Manufacturing method of polystyrene resin extruded foam board

A controlled blend of HFO-1224yd and isobutane in extruded polystyrene foam boards addresses solubility and flammability issues, achieving stable thermal conductivity and density for enhanced insulation and safety.

JP7568523B2Active Publication Date: 2024-10-16JSP CORP
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
JP2021007226
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-20
Publication Date
2024-10-16
Estimated Expiration
2041-01-20

AI Technical Summary

Technical Problem

Existing extruded polystyrene foam boards using hydrofluoroolefins like HFO-1234ze and HFO-1233zd face issues with maintaining low thermal conductivity due to solubility and foaming properties, leading to inconsistent density and flammability concerns.

Method used

A manufacturing method involving a specific blend of 1-chloro-2,3,3,3-tetrafluoropropene (HFO-1224yd) and saturated hydrocarbons like isobutane, with controlled ratios to achieve optimal foamability, appearance, and long-term thermal conductivity.

Benefits of technology

The method produces foam boards with stable low thermal conductivity over time, balanced density, and improved flammability resistance, ensuring effective heat insulation and mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568523000001
    Figure 0007568523000001
  • Figure 0007568523000002
    Figure 0007568523000002
Patent Text Reader

Abstract

To provide a method for producing a polystyrene-based resin extruded foam plate capable of reducing the thermal conductivity of a foam plate.SOLUTION: There is provided a method for producing a polystyrene-based resin extruded foam plate which comprises a step of extruding and foaming a foamable resin composition obtained by kneading a base material resin composed mainly of a polystyrene-based resin and a physical foaming agent, followed by molding it into a plate shape by a molding tool, wherein the physical foaming agent contains a foaming agent (a) composed of 1-chloro-2,3,3,3-tetrafluoropropene and a foaming agent (b) composed of a saturated hydrocarbon having 3 to 5 carbon atoms; the total addition amount of the physical foaming agent is 0.8 to 1.5 mol based on 1 kg of the base material resin; the addition amount of the foaming agent (a) is 0.7 to 1.3 mol based on 1 kg of the base material resin; the addition amount of the foaming agent (b) is 0.1 mol or more based on 1 kg of the base material resin; and the ratio of the addition amount of the foaming agent (b) based on 1 kg of the base material resin to the addition amount of the foaming agent (a) based on 1 kg of the base material resin is 0.6 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an extruded polystyrene foam board, and more particularly to a method for producing an extruded polystyrene foam board that can be suitably used as an insulating material for the walls, floors, roofs, etc. of buildings. [Background technology]

[0002] Polystyrene resin extruded foam boards (hereinafter, simply referred to as "extruded foam boards") are widely used as heat insulating materials due to their excellent heat insulating properties and mechanical strength. Such extruded foam boards in the form of a plate are generally produced by heating and melting a polystyrene resin in an extruder, then injecting a physical foaming agent into the resulting molten material, kneading the resulting foamable molten resin mixture, and extruding the mixture into a low pressure region through a flat die or the like attached to the tip of the extruder to foam it, and forming the mixture into a plate shape using a molding tool.

[0003] As the blowing agent used in the production of the extruded foam board, butanes such as normal butane and isobutane are used because they have excellent foaming properties, an ozone depletion potential of 0, a small global warming potential, and excellent heat insulation properties. However, these butanes are highly flammable and remain in the extruded foam board for a long period of time, making it flammable, so there is an upper limit to the amount of butane added.

[0004] In order to solve the above-mentioned problem of flammability, extruded foam boards have been produced by combining butane with a quick-dissipating blowing agent such as water, carbon dioxide, ether, or alcohol, to produce extruded foam boards with low residual butane even at low apparent density. Furthermore, in recent years, hydrofluoroolefins such as 1,3,3,3-tetrafluoropropene and 1-chloro-3,3,3-trifluoropropene have been used in combination with butane and a quick-dissipating blowing agent. These hydrofluoroolefins are soluble in polystyrene resins and have foaming properties, so that extruded foam boards with low apparent density can be produced. In addition, hydrofluoroolefins are non-flammable, have low thermal conductivity in a gaseous state, have excellent heat insulation properties, and remain in the extruded foam board for a long period of time, so that they can provide long-term heat insulation properties.

[0005] Furthermore, hydrofluoroolefins are environmentally friendly blowing agents because they have very low ozone depletion potential and global warming potential. As extruded foam boards produced using the hydrofluoroolefins, for example, foam boards disclosed in Patent Documents 1 to 3 have been proposed. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2013-82805 A [Patent Document 2] JP 2015-229771 A [Patent Document 3] JP 2017-95618 A Summary of the Invention [Problem to be solved by the invention]

[0007] Examples of the hydrofluoroolefin that are easily available include 1,3,3,3-tetrafluoropropene (hereinafter also referred to as HFO-1234ze) and 1-chloro-3,3,3-trifluoropropene (hereinafter also referred to as HFO-1233zd).

[0008] Among these hydrofluoroolefins, HFO-1234ze is more effective at maintaining low thermal conductivity (low thermal conductivity) than HFO-1233zd, but because it has low solubility in polystyrene resins, if a large amount of HFO-1234ze is added, it will dissipate from the polystyrene resin immediately after foaming, making it impossible to obtain an extruded foam board with a low apparent density.

[0009] On the other hand, although HFO-1233zd has superior foaming properties compared to HFO-1234ze, its effect of maintaining the thermal conductivity of the extruded foam plate low for a long period of time is slightly lower than that of HFO-1234ze, and therefore, depending on the blending amount and blending ratio, its contribution to the effect of lowering the thermal conductivity may be insufficient.

[0010] An object of the present invention is to provide a method for producing an extruded polystyrene resin foam board using a foaming agent containing a hydrofluoroolefin, which has excellent foamability, a good appearance, and can maintain low thermal conductivity of the foam board. [Means for solving the problem]

[0011] According to the present invention, there is provided a method for producing an extruded polystyrene resin foam board as described below. [1] A method for producing an extruded polystyrene-based resin foam plate, comprising the steps of extruding and foaming a foamable resin composition obtained by kneading a base resin mainly composed of a polystyrene-based resin with a physical foaming agent, and forming the composition into a plate using a molding tool, wherein the physical foaming agent comprises a foaming agent (a) made of 1-chloro-2,3,3,3-tetrafluoropropene and a foaming agent (b) made of a saturated hydrocarbon having 3 to 5 carbon atoms, the total amount of the physical foaming agents added is 0.8 to 1.5 mol per kg of the base resin, the amount of the foaming agent (a) added is 0.7 to 1.3 mol per kg of the base resin, the amount of the foaming agent (b) added is 0.1 mol or more per kg of the base resin, and the ratio of the amount of the foaming agent (a) added per kg of the base resin to the amount of the foaming agent (b) added per kg of the base resin is 0.6 or less. [2] The method for producing an extruded polystyrene resin foam board according to the above aspect 1, wherein the amount of the foaming agent (b) added is less than 0.4 mol per kg of the base resin. [3] The method for producing an extruded polystyrene foam board according to the above aspect 1 or 2, wherein the amount of the foaming agent (a) added is more than 0.8 mol and not more than 1.3 mol per kg of the base resin. [4] In the method for producing an extruded polystyrene foam board according to any one of the above items 1 to 3, the ratio of the amount of the foaming agent (a) added per kg of the base resin to the amount of the foaming agent (b) added per kg of the base resin is 0.4 or less. Effect of the Invention

[0012] According to the manufacturing method of the present invention, by using a blowing agent in which a hydrofluoroolefin mainly composed of 1-chloro-2,3,3,3-tetrafluoropropene and a saturated hydrocarbon such as butane are added in a specific ratio, a method for manufacturing an extruded polystyrene resin foam board that has excellent foamability, good appearance, and can maintain low thermal conductivity of the foam board even after a long period of time is provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The method for producing an extruded polystyrene foam plate of the present invention will be described in detail below. The manufacturing method of the present invention is a method for manufacturing a polystyrene-based resin extruded foam board (hereinafter, also simply referred to as an extruded foam board) by a method including a step of extruding and foaming a foamable resin composition obtained by kneading a base resin mainly composed of a polystyrene-based resin and a physical foaming agent, and molding the composition into a board shape using a molding tool.

[0014] Specifically, a base resin consisting of a polystyrene resin and other resins added as necessary, a flame retardant, and other additives added as necessary are melted and kneaded under heating in an extruder, a specific foaming agent is injected into the resulting molten mixture and further kneaded to form a foamable resin melt, which is adjusted to a temperature suitable for foaming and extruded from the high-pressure extruder to a low-pressure region through a flat die to foam, and the mixture is passed through a molding die (for example, a molding die (guider) consisting of two upper and lower plates of polytetrafluoroethylene resin or the like arranged in parallel or so as to gradually expand from the entrance to the exit direction) arranged at the exit of the flat die, or a shaping device such as a molding roll, to produce a plate-shaped extruded foam plate.

[0015] <Base resin> (Polystyrene resin) Examples of the polystyrene resin used in the production method of the present invention include polystyrene, styrene-methyl acrylate copolymers containing 50 mol% or more of styrene unit components, styrene-ethyl acrylate copolymers, styrene-methyl methacrylate copolymers, styrene-ethyl methacrylate copolymers, styrene-acrylic acid copolymers, styrene-methacrylic acid copolymers, styrene-maleic anhydride copolymers, styrene-polyphenylene ether copolymers, styrene-acrylonitrile copolymers, styrene-methylstyrene copolymers, styrene-dimethylstyrene copolymers, styrene-ethylstyrene copolymers, and styrene-diethylstyrene copolymers. Among these, polystyrene can be preferably used. In addition to the styrene unit components, polystyrene may contain unit components derived from a branching agent such as a polyfunctional monomer or a polyfunctional macromonomer. The content of the styrene component units in the above copolymer is preferably 60 mol% or more, more preferably 80 mol% or more, and even more preferably 90 mol% or more.

[0016] In addition, the base resin preferably contains an amorphous polyethylene terephthalate copolymer to improve the heat insulation of the extruded foam board. In this case, the amorphous polyethylene terephthalate resin is preferably blended in the base resin so as to be 5% by mass or more and less than 50% by mass, more preferably 10% by mass or more and 40% by mass or less, and even more preferably 15% by mass or more and 30% by mass or less. In addition, the amorphous polyethylene terephthalate copolymer has a heat of fusion associated with melting of the resin based on JIS K7122 of less than 5 J / g. The heat of fusion is measured based on a DSC curve obtained using a heat flux differential scanning calorimeter, employing "when measuring heat of fusion after performing a certain heat treatment" (the heating rate and cooling rate in the condition adjustment of the test piece are both 10°C / min) described in JIS K7122 (1987).

[0017] In addition, the melt viscosity of the polystyrene resin used in the manufacturing method of the present invention is 200°C, a shear rate of 100 sec.-1 Under these conditions, the viscosity is preferably 500 to 3000 Pa·s, more preferably 1000 to 2500 Pa·s, and further preferably 1500 to 2300 Pa·s.

[0018] (Other polymers) The base resin may contain polymers other than the polystyrene resin and the amorphous polyethylene terephthalate copolymer within the scope of the present invention. Examples of other polymers include polyethylene resins (a mixture of one or more selected from the group consisting of ethylene homopolymers and ethylene copolymers having an ethylene unit content of 50 mol% or more), polypropylene resins (a mixture of one or more selected from the group consisting of propylene homopolymers and propylene copolymers having an ethylene unit content of 50 mol% or more), polyphenylene ether resins, and polymethyl methacrylate, as well as thermoplastic elastomers such as styrene-butadiene-styrene block copolymers, styrene-isoprene-styrene block copolymers, hydrogenated styrene-butadiene-styrene block copolymers, hydrogenated styrene-isoprene-styrene block copolymers, and styrene-ethylene copolymers. These other polymers may be blended according to the purpose so as to be less than 50% by mass in the base resin, preferably 30% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less.

[0019] In the manufacturing method of the present invention, a base resin mainly composed of a polystyrene-based resin means that 50% by mass or more of the base resin is a polystyrene-based resin, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more.

[0020] <Physical foaming agent> The physical blowing agent used in the present invention contains at least a blowing agent (a) made of 1-chloro-2,3,3,3-tetrafluoropropene (HFO-1224yd) and a blowing agent (b) made of a saturated hydrocarbon having 3 to 5 carbon atoms as essential components.

[0021] Among hydrofluoroolefins, HFO-1224yd (1-chloro-2,3,3,3-tetrafluoropropene) as the blowing agent (a) has moderate solubility in polystyrene resins and excellent foaming properties, which makes it easier to produce extruded foam boards with low apparent density. In addition, since HFO-1224yd is non-flammable, it can reduce the risk of ignition due to static electricity during the production of extruded foam boards. Furthermore, HFO-1224yd has a low ozone depletion potential and a very small global warming potential, making it a blowing agent with a small burden on the environment. However, compared to HFO-1234ze, HFO-1224yd is more likely to escape from the extruded foam board, and the thermal conductivity of the extruded foam board cannot be maintained low for a long period of time. In particular, the more HFO-1224yd is added, the more likely it is to escape from the extruded foam board. In the present invention, by adding HFO-1224yd and saturated hydrocarbons having 3 to 5 carbon atoms in a specific ratio, it is possible to suppress the loss of HFO-1224yd from the extruded foam plate and maintain low thermal conductivity of the extruded foam plate even after a long period of time, compared to when no saturated hydrocarbons having 3 to 5 carbon atoms are added.

[0022] Examples of the saturated hydrocarbon having 3 to 5 carbon atoms as the blowing agent (b) include propane, normal butane, isobutane (2-methylpropane), normal pentane, isopentane (2-methylbutane), cyclobutane, neopentane (2,2-dimethylpropane), and cyclopentane. Two or more of these can also be used in combination. Among these, isobutane is preferably used.

[0023] (Other foaming agents) As the physical blowing agent used in the present invention, in addition to the above-mentioned essential blowing agent (a) and blowing agent (b), one or more other blowing agents selected from water, carbon dioxide, alkyl chloride, aliphatic alcohols having 1 to 5 carbon atoms, dialkyl ethers having an alkyl chain of 1 to 3 carbon atoms, and hydrofluoroolefins having 3 or 4 carbon atoms other than the above-mentioned HFO-1224yd can be used.

[0024] By using the other foaming agents together with foaming agent (a) and foaming agent (b), it becomes easier to obtain an extruded foam board having a high expansion ratio, a low apparent density, and a good appearance.

[0025] Water and carbon dioxide can reduce the environmental load and dissipate quickly from the extruded foam board, allowing the dimensions of the resulting extruded foam board to be stabilized quickly.

[0026] Examples of alkyl chlorides include methyl chloride and ethyl chloride. Alkyl chlorides are easy to foam polystyrene resins, and by using them together with the above-mentioned foaming agent (a) and foaming agent (b), an extruded foam board with a desired apparent density can be obtained. Furthermore, alkyl chlorides have a high permeation rate into polystyrene resins and dissipate quickly after the production of the extruded foam board, so that the dimensions of the extruded foam board obtained can be stabilized quickly.

[0027] The aliphatic alcohol having 1 to 5 carbon atoms does not destroy the ozone layer, does not warm the earth, and is quickly dispersed from the extruded foam board, so that the shape of the extruded foam board can be quickly stabilized. The aliphatic alcohol, when used together with the blowing agent (a) and the blowing agent (b), can contribute to obtaining an extruded foam board with a low apparent density (high expansion ratio).

[0028] Examples of aliphatic alcohols having 1 to 5 carbon atoms include methyl alcohol (methanol), ethyl alcohol (ethanol), n-propyl alcohol, isopropyl alcohol, butyl alcohol, sec-butyl alcohol, tert-butyl alcohol, aryl alcohol, crotyl alcohol, propargyl alcohol, n-amyl alcohol, sec-amyl alcohol, isoamyl alcohol, tert-amyl alcohol, neopentyl alcohol, 3-pentanol, 2-methyl-1-butanol, 3-methyl-2-butanol, etc. Among these, ethanol can be preferably used from the viewpoint of safety to the environment and the human body.

[0029] In addition, in the present invention, in addition to the above-mentioned essential blowing agent (a) HFO-1224yd, trans-1,3,3,3-tetrafluoropropene (transHFO-1234ze), cis-1,3,3,3-tetrafluoropropene (cisHFO-1234ze), 2,3,3,3-tetrafluoropropene (HFO-1234yf), 1,1,1,4,4,4-hexafluoro-2-butene (HFO-1336mzz), etc. can be used as hydrofluoroolefins having 3 or 4 carbon atoms. Note that these hydrofluoroolefins also include hydrochlorofluoroolefins in which chlorine has been introduced. These blowing agents can be used alone or in combination of two or more kinds.

[0030] <Amount of foaming agent added> In the present invention, the total amount of the physical foaming agent is 0.8 to 1.5 mol per kg of the base resin. If the amount of the physical foaming agent is too small, the apparent density of the resulting extruded foam board is high, and it may not be possible to obtain an extruded foam board with a desired low apparent density. If the amount is too large, the apparent density may be too small, the strength of the resulting extruded foam board may be reduced, and the board may not be usable as a heat insulating material for building materials, or many gas spots may occur, resulting in a poor appearance of the resulting extruded foam board. For these reasons, the total amount of the physical foaming agent is preferably more than 0.9 mol, more preferably 1 mol or more. The upper limit is preferably 1.4 mol, more preferably 1.35 mol.

[0031] The amount of the foaming agent (a) is 0.7 to 1.3 mol per kg of base resin. If the amount of the foaming agent (a) is too small, the apparent density of the resulting extruded foam board may be too high, making it difficult to obtain an extruded foam board with the desired low apparent density. From this viewpoint, the amount of the foaming agent (a) is preferably more than 0.8 mol per kg of base resin, and more preferably 0.9 mol or more per kg of base resin. If it is difficult to produce the extruded foam board under conditions where a large amount of the foaming agent (a) is added, it is possible to easily produce the extruded foam board by using a screw having a large ratio of the axial length of the screw to the diameter of the screw, or a high-mixing screw such as a twin screw, as necessary. If the amount of the foaming agent (a) is too large, many gas spots may occur, and the appearance of the resulting extruded foam board may be deteriorated. From this viewpoint, the amount of the foaming agent (a) is preferably 1.2 mol or less per kg of base resin, and more preferably 1.1 mol or less per kg of base resin.

[0032] The amount of foaming agent (b) added is 0.1 mol or more per kg of base resin. If the amount of foaming agent (b) added is too small, the thermal conductivity of the foamed board may not be maintained low even after a long period of time. From this viewpoint, the amount of foaming agent (b) added is preferably 0.15 mol or more per kg of base resin, and more preferably 0.2 mol or more per kg of base resin. On the other hand, from the viewpoint of maintaining the appearance and high flame retardancy of the foamed board, the amount of foaming agent (b) added is preferably less than 0.4 mol per kg of base resin, more preferably 0.35 mol or less per kg of base resin, and even more preferably 0.3 mol or less per kg of base resin.

[0033] In the present invention, the ratio of the amount of foaming agent (b) added to 1 kg of base resin to the amount of foaming agent (a) added to 1 kg of base resin is 0.6 or less. When the ratio of the amount of foaming agent (b) added to the amount of foaming agent (a) added is within the above range, a foamed board with a low apparent density can be obtained and the thermal conductivity after a long period of time can be maintained low. From this viewpoint, the ratio of the amount of foaming agent (b) added to 1 kg of base resin to the amount of foaming agent (a) added to 1 kg of base resin is preferably 0.5 or less, more preferably 0.4 or less, and even more preferably 0.3 or less. On the other hand, the lower limit of the ratio is about 0.1.

[0034] According to the manufacturing method of the present invention, by using a foaming agent containing a hydrofluoroolefin mainly composed of 1-chloro-2,3,3,3-tetrafluoropropene and a saturated hydrocarbon such as butane in a specific ratio, the thermal conductivity of the foamed board after a long period of time can be reduced. The reason for this is unclear, but it is thought that the thermal conductivity of the gas phase calculated from the molar fraction of the foaming agent present in the bubbles of the foamed board after a long period of time is calculated to be lower when a saturated hydrocarbon is added in a specific ratio.

[0035] When one or more blowing agents selected from water, carbon dioxide, alkyl chloride, aliphatic alcohols having 1 to 5 carbon atoms, dialkyl ethers having 1 to 3 carbon atoms in the alkyl chain, and hydrofluoroolefins having 3 or 4 carbon atoms other than HFO-1224yd are added as blowing agents other than blowing agent (a) and blowing agent (b), the amount of each is preferably 0.3 mol or less, more preferably 0.2 mol or less, and even more preferably 0.1 mol or less per kg of the base resin.

[0036] <Other ingredients> (Flame retardant) The extruded foam board obtained by the production method of the present invention is used mainly as a heat insulating material for building materials, and flame retardancy is imparted to the foam board by blending a flame retardant with the base resin. The flame retardant used in the present invention is not particularly limited, but a bromine-based flame retardant is preferred. Examples of the bromine-based flame retardant include brominated butadiene-based polymers such as brominated butadiene-styrene copolymers, tetrabromobisphenol-A-bis(2,3-dibromo-2-methylpropyl ether), tetrabromobisphenol-S-bis(2,3-dibromo-2-methylpropyl ether), tetrabromobisphenol-F-bis(2,3-dibromo-2-methylpropyl ether), tetrabromobisphenol-A-bis(2,3-dibromopropyl ether), tetrabromo Examples of the brominated bisphenol compounds include bisphenol-S-bis(2,3-dibromopropyl ether) and tetrabromobisphenol-F-bis(2,3-dibromopropyl ether), and brominated isocyanurates include tris(2,3-dibromopropyl)isocyanurate, mono(2,3,4-tribromobutyl)isocyanurate, di(2,3,4-tribromobutyl)isocyanurate, and tris(2,3,4-tribromobutyl)isocyanurate. These brominated flame retardants can be used alone or in combination of two or more.

[0037] In addition to these bromine-based flame retardants, nitrogen-containing cyclic compounds such as cresyl di-2,6-xylenyl phosphate, antimony trioxide, diantimony pentoxide, ammonium sulfate, zinc stannate, cyanuric acid, pentabromotoluene, isocyanuric acid, triallyl isocyanurate, melamine cyanurate, melamine, melam, and melem; silicone-based compounds; inorganic compounds such as boron oxide, zinc borate, and zinc sulfide; and phosphorus-based compounds such as phosphate esters represented by triphenyl phosphate, red phosphorus, ammonium polyphosphate, phosphazene, and hypophosphites.

[0038] Among these flame retardants, it is preferable to use a flame retardant containing one or more of brominated butadiene-styrene copolymer, tetrabromobisphenol A-bis(2,3-dibromopropyl ether), tetrabromobisphenol A-bis(2,3-dibromo-2-methylpropyl ether), and tris(2,3-dibromopropyl)isocyanurate, because it can impart high flame retardancy to the extruded foam board. Among these, it is more preferable to use a flame retardant containing a brominated butadiene-styrene copolymer, or a flame retardant containing a combination of tetrabromobisphenol A-bis(2,3-dibromopropyl ether) and tetrabromobisphenol A-bis(2,3-dibromo-2-methylpropyl ether), because it can impart high flame retardancy, is less likely to decompose the polystyrene resin during extrusion, and makes it easy to stably obtain an extruded foam board even in the case of a low apparent density (high expansion ratio) and a large cross-sectional area.

[0039] The amount of the flame retardant is about 0.1 to 10 parts by mass, more preferably 1 to 8 parts by mass, and even more preferably 3 to 7 parts by mass, relative to 100 parts by mass of the polystyrene resin, since the amount can impart high flame retardancy to the extruded foam board and can suppress deterioration of extrusion foamability and mechanical properties. If it is within this range, the flame retardant does not inhibit foamability, and an extruded foam board having high flame retardancy such as the flammability standard for extruded polystyrene foam insulation boards described in "Test Method A" specified in the flammability test method of JIS A9521:2017 can be obtained.

[0040] (Flame retardant assistant) In the method of the present invention, a flame retardant auxiliary can be used in combination with the flame retardant to further improve the flame retardancy of the extruded foam board. Examples of the flame retardant auxiliary include one or more selected from diphenylalkanes and diphenylalkenes such as 2,3-dimethyl-2,3-diphenylbutane, 2,3-diethyl-2,3-diphenylbutane, 3,4-dimethyl-3,4-diphenylhexane, 3,4-diethyl-3,4-diphenylhexane, 2,4-diphenyl-4-methyl-1-pentene, and 2,4-diphenyl-4-ethyl-1-pentene, and polyalkylated aromatic compounds such as poly-1,4-diisopropylbenzene. The amount of the flame retardant auxiliary is generally 0.01 to 1 part by mass, more preferably 0.05 to 0.5 parts by mass, based on 100 parts by mass of the polystyrene resin.

[0041] (Radiation suppressant) In the manufacturing method of the present invention, graphite can be blended as a radiation suppressant in the foamable resin composition in order to improve the heat insulating property of the extruded foam board by reflecting infrared rays.

[0042] Examples of graphite include flake graphite, scaly graphite, artificial graphite, and earthy graphite, and it is preferable to use graphite whose main component is flake graphite. As described later, it is preferable to use graphite as a master batch in which the graphite is mixed at a high concentration with a polystyrene resin. Graphite having a fixed carbon content of 90% or more is preferable because it has good workability when producing a master batch and has an excellent effect of improving the heat insulation of the resulting extruded foam board. In order to further improve the heat insulation of the extruded foam board, graphite having a fixed carbon content of 93% or more is more preferable, and graphite having a fixed carbon content of 95% or more is even more preferable. The fixed carbon content of the graphite refers to a value measured by the method described in JIS M8511 (1976).

[0043] The amount of graphite is preferably 0.2 to 10 parts by mass per 100 parts by mass of the base resin. When the amount is within this range, the heat insulation is improved, and an extruded foam plate with the desired low thermal conductivity can be obtained. From this viewpoint, the amount of graphite is more preferably 0.3 to 5 parts by mass, and even more preferably 0.4 to 3 parts by mass, per 100 parts by mass of the base resin of the extruded foam plate.

[0044] In the manufacturing method of the present invention, the extruded foam board may contain a radiation suppressant other than the graphite in order to further improve the heat insulating properties. Examples of radiation suppressants other than graphite include one or more selected from metal oxides such as titanium oxide, metals such as aluminum, ceramics, carbon black, graphite, infrared shielding pigments, hydrotalcite, etc. The amount of the radiation suppressant other than graphite to be added is generally 0.5 to 5 parts by mass, and more preferably 1 to 4 parts by mass, based on 100 parts by mass of the base resin.

[0045] In the method of the present invention, other known additives may be appropriately blended with the base resin as necessary, such as, for example, a cell regulator, a colorant such as a pigment or a dye, a heat stabilizer, a filler, and the like.

[0046] (Foam regulator) In the production method of the present invention, it is preferable to form the foamable resin composition by blending a cell control agent with the base resin. As the bubble regulator, inorganic powders such as talc, kaolin, mica, silica, calcium carbonate, barium sulfate, titanium oxide, clay, aluminum oxide, bentonite, and diatomaceous earth can be used. Among them, talc is preferred because it is easy to adjust the bubble diameter and to reduce the bubble diameter without impairing flame retardancy, and fine talc with a 50% particle size (light transmission centrifugal sedimentation method) of 0.1 to 20 μm is particularly preferred, and fine talc with a 50% particle size (light transmission centrifugal sedimentation method) of 0.5 to 15 μm is particularly preferred. The amount of the bubble regulator to be added varies depending on the type of regulator, the target bubble diameter, etc., but when talc is used as the bubble regulator, it is preferably 0.1 to 7 parts by weight, more preferably 0.2 to 5 parts by weight, and even more preferably 0.3 to 3 parts by weight per 100 parts by weight of the polystyrene resin.

[0047] (Heat stabilizer) The thermal stabilizer can improve the thermal stability of the bromine-based flame retardant by blending it with raw materials or scraps when producing an extruded foam board or when recycling scraps of an extruded foam board to make pellets. Examples of the thermal stabilizer include one or more thermal stabilizers selected from bisphenol-type epoxy compounds and novolac-type epoxy compounds such as EPICLON series manufactured by DIC, hindered phenol compounds such as pentaerythritol tetrakis [3- (3,5-di-tert-butyl-4-hydroxyphenyl) propionate], and phosphite compounds such as bis (2,6-di-t-butyl-4-methylphenyl) pentaerythritol diphosphite. The blending amount of the thermal stabilizer is preferably 0.1 to 40 parts by mass with respect to 100 parts by mass of the total amount of the flame retardant.

[0048] In the manufacturing method of the present invention, as a method of blending the flame retardant and other additives into the base resin, a method of feeding a predetermined ratio of the flame retardant and other additives together with the base resin to a feed section provided upstream of the extruder and kneading them in the extruder can be adopted. In addition, a method of feeding the flame retardant and other additives into the molten polystyrene resin from a feed section provided in the middle of the extruder can also be adopted. Specifically, a method of feeding a dry blend of the flame retardant, other additives, and base resin to the extruder and melt-kneading it, a method of feeding a melt-kneaded product obtained by kneading the flame retardant, other additives, and base resin with a kneader or the like to the extruder, a method of preparing a master batch in which a high concentration of the flame retardant and other additives is blended in advance with a polystyrene resin, feeding the master batch to the extruder and melt-kneading it with the base resin, etc. can be adopted. In particular, from the viewpoint of dispersibility, it is preferable to adopt a method of preparing a flame retardant master batch and feeding it to the extruder. The flame retardant masterbatch is prepared by using a polystyrene resin having an MFR of about 0.5 to 30 g / 10 min as the base resin, and adjusting the masterbatch so that the flame retardant content is 10 to 95 mass %, more preferably 30 to 90 mass %, and even more preferably 50 to 85 mass %.

[0049] In the method of the present invention, the molten foamable resin composition containing the base resin, additives such as a flame retardant, and a physical foaming agent as described above is extruded and foamed under atmospheric pressure, and then shaped into a plate using a molding tool, thereby obtaining an extruded polystyrene resin foam plate.

[0050] <Physical properties of foam board> Next, the extruded polystyrene resin foam board obtained by the production method of the present invention will be described. (Cross-sectional area, dimensions, etc.) The extruded foam board of the present invention is in the form of a plate. The extruded foam board has a cross-sectional area perpendicular to the extrusion direction of 100 cm2. 2 More preferably, 200 cm 2 More preferably, the upper limit of the cross-sectional area is approximately 1500 cm 2 It is. In this specification, the cross-sectional area perpendicular to the extrusion direction refers to the area of ​​a cross section of the extruded foam plate perpendicular to the extrusion direction.

[0051] The extruded foam board of the present invention is usually produced by preparing an original board having a size at least one size larger than the desired size, and then cutting the original board to adjust the width, length, and in some cases the thickness.

[0052] However, if the width of the base plate changes significantly during production and becomes narrower than the specified width, it becomes impossible to obtain an extruded foam board of the specified size, resulting in poor yield. In addition, as described above, in the production of extruded foam boards, the smaller the apparent density and the larger the cross-sectional area, the more difficult it tends to be to expand. According to the production method of the present invention, even when producing an extruded foam board with a large thickness and cross-sectional area, an extruded foam board with good appearance can be stably produced.

[0053] When the extruded foam board is used as a heat insulating material, its thickness is preferably from 10 to 150 mm, more preferably from 15 to 120 mm.

[0054] The width of the extruded foam board is preferably 800 mm or more, more preferably 900 mm or more, with the upper limit being approximately 1200 mm.

[0055] (Apparent density) The apparent density of the extruded foam board is 20 to 45 kg / m 3 and preferably 30 to 45 kg / m 3 When the apparent density is within the above range, the material has sufficient mechanical strength and is lightweight, and can be suitably used, for example, as a heat insulating material.

[0056] (Closed bubble rate) The closed cell ratio of the extruded foam board is preferably 85% or more, more preferably 90% or more, and even more preferably 93% or more. If the closed cell ratio is within this range, the foaming agent (a) and the foaming agent (b) tend to remain in the bubbles, and the high heat insulating performance of the extruded foam board can be maintained for a long period of time. In addition, the extruded foam board can have excellent mechanical strength such as compressive strength.

[0057] (Thermal Conductivity) (after 7 days) In the extruded foam board of the present invention, the thermal conductivity 7 days after production is preferably 0.025 W / m·K or less, more preferably 0.023 W / m·K or less, and even more preferably 0.021 W / m·K or less. (100 days later) Furthermore, the thermal conductivity 100 days after production is preferably 0.027 W / m·K or less, more preferably 0.026 W / m·K or less, and even more preferably 0.025 W / m·K or less. (After 300 days) Furthermore, the thermal conductivity 300 days after production is preferably 0.030 W / m·K or less, more preferably 0.028 W / m·K or less, and even more preferably 0.026 W / m·K or less.

[0058] The thermal conductivity can be measured based on the heat flow meter method (one test piece, symmetrical configuration, high temperature side 38°C, low temperature side 8°C, average temperature 23°C) described in JIS A1412-2:1999. A specific measurement method will be described in the Examples.

[0059] Long-term thermal conductivity is measured on samples that have undergone accelerated testing as described in Test Method A of Accelerated Tests of Long-term Changes in Thermal Resistance in accordance with JIS A1486 (2014). According to this method, for example, the thermal conductivity of a sample obtained by slicing a 25 mm-thick extruded foam board to a thickness of 10 mm measured 16 days after production corresponds to the thermal conductivity of the extruded foam board approximately 100 days after production, and the thermal conductivity measured 80 days after production corresponds to the thermal conductivity of the extruded foam board approximately 300 days after production.

[0060] (Residual amount of foaming agent) As described above, the extruded foam board of the present invention is extruded and foamed using blowing agent (a) and blowing agent (b), so that a specific amount of 1-chloro-2,3,3,3-tetrafluoropropene remains in the extruded foam board. The remaining amount of blowing agent (a) in the extruded foam board of the present invention is a value measured by an internal standard method using a gas chromatograph. Specifically, a sample of the extruded foam board is placed in a lidded sample bottle containing an appropriate amount of toluene and an internal standard substance, and the bottle is closed with a lid. The sample is thoroughly stirred, and the blowing agent (a) in the extruded foam board is dissolved in toluene. The solution is used as a measurement sample and gas chromatographic analysis is performed to determine the remaining amount of blowing agent (a) in the extruded foam board.

[0061] In the extruded foam board of the present invention, the remaining amount of the foaming agent (a) is preferably 0.6 mol or more per kg of the extruded foam board 7 days after production, and 0.5 mol or more per kg of the extruded foam board 100 days after production. If the remaining amount is within this range, the foaming agents (a) and (b) will exhibit an effect of improving the heat insulation, resulting in an extruded foam board with excellent heat insulation. In the extruded foam board of the present invention, the ratio (%) of the amount of foaming agent (a) remaining 100 days after production to the amount of foaming agent (a) remaining 7 days after production is preferably 70% or more.

[0062] (Compressive strength) The extruded foam board according to the present invention has excellent compressive strength 7 days after production. In particular, when the base resin contains a non-crystalline polyethylene terephthalate copolymer together with a polystyrene resin, the foam board has an improved compressive strength if the foam board satisfies the foaming agent composition according to the present invention. The compressive strength of the extruded foam board is measured as follows. According to JIS K7181 (2011), it can be measured by the following method using, for example, a Tensilon universal material testing machine manufactured by A&D Co., Ltd. The test piece obtained by cutting out the center of the extruded foam, excluding the skin layer, is compressed by 10% at a speed of 10 mm / min to obtain a stress-strain curve. The stress at 10% compression is read from the obtained stress-strain curve and divided by the compressed area of ​​the test piece to obtain the 10% compression strength. However, if the stress-strain curve shows a yield point before reaching the target strain amount, and the yield point stress is greater than the stress corresponding to the target strain amount, the compressive strength of the target strain amount is calculated based on the yield point stress. The compressive strength in the present invention is determined by carrying out the above measurements in three directions, namely the extrusion direction, width direction, and thickness direction of the extruded foam plate, and adopting the arithmetic average value. EXAMPLES

[0063] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples in any way.

[0064] In the examples and comparative examples, the following devices and raw materials were used.

[0065] The extrusion device used was a first extruder with an inner diameter of 115 mm and a second extruder equipped with a high-mixing type screw with an inner diameter of 180 mm connected in series, a physical foaming agent injection port was provided near the end of the first extruder, and a flat die equipped with a resin discharge port (die lip) with a rectangular cross section with a gap of 1 mm and a width of 440 mm was connected to the outlet of the second extruder. In addition, a molding device (guider) consisting of a pair of upper and lower plates made of polytetrafluoroethylene resin installed horizontally at a substantially constant interval was attached to the resin outlet of the second extruder.

[0066] (1) Base resin Polystyrene resin: DIC Corporation polystyrene "HP780AN", melt viscosity (200℃, 100sec -1 )1900 Pa·s Polyester resin: Mitsubishi Gas Chemical Company, Inc. spiroglycol modified polyethylene terephthalate "ALTESTER3012", terephthalic acid 100% by mass, spiroglycol / ethylene glycol = 30% by mass / 70% by mass, melt viscosity (200°C, 100 sec -1 )2000 Pa·s

[0067] (2) Physical foaming agents (a-1) 1-chloro-2,3,3,3-tetrafluoropropene (HFO-1224yd): manufactured by AGC (a-2) 1-chloro-3,3,3-trifluoropropene (HFO-1233zd): manufactured by Honeywell Japan (b) Isobutane: manufactured by Taiyo Liquefied Gas Co., Ltd. (c-1) Water (c-2) Ethanol: Yamaichi Chemical Industry Co., Ltd.

[0068] (3) Flame retardants A flame retardant masterbatch (GR-134BG manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) containing 82 mass% of a mixed flame retardant of 60 mass% (tetrabromobisphenol A bis (2,3-dibromo-2-methylpropyl ether): Daiichi Kogyo Seiyaku "SR-130" / 40 mass% (tetrabromobisphenol A bis (2,3-dibromopropyl ether): Daiichi Kogyo Seiyaku "SR-720") was used, and the masterbatch was added so as to obtain the amount of flame retardant shown in the table.

[0069] (4) Foam regulator Talc (manufactured by Matsumura Sangyo Co., Ltd., product name "Hi-Filler #12") (5) Radiation suppressants Graphite ("CP-N" (flake graphite) manufactured by Nippon Graphite Industries Co., Ltd., primary particle size (d50) = 10 μm) Titanium oxide ("JR-405" manufactured by Teika Co., Ltd., primary particle size (d50) = 0.2 μm)

[0070] Examples 1 to 6, Comparative Examples 1 to 4 The types and amounts of base resin, flame retardant master batch, talc (cell foam regulator), and radiation inhibitor shown in Table 1 (Examples 1 to 5, Comparative Examples 1 to 3) and Table 2 (Example 6, Comparative Example 4) below were supplied to a first extruder, heated to 200°C and kneaded, and the types and amounts of physical foaming agents shown in Tables 1 and 2 were supplied from a physical foaming agent injection port provided in the first extruder, and further kneaded to form a foamable resin melt. Next, the obtained foamable resin melt was transferred to a second extruder to adjust the resin temperature, and then extruded into a guider at a discharge rate of 400 kg / hr. While foaming, the melt was passed through the guider to be molded (shaped) into a plate to produce an original plate of an extruded foam plate having a thickness of 30 mm. Further, the width and length of the original plate were adjusted by cutting, and the molded skins on both sides were evenly cut to produce a rectangular parallelepiped polystyrene resin foam plate without a molded skin (width: 910 mm, length: 1820 mm, thickness: 25 mm, cross-sectional area perpendicular to the extrusion direction: 227.5 cm). 2 ) was manufactured.

[0071] [Table 1] [Table 2]

[0072] For the extruded foam boards obtained in the Examples and Comparative Examples, the apparent density, closed cell ratio, thermal conductivity (after 7 days, 100 days, and 300 days), remaining HFO amount (after 7 days and 100 days), remaining HFO ratio, and compressive strength were measured by the methods described below, and the flammability and appearance were evaluated according to the following criteria.

[0073] (Apparent density) The apparent density of the extruded foam board was determined as follows: A rectangular parallelepiped sample of 50 mm length × 50 mm width × 25 mm thickness was cut out from the center and both ends of the obtained extruded foam board in the width direction, the mass was measured, and the apparent density of each sample was determined by dividing the mass by the volume, and the arithmetic average of the masses was regarded as the apparent density.

[0074] (Closed bubble rate) The closed cell ratio of the foam board was calculated from the true volume Vx of the extruded foam board measured using an air comparison type specific gravity meter (Toshiba Beckman Co., Ltd., air comparison type specific gravity meter, model: 930) according to procedure C of ASTM-D2856-70, using the following formula (1).

[0075] Specifically, cut samples were cut from three locations, the center and both ends in the width direction of the extruded foam plate, and each cut sample was used as a measurement sample to measure the closed cell ratio of each measurement sample and calculate the arithmetic average value of the closed cell ratio at the three locations. The cut samples used were cut from the extruded foam plate to a size of 25 mm length x 25 mm width x 25 mm thickness.

[0076] S(%)=(Vx-W / ρ)×100 / (Va-W / ρ) (1) In the formula, Vx, Va, W, and ρ are as follows: Vx: The true volume (cm) of the cut sample obtained by measurement using the air comparison type specific gravity meter 3 ) (This corresponds to the sum of the volume of the resin that constitutes the cut sample of the extruded foam board and the total volume of the air bubbles in the closed cell portion of the cut sample.) Va: Apparent volume (cm) of the cut sample calculated from the outer dimensions of the cut sample used in the measurement 3 ) W: Total mass of cut samples used for measurement (g) ρ: density of the resin composition constituting the extruded foam board (g / cm 3 )

[0077] (Thermal conductivity 7 days after manufacture) Test pieces measuring 200 mm in length, 200 mm in width, and 25 mm in thickness were cut out from the center of the width direction of the extruded foam board immediately after production, and the test pieces were stored in a constant temperature and humidity room at a temperature of 23°C and a relative humidity of 50%. Seven days after production, the thermal conductivity was measured based on the flat plate heat flow meter method described in JIS A1412-2 (1999) (two heat flow meter method, high temperature side 38°C, low temperature side 8°C, average temperature 23°C).

[0078] (Thermal conductivity 100 days and 300 days after manufacture) In addition, the thermal conductivity measured 100 and 300 days after manufacture was the value obtained by measuring the thermal conductivity of the extruded foam board according to Test Method A of the accelerated long-term change test of thermal resistance in accordance with JIS A1486 (2014). Specifically, a rectangular parallelepiped measuring 200 mm long x 200 mm wide x 25 mm thick was cut out from the center of the width direction of the extruded foam board immediately after production, and then test pieces measuring 200 mm long x 200 mm wide x 10 mm thick were cut out by evenly shaving both sides. These were then stored in a temperature-constant humidity room at a temperature of 23°C and a relative humidity of 50%. The thermal conductivity of the test pieces 16 days after production (corresponding to 100 days after production of a 25 mm thick extruded foam board) and 48 days after production (corresponding to 300 days after production of a 25 mm thick extruded foam board) was measured based on the flat plate heat flow meter method (two heat flow meter method, high temperature side 38°C, low temperature side 8°C, average temperature 23°C) described in JIS A1412-2 (1999).

[0079] (HFO remaining 7 days after manufacture) A test piece measuring 200 mm x 200 mm x 25 mm was cut from the centre of the width direction of the extruded foam plate immediately after production and stored in a constant temperature and humidity room at a temperature of 23°C and a relative humidity of 50%. Seven days after production, an appropriate amount of sample was cut out from the test piece and placed in a lidded sample bottle containing an appropriate amount of toluene and an internal standard substance, the lid was closed, and the mixture was thoroughly stirred. The HFO in the extruded foam plate was dissolved in toluene, and the solution was used as the measurement sample for gas chromatographic analysis to determine the amount of HFO remaining in the extruded foam plate. (HFO remaining 100 days after manufacture) Immediately after production, a rectangular prism measuring 200 mm long x 200 mm wide x 25 mm thick was cut out from the centre of the width direction of the extruded foam board and then evenly shaved from both sides to cut out a test piece measuring 200 mm long x 200 mm wide x 10 mm thick. The test piece was stored in a constant temperature and humidity room at a temperature of 23°C and a relative humidity of 50%. An appropriate amount of sample was cut out from the test piece 16 days after production (equivalent to 100 days after the production of a 25 mm thick extruded foam board). This sample was placed in a lidded sample bottle containing an appropriate amount of toluene and an internal standard, the lid was closed, and the solution was thoroughly stirred and the HFOs in the extruded foam board dissolved in toluene was used as the measurement sample for gas chromatographic analysis to determine the amount of HFO remaining in the extruded foam board.

[0080] (HFO residual rate) The amount of HFO remaining 7 days after production was divided by the amount of HFO remaining 100 days after production to obtain the HFO remaining rate.

[0081] (flammability) Immediately after production, the extruded foam board was stored in a constant temperature and humidity room at a temperature of 23°C and a relative humidity of 50%. Four weeks after production, five test pieces (N=5) were randomly cut out from the extruded foam board. The flammability was measured based on "Test Method A" specified in the flammability test method of JIS A9521:2017, and the flame retardancy of the extruded foam board was evaluated according to the following criteria. Evaluation criteria ○: Disappeared within 3 seconds for all five test pieces. ×: The average burning time of the five test pieces is more than 3 seconds. (Not applicable)

[0082] (Compressive strength) The compressive strength of the extruded foam board was measured as follows. In accordance with JIS K7181 (2011), the measurement was performed using a Tensilon universal material testing machine manufactured by A&D Co., Ltd., using the following method. A test piece (50 mm in the extrusion direction × 50 mm in the width direction × 25 mm thick [excluding the skin layer]) cut from the center of the extruded foam board was compressed by 10% at a speed of 10 mm / min to obtain a stress-strain curve. The stress at 10% compression was read from the obtained stress-strain curve, and the compressed area of ​​the test piece (25 cm 2 The above measurements were carried out in the three directions of the extrusion direction, width direction, and thickness direction of the extruded foam board, and the arithmetic average value was taken as the compressive strength.

[0083] (exterior) The appearance was evaluated according to the following criteria. ⊚: The foaming state was good, and the surface of the base plate was free of roughness or spot holes. By removing the molding skin from the base plate, an extruded foam plate with an extremely good appearance was stably obtained. ◯: Some roughness was observed on the surface of the original plate, but the foaming state was good, there were no spot holes on the surface, and an extruded foam plate with a good appearance was obtained by scraping off the molding skin of the original plate. ×: Roughness and multiple spot holes were observed on the surface of the original plate, and a good-looking extruded foam plate was not obtained.

[0084] From the above results, in Comparative Examples 1 and 4, in which isobutane was not added, the HFO remaining amount and HFO remaining rate after 100 days were lower than those in Examples 1 to 6, and in Comparative Example 1, the compressive strength was also low. In Comparative Example 2, in which the amount of HFO-1224yd was increased and isobutane was not added, and in Comparative Example 3, in which the balance between the amounts of HFO-1224yd and isobutane added was outside the range specified in the present invention, the moldability of the extruded foam board was poor, and the appearance showed roughness and multiple spot holes on the surface, and a good extruded foam board was not obtained. In Comparative Examples 2 and 3, since a good extruded foam board was not obtained, the flammability evaluation and the compressive strength measurement were not performed. In contrast, the extruded foam boards of Examples 1 to 6, which were produced using a base resin mainly composed of a polystyrene resin and adding physical foaming agents of HFO-1224yd and isobutane within the ranges specified in the present invention, were good and well-balanced in terms of apparent density, thermal conductivity, compressive strength, flammability, and appearance.

Claims

1. A method for producing an extruded polystyrene-based resin foam plate, comprising the steps of extruding and foaming a foamable resin composition obtained by kneading a base resin mainly composed of a polystyrene-based resin with a physical foaming agent, and forming the foamed resin into a plate shape using a molding tool, the physical blowing agent comprises a blowing agent (a) made of 1-chloro-2,3,3,3-tetrafluoropropene and a blowing agent (b) made of a saturated hydrocarbon having 3 to 5 carbon atoms; the total amount of the physical foaming agent added is 0.8 to 1.5 mol per kg of the base resin; The amount of the foaming agent (a) added is 0.7 to 1.3 mol per kg of the base resin, the amount of the foaming agent (b) added is 0.1 mol or more per kg of the base resin, A method for producing an extruded polystyrene resin foam board, characterized in that the ratio of the amount of the foaming agent (a) added per 1 kg of the base resin to the amount of the foaming agent (b) added per 1 kg of the base resin is 0.6 or less.

2. 2. The method for producing an extruded polystyrene foam board according to claim 1, wherein the amount of the foaming agent (b) added is less than 0.4 mol per 1 kg of the base resin.

3. 3. The method for producing an extruded polystyrene foam board according to claim 1, wherein the amount of the foaming agent (a) added is more than 0.8 mol and not more than 1.3 mol per kg of the base resin.

4. 4. The method for producing a polystyrene-based resin extruded foam board according to claim 1, wherein the ratio of the amount of the foaming agent (a) added per 1 kg of the base resin to the amount of the foaming agent (b) added per 1 kg of the base resin is 0.4 or less.

Citation Information

Patent Citations

  • Polyether for thermal insulation of refrigerator / freezer, and method for preparing rigid polyurethane foam from polyether

    CN113461893A

  • Refrigeration cycle device

    JP2010002105A

  • Cooling cycle device

    JP2010101530A

  • Thermoplastic resin extrusion foamed heat insulating plate

    JP2013082805A

  • Method for producing thermoplastic resin extruded foam insulation board

    JP2015229771A