Expandable styrene resin particles, pre-expanded styrene resin particles, and styrene resin foamed molded product

By optimizing the composition and properties of expandable styrenic resin particles with specific ratios of styrene, (meth)acrylic acid ester monomer, blowing agent, and additives, the challenges of shrinkage and moldability are addressed, resulting in high-quality foam molded products with balanced energy efficiency.

JP7568529B2Active Publication Date: 2024-10-16SEKISUI PLASTICS CO LTD
View PDF 20 Cites 0 Cited by

Patent Information

Application Number
JP2021011688
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-28
Publication Date
2024-10-16
Estimated Expiration
2041-01-28

AI Technical Summary

Technical Problem

Existing foam molding technologies face challenges in achieving both energy savings and moldability while minimizing shrinkage during in-mold foam molding of expandable styrenic resin particles, often resulting in undesired product shapes.

Method used

The use of expandable styrenic resin particles containing specific ratios of styrene monomer, (meth)acrylic acid ester monomer, blowing agent (isobutane), solvent, and plasticizer, along with controlled molecular weight, to achieve balanced energy savings and moldability, reducing shrinkage during foam molding.

Benefits of technology

The solution enables the production of foam molded products with suppressed shrinkage, maintaining excellent energy efficiency and moldability, ensuring consistent product shape and quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568529000001
    Figure 0007568529000001
Patent Text Reader

Abstract

To provide expandable styrene resin particles which have an excellent energy-saving property when expansion-molded in a mold and excellent moldability, and which can form an expansion-molded body with suppressed shrinkage.SOLUTION: Expandable styrene resin particles of the present invention comprise a styrene resin and a blowing agent. The styrene resin is a polymer of a monomer mixture containing 90 mass% to 99 mass% of a styrene monomer and 1 mass% to 10 mass% of a (meth)acrylate monomer, and a weight average molecular weight Mw, thereof is 240000 to 500000. A content of the blowing agent in the expandable styrene resin particles is 3 mass% to 8.5 mass%, and the blowing agent contains 35 mass% to 85 mass% of isobutane relative to the whole weight. And a total amount of a solvent and a plasticizer in the expandable styrene resin particles is 0.5 mass% to 3 mass%, and an amount of a residual unreacted monomer is 0.15 mass% to 0.7 mass%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to expandable styrene-based resin particles, pre-expanded styrene-based resin particles, and expanded molded styrene-based resin articles. [Background technology]

[0002] Since foam molded articles are lightweight and have excellent heat insulation and mechanical strength, they are widely used as heat insulation materials for houses and automobiles, heat retaining materials for building materials, transport packaging materials for fish boxes and food containers, and cushioning materials. Among them, in-mold foam molded articles manufactured using expandable particles as raw materials are widely used. In-mold foam molding requires energy saving and moldability. Examples of energy saving include a small amount of steam used and a short heating time. Examples of moldability include the fact that the expandable particles do not break during molding, that the appearance of the resulting foam molded article is good, that the vapor pressure at which a good molded article is obtained is appropriate, and that the cooling time is short. As is clear from this explanation, energy saving and moldability are characteristics that can be related to each other. Various technologies have been proposed to improve energy saving and moldability. However, in many cases, when trying to improve energy saving and moldability, excessive shrinkage occurs during in-mold foam molding, and a foam molded article of the desired shape cannot be obtained. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-184393 A [Patent Document 2] JP 2011-026506 A [Patent Document 3] Patent No. 6424037 [Patent Document 4] Patent No. 3532323 Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention has been made to solve the above-mentioned problems of the prior art, and its main object is to provide expandable styrene-based resin particles that are excellent in energy saving and moldability during in-mold foam molding and can form foamed molded articles with suppressed shrinkage. The present invention also provides pre-expanded styrene-based resin particles and styrene-based resin foamed molded articles using such expandable styrene-based resin particles. [Means for solving the problem]

[0005] The expandable styrene-based resin particles according to an embodiment of the present invention comprise a styrene-based resin and a blowing agent; the styrene-based resin is a polymer of a monomer mixture containing 90% by mass to 99% by mass of a styrene-based monomer and 1% by mass to 10% by mass of a (meth)acrylic acid ester monomer, and has a weight average molecular weight Mw of 240,000 to 500,000; the content of the blowing agent in the expandable styrene-based resin particles is 3% by mass to 8.5% by mass, and the blowing agent contains 35% by mass to 85% by mass of isobutane relative to the total amount of the blowing agent; the total amount of the solvent and plasticizer in the expandable styrene-based resin particles is 0.5% by mass to 3% by mass, and the amount of remaining unreacted monomer is 0.15% by mass to 0.7% by mass. According to another embodiment of the present invention, there is provided a pre-expanded styrene-based resin particle, which is obtained by pre-expanding the above-mentioned expandable styrene-based resin particle. According to yet another embodiment of the present invention, there is provided a styrene-based resin foamed molded article. The styrene-based resin foamed molded article contains expanded styrene-based resin particles obtained by expanding the pre-expanded styrene-based resin particles, and is composed of a plurality of the expanded styrene-based resin particles fused together. Effect of the Invention

[0006] According to an embodiment of the present invention, by controlling in combination the foaming agent content, the solvent and plasticizer content, and the amount of remaining unreacted monomer in the foaming styrene-based resin particles, as well as the ratio of the styrene-based monomer to the (meth)acrylic acid ester monomer in the styrene-based resin, and the isobutane content in the foaming agent, it is possible to obtain foaming styrene-based resin particles that are excellent in energy saving and moldability during in-mold foaming and can form foamed molded articles with suppressed shrinkage. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments. The definitions of terms used in this specification are as follows. Expandable styrene-based resin particles (sometimes simply referred to as expandable particles): These refer to particles impregnated with a blowing agent before foaming. Pre-expanded styrene-based resin particles (sometimes simply referred to as pre-expanded particles): These refer to particles obtained by pre-expanding expandable particles before being subjected to expansion molding. Expanded styrene-based resin particles (sometimes simply referred to as expanded particles): These refer to particles that form an expanded molded article when pre-expanded particles are further expanded by expansion molding. Styrene-based expanded resin molded article (sometimes simply referred to as expanded molded article): refers to an article molded from expanded styrene-based resin particles.

[0008] A. Expandable styrene resin particles A-1.Overall configuration The expandable styrene-based resin particles (expandable particles) according to an embodiment of the present invention contain a styrene-based resin and a foaming agent, and have a particle shape as a whole. The particle size of the expandable particles is, for example, 0.3 mm to 3.0 mm, and preferably 0.3 mm to 1.7 mm. The particle size can be measured in accordance with JIS Z 8815. Specifically, the particle size is a value measured as a particle size at an integrated value of 50% from the particle size distribution by the sieving test of JIS Z 8815. Any appropriate shape can be adopted as the shape of the expandable particles. Specific examples of the shape include a spherical shape, a substantially spherical shape, an oval spherical shape (egg-shaped), a cylindrical shape, and a substantially cylindrical shape.

[0009] In an embodiment of the present invention, the expandable particles have the following configuration. The styrene-based resin is a polymer of a monomer mixture containing 90% by mass to 99% by mass of a styrene-based monomer and 1% by mass to 10% by mass of a (meth)acrylic acid ester monomer. The content of the blowing agent in the expandable particles is 3% by mass to 8.5% by mass. The blowing agent contains 35% by mass to 85% by mass of isobutane relative to the total amount of the blowing agent. Furthermore, the total amount of the solvent and plasticizer in the expandable particles is 0.5% by mass to 3% by mass, and the amount of the remaining unreacted monomer (hereinafter sometimes simply referred to as the remaining monomer) is 0.15% by mass to 0.7% by mass. By having such a configuration, it is possible to realize expandable styrene-based resin particles that are excellent in energy saving and moldability during in-mold expansion molding and can form an expanded molded product with suppressed shrinkage. The components of the expandable particles will be specifically described below.

[0010] A-2. Styrene-based resin The styrene resin is a polymeric compound containing a styrene monomer as a monomer component. The styrene monomer contains styrene or a styrene derivative. Examples of the styrene derivative include α-methylstyrene, vinyltoluene, chlorostyrene, ethylstyrene, i-propylstyrene, dimethylstyrene, and bromostyrene. The styrene monomer may be used alone or in combination of two or more. The styrene monomer preferably contains at least styrene. The styrene monomer preferably contains 50% or more of styrene based on the total amount of the styrene monomer, more preferably 70% or more, and even more preferably 90% or more.

[0011] The styrene-based resin may contain a styrene-based monomer as a main component of the monomer components, and may be a copolymer of a styrene-based monomer and a copolymer component. A representative example of the copolymer component is a vinyl monomer. In the embodiment of the present invention, the styrene-based resin is a polymer of a monomer mixture containing 90% by mass to 99% by mass of a styrene-based monomer and 1% by mass to 10% by mass of a (meth)acrylic acid ester monomer as a vinyl monomer, as described above. The content of the styrene-based monomer in the monomer mixture is preferably 95% by mass to 99% by mass, more preferably 97% by mass to 99% by mass. The content of the (meth)acrylic acid ester monomer in the monomer mixture is preferably 1% by mass to 5% by mass, more preferably 1% by mass to 3% by mass.

[0012] Specific examples of the (meth)acrylic acid ester monomer include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and hexyl (meth)acrylate. Butyl acrylate, 2-ethylhexyl acrylate, and ethyl acrylate are preferred, and butyl acrylate is more preferred. By using the (meth)acrylic acid ester monomer, the glass transition temperature (Tg) of the styrene resin can be lowered, and excellent energy saving properties and moldability can be achieved. On the other hand, when the (meth)acrylic acid ester monomer is used, a foam molded product of a desired shape may not be obtained due to shrinkage during foam molding. According to an embodiment of the present invention, the blending ratio of the (meth)acrylic acid ester monomer is set to the above range, and further, the content of the foaming agent, the content of isobutane in the foaming agent, the content of the solvent and the plasticizer, and the amount of the remaining monomer are controlled in combination, thereby making it possible to suppress the shrinkage of the foam molded product while maintaining excellent energy saving properties and moldability. In this specification, "(meth)acrylic" means acrylic and / or methacrylic.

[0013] As described above, the styrene-based resin may be a polymer of a monomer mixture containing a copolymerization component (other copolymerization component) other than a styrene-based monomer and a (meth)acrylic acid ester monomer. The content of the other copolymerization component in the monomer mixture is defined as the remainder of the total content of the styrene-based monomer and the (meth)acrylic acid ester monomer when the entire monomer mixture is taken as 100 mass%. The other copolymerization component may typically be a vinyl monomer (other vinyl monomer) other than a (meth)acrylic acid ester monomer. Examples of the other vinyl monomer include a (meth)acrylic acid ester monomer, a multifunctional monomer, a maleic acid ester monomer, and a fumaric acid ester monomer. The other vinyl monomer may be used alone or in combination of two or more kinds. The number, type, combination, amount, etc. of the other vinyl monomer may be appropriately set according to the purpose.

[0014] Specific examples of the polyfunctional monomer include divinylbenzenes such as o-divinylbenzene, m-divinylbenzene, and p-divinylbenzene, and alkylene glycol di(meth)acrylates such as ethylene glycol di(meth)acrylate and polyethylene glycol di(meth)acrylate. By using a polyfunctional monomer, a branched structure can be imparted to the styrene-based resin.

[0015] An example of a maleate monomer is dimethyl maleate.

[0016] Examples of fumarate monomers include dimethyl fumarate, diethyl fumarate, and ethyl fumarate.

[0017] The weight average molecular weight Mw of the styrene resin is, for example, 240,000 to 500,000, or, for example, 240,000 to 450,000, or, for example, 240,000 to 400,000. The weight average molecular weight Mw of the styrene resin may be, for example, 280,000 to 400,000, or, for example, 350,000 to 400,000. If the weight average molecular weight is too large, the energy saving properties and moldability may be insufficient. If the weight average molecular weight is too small, a foam molded product of the desired shape may not be obtained due to shrinkage during foam molding.

[0018] A-3. Foaming agent Any suitable blowing agent can be used as the blowing agent. The blowing agent is preferably an organic compound whose boiling point is equal to or lower than the softening point of the styrene-based resin and is in a gaseous or liquid state at normal pressure. Specific examples include aliphatic hydrocarbons such as propane, n-butane, isobutane, pentane (n-pentane, isopentane or neopentane), and n-hexane; alicyclic hydrocarbons such as cyclopentane and cyclopentadiene; ketones such as acetone and methyl ethyl ketone; alcohols such as methanol, ethanol, and isopropyl alcohol; low-boiling ether compounds such as dimethyl ether, diethyl ether, dipropyl ether, and methyl ethyl ether; and halogen-containing hydrocarbons such as trichloromonofluoromethane and dichlorodifluoromethane. Inorganic gases such as carbon dioxide, nitrogen, and ammonia may be used as the blowing agent. The blowing agent may be used alone or in combination of two or more kinds. Aliphatic hydrocarbons are preferred. This is because they can prevent the destruction of the ozone layer and can be quickly replaced with air, thereby suppressing the deterioration of the foamed molded body over time. More preferred are propane, n-butane, isobutane, and combinations thereof.

[0019] In the embodiment of the present invention, n-butane and isobutane can be particularly preferably used. Furthermore, in the embodiment of the present invention, the foaming agent contains 35% by mass to 85% by mass, preferably 35% by mass to 80% by mass, more preferably 40% by mass to 80% by mass, and further preferably 40% by mass to 70% by mass of isobutane based on the total amount of the foaming agent. If the content of isobutane is too small, a foam molded product having a desired shape may not be obtained due to shrinkage during foam molding. If the content of isobutane is too large, energy saving or moldability may be insufficient (especially, the cooling time after molding may be long).

[0020] Furthermore, in an embodiment of the present invention, the content of pentane (n-pentane and isopentane) in the foaming agent is preferably less than 10% by mass, more preferably less than 5% by mass, and even more preferably less than 3% by mass. The content of pentane may be 0 (zero). If the content of pentane is too high, the strength of the foamed molded article may be insufficient.

[0021] The content of the foaming agent in the expandable particles is 3% by mass to 8.5% by mass, preferably 3% by mass to 8% by mass, and more preferably 4% by mass to 6% by mass, as described above. If the content of the foaming agent is too small, the foamed molded article itself may not be obtained. If the content of the foaming agent is too large, the energy saving or moldability may be insufficient (especially, the cooling time after molding may be long).

[0022] A-4. Plasticizers and solvents The expandable particles may contain a plasticizer and / or a solvent. Examples of the plasticizer include aliphatic esters such as diisobutyl adipate and dibutyl sebacate, fatty acid glycerides such as stearic acid triglyceride, glycerol tristearate, and glycerol tricaprylate, vegetable oils such as coconut oil, palm oil, and olive oil, and liquid paraffin. Among these plasticizers, diisobutyl adipate, coconut oil, and liquid paraffin are preferred. It is preferable not to use chemical substances prohibited from use under laws and regulations such as the RоHS Directive (RоHS2) and the Food Sanitation Act as plasticizers. Examples of such chemical substances include phthalates. Examples of phthalates include di-2-ethylhexyl phthalate and n-octyl phthalate. Examples of the solvent include aliphatic hydrocarbons with C6 or more such as hexane and heptane, alicyclic hydrocarbons with C6 or more such as cyclohexane and cyclooctane, and aromatic hydrocarbons such as toluene and ethylbenzene. Among these solvents, cyclohexane is preferred from the viewpoint of good foaming power and environmental and health aspects. In an embodiment of the present invention, the total amount of the solvent and the plasticizer in the expandable particles is 0.5% by mass to 3% by mass, preferably 0.8% by mass to 2.5% by mass, and more preferably 1.5% by mass to 2.2% by mass, as described above. If the total amount is too small, the energy saving properties and moldability may be insufficient. If the total amount is too large, a foam molded product of the desired shape may not be obtained due to shrinkage during foam molding. The total amount can be adjusted by the amount of each added during production.

[0023] A-5. Residual monomer Unreacted monomers may remain in the expandable particles. In the embodiment of the present invention, the amount of the residual monomer is 0.15% by mass to 0.7% by mass, preferably 0.15% by mass to 0.6% by mass, and more preferably 0.15% by mass to 0.5% by mass, as described above. If the amount of the residual monomer is too small, moldability may be insufficient. If the amount of the residual monomer is too large, a foamed molded product of a desired shape may not be obtained due to shrinkage during foam molding. The amount of the residual monomer can be adjusted by adjusting the polymerization reaction temperature, polymerization reaction time, amount of polymerization initiator added, etc. during production, or by intentionally adding it to the styrene-based resin particles.

[0024] A-6.Average bubble diameter When the expandable particles are expanded 60 times (which may be pre-expanded particles or expanded particles), the average bubble diameter of the surface layer is preferably 20 μm to 200 μm, more preferably 40 μm to 150 μm, and even more preferably 50 μm to 120 μm. If the average bubble diameter is in such a range, there is an advantage that the appearance of the foamed molded product is beautiful. The surface layer of the expanded particles refers to the region from the surface of the expanded particles to 300 μm in the center direction (i.e., in the diameter direction). The average bubble diameter can be measured, for example, in accordance with ASTM D2482-69.

[0025] A-7.Other The expandable particles may further contain additives. Examples of additives include radiant heat transfer suppressing components, resins other than styrene-based resins, crosslinking agents, fillers, flame retardants, flame retardant assistants, lubricants, colorants, antistatic agents, spreading agents, cell regulators, weather resistance agents, antioxidants, antifogging agents, and fragrances. The type, number, combination, and content of additives can be appropriately set depending on the purpose.

[0026] The expandable particles may further contain a surface additive. For example, examples of surface additives for suppressing adhesion between pre-expanded particles during pre-expanding of the expandable particles include powdered metal soaps (e.g., zinc stearate, magnesium stearate, etc.) and silicone oil. For example, examples of surface additives for promoting fusion of pre-expanded particles during molding include fatty acid esters (e.g., hydrogenated castor oil, stearic acid triglyceride, medium-chain fatty acid triglyceride, etc.), vegetable oils (coconut oil, olive oil, etc.), liquid paraffin, etc. Examples of surface additives for preventing static electricity include polyethylene glycol, propylene glycol, glycerin, etc.

[0027] The expandable granules can be produced by a method well known and commonly used in the art, and therefore, a description of the method for producing the expandable granules will be omitted.

[0028] B. Pre-expanded styrene resin particles The pre-expanded particles according to an embodiment of the present invention are obtained by pre-expanding the expandable particles described in the above item A. The pre-expanding step includes expanding the expandable particles to a desired bulk expansion ratio (bulk density) using steam or the like. The bulk expansion ratio of the pre-expanded particles is preferably 3 to 100 times, more preferably 30 to 90 times, and further preferably 50 to 70 times. The bulk density is the reciprocal of the bulk expansion ratio. The bulk expansion ratio and the bulk density can be determined, for example, as follows. The expandable particles are collected as a measurement sample, W (g). The measurement sample is allowed to fall naturally into a measuring cylinder, and the volume of the measurement sample that fell into the measuring cylinder, V (cm 3 ) is measured using an apparent density measuring device conforming to JIS K 6911. From the mass and volume of the measurement sample, the bulk expansion ratio and bulk density can be calculated according to the following formula. Bulk foaming ratio (times = cm 3 / g) = volume of measurement sample (V) / mass of measurement sample (W) Bulk density (g / cm 3 ) = mass of measurement sample (W) / volume of measurement sample (V)

[0029] In one embodiment, the pre-expanded particles can be used for forming a foamed molded article. In another embodiment, the pre-expanded particles can be used as they are as a buffer material, a heat insulating material, etc. When the pre-expanded particles are used as they are, the pre-expanded particles can be preferably used as a filling material in which a large number of the pre-expanded particles are filled in a bag.

[0030] C. Styrene resin foam molding The foamed molded article according to the embodiment of the present invention contains expanded styrene-based resin particles (expanded particles) obtained by further expanding the pre-expanded particles described in the above section B. The foamed molded article is typically composed of a plurality of expanded particles fused together.

[0031] The foamed molded article can be typically produced by placing pre-expanded particles in a mold having a predetermined shape according to the purpose and performing in-mold foaming. More specifically, in-mold foaming includes (i) filling pre-expanded particles into a closed mold having a large number of small holes, (ii) heating and foaming the pre-expanded particles with a heat medium (e.g., pressurized steam, etc.) to obtain foamed particles, and (iii) filling the voids between the foamed particles by the heating and foaming, and fusing the foamed particles to each other to integrate them. The density of the foamed molded article can be appropriately set according to the purpose. The density of the foamed molded article can be adjusted, for example, by previously adjusting the bulk expansion ratio of the pre-expanded particles to be filled in the mold, or by adjusting the amount of pre-expanded particles filled in the mold.

[0032] The heat-foaming temperature (substantially the temperature of the heat transfer medium) is preferably 90°C to 150°C, more preferably 110°C to 130°C. The heat-foaming time is preferably 5 seconds to 50 seconds, more preferably 10 seconds to 50 seconds. The molding vapor pressure of the heat-foaming (gauge pressure of the heat transfer medium blowing in) is preferably 0.06 MPa to 0.08 MPa. If the heat-foaming is performed under such conditions, the expanded particles can be well fused to each other.

[0033] If necessary, the pre-expanded particles may be aged before forming into a foamed molded article. The aging temperature of the pre-expanded particles is preferably 20°C to 60°C. If the aging temperature is too low, an excessively long aging time may be required. If the aging temperature is too high, the blowing agent in the pre-expanded particles may dissipate, resulting in a decrease in moldability.

[0034] The bulk expansion ratio of the expanded beads in the expanded molded product is preferably 3 to 100 times, more preferably 30 to 90 times, and further preferably 50 to 70 times.

[0035] In the embodiment of the present invention, shrinkage during foam molding is suppressed, so that foam molded articles having desired shapes can be obtained stably and with high yields. EXAMPLES

[0036] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring and evaluating each property are as follows.

[0037] (A) Unreacted monomer content and solvent content of expandable particles The unreacted monomer content and the solvent content of the expandable particles were measured by gas chromatography. 1 g of each expandable particle was precisely weighed out, and 1 mL of a dimethylformamide solution containing 0.1% by volume of cyclopentanol was added to the precisely weighed sample as an internal standard solution, and then dimethylformamide was further added to prepare 25 mL of a measurement solution. Next, 1.8 μL of this measurement solution was supplied to a gas chromatograph (manufactured by Shimadzu Corporation, product name "GC-2014") for measurement. The unreacted monomer content and the solvent content relative to the total weight of the expandable particles were calculated based on a calibration curve that had been measured in advance, and the respective contents (ppm) were calculated. The measurement conditions were as follows. <Measurement conditions> Detector: FID Column: GL Sciences (φ3mm×2m) Liquid phase: PEG-20MPT25% Support: Chromosorb WAW-DWCS Mesh:60 / 80 Column temperature: 95℃ DET temperature:220℃ Detector temperature: 220℃ Carrier gas: Nitrogen Nitrogen flow rate: 40mL / min

[0038] (B) Weight average molecular weight of expandable particles The weight-average molecular weight was measured by gel permeation chromatography (GPC) using the average molecular weight converted to polystyrene (PS). Specifically, 3 mg of the expandable particle sample was added to 10 mL of tetrahydrofuran (THF) and left to dissolve for 72 hours (complete dissolution), and the resulting solution was filtered with a non-aqueous 0.45 μm chromatodisk (13N) manufactured by Kurabo Industries, Ltd. and measured. The average molecular weight of the sample was obtained from the calibration curve of standard polystyrene that had been measured and prepared in advance. The chromatographic conditions were as follows: <Measurement conditions> Equipment used: High-speed GPC equipment, Tosoh Corporation, HLC-8320GPC EcoSEC system (with built-in RI detector) Guard column: Tosoh Corporation, TSKguardcolumn SuperHZ-H (4.6mm ID x 2cm L) x 1 Column: Tosoh Corporation, TSKgel SuperHZM-H (4.6 mm ID x 15 cm L) x 2 Column temperature: 40℃ System temperature: 40℃ Mobile phase: Tetrahydrofuran Mobile phase flow rate: Sample side = 0.175 mL / min, Reference side = 0.175 mL / min Detector: RI detector, sample concentration = 0.3 g / L Injection volume: 50μL Measurement time: 0 to 25 minutes Runtime: 25 minutes Sampling pitch: 200msec <Creating a calibration curve> The standard polystyrene samples used for the calibration curve were those manufactured by Tosoh Corporation under the trade name "TSK standard POLYSTYRENE" with weight average molecular weights of 5,480,000, 3,840,000, 355,000, 102,000, 37,900, 9,100, 2,630, and 500, and those manufactured by Showa Denko KK under the trade name "Shodex STANDARD" with a weight average molecular weight of 1,030,000. The calibration curve was created as follows. The standard polystyrene samples for the calibration curve were divided into group A (weight average molecular weight of 1,030,000), group B (weight average molecular weights of 3,840,000, 102,000, 9,100, and 500), and group C (weight average molecular weights of 5,480,000, 355,000, 37,900, and 2,630). 5 mg of group A was weighed out and dissolved in 20 mL of tetrahydrofuran (solution A), 5 mg to 10 mg of group B was weighed out and dissolved in 50 mL of tetrahydrofuran (solution B), and 1 mg to 5 mg of group C was weighed out and dissolved in 40 mL of tetrahydrofuran (solution C). The standard polystyrene calibration curve was obtained by injecting 50 μL of each of the prepared solutions A, B, and C, and creating a calibration curve (cubic equation) from the retention times obtained after measurement using a data analysis program for HLC-8320GPC, GPC Workstation (EcoSEC-WS). Measurements were performed using the calibration curve. The weight average molecular weight can also be measured using a sample from the expanded beads or the expanded molded article.

[0039] (C) Foaming agent content and foaming agent composition of expandable particles The blowing agent content (mass%) and blowing agent composition of the expandable particles were measured as follows. Approximately 20 mg of the expandable particles were precisely weighed and placed at the inlet of a Shimadzu PYR-1A pyrolysis furnace, and the furnace was purged with helium for about 15 seconds to expel any gas that had been mixed in when the sample was placed. After sealing, the sample was inserted into the furnace core at 180°C and heated for 120 seconds to release gas, and the released gas was measured and quantified under the following conditions. The blowing agent composition was calculated from the content of each blowing agent type relative to the total amount of blowing agent. <Measurement conditions> Measurement equipment: Gas chromatograph GC-14B, pyrolysis furnace PYR-1A (manufactured by Shimadzu Corporation) Column: Shimalite 60 / 80 NAW (Squalane 25%) 3m x 3φ Detector: FID Measurement conditions: column temperature (70°C), injection port temperature (110°C), detector temperature (110°C) Carrier gas (N2), N2 flow rate (50mL / min), absolute calibration method

[0040] (1)Energy saving The heating time during expansion was used as an index for evaluating energy saving. Specifically, it was as follows: The expandable particles obtained in the examples and comparative examples were fed to a cylindrical batch-type pre-expander and heated with steam at a blowing pressure of 0.07 MPa until the bulk density reached 0.017 g / cm. 3 The time required for the expansion ratio to reach 60 times was taken as the heating time, and the results were evaluated according to the following criteria. ◎: Heating time is 90 seconds or less 〇: Heating time is more than 90 seconds and less than 120 seconds △: Heating time is more than 120 seconds and less than 150 seconds ×: Heating time exceeds 150 seconds

[0041] (2) Formability For in-mold foam molding, an ACE-3SP molding machine manufactured by Sekisui Machinery Co., Ltd. was used, and the pre-expanded particles obtained in the Examples and Comparative Examples were filled into a plate-shaped mold measuring 400 mm in length, 300 mm in width, and 30 mm in thickness, with the heating time set to 20 seconds and the molding steam pressure (steam injection gauge pressure) set to 0.03 MPa to 0.08 MPa (adjusted in 0.01 MPa increments). The following four items were evaluated.

[0042] (2-1) Weldability Molding was performed at a molding steam pressure of 0.05 MPa. The obtained foamed molded product was broken, and the fracture surface was observed to determine the proportion of particles that had broken, rather than the particle interface, and evaluated according to the following criteria. ◎: Particle breakage rate is 90% or more 〇: The rate of particle breakage is 80% or more but less than 90% △: The rate of particle breakage is 70% or more but less than 80%. ×: The rate of particle breakage is less than 70%.

[0043] (2-2) Surface properties Molding was performed at a molding steam pressure of 0.05 MPa. The surface condition of the obtained foamed molded article was visually observed and evaluated according to the following criteria. ◎: Surface melting, no grains, very beautiful 〇: Surface melting, few grains, beautiful △: Surface melting, grain gaps, slightly poor appearance ×: Surface melting, many intergranular spaces, poor appearance

[0044] (2-3) Forming steam pressure Molding was performed at a molding steam pressure of 0.03 MPa to 0.08 MPa. The molding steam pressure at which both the above "(2-1) Weldability" and "(2-2) Surface property" were rated as "◎" or "〇" was specified, and the molded product was evaluated according to the following criteria. ◎: 0.04MPa or less ○: More than 0.04MPa and less than 0.05MPa △: More than 0.05MPa and less than 0.06MPa ×: Exceeds 0.06MPa

[0045] (2-4) Cooling time At the molding steam pressure specified in "(2-3) Molding steam pressure" above, the cooling time during molding was evaluated according to the following criteria. ◎: 80 seconds or less ○: More than 80 seconds and less than 100 seconds △: More than 100 seconds and less than 120 seconds ×: More than 120 seconds

[0046] (3) Contraction The expandable granules obtained in the examples and comparative examples were fed to a cylindrical batch-type pre-expander and heated with steam at a blowing pressure of 0.07 MPa to produce a bulk density of 0.017 g / cm. 3After pre-expanding to a volume expansion ratio of 70, the mixture was left to stand for 24 hours to obtain pre-expanded particles. For in-mold foaming, an ACE-3SP molding machine manufactured by Sekisui Kogyo Co., Ltd. was used, and the pre-expanded particles obtained above were filled into a plate-shaped mold having a size of 400 mm long x 300 mm wide x 10 mm thick. The heating time was 20 seconds, and the molding steam pressure (steam injection gauge pressure) was 0.08 MPa to obtain a foamed molded body. Five minutes after removal from the mold, the linear distances of the four sides of the length and width of the foamed molded body were measured, and the ratio to the mold dimensions was taken as the dimensional shrinkage rate. The same measurement was also performed one hour after removal from the mold. Of the four sides measured, the side with the largest shrinkage was evaluated according to the following criteria. ◎: The shrinkage rate after 5 minutes is 5% or less, and the shrinkage rate after 1 hour is smaller than the shrinkage rate after 5 minutes. ○: The shrinkage rate after 5 minutes is more than 5% and 6% or less, and the shrinkage rate after 1 hour is smaller than the shrinkage rate after 5 minutes. △: The shrinkage rate after 5 minutes is more than 6% and the shrinkage rate after 1 hour is smaller than the shrinkage rate after 5 minutes. ×: The shrinkage rate after 5 minutes is more than 6% and the shrinkage rate after 1 hour is greater than the shrinkage rate after 5 minutes.

[0047] (4) Overall evaluation Based on the evaluation of the above six items, an overall evaluation was conducted using the following criteria. ◎: No △ or × in any of the six evaluation items, and 5 or more ◎ 〇: No △ or × in any of the six evaluation items, and 4 or less ◎ △: Any of the six evaluation items has △ and no × ×: Any of the six evaluation items has an ×.

[0048] [Example 1] (Preparation of styrene-based resin particles) In a 100L autoclave equipped with a stirrer, 40,000 parts by mass of pure water, 100 parts by mass of calcium phosphate, and 3.2 parts by mass of sodium dodecylbenzenesulfonate were charged, and further, 40,000 parts by mass of styrene, 102 parts by mass of benzoyl peroxide, and 24 parts by mass of t-butylperoxy-2-ethylhexyl monocarbonate were charged while stirring. The temperature was then raised to 90°C, and the mixture was kept at 90°C for 6 hours, then raised to 125°C, and kept at 125°C for 2 hours, and then cooled to obtain styrene-based resin particles. The obtained styrene-based resin particles were sieved to obtain styrene-based resin seed particles having a particle diameter of 0.5 mm to 0.71 mm as seed particles. The rotation speed of the stirrer was adjusted so that such a particle diameter was obtained.

[0049] (Preparation of expandable styrene resin particles) In a 25L autoclave equipped with a stirrer, 2150 parts by mass of the seed particles obtained above, 30 parts by mass of magnesium pyrophosphate, and 1.0 parts by mass of sodium dodecylbenzenesulfonate were charged, and the mixture was stirred at 230 rpm to prepare a dispersion. The temperature was then raised to 72°C, and a solution in which 31 parts by mass of benzoyl peroxide and 8 parts by mass of t-butylperoxy-2-ethylhexyl monocarbonate were dissolved in a monomer mixture of 786 parts by mass of styrene and 137 parts by mass of butyl acrylate was added to the dispersion. After all the solution was added, the mixture was kept at 72°C for 60 minutes. Next, the temperature was raised to 87°C over 1 hour, while a constant supply of 2346 parts by mass of styrene was added, and a monomer mixture in which 2.7 parts by mass of divinylbenzene were dissolved in 3744 parts by mass of styrene was added at a constant supply, while the mixture was kept at 87°C for 1 hour and 30 minutes, and the mixture was kept for another 30 minutes. The temperature was then raised to 125°C, held at that temperature for 30 minutes, and then cooled to 100°C. Next, 92 parts by mass of cyclohexane, 82 parts by mass of diisobutyl adipate (plasticizer), and 45 parts by mass of styrene were added, and then 640 parts by mass of mixed butane (n-butane / isobutane=50% / 50%) was pressed in and held for 2 hours, and then cooled to 25°C. The slurry was removed from the autoclave, washed, dehydrated, and dried to obtain expandable particles. The content of butyl acrylate in the monomer mixture, the content of the blowing agent in the expandable particles, the content of isobutane in the blowing agent, the content of the remaining monomer in the expandable particles, the total amount of the plasticizer and the solvent in the expandable particles, and the weight average molecular weight of the styrene-based resin were as shown in Table 1. The content of the remaining monomer, the amount of the plasticizer, and the amount of the solvent were adjusted by making some changes to the above-mentioned addition amounts in the preparation of the expandable particles. The resulting expandable granules were coated with surface additives, which consisted of 0.05 parts by mass of zinc stearate, 0.05 parts by mass of triglyceride stearate, 0.05 parts by mass of monoglyceride stearate, and 0.05 parts by mass of polyethylene glycol, relative to 100 parts by mass of the expandable granules.

[0050] (Preparation of pre-expanded styrene-based resin particles) The expandable particles are fed into a cylindrical batch type pre-expander and heated with steam at a blowing pressure of 0.07 MPa to produce a bulk density of 0.017 g / cm. 3 After pre-expanding to a bulk expansion ratio of 60 times, the mixture was left to stand for 24 hours to obtain pre-expanded particles.

[0051] (Preparation of styrene-based resin foam molded bodies) An ACE-3SP molding machine manufactured by Sekisui Machinery Co., Ltd. was used for in-mold foam molding. A plate-shaped mold measuring 400 mm in length, 300 mm in width, and 30 mm in thickness was filled with the pre-expanded particles obtained in the Examples and Comparative Examples. The heating time was set to 20 seconds, and the molding steam pressure (steam injection gauge pressure) was set to 0.03 MPa to 0.08 MPa (adjusted in increments of 0.01 MPa), to obtain a foam molded product.

[0052] The obtained expandable particles, pre-expanded particles, and foamed molded articles were subjected to the above evaluations (1) to (3). The results are shown in Table 1.

[0053] [Examples 2 to 12 and Comparative Examples 1 to 11] Expandable particles, pre-expanded particles, and foamed molded articles were obtained in the same manner as in Example 1, except that the formulation and production method were changed so that the content of butyl acrylate in the monomer mixture, the content of the foaming agent in the expandable particles, the content of isobutane in the foaming agent, the content of the residual monomer in the expandable particles, the total amount of the plasticizer and the solvent in the expandable particles, and the weight average molecular weight of the styrene-based resin were the values ​​shown in Table 1. The obtained expandable particles, pre-expanded particles, and foamed molded articles were subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0054] [Table 1]

[0055] As is clear from Table 1, according to the examples of the present invention, it is possible to obtain a foamed molded article in which shrinkage is suppressed while maintaining excellent energy saving properties and excellent moldability. [Industrial Applicability]

[0056] The expandable styrene-based resin particles according to the embodiment of the present invention, and the pre-expanded styrene-based resin particles and styrene-based resin foam molded products using the same are suitable for use as insulation materials for houses and automobiles, heat-retaining materials for building materials, transport packaging materials for fish boxes and food containers, cushioning materials, etc. More specifically, the expandable styrene-based resin particles, pre-expanded styrene-based resin particles and styrene-based resin foam molded products are suitable for use as wall insulation materials, floor insulation materials, roof insulation materials, automobile insulation materials, heat-retaining materials for hot water tanks, heat-retaining materials for piping, heat-retaining materials for solar systems, heat-retaining materials for water heaters, containers for food and industrial products, packaging materials for fish and agricultural products, embankment materials, core materials for tatami mats, etc.

Claims

1. Expandable styrene-based resin particles containing a styrene-based resin and a blowing agent, the styrene-based resin is a polymer of a monomer mixture containing 90% by mass to 99% by mass of a styrene-based monomer and 1% by mass to 10% by mass of a (meth)acrylic acid ester monomer, and has a weight average molecular weight Mw of 240,000 to 500,000; The content of the blowing agent in the expandable styrene-based resin particles is 3% by mass to 8.5% by mass, and the blowing agent contains 35% by mass to 85% by mass of isobutane relative to the total amount of the blowing agent, the total amount of the solvent and the plasticizer in the expandable styrene-based resin particles is 1.5% by mass to 3% by mass, and the amount of the remaining unreacted monomer is 0.15% by mass to 0.7% by mass; Expandable styrene resin particles.

2. 2. Pre-expanded styrene-based resin particles obtained by pre-expanding the expandable styrene-based resin particles according to claim 1.

3. A styrene-based resin foamed molded article comprising a plurality of expanded styrene-based resin particles obtained by expanding the pre-expanded styrene-based resin particles according to claim 2, the expanded styrene-based resin particles being fused together.

Citation Information

Patent Citations

  • Expandable methyl methacrylate resin particle

    JP1983141219A

  • Device for supplying inorganic melt to fiberizing device

    JP1989024037A

  • Highly foamable styrene resin particle

    JP1997100366A

  • Foamable styrenic resin particle

    JP2001220458A

  • Expandable styrene-based resin particle

    JP2002284917A