 50 μm, and even more preferably 3 μm to 10 μm, which is the average thickness of 10 or more arbitrarily selected dry solids.
[0029] When the water-absorbing composition is a powdered dry solid, from the viewpoint of improving the amount of water absorbed, the average particle size of the particles of the water-absorbing composition is preferably 100 μm or more and 500 μm or less, and more preferably 200 μm or more and 400 μm or less. The particle size refers to the maximum length in the form of powder, and is measured, for example, by sieve classification, dynamic light scattering method, laser diffraction method, etc.
[0030] The water-absorbing composition is preferably capable of absorbing and retaining artificial urine at 10 times or more its own weight, more preferably at 15 times or more its own weight, more preferably at 20 times or more its own weight, and even more preferably at 30 times or more its own weight. There is no particular limit to the upper limit of the amount of artificial urine that can be absorbed and retained, but 150 times its own weight can be used as a guideline for the upper limit. The amount of artificial urine that can be absorbed and retained is determined, for example, as the maximum liquid retention amount in [Evaluation of gelation] in the Examples described later. The composition of the artificial urine is described later.
[0031] As described above, the water-absorbing composition of the present invention is preferably used as an absorbent material for absorbent articles such as diapers. Absorbent articles are primarily used to absorb and retain body fluids such as urine and menstrual blood excreted from the body. Absorbent articles include, but are not limited to, disposable diapers, sanitary napkins, incontinence pads, panty liners, and the like, and broadly include articles used to absorb fluids excreted from the human body. Absorbent articles typically include a top sheet, a back sheet, and a liquid-retentive absorbent interposed between the two sheets. The absorbent is the main liquid-absorbing portion of the absorbent article and contains an absorbent material. The absorbent article may further include various members according to its specific use. Such members are known to those skilled in the art.
[0032] Next, the method for producing the water-absorbing composition of the present invention will be described based on its preferred embodiment. In this production method, the above-mentioned CNF and water-soluble polymer are mixed in a liquid consisting of a dispersion medium such as water, and the resulting mixed solution is dried to produce the water-absorbing composition. Hereinafter, in this production method, the process of mixing the CNF and the water-soluble polymer in a liquid to obtain a mixed solution is also referred to as the "mixing process," and the process of drying the mixed liquid is also referred to as the "drying process."
[0033] In this manufacturing method, the CNF and water-soluble polymer that are the raw materials of the water-absorbing composition can be purchased and used as commercially available products. Examples of commercially available CNF products include "LeoCrysta" manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "BiNFi-S" manufactured by Sugino Machine Co., Ltd., and "Cerish" manufactured by Daicel FineChem Co., Ltd. CNF is generally commercially available in a state dispersed in water. Commercially available cellulose derivatives, which are water-soluble polymers, include, for example, "Cellogen" and "BSH-12" manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "CEKOL" manufactured by Sansho Co., Ltd., and "CMC Daicel" manufactured by Daicel FineChem Ltd.
[0034] In this manufacturing method, the above-mentioned CNF and water-soluble polymer are used. The CNF is dispersed in a dispersion medium such as water, i.e., a CNF dispersion is used. In the mixing step, the CNF dispersion and a cellulose derivative are mixed to obtain a mixed solution. At this time, water or an alcohol-based dispersion medium may be added to prepare the mixed solution. Examples of the alcohol-based dispersion medium include monohydric alcohols such as ethanol, 2-propanol, methanol, and butanol, ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, and ester-based solvents such as ethyl acetate and butyl acetate.
[0035] From the viewpoint of easily mixing the CNF and the water-soluble polymer, the content of the CNF in the mixed solution is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, and also preferably 1% by mass or less, more preferably 0.8% by mass or less, and also preferably 0.1% by mass to 1% by mass or less, and more preferably 0.2% by mass to 0.8% by mass or less. From the same viewpoint as above, the content of the water-soluble polymer in the mixed solution is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, and also preferably 1% by mass or less, more preferably 0.8% by mass or less, and also preferably 0.1% by mass to 1% by mass or less, and more preferably 0.2% by mass to 0.8% by mass or less.
[0036] It is preferable that the CNF content and the water-soluble polymer content in the mixed solution are such that the ratio of their contents in the water-absorbing composition (C1:C2) falls within the above-mentioned ranges.
[0037] From the viewpoint of uniformly dispersing the CNF and the cellulose derivative in the mixed solution, it is preferable that the dispersion medium in the mixed solution is mainly water. Specifically, the content of water in the mixed solution is preferably 80% by mass or more, more preferably 90% by mass or more, and also preferably less than 100% by mass, and also preferably 80% by mass or less. End It is less than 100% by mass, and more preferably from 90% to less than 100% by mass.
[0038] In the mixing step, the CNF and the water-soluble polymer are dissolved in a dispersion medium to obtain a mixed solution. In this step, the method for dissolving, i.e. dispersing, the CNF and the water-soluble polymer in the dispersion medium is not particularly limited, and a known dispersion method can be used. Examples of known dispersion methods include dispersion treatments such as shearing treatment, ultrasonic treatment, high-pressure injection treatment, and shaking treatment. In the mixing step, one or more of these treatments can be combined. For the shearing treatment, a shear treatment device such as a stirrer can be used. For the ultrasonic treatment, an ultrasonic treatment device such as an ultrasonic homogenizer can be used. For the high-pressure injection treatment, a high-pressure injection treatment device such as a pressure homogenizer can be used. For the shaking treatment, a shaking treatment device such as a paint shaker can be used. In the mixing step, the dispersion treatment of the CNF and the cellulose derivative may be performed at room temperature (25°C), or the mixing tank may be heated (to about 40°C).
[0039] In the mixing step, the order in which the CNF and the water-soluble polymer are dispersed in the dispersion medium is not particularly limited. That is, the water-soluble polymer may be added to the dispersion liquid in which the CNF is dispersed and then mixed, or the CNF may be added to the dispersion liquid in which the water-soluble polymer is dispersed and then mixed. In addition, the CNF and the water-soluble polymer may be added simultaneously to a mixing tank containing the dispersion medium.
[0040] In the drying step, the mixed solution is dried to obtain a water-absorbing composition. The drying method used in the drying step is not particularly limited as long as it can maintain the quality of the water-absorbing composition, and examples of the drying method include freeze-drying using hot air, a heater, or vacuum, freeze-drying, spray-drying, and the like, and one or more of these methods may be used in combination. The water-absorbing composition is obtained as a dry solid in various forms, such as a sheet or powder, depending on the drying method used in the drying step. When the dry solid is in the form of a flake, it is preferable to cut the dry solid into 1 mm to 3 mm squares in order to improve the handleability as an absorbent material.
[0041] From the viewpoint of easily producing the water-absorbing composition, it is preferable to freeze-dry the mixed solution in the drying step. From the same viewpoint as above, it is preferable to perform freeze-drying under the following conditions. The freezing temperature is preferably -20°C or lower, more preferably -50°C or lower. The lower limit of the freezing temperature is not particularly limited, but from the viewpoint of production, it is preferably -100°C or higher. The pressure in the freeze-drying may be selected according to the freezing temperature.
[0042] The present production method preferably includes a pulverization step in which the water-absorbing composition obtained in the drying step is pulverized. The pulverization step is effective in that the specific surface area is within the above-mentioned range, and is particularly effective when the water-absorbing composition is produced by a method other than freeze-drying. In the pulverization step, the water-absorbing composition is pulverized by dry pulverization. Examples of pulverization devices used in dry pulverization include container-driven media mills such as roller mills, rolling ball mills, vibrating ball mills, vibrating rod mills, vibrating tube mills, planetary ball mills, and centrifugal fluidization mills, media-agitated mills such as tower-type pulverizers, agitation tank-type mills, flow tank-type mills, and annular-type mills, consolidation shear mills such as high-speed centrifugal roller mills and ong mills, mortars, stone mills, mass colloiders, fret mills, edge runner mills, knife mills, pin mills, cutter mills, and hammer mills. The water-absorbing composition obtained through the pulverization step may be sieved to a desired particle size, if necessary.
[0043] In addition, when the water-absorbing composition contains the other components described above, the other components may be contained in the mixed solution in the mixing step, or the other components may be added to the water-absorbing composition obtained in the drying step.
[0044] Although the present invention has been described above, the present invention is not limited to the above-described embodiment, and can be modified as appropriate without departing from the spirit of the present invention.
[0045] In relation to the above-mentioned embodiment, the present invention further discloses the following water-absorbing composition and a method for producing the same. <1> It contains cellulose nanofibers and water-soluble polymers, and has a specific surface area of 1.0 m 2 / g or more. <2> The specific surface area is 5.0 m 2 / g or more, preferably 10.0m 2 / g or more, more preferably 15.0m 2 / g or more and 200m 2 / g or less, preferably 150m 2 / g or less, more preferably 100m 2 / g or less, more preferably 50m 2 / g or less. <1> The water-absorbing composition according to claim 1. <3> The specific surface area is 200 m 2 / g or less, preferably 150m 2 / g or less, more preferably 100m 2 / g or less, more preferably 50m 2 / g or less. <1> or <2> The water-absorbing composition according to claim 1. <4> The specific surface area is 1.0 m 2 / g or more 200m 2 / g or less, preferably 5.0m 2 / g or more 150m 2 / g or less, more preferably 10.0m 2 / g or more 100m 2 / g or less, more preferably 15.0m 2 / g or more 50m 2 / g or less. <1> The water-absorbing composition according to claim 1. <5> The water-soluble polymer has a viscosity of 5000 mPa·s or more in a 1% by mass aqueous solution at 25° C., preferably 5000 mPa·s or more and 30000 mPa·s or less, more preferably 6000 mPa·s or more and 20000 mPa·s or less, and further preferably 7500 mPa·s or more and 15000 mPa·s or less. <1> ~ <4> 13. The water-absorbing composition according to claim 12 . <6> The water-soluble polymer is a cellulose derivative or a salt thereof. <1> ~ <5> 13. The water-absorbing composition according to claim 12 . <7> The cellulose derivative or a salt thereof is at least one selected from the group consisting of carboxymethyl cellulose, carboxyethyl cellulose, methyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl cellulose, and salts thereof. <6> The water-absorbing composition according to claim 1. <8> The etherification degree of the cellulose derivative is 1.0 or less, preferably 0.4 to 1.0, more preferably 0.4 to 0.9, and even more preferably 0.6 to 0.8. <6> or <7> The water-absorbing composition according to claim 1. <9> When the content of the cellulose nanofiber in the water absorbent composition is C1 and the content of the water-soluble polymer in the water absorbent composition is C2, the ratio of C1 to C2, C1:C2, is 1:0.5 to 1:20, preferably 1:0.8 to 1:15, and more preferably 1:1 to 1:10. <1> ~ <8> 13. The water-absorbing composition according to claim 12 . <10> The above <1> ~ <9> A method for producing the water-absorbing composition according to any one of claims 1 to 4, A method for producing a water-absorbing composition, comprising mixing the cellulose nanofibers and the water-soluble polymer in a liquid, and freeze-drying the resulting mixed solution. EXAMPLES
[0046] The present invention will be described in more detail below with reference to examples, but the scope of the present invention is not limited to these examples. It should be noted that Examples 1 and 3 are reference examples.
[0047] Example 1 As the CNF, an aqueous dispersion of CNF with a carboxyl group introduced therein (CNF 2.5% by mass, trade name "Leo Crystal", manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) and sodium carboxymethylcellulose (trade name "Cellogen MP-60", manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) were prepared as the water-soluble polymer. Hereinafter, sodium carboxymethylcellulose is also referred to as CMC-Na. CMC-Na and ion-exchanged water were mixed with the aqueous dispersion of CNF to prepare a mixed solution of CNF and CMC-Na. The content of CNF and the content of cellulose derivative in this mixed solution were each 0.01% by mass. Next, a Teflon (registered trademark) sheet (TOMBO9001, manufactured by Nichias Corporation) was laid on a metal plate measuring 280 mm x 200 mm and a depth of 20 mm, and approximately 50 mL of the mixed solution was poured on top of it, which was dried for approximately 5 hours in an electric drying oven set at 105 ° C., and then left in a room temperature environment for approximately 30 minutes to form a film-like dried product with an average thickness of 4.9 μm on the plate. The obtained film-like dried product was cut into pieces of about 1.0 mm square using scissors to obtain flakes. The flakes were then sieved through a sieve with a mesh size of 4 μm, and the dried product that passed through the sieve was used as the water-absorbing composition of Example 1.
[0048] Example 2 A mixed solution was prepared in the same manner as in Example 1, except that the content of CNF and the content of the cellulose derivative in the mixed solution were each 0.4% by mass. Next, the mixed solution was placed in a metal mold (Sansho Co., Ltd. stainless steel cylindrical tray diameter x depth = 72 mm x 53 mm) and frozen in a freezer at -80 ° C. for 1 hour. Thereafter, freeze-drying was performed for about 48 hours until drying was completed in a freeze dryer. The freezer used was Deep Freezer LAB-11 manufactured by Kanou Refrigeration Co., Ltd., and the freeze dryer used was Freeze Dryer FDU-1200 manufactured by Tokyo Rikakikai Co., Ltd. The dried product obtained after this freeze-drying was used as the water-absorbing composition in Example 2.
[0049] [Examples 3 and 4] In Example 3, a water-absorbing composition was obtained in the same manner as in Example 1, except that sodium carboxymethylcellulose (product name "BSH-12", manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) was used as the water-soluble polymer, and the viscosity of a 1% by mass aqueous solution of the cellulose derivative at 25°C was varied as shown in Table 1. The average thickness of the film-like dried product produced in the process of obtaining the water-absorbing composition was 6.1 μm. In Example 4, a water-absorbing composition was obtained in the same manner as in Example 2, except that the cellulose derivative of Example 3 was used.
[0050] Comparative Examples 1 and 2 In Comparative Example 1, a water-absorbing composition was obtained by the same method as in Example 1, except that the content of CNF and the content of the cellulose derivative in the mixed solution before drying in the electric oven were each 0.6% by mass. As a result, in Comparative Example 1, the average thickness of the film-like dried material obtained by drying in the electric oven was 15.2 μm, which was thicker than the sample in Example 1. As shown in Table 1, the dried material was a water-absorbing composition with a smaller specific surface area than that of Example 1. In Comparative Example 2, a water-absorbing composition was obtained in the same manner as in Comparative Example 1, except that the cellulose derivative of Example 3 was used. The average thickness of the film-like dried product produced in the process of obtaining the water-absorbing composition was 17.8 μm.
[0051] [Reference example] As the water-absorbing composition, a polyacrylic acid sodium salt polymer was used. Such a polymer is used as the water-absorbing polymer in Kao Corporation's 2018 Merries Pants.
[0052] The specific surface area, the viscosity of a 1% by mass aqueous solution of the cellulose derivative at 25°C, and the degree of etherification of the cellulose derivative were measured for each of the water-absorbing compositions of the Examples, Comparative Examples, and Reference Examples by the above-mentioned measuring methods. The results of these measurements are shown in Table 1 below. In addition, the ratio (C1:C2) of the CNF content C1 to the cellulose derivative content C2 based on the content in the mixed solution is shown in Table 1 below.
[0053] [Evaluation of gelation] 0.03 g of the water-absorbing composition was placed in a 20 mL vial (trade name "screw bottle", manufactured by Maruemu Co., Ltd.), and a predetermined amount of artificial urine was further added. The composition of the artificial urine was 1.940 mass% urea, 0.795 mass% sodium chloride, 0.111 mass% magnesium sulfate, 0.062 mass% calcium chloride, 0.198 mass% potassium sulfate, 0.005 mass% Red No. 2 (dye), water (96.882 mass%), and polyoxyethylene lauryl ether (0.007 mass%), and the surface tension was adjusted to 53±1 dyne / cm (23°C). Next, the 20 mL vial was shaken by hand for 5 seconds with the cap vertically up and the bottom vertically down to thoroughly mix the contents of the vial, and the contents were visually checked to see if they had gelled. The vial was then continued to be shaken by hand, and the contents of the vial were visually checked every 10 seconds to see if they had gelled. In this visual check, the vial was placed upside down so that the cap of the vial was vertically down and the bottom was vertically up, and if a portion of the contents of the vial did not fall from the bottom to the cap within 30 seconds, it was judged to have "gelled". For samples in which gelling was confirmed, the time from when the liquid was poured to when it gelled minus the 30 seconds required to confirm that the contents of the vial did not fall was measured as the "gelling time". If gelling did not occur even after 60 minutes had passed since the start of shaking, it was judged not to have gelled. This evaluation and measurement were carried out by sequentially changing the amount of artificial urine to 17 times, 33 times, 50 times, 66 times, and 80 times (2.4 g) the weight of the water-absorbing composition. In addition, when the artificial urine was added and gelation did not occur even after 60 minutes had passed since the start of shaking, the maximum liquid retention of the water-absorbing composition was measured. Specifically, the vial was placed upside down and the amount of the contents of the vial that had fallen, i.e., the amount of dripping liquid, was measured, and the amount of dripping liquid was subtracted from the amount of artificial urine added to the vial before shaking to obtain the maximum liquid retention of the water-absorbing composition. The maximum liquid retention is expressed as a ratio (amount) to the weight of the water-absorbing composition. The presence or absence of gelation, the gelation time, and the maximum liquid retention of each sample are shown in Table 1 below.
[0054] [Table 1]
[0055] As is clear from the results shown in Table 1, the water-absorbing compositions of Examples 1 to 4 were able to gelatinize artificial urine in an amount 33 times or more their own weight. In other words, the water-absorbing compositions of Examples 1 to 4 were able to absorb and retain water in an amount 33 times or more their own weight. This is believed to be due to the high dispersibility and contact efficiency of the CNF in the water-absorbing compositions in water. Therefore, the results shown in Table 1 This indicates that the water-absorbing compositions of Examples 1 to 4 have sufficient absorption performance as absorbent materials used in absorbent articles such as diapers. Furthermore, the results of Examples 1 to 4 indicate that the higher the specific surface area of the water-absorbing composition, the more effective it is in improving the liquid retention of the water-absorbing composition. Furthermore, when the specific surface area of the water-absorbing composition is 14 m 2 / g or more, it resulted in a higher liquid retention than the water-absorbent polymer of the reference example. Furthermore, when the water-absorbent composition of Example 2 was added with 80 times its own weight in water to test for gelation, the contents of the vial, i.e., the mixture of the water-absorbent composition and water, became sol-like, and when the vial was placed upside down, the entire contents fell out. A similar phenomenon was observed for the water-absorbent composition of Example 4 in a test in which 50 times its own weight in water was added. In these samples, water separation from the mixture of the water-absorbent composition and water was not observed, and the above-mentioned dripping could not be measured. The maximum liquid retention amounts of Examples 2 and 4 in Table 1 are the amounts of water at which gelation was confirmed in the test for gelation (66 times its own weight, 100 times its own weight). 50 (double amount) should be indicated.
Claims
1. It contains cellulose nanofibers and water-soluble polymers and has a specific surface area of 14 m 2 / g or more, the water-soluble polymer is a cellulose derivative or a salt thereof, and the etherification degree of the cellulose derivative or the salt thereof is 0.4 or more and 1.0 or less; The water-soluble polymer has a viscosity of 5000 mPa·s or more in a 1% by mass aqueous solution at 25°C, The water-absorbent composition, wherein the content of the cellulose nanofiber in the water-absorbent composition is C1 and the content of the water-soluble polymer in the water-absorbent composition is C2, and the ratio of C1 to C2, C1:C2, is 1:0.5 to 1:
20.
2. The specific surface area is 200 m 2 The water-absorbing composition according to claim 1, wherein the water-absorbing composition has a water-absorbent property of 0.1 to 1.0% by mass.
3. The water-absorbing composition according to claim 1 or 2, wherein the cellulose derivative or its salt is at least one selected from the group consisting of carboxymethyl cellulose, carboxyethyl cellulose, methyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl cellulose, and salts thereof.
4. A method for producing the water-absorbing composition according to any one of claims 1 to 3, A method for producing a water-absorbing composition, comprising mixing the cellulose nanofibers and the water-soluble polymer in a liquid, and freeze-drying the resulting mixed solution.
Citation Information
Patent Citations
Supplementation of Carboxycellulose with a High Degree of Substitution to Essentially Amorphous Cellulose Nanofibrils
JP2000503704A
Cellulose porous body and method for producing the same
JP2010215872A
Porous cellulose body and method for producing the same
JP2013253137A
Water-absorbing composition and production method therefor
JP2020139089A
Dry solid of anion-modified cellulose nanofiber and method for producing same
WO2015107995A1