Blowing Agent Blends for Thermoplastic Polymers

A blend of HFO-1336mzz-Z and cyclopentane addresses the high GWP and ODP issues of CFCs by enhancing solubility in polystyrene, producing low-density, thermally insulating foams with reduced environmental impact.

JP7568650B2Active Publication Date: 2024-10-16THE CHEMOURS CO FC LLC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021568576
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-29
Filing Date
2020-05-29
Publication Date
2024-10-16
Estimated Expiration
2040-05-29

AI Technical Summary

Technical Problem

Existing blowing agents for thermoplastic foams, such as chlorofluorocarbons (CFCs), have high global warming potential (GWP) and ozone depletion potential (ODP), necessitating the development of low-ODP and low-GWP alternatives.

Method used

A blend of Z-1,1,1,4,4,4-hexafluoro-2-butene (HFO-1336mzz-Z) and cyclopentane is used as a blowing agent, which significantly enhances solubility in softened polystyrene, allowing for the production of thermoplastic polymer foams with improved properties.

Benefits of technology

The HFO-1336mzz-Z/cyclopentane blend achieves higher solubility in polystyrene, resulting in foams with reduced density and improved thermal insulation capabilities while minimizing environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568650000002
    Figure 0007568650000002
  • Figure 0007568650000003
    Figure 0007568650000003
  • Figure 0007568650000001
    Figure 0007568650000001
Patent Text Reader

Abstract

The present invention relates to the use of HFO-1336mzz-Z / cyclopentane blends as blowing agents for thermoplastic polymers (e.g., polystyrene).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to blends of HFO-1336mzz-Z and cyclopentane, which are useful as blowing agents for thermoplastic polymers, such as polystyrene. [Background technology]

[0002] Chlorofluorocarbons (i.e., CFCs) have been used as blowing agents in the manufacture of various types of foams. In general, CFCs produce foams that have good thermal insulation properties, low flammability, and good dimensional stability. However, despite these advantages, CFCs have fallen into disfavor due to their involvement in the destruction of stratospheric ozone and their general high contribution to global warming. Summary of the Invention [Problem to be solved by the invention]

[0003] Therefore, there is a need for blowing agents that have both low ODP (ozone depletion potential) and low GWP (global warming potential). [Means for solving the problem]

[0004] The present application provides, inter alia, a process for preparing a thermoplastic polymer foam, the process comprising: (a) providing a foamable composition comprising a thermoplastic polymer and a blowing agent, the blowing agent comprising about 95% to about 1% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene and about 1% to about 95% by weight of cyclopentane; (b) expanding the foamable composition to produce a thermoplastic polymer foam; Includes.

[0005] The present application further provides a thermoplastic polymer foam, the thermoplastic polymer foam comprising: (a) a thermoplastic polymer selected from the group consisting of polystyrene homopolymer, polystyrene copolymer, and styrene-acrylonitrile copolymer, or blends thereof; (b) a blowing agent comprising 95% by weight to 1% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene and 1% by weight to 95% by weight of cyclopentane; Includes.

[0006] In some embodiments, the thermoplastic polymer foams provided herein are prepared according to one or more of the processes described herein.

[0007] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this invention belongs. Methods and materials for use in the present invention are described herein, and other suitable methods and materials known in the art may be used. The materials, methods, and examples are merely illustrative and are not intended to be limiting. All publications, patent applications, patents, sequences, database entries, and other references mentioned herein are incorporated herein by reference in their entirety. In case of conflict, the present specification, including definitions, will control. [Brief description of the drawings]

[0008] [Figure 1] The solubility at 176°C of an HFO-1336mzz-Z / cyclopentane blend containing 20 wt% cyclopentane in a polystyrene homopolymer with a melt flow index (MFI) at 200°C of approximately 5.00 g / 10 min (measured using a 5 kg load on the molten polymer according to the procedure of ASTM D 1238) is compared to the solubility of neat HFO-1336mzz-Z in polystyrene. [Diagram 2]The solubility at 176°C of an HFO-1336mzz-Z / cyclopentane / HFC-152a blend, containing 40 wt% HFO-1336mzz-Z, 40 wt% HFC-152a, and 20 wt% cyclopentane, in a polystyrene homopolymer with an MFI of 5.00 g / 10 min at 200°C (measured using a 5 kg load on the molten polymer according to the procedure of ASTM D 1238) is compared to the solubility of an HFO-1336mzz-Z / HFC-152a blend (50 wt% / 50 wt%) in polystyrene homopolymer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Current agents with high global warming potential (GWP) for expanding thermoplastic foams, such as extruded polystyrene foam (XPS), are under regulatory pressure. Z-1,1,1,4,4,4-hexafluoro-2-butene (i.e., HFO-1336mzz-Z) could in principle be used as a low GWP agent for expanding polystyrene (or other thermoplastic polymers) into foams with high thermal insulation. However, HFO-1336mzz-Z has low solubility in softened polystyrene under the operating conditions of current extrusion processes. As a result, they result in suboptimal foam properties (e.g., higher than desired foam density).

[0010] Blowing agents for expanding thermoplastic foams (e.g., polystyrene foams) must be sufficiently soluble in the molten thermoplastic polymer (e.g., polystyrene resin) under foam-forming conditions so that an adequate amount of blowing agent is available during the foam expansion and cooling stages to form cells and reduce the effective foam density to a target value. Blowing agents present beyond their solubility can lead to foam defects.

[0011] As described herein, it has been unexpectedly discovered that blends of HFO-1336mzz-Z and cyclopentane can exhibit solubilities in softened polystyrene that significantly exceed the solubility of neat HFO-1336mzz-Z at the same conditions (see, e.g., Figure 1). For example, the solubility of neat HFO-1336mzz-Z in a softened polystyrene homopolymer having a melt flow index (MFI) of 5.0 g / 10 min at 179°C and 1374 psia is measured to be 5.7 g per 100 g of polystyrene (or 5.7 phr, i.e., 5.7 parts solute per 100 parts resin by mass). In contrast, the solubility of an exemplary HFO-1336mzz-Z / cyclopentane blend containing 20 wt. % cyclopentane has a solubility of 32.24 g per 100 g of polystyrene in the same polystyrene at the same temperature and pressure (i.e., 465.6% greater than the solubility of neat HFO-1336mzz-Z).

[0012] It has also been unexpectedly found that ternary blends of HFO-1336mzz-Z with cyclopentane and HFC-152a can exhibit solubilities in softened polystyrene that are significantly greater than the solubility of binary blends of HFO-1336mzz-Z with HFC-152a (50 wt.% / 50 wt.% blends) at similar conditions (see, e.g., FIG. 2). For example, the solubility of an HFO-1336mzz-Z / HFC-152a blend containing 50 wt.% HFC-152a in a softened polystyrene homopolymer having a melt flow index (MFI) of 5.0 g / 10 min at 179° C. and 2980 psia is measured to be 11.8 g per 100 g of polystyrene (or 11.8 phr, i.e., 5.7 parts solute per 100 parts resin by mass). In contrast, the solubility of an exemplary HFO-1336mzz-Z / cyclopentane / HFC-152a blend containing 20 wt. % cyclopentane and 40 wt. % HFC-152a has a solubility of 17.83 g per 100 g of polystyrene in the same polystyrene at the same temperature and approximately the same pressure (2968 psia) (i.e., 51.1% greater than the solubility of a 50 wt. % / 50 wt. % HFO-1336mzz-Z / HFC-152a blend).

[0013] Thus, binary blends of HFO-1336mzz-Z and cyclopentane, and ternary blends of HFO-1336mzz-Z, cyclopentane, and HFC-152a, each optionally in combination with at least one additional compound provided herein (e.g., an additional compound selected from the group consisting of HFOs, HCFOs, HFCs, HFEs, HCFCs, CFCs, CO2, N2, olefins, hydrochloroolefins, chlorinated hydrocarbons, organic acids, alcohols, hydrocarbons, ethers, aldehydes, ketones, water, methyl formate, ethyl formate, formic acid, and trans-1,2-dichloroethylene (DCE)), may be useful as blowing agents having a low or moderate GWP for the expansion of thermoplastic foams, including extruded polystyrene foams.

[0014] Definitions and Abbreviations As used herein, the terms "comprises," "comprising," "includes," "including," "has," "having," or any other variation thereof, are intended to cover non-exclusive inclusions. For example, a process, method, article, or apparatus that includes a list of elements is not necessarily limited to those elements, but may include other elements not expressly listed or inherent to such process, method, article, or apparatus. Furthermore, unless expressly stated to the contrary, "or" refers to an inclusive "or" and not an exclusive "or." For example, a condition A or B is satisfied by any one of the following: A is true (or present) and B is false (or absent), A is false (or absent) and B is true (or present), and both A and B are true (or present).

[0015] Additionally, the use of "a" or "an" is employed to describe a plurality of elements and components described herein. This is done merely for convenience and to give a general sense of the scope of the invention. This description should be interpreted to include one or at least one, and the singular also includes the plural unless it is clear that a different meaning is intended.

[0016] As used herein, the term "about" is meant to account for variations due to experimental error (e.g., plus or minus about 10% of the indicated value). All measurements reported herein are understood to be modified by the term "about," unless otherwise indicated, regardless of whether the term "about" is explicitly used.

[0017] As used herein, the term "consisting of" excludes any element, step, or ingredient not specified. In the claims, such phrases limit the claim to include materials other than those recited, except for impurities normally accompanying the materials. When the phrase "consisting of" appears within a clause in the body of a claim rather than immediately following the preamble, it is intended to limit only the elements recited in that clause and does not exclude other elements from the claim as a whole.

[0018] As used herein, "consisting essentially of" is used to define compositions, methods that include materials, steps, features, ingredients, or elements in addition to those literally disclosed, provided that these additionally included materials, steps, features, components, or elements do not substantially affect the basic and novel characteristic(s) of the claimed invention, particularly the mechanism of action for achieving any desired result of the inventive process. The terms "consists essentially of" or "consisting essentially of" occupy a middle ground between "comprising" and "consisting of."

[0019] When an amount, concentration, or other value or parameter is given as either a range or a list of upper and / or lower values, it is understood to specifically disclose all ranges formed from any pair of any range upper limit or value and any range lower limit or value, whether or not a range is otherwise disclosed. When a numerical range is described herein, unless otherwise indicated, the range is intended to include the endpoints, and to include all integers and fractions within the range.

[0020] Global warming potential (GWP) is an index used to estimate the relative global warming contribution resulting from the atmospheric emission of one kilogram of a particular greenhouse gas compared to the emission of one kilogram of carbon dioxide. GWP can be calculated for various time horizons and indicates the impact of a given gas over its atmospheric lifetime. The GWP for a 100-year time horizon is the value usually referred to.

[0021] As used herein, the term "Ozone Depletion Potential (ODP)" is defined in Section 1.4.4, pages 1.28-1.31 of The Scientific Assessment of Ozone Depletion, 2002, A report of the World Meteorological Association's Global Ozone Research and Monitoring Project (see the first paragraph of this section). Ozone Depletion Potential (ODP) measures the stratospheric ozone depletion expected from a compound on a mass-by-mass basis relative to fluorotrichloromethane (CFC-11).

[0022] The following abbreviations may be used herein: CFCs: Chlorofluorocarbons GWP: Global Warming Potential HCFC: Hydrochlorofluorocarbons HCFO: Hydrochlorofluoroolefin HFC: Hydrofluorocarbon HFE: Hydrofluoroether HFO: Hydrofluoroolefin HFC-152a: 1,1-difluoroethane HFO-1336mzz-Z or 1336mzz-Z: Z-1,1,1,4,4,4-hexafluoro-2-butene MFI: Melt Flow Index ODP: Ozone Depletion Potential PS: Polystyrene wt%: weight percent or weight percentage

[0023] Process and foam of the present invention The present application provides a process for preparing thermoplastic polymer foams.

[0024] In some embodiments, the process provided herein comprises: (a) providing a foamable composition comprising a thermoplastic polymer and a blowing agent, the blowing agent comprising about 95% to about 1% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene and about 1% to about 95% by weight of cyclopentane; (b) expanding the foamable composition to produce a thermoplastic polymer foam; Includes.

[0025] In some embodiments, the blowing agent comprises about 1% to about 90% by weight cyclopentane, e.g., about 1% to about 70% by weight, about 1% to about 50% by weight, about 1% to about 30% by weight, about 1% to about 10% by weight, about 10% to about 90% by weight, about 10% to about 70% by weight, about 10% to about 50% by weight, about 10% to about 30% by weight, about 30% to about 90% by weight, about 30% to about 70% by weight, about 30% to about 50% by weight, about 50% to about 90% by weight, about 50% to about 70% by weight, or about 70% to about 90% by weight cyclopentane.

[0026] In some embodiments, the blowing agent comprises about 2% to about 45% by weight cyclopentane. In some embodiments, the blowing agent comprises about 10% to about 40% by weight cyclopentane. In some embodiments, the blowing agent comprises about 1% to about 30% by weight cyclopentane. In some embodiments, the blowing agent comprises about 15% to about 30% by weight cyclopentane. In some embodiments, the blowing agent comprises about 1% to about 25% by weight cyclopentane. In some embodiments, the blowing agent comprises about 5% to about 15% by weight cyclopentane. In some embodiments, the blowing agent comprises about 5% to about 10% by weight cyclopentane.

[0027] In some embodiments, the blowing agent comprises up to about 45% cyclopentane by weight, e.g., up to about 40%, 30%, 25%, 20%, 15%, 10%, 5%, or 1% cyclopentane by weight, hi some embodiments, the blowing agent comprises up to about 20% cyclopentane by weight.

[0028] In some embodiments, the blowing agent comprises about 90% to about 5% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene, e.g., about 90% to about 10% by weight, about 90% to about 30% by weight, about 90% to about 50% by weight, about 90% to about 70% by weight, about 70% to about 5% by weight, about 70% to about 10% by weight, about 70% to about 30% by weight, about 70% to about 50% by weight, about 50% to about 5% by weight, about 50% to about 10% by weight, about 50% to about 30% by weight, about 30% to about 5% by weight, about 30% to about 10% by weight, or about 10% to about 5% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene.

[0029] In some embodiments, the blowing agent comprises about 75% to about 10% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. In some embodiments, the blowing agent comprises about 75% to about 50% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. In some embodiments, the blowing agent comprises about 60% to about 10% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. In some embodiments, the blowing agent comprises about 55% to about 35% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. In some embodiments, the blowing agent comprises about 50% to about 10% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. In some embodiments, the blowing agent comprises about 40% to about 15% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. In some embodiments, the blowing agent comprises about 30% to about 20% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. In some embodiments, the blowing agent comprises about 30% to about 10% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene.

[0030] In some embodiments, the blowing agent comprises up to about 95% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene, for example up to about 90%, 80%, 70%, 60%, 50%, 40%, 30%, 20%, or 10% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. In some embodiments, the blowing agent comprises up to about 80% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene.

[0031] In some embodiments, the blowing agent comprises up to about 80% by weight Z-1,1,1,4,4,4-hexafluoro-2-butene and up to about 20% by weight cyclopentane.

[0032] In some embodiments, the blowing agent consists essentially of Z-1,1,1,4,4,4-hexafluoro-2-butene and cyclopentane. In some embodiments, the blowing agent consists of Z-1,1,1,4,4,4-hexafluoro-2-butene and cyclopentane.

[0033] In some embodiments, the solubility of the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene and cyclopentane in the polymer is greater than the solubility of Z-1,1,1,4,4,4-hexafluoro-2-butene alone in the polymer. In some embodiments, the solubility of the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene and cyclopentane in the polymer is increased by more than about 10%, more than about 25%, more than about 50%, more than about 100%, more than about 100%, more than about 200%, more than about 300%, or more than about 400% compared to the solubility of Z-1,1,1,4,4,4-hexafluoro-2-butene alone in the polymer. In some embodiments, the solubility of the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene and cyclopentane in the polymer is increased by about 400% to about 500% compared to the solubility of Z-1,1,1,4,4,4-hexafluoro-2-butene alone in the polymer. In some embodiments, the solubility of the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene and cyclopentane in the polymer is increased by about 450% to about 475% compared to the solubility of Z-1,1,1,4,4,4-hexafluoro-2-butene alone in the polymer. In some embodiments, the solubility of the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene and cyclopentane in the polymer is increased by about 460% to about 470% compared to the solubility of Z-1,1,1,4,4,4-hexafluoro-2-butene alone in the polymer.

[0034] In some embodiments, the blowing agents provided herein further comprise HFC-152a.

[0035] In some embodiments, the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a is from about 5% to about 75% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene, e.g., from about 5% to about 60% by weight, from about 5% to about 50% by weight, from about 5% to about 40% by weight, from about 5% to about 20% by weight, from about 5% to about 10% by weight, from about 10% to about 75% by weight, from about 10% to about 6 ... % to about 50% by weight, about 10% to about 40% by weight, about 10% to about 20% by weight, about 20% to about 75% by weight, about 20% to about 60% by weight, about 20% to about 50% by weight, about 20% to about 40% by weight, about 40% to about 75% by weight, about 40% to about 60% by weight, about 40% to about 50% by weight, about 50% to about 75% by weight, about 50% to about 60% by weight, or about 60% to about 75% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene.

[0036] In some embodiments, the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a comprises about 75% to about 10% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. In some embodiments, the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a comprises about 75% to about 50% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. In some embodiments, the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a comprises about 10% to about 50% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. In some embodiments, the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a comprises about 30% to about 50% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. In some embodiments, the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a comprises about 55% to about 35% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. In some embodiments, the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a comprises about 30% to about 10% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. In some embodiments, the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a comprises about 15% to about 45% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. In some embodiments, the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a comprises about 35% to about 45% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. In some embodiments, the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a comprises about 20% to about 30% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene.In some embodiments, the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a comprises about 40% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene.

[0037] In some embodiments, the blowing agent, including Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a, is from about 1% by weight to about 45% by weight of cyclopentane, for example, from about 5% by weight to about 95% by weight of cyclopentane, for example, from about 5% by weight to about 80% by weight, from about 5% by weight to about 50% by weight, from about 5% by weight to about 25% by weight, from about 5% by weight to about 50 ... about 10% by weight, about 10% by weight to about 95% by weight, about 10% by weight to about 80% by weight, about 10% by weight to about 50% by weight, about 10% by weight to about 25% by weight, about 25% by weight to about 95% by weight, about 25% by weight to about 80% by weight, about 25% by weight to about 50% by weight, about 50% by weight to about 95% by weight, about 50% by weight to about 80% by weight, or about 80% by weight to about 95% by weight of cyclopentane.

[0038] In some embodiments, the blowing agent containing Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a contains about 1% to about 50% by weight of cyclopentane. In some embodiments, the blowing agent containing Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a contains about 2% to about 45% by weight of cyclopentane. In some embodiments, the blowing agent containing Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a contains about 10% to about 40% by weight of cyclopentane. In some embodiments, the blowing agent containing Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a contains about 15% to about 30% by weight of cyclopentane. In some embodiments, the blowing agent containing Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a contains about 1% to about 25% by weight of cyclopentane. In some embodiments, the blowing agent containing Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a contains about 10% to about 25% by weight of cyclopentane. In some embodiments, the blowing agent containing Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a contains about 15% to about 25% by weight of cyclopentane. In some embodiments, the blowing agent containing Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a contains about 5% to about 10% by weight of cyclopentane. In some embodiments, the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a comprises about 20% by weight cyclopentane.

[0039] In some embodiments, the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a comprises about 5% by weight to about 95% by weight of HFC-152a, e.g., about 5% by weight to about 80% by weight, about 5% by weight to about 50% by weight, about 5% by weight to about 25% by weight, about 5% by weight to about 10% by weight, about 10% by weight to about 95% by weight, about 10% by weight to about 80% by weight, about 10% by weight to about 50% by weight, about 10% by weight to about 25% by weight, about 25% by weight to about 95% by weight, about 25% by weight to about 80% by weight, about 25% by weight to about 50% by weight, about 50% by weight to about 95% by weight, about 50% by weight to about 80% by weight, or about 80% by weight to about 95% by weight of HFC-152a.

[0040] In some embodiments, the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a comprises about 5% to about 90% by weight of HFC-152a. In some embodiments, the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a comprises about 75% to about 85% by weight of HFC-152a. In some embodiments, the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a comprises about 50% to about 70% by weight of HFC-152a. In some embodiments, the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a comprises about 10% to about 55% by weight of HFC-152a. In some embodiments, the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a comprises about 20% to about 80% by weight of HFC-152a. In some embodiments, the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a comprises about 30% to about 50% by weight of HFC-152a. In some embodiments, the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a comprises about 1% to about 20% by weight of HFC-152a. In some embodiments, the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a comprises about 10% to about 50% by weight of HFC-152a. In some embodiments, the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a comprises about 35% to about 45% by weight of HFC-152a. In some embodiments, the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a comprises about 40% by weight HFC-152a.

[0041] In some embodiments, the solubility of the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a in the polymer is greater than the solubility of the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene and HFC-152a without cyclopentane in the polymer. In some embodiments, the solubility of the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a in the polymer is greater than the solubility of the blowing agent consisting essentially of Z-1,1,1,4,4,4-hexafluoro-2-butene and HFC-152a without cyclopentane in the polymer. In some embodiments, the solubility of the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a in the polymer is greater than the solubility of the blowing agent consisting of Z-1,1,1,4,4,4-hexafluoro-2-butene and HFC-152a in the polymer.

[0042] In some embodiments, the solubility of the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a in the polymer is increased by more than about 10%, more than about 20%, more than about 30%, more than about 40%, or more than about 50% compared to the solubility of the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene and HFC-152a in the polymer. In some embodiments, the solubility of the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a in the polymer is increased by about 10% to about 60% compared to the solubility of the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene and HFC-152a in the polymer. In some embodiments, the solubility of the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a in the polymer is increased by about 40% to about 60% compared to the solubility of the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene and HFC-152a in the polymer. In some embodiments, the solubility of the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a in the polymer is increased by about 45% to about 55% compared to the solubility of the blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene and HFC-152a in the polymer.

[0043] In some embodiments, the blowing agent consists essentially of Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a. In some embodiments, the blowing agent consists essentially of Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a.

[0044] In some embodiments, the blowing agent is about 10% to about 75% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene; about 2% to about 45% by weight of cyclopentane, and Contains about 90% to about 5% by weight of HFC-152a.

[0045] In some embodiments, the blowing agent is about 10% by weight to about 50% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene; about 5% to about 10% by weight of cyclopentane, and Contains about 75% to about 85% by weight of HFC-152a.

[0046] In some embodiments, the blowing agent is about 10% by weight to about 30% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene; about 15% to about 30% by weight of cyclopentane, and Contains about 50% to about 70% by weight of HFC-152a.

[0047] In some embodiments, the blowing agent is about 35% to about 55% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene; about 10% to about 40% by weight of cyclopentane, and Contains about 50% to about 70% by weight of HFC-152a.

[0048] In some embodiments, the blowing agent is about 50% to about 75% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene; about 10% to about 40% by weight of cyclopentane, and Contains about 10% to about 55% by weight of HFC-152a.

[0049] In some embodiments, the blowing agent is about 30% to about 50% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene; about 10% to about 30% by weight of cyclopentane, and Contains about 30% to about 50% by weight of HFC-152a.

[0050] In some embodiments, the blowing agent is about 35% to about 45% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene; about 15% to about 25% by weight of cyclopentane, and Contains about 35% to about 45% by weight of HFC-152a.

[0051] In some embodiments, the blowing agent is about 40% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene, About 20% by weight of cyclopentane, and It contains about 40% by weight of HFC-152a.

[0052] In some embodiments, the blowing agent is about 10% by weight to about 40% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene; about 50% to about 10% by weight of cyclopentane, and Contains about 50% to about 85% by weight of HFC-152a.

[0053] In some embodiments, the blowing agent is about 10% by weight to about 40% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene; about 6% to about 9% by weight of cyclopentane, and Contains about 54% to about 81% by weight of HFC-152a.

[0054] In some embodiments, the blowing agent is about 25% to about 35% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene; about 1% to about 10% by weight of cyclopentane, and Contains about 60% to about 70% by weight of HFC-152a.

[0055] In some embodiments, the blowing agent is about 25% to about 30% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene; about 5% to about 10% by weight of cyclopentane, and Contains about 60% to about 65% by weight of HFC-152a.

[0056] In some embodiments, the blowing agent is about 28% to about 30% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene; about 6% to about 8% by weight of cyclopentane, and Contains about 63% to about 65% by weight of HFC-152a.

[0057] In some embodiments, the blowing agent is about 29% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene; about 7% by weight of cyclopentane, and It contains about 64% by weight of HFC-152a.

[0058] In some embodiments, the blowing agent is about 80% by weight Z-1,1,1,4,4,4-hexafluoro-2-butene and about 20% by weight cyclopentane, or about 80% by weight Z-1,1,1,4,4,4-hexafluoro-2-butene, about 15% by weight cyclopentane, and about 5% by weight HFC-152a, or about 80% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene, about 10% by weight of cyclopentane, and about 10% by weight of HFC-152a, or about 80% by weight Z-1,1,1,4,4,4-hexafluoro-2-butene, about 5% by weight cyclopentane, and about 15% by weight HFC-152a, or about 70% by weight Z-1,1,1,4,4,4-hexafluoro-2-butene and about 30% by weight cyclopentane, or about 70% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene, about 20% by weight of cyclopentane, and about 10% by weight of HFC-152a, or about 70% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene, about 10% by weight of cyclopentane, and about 20% by weight of HFC-152a, or about 70% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene, about 5% by weight of cyclopentane, and about 25% by weight of HFC-152a, or about 60% by weight Z-1,1,1,4,4,4-hexafluoro-2-butene and about 40% by weight cyclopentane, or about 60% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene, about 30% by weight of cyclopentane, and about 10% by weight of HFC-152a, or about 60% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene, about 20% by weight of cyclopentane, and about 20% by weight of HFC-152a, or about 60% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene, about 10% by weight of cyclopentane, and about 30% by weight of HFC-152a, or about 60% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene, about 5% by weight of cyclopentane, and about 35% by weight of HFC-152a, or about 50% by weight Z-1,1,1,4,4,4-hexafluoro-2-butene and about 50% by weight cyclopentane, or about 50% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene, about 40% by weight of cyclopentane, and about 10% by weight of HFC-152a, or about 50% by weight Z-1,1,1,4,4,4-hexafluoro-2-butene, about 30% by weight cyclopentane, and about 20% by weight HFC-152a, or about 50% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene, about 20% by weight of cyclopentane, and about 30% by weight of HFC-152a, or about 50% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene, about 10% by weight of cyclopentane, and about 40% by weight of HFC-152a, or about 50% by weight Z-1,1,1,4,4,4-hexafluoro-2-butene, about 5% by weight cyclopentane, and about 45% by weight HFC-152a. about 40% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene, about 55% by weight of cyclopentane, and about 5% by weight of HFC-152a; about 40% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene, about 50% by weight of cyclopentane, and about 10% by weight of HFC-152a, or about 40% by weight Z-1,1,1,4,4,4-hexafluoro-2-butene, about 40% by weight cyclopentane, and about 20% by weight HFC-152a, or about 40% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene, about 30% by weight of cyclopentane, and about 30% by weight of HFC-152a, or about 40% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene, about 20% by weight of cyclopentane, and about 40% by weight of HFC-152a, or about 40% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene, about 10% by weight of cyclopentane, and about 50% by weight of HFC-152a, or It contains about 40% by weight Z-1,1,1,4,4,4-hexafluoro-2-butene, about 5% by weight cyclopentane, and about 55% by weight HFC-152a.

[0059] In some embodiments, the blowing agent comprises about 80% by weight Z-1,1,1,4,4,4-hexafluoro-2-butene and about 20% by weight cyclopentane.

[0060] In some embodiments, the blowing agent comprises about 40% by weight Z-1,1,1,4,4,4-hexafluoro-2-butene, about 20% by weight cyclopentane, and about 40% by weight HFC-152a.

[0061] Without being bound by theory, it is believed that blowing agent blends having lower HFO-1336mzz-Z content serve as low cost, low GWP replacements for existing XPS blowing agents while maintaining foam qualities such as heat resistance, while compositions containing higher HFO-1336mzz-Z content serve as low GWP XPS blowing agents that enable higher foam heat resistance while maintaining other foam quality attributes.

[0062] In some embodiments, the process of the present invention further comprises heating the polymer and blowing agent in the presence of one or more additives. Exemplary additives include, but are not limited to, nucleating agents, cell stabilizers, surfactants, preservatives, colorants, antioxidants, reinforcing agents, fillers, antistatic agents, IR attenuators, extrusion aids, plasticizers, and viscosity modifiers, or any combination thereof, in amounts to achieve the desired effect.

[0063] In some embodiments, the blowing agents provided herein are substantially free of additives, hi some embodiments, the blowing agents include one or more additives (e.g., 1, 2, 3, 4, or 5 additives).

[0064] In some embodiments, the process of the present invention is carried out in the presence of a nucleating agent, hi some embodiments, the nucleating agent is selected from talc, graphite, and magnesium silicate.

[0065] In some embodiments, the foamable composition further comprises a flame retardant. In some embodiments, the flame retardant comprises a polymeric flame retardant or a halogenated flame retardant. In some embodiments, the flame retardant is a brominated flame retardant or a chlorinated flame retardant. In some embodiments, the flame retardant is PolyFR.

[0066] In some embodiments, the foamable composition further comprises an infrared attenuating agent.

[0067] As used herein, the term "molten composition" refers to a foamable composition. The amount of blowing agent in the molten composition depends on the amount of additives other than the blowing agent and the density desired in the foamed product. In some embodiments, the amount of blowing agent in the foamable composition is about 5% to about 20% by weight. In some embodiments, the amount of blowing agent in the foamable composition is about 5% to about 15% by weight based on the weight of the foamable composition. It is understood that the weight percent of the blowing agent in the foamable composition can be adjusted based on the desired density of the foam and the ratio of the components in the blowing agent.

[0068] In some embodiments, the blowing agent is about 5 parts to about 25 parts per 100 parts by weight of the polymer, e.g., about 5 parts to about 20 parts, about 5 parts to about 15 parts, about 5 parts to about 10 parts, about 10 parts to about 25 parts, about 10 parts to about 20 parts, about 10 parts to about 15 parts, about 15 parts to about 25 parts, about 15 parts to about 20 parts, or about 20 parts to about 25 parts per 100 parts by weight of the polymer. In some embodiments, the blowing agent is about 7 parts to about 18 parts per 100 parts by weight of the polymer.

[0069] In some embodiments, the thermoplastic polymers provided herein are alkenyl aromatic polymers. As used herein, the term "alkenyl aromatic polymer" refers to a polymer formed from alkenyl-aromatic monomer units. In some embodiments, the alkenyl-aromatic monomer units are C 2~6 Alkenyl-C 6~10 In some embodiments, the alkenyl-aromatic monomeric unit is 2~6 alkenyl-phenyl monomeric units, wherein the phenyl is optionally substituted. In some embodiments, the alkenyl aromatic polymer is polystyrene.

[0070] The polystyrene may be a styrene homopolymer or may contain copolymerized monomers other than styrene (i.e., polystyrene copolymers). In some embodiments, the thermoplastic polymer comprises a blend of polystyrene and an additional thermoplastic polymer. In some embodiments, the additional thermoplastic polymer is a copolymer of styrene and a monomer other than styrene (e.g., acrylonitrile).

[0071] In some embodiments, the thermoplastic polymer is selected from polystyrene, polyethylene, polyethylene copolymers, polypropylene, polypropylene copolymers, acrylonitrile butadiene styrene, styrene acrylonitrile copolymers, and blends thereof. In some embodiments, the thermoplastic polymer is selected from polystyrene, polyethylene, and polypropylene. In some embodiments, the thermoplastic polymer is a polyethylene-polypropylene copolymer. In some embodiments, the thermoplastic polymer is polystyrene.

[0072] Whether the thermoplastic polymer being foamed is polystyrene or a blend of polystyrene with other thermoplastic polymers, in some embodiments styrene is the predominant polymerized monomer (unit) in the foamed thermoplastic polymer, hi some embodiments, polymerized units of styrene make up at least 70 mol%, at least 80 mol%, at least 90 mol%, or at least 100 mol% of the polymerized monomer units of the thermoplastic polymer.

[0073] When the thermoplastic polymer contains a styrene copolymer, the amount of additional monomer copolymerized with styrene is such that the styrene content of the copolymer is at least 60 mol % of the copolymer, at least 70 mol % of the copolymer, at least 80 mol %, or at least 90 mol % of the copolymer, based on the total moles of the copolymer (i.e., 100%). It is understood that these ratios apply whether the styrene copolymer is the only styrene-containing polymer in the thermoplastic polymer or is a blend with other thermoplastic polymers, such as styrene homopolymers or other styrene copolymers.

[0074] In some embodiments, the thermoplastic polymer comprises a styrene homopolymer (i.e., polystyrene homopolymer). When the thermoplastic polymer is a blend of polystyrene and other thermoplastic polymers as described above, the polystyrene component of the blend is, in some embodiments, a styrene homopolymer that constitutes at least 80% by weight of the combined weight of the polystyrene and other thermoplastic polymers.

[0075] The molecular weight of the thermoplastic polymer, including polystyrene, being expanded is high enough to provide the strength required for the foam application requirements. The strength requirement determines the minimum density of the expanded product. The high molecular weight of the thermoplastic polymer, including polystyrene, also contributes to the strength of the expanded product. An indication of molecular weight is the rate at which the molten polymer flows through a specified orifice under a specified load. The slower the flow rate, the higher the molecular weight. Melt flow rate measurements are made according to ASTM D 1238 at 200°C and using a load of 5 kg on the molten polymer. The weight of the molten polymer that flows through the orifice in a specified time allows the melt flow rate to be reported in g / 10 min. In some embodiments, the melt flow rate of the thermoplastic polymer, including polystyrene, is 20 g / 10 min or less, 15 g / 10 min or less, or 10 g / 10 min or less. In some embodiments, the minimum melt flow rate of all melt flow rates disclosed herein is at least 1 g / 10 min, whereby the melt flow rate ranges disclosed herein include, but are not limited to, 1-25, 1-20, 1-15, and 1-10 g / 10 min. In some embodiments, the melt flow rate is about 25 g / 10 min or less when measured according to the procedure of ASTM D 1238 at 200° C. using a 5 kg load on the molten polymer.

[0076] References to thermoplastic polymers, including polystyrene, also apply to polystyrene itself, so for example, the disclosure of thermoplastic polymers, including polystyrene, in the preceding paragraph can be substituted for polystyrene in the present disclosure.

[0077] In some embodiments, the process of the present invention further comprises the step of extruding a thermoplastic polymer to form a thermoplastic polymer foam comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and optionally HFC-152a.

[0078] In some embodiments, the extrusion is carried out at a die temperature of about 100°C to about 150°C, e.g., about 100°C to about 140°C, about 100°C to about 130°C, about 100°C to about 120°C, about 100°C to about 110°C, about 110°C to about 150°C, about 110°C to about 140°C, about 110°C to about 130°C, about 110°C to about 120°C, about 120°C to about 150°C, about 120°C to about 140°C, about 120°C to about 130°C, about 130°C to about 150°C, about 130°C to about 140°C, or about 140°C to about 150°C. In some embodiments, the extrusion is carried out at a temperature of about 110°C to about 140°C. In some embodiments, the extrusion is carried out at a temperature of about 120°C to about 130°C.

[0079] In some embodiments, the process of the present invention is carried out in an extruder to 1) form the foamable composition into a desired form and 2) extrude the foamable composition to form a thermoplastic polymer foam comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and optionally HFC-152a.

[0080] When the process of the present invention is carried out in an extruder, the thermoplastic polymer forms the feedstock to the extruder. In some embodiments, the blowing agent and co-blowing agent are fed into the extruder at a location intermediate the feed end and the extrusion end of the extruder, typically to the foamable composition created when the extrusion screw advances the feedstock along the length of the extruder. Additional additives may be added when convenient, as may be determined by the state of the additives. For example, solid additives may be conveniently added to the extruder at the feed end of the extruder, possibly as a mixture with the polymer feedstock in particulate form. The foamable composition obtained in the extruder is extruded through a die, thereby expanding the foamable composition into a foamed product of the desired shape (e.g., sheet, plate, rod, or tube), and then cooled.

[0081] The "melt mixing zone" is the area in the extruder where the composition melts to form a molten composition. This melting occurs due to the input of heat and the heat generated in the mixing process to form the melt. In some embodiments, the temperature of the melt mixing zone is at least 185°C, at least 190°C, at least 200°C, or at least 210°C. In some embodiments, the maximum temperature for all melt mixing temperatures disclosed herein is 250°C. The melt mixing temperatures disclosed herein are the temperatures of the melt in the mixing zone during mixing. In some embodiments, the pressure at which melt mixing is performed is at least 1750 psi, at least 2000 psi, at least 2500, at least 3000 psi (207 bar), at least 3500 psi (241 bar), or at least 4000 psi (276 bar). In some embodiments, the maximum for all disclosed minimum pressures at which melt mixing is performed is 5000 psi (345 bar) or less. The pressures disclosed herein are gauge pressures.

[0082] In the region within the extruder where the molten composition is extruded, the molten composition is cooled such that the temperature at which extrusion occurs is, in some embodiments, at least 105° C., at least 110° C., or at least 125° C. In some embodiments, the maximum for all minimum extrusion temperatures disclosed herein is no greater than 140° C. The extrusion temperatures disclosed herein are the temperatures of the melt as it is extruded.

[0083] In some embodiments, extrusion is carried out at a pressure of at least 750 psi, at least 1000 psi, at least 1250 psi, 1500 psi (103 bar), or at least 1600 psi (110 bar). The maximum for the minimum extrusion pressure disclosed herein is, in some embodiments, no greater than 2000 psi (138 bar). The extrusion pressure is the pressure inside the extrusion die.

[0084] In some embodiments, the process is carried out at a pressure just prior to foaming of about 100 psi to about 5000 psi, e.g., about 100 psi to about 4000 psi, about 100 psi to about 3000 psi, about 100 psi to about 2000 psi, about 100 psi to about 1000 psi, about 750 psi to about 1250 psi, about 1000 psi to about 5000 psi, about 1000 psi to about 4000 psi, about 1000 psi to about 3000 psi, about 1000 psi to about 2000 psi, about 2000 psi to about 5000 psi, about 2000 psi to about 4000 psi, about 2000 psi to about 3000 psi, about 3000 psi to about 5000 psi, about 3000 psi to about 4000 psi, or about 4000 psi to about 5000 psi. In some embodiments, the process is carried out at a pressure just below foaming of about 500 psi to about 4000 psi. In some embodiments, the process is carried out at a pressure just below foaming of about 800 psi to about 3000 psi. In some embodiments, the process is carried out at a pressure just below foaming of about 1000 psi to about 2500 psi.

[0085] The above disclosure of multiple ranges for melt flow rate, temperature, and pressure can be used in any combination in the practice of the present invention to obtain a particular foam structure desired. For example, a melt mixing pressure of 3000-5000 psi (207-345 bar) can be used to obtain a foam product with low bubble density, and this pressure range can be used with any of the melt mixing and extrusion temperature ranges to form any of the smooth skin closed cell foam product densities disclosed herein. The same is true for the melt extrusion pressure range of 1500-2000 psi (103-138 bar) along with the pressure range of 3000-5000 psi (207-345 bar) for melt mixing. In some embodiments, the two pressure ranges for melt mixing (207-345 bar) and extrusion (103-138 bar) are used together. Any melt flow rate of the polymer being foamed (eg, at least 1, and up to 25, 20, 15, or 10 g / 10 min) can be used with any combination of pressure and temperature depending on the foam product result desired.

[0086] When the process of the present invention is carried out in an extruder, the thermoplastic polymer (i.e., the foamable composition) is cooled such that the temperature at which extrusion occurs is, in some embodiments, at least 125°C or at least 130°C. In some embodiments, the temperature at which extrusion occurs is lower than the first temperature of the process of the present invention. In some embodiments, the maximum for all minimum extrusion temperatures disclosed herein is about 150°C or less. In some embodiments, the extrusion occurs at a temperature of about 100°C to about 150°C. In some embodiments, the extrusion occurs at a temperature of about 110°C to about 140°C.

[0087] In some embodiments, the extrusion temperature disclosed herein is the temperature of the polymer melt during extrusion.

[0088] When the process of the present invention is carried out in an extruder, extrusion is carried out at a pressure of at least 750 psi, or at least 1000 psi, or at least 1250 psi, or at least 1500 psi (103 bar), or at least 1600 psi (110 bar), in some embodiments. The maximum for the minimum extrusion pressure disclosed herein is, in some embodiments, no greater than 2000 psi (138 bar). In some embodiments, extrusion is carried out at a pressure of about 1500 psi to about 2000 psi. In some embodiments, the extrusion pressure disclosed herein is the pressure inside the extrusion die.

[0089] In some embodiments, the extrusion is carried out at a pressure of about 100 psi to about 5000 psi, e.g., about 100 psi to about 4000 psi, about 100 psi to about 2000 psi, about 100 psi to about 1000 psi, about 750 psi to about 1250 psi, about 1000 psi to about 5000 psi, about 1000 psi to about 4000 psi, about 1000 psi to about 2000 psi, about 2000 psi to about 5000 psi, about 2000 psi to about 4000 psi, or about 4000 psi to about 5000 psi.

[0090] In some embodiments, the extrusion is carried out at a pressure of from about 500 psi to about 4000 psi.

[0091] In some embodiments, the extrusion is carried out at a pressure of from about 750 psia to about 3000 psia.

[0092] In some embodiments, the extrusion is carried out at a pressure of from about 900 psia to about 2750 psia.

[0093] In some embodiments, the present application provides foam products (eg, thermoplastic polymer foams) prepared according to one or more of the processes described herein.

[0094] In some embodiments, the foam comprises: (a) a thermoplastic polymer selected from the group consisting of polystyrene homopolymer, polystyrene copolymer, and styrene-acrylonitrile copolymer, or blends thereof; (b) a blowing agent provided herein (i.e., a blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and optionally HFC-152a); and Includes.

[0095] In some embodiments, the foam comprises: (a) a thermoplastic polymer selected from the group consisting of polystyrene homopolymer, polystyrene copolymer, and styrene-acrylonitrile copolymer, or blends thereof; (b) a blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene and cyclopentane as provided herein; Includes.

[0096] In some embodiments, the foam comprises: (a) a thermoplastic polymer selected from the group consisting of polystyrene homopolymer, polystyrene copolymer, and styrene-acrylonitrile copolymer, or blends thereof; (b) a blowing agent comprising Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a as provided herein; Includes.

[0097] In some embodiments, the foams provided herein further comprise one or more additives described herein.

[0098] It is understood that the blowing agent blends, additives, melt flow rates, temperatures, pressures, and other process parameters described herein may be used in any combination in the practice of the present invention to obtain the particular foam structure desired.

[0099] In some embodiments, the thermoplastic polymer foams provided herein include one or more of the following properties: Closed Cells - at least 70%, at least 80%, at least 90%, or at least 95% closed cells. Closed cell content can be measured according to ASTM method D6226-05. Average bubble size: about 0.005 mm to about 5 mm (i.e., 5 μm to about 5000 μm), for example, about 0.01 mm to about 5 mm, about 0.05 mm to about 5 mm, about 0.05 mm to about 0.5 mm. In some embodiments, the average bubble size is about 0.01 mm to about 1 mm. In some embodiments, the average bubble size is about 0.02 mm to about 0.5 mm. In some embodiments, the average bubble size is about 0.1 mm to about 0.3 mm. ·Density: Approx. 60kg / m 3 Below, approximately 45kg / m 3 Below, about 40kg / m 3 Below, about 35kg / m 3 or less than 23 kg / m 3 Density can be measured according to ISO method 845 85. -Smooth skin. Virtually free of blowholes. EXAMPLES

[0100] The present invention will now be described in more detail with reference to specific examples. The following examples are provided for illustrative purposes and are not intended to limit the present invention in any way.

[0101] Example 1. Solubility of HFO-1336mzz-Z / Cyclopentane Blends in Softened Polystyrene Homopolymer This example shows that the solubility of Z-1,1,1,4,4,4-hexafluoro-2-butene (i.e., HFO-1336mzz-Z) / cyclopentane blends in softened polystyrene is improved compared to the solubility of neat HFO-1336mzz-Z in softened polystyrene.

[0102] The solubility of HFO-1336mzz-Z and HFO-1336mzz-Z / cyclopentane blends containing 20 wt. % cyclopentane in softened polystyrene was determined by the following procedure: Approximately 78 g of polystyrene was charged to a 125 cc stainless steel Parr© reactor. The reactor was weighed, attached to inlet / outlet piping, immersed in an oil bath, and evacuated. A quantity of blowing agent in excess of the expected solubility was charged to the evacuated reactor using a HIP pressure generator (manufactured by High Pressure Equipment Company). The oil bath was heated and maintained at a temperature of 179° C. for 30 minutes, after which the final pressure was recorded. The Parr© reactor was removed from the oil bath and allowed to cool to room temperature. After venting or releasing the excess (undissolved in polystyrene) blowing agent, the reactor (with resolidified polystyrene inside) was weighed. The weight gain was recorded as the solubility according to the following formula: Formula 1. Solubility (wt%) = (increase in resin weight ÷ 78) × 100.

[0103] Unexpectedly, blends of HFO-1336mzz-Z with cyclopentane were found to exhibit solubilities in softened polystyrene that significantly exceeded the solubility of neat HFO-1336mzz-Z at the same conditions (Figure 1). For example, the solubility of neat HFO-1336mzz-Z in softened polystyrene homopolymer with a melt flow index (MFI) of 5.0 g / 10 min at 179°C and 1,374 psia was estimated to be 5.7 g / 100 g of polystyrene (5.7 phr). In contrast, the solubility of the HFO-1336mzz-Z / cyclopentane blend containing 20 wt% cyclopentane was 32.24 g / 100 g of polystyrene in the same polystyrene at the same temperature and pressure, i.e., 465.6% higher than the solubility of neat HFO-1336mzz-Z.

[0104] Example 2. Solubility of HFO-1336mzz-Z / HFC-152a / Cyclopentane Blends in Softened Polystyrene Homopolymer This example shows that the solubility of Z-1,1,1,4,4,4-hexafluoro-2-butene / HFC-152a / cyclopentane blends in softened polystyrene is improved compared to the solubility of HFO-1336mzz-Z / HFC-152a blends in softened polystyrene.

[0105] The solubilities in softened polystyrene of HFO-1336mzz-Z / HFC-152a (50 wt% / 50 wt%) blends and HFO-1336mzz-Z / HFC-152a / cyclopentane blends containing 40 wt% HFO-1336mzz-Z, 40 wt% HFC-152a, and 20 wt% cyclopentane were determined according to the procedure described in Example 1.

[0106] Unexpectedly, blends of HFO-1336mzz-Z with HFC-152a and cyclopentane were found to exhibit solubilities in softened polystyrene that significantly exceeded those of binary blends of HFO-1336mzz-Z with HFC-152a at similar conditions (Figure 2). For example, the solubility of a binary blend of HFO-1336mzz-Z / HFC-152a (50 wt% / 50 wt%) in softened polystyrene homopolymer having a melt flow index (MFI) of 5.0 g / 10 min at 179°C and 2980 psia was estimated to be 11.8 g / 100 g of polystyrene (11.8 phr). In contrast, the solubility of an HFO-1336mzz-Z / HFC-152a / cyclopentane blend, containing 40 wt. % HFO-1336mzz-Z, 40 wt. % HFC-152a, and 20 wt. % cyclopentane, showed a solubility of 17.83 g / 100 g of polystyrene in the same polystyrene at the same temperature and similar pressure (2968 psia), i.e., 51.1% higher than the solubility of the binary HFO-1336mzz-Z / HFC-152a blend.

[0107] Example 3. Polystyrene Foam Extrusion Using HFO-1336mzz-Z / HFC-152a / Cyclopentane Blend as Blowing Agent This example shows the reduction in XPS foam density resulting from the addition of cyclopentane to a blowing agent blend containing HFO-1336mzz-Z and HFC-152a. The polystyrene was a styrene homopolymer (Total Petrochemicals, PS 535B) with a melt flow rate of 4 g / 10 min. A nucleating agent (talc) was present with the polystyrene and blowing agent in the molten composition formed in the extruder.

[0108] A 50 mm twin screw laboratory extruder with nine independently controlled, electrically heated zones was used. The first four zones of the extruder were used to heat and soften the polymer. The remaining barrel section from the blowing agent injection location to the end of the extruder was set at the selected, lower temperature. A rod die with a 3 mm opening was used to extrude the foam rod samples. The results are summarized in Table 1.

[0109] [Table 1] * Parts per 100 parts of polystyrene resin (mass)

[0110] The results in Table 1 show that when the Z-HFO-1336mzz / HFC-152a / cyclopentane blend containing 10.7 wt. % cyclopentane is used as the blowing agent, it is possible to form an extruded polystyrene foam having a density about 13.6% lower than that obtained with a foamed blend containing Z-HFO-1336mzz and HFC-152a at a mass ratio of Z-HFO-1336mzz to HFC-152a (about 0.72) similar to the mass ratio of Z-HFO-1336mzz to HFC-152a in the Z-HFO-1336mzz / HFC-152a / cyclopentane blend (about 0.74).

[0111] Other embodiments 1. A process for preparing a thermoplastic polymer foam, comprising: (a) providing a foamable composition comprising a thermoplastic polymer and a blowing agent, the blowing agent comprising about 95% to about 1% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene and about 1% to about 95% by weight of cyclopentane; (b) expanding the foamable composition to produce a thermoplastic polymer foam; The process includes: 2. The process of embodiment 1, wherein the solubility of the blowing agent in the polymer is greater than the solubility of Z-1,1,1,4,4,4-hexafluoro-2-butene alone in the polymer. 3. The process of any one of the preceding claims, wherein the blowing agent comprises about 75% to about 10% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. 4. The process of any one of the preceding claims, wherein the blowing agent comprises about 50% to about 10% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. 5. The process of any one of the preceding embodiments, wherein the blowing agent comprises about 2% to about 45% by weight of cyclopentane. 6. The process of any one of the preceding embodiments, wherein the blowing agent comprises about 15% to about 25% by weight of cyclopentane. 7. The process of any one of the preceding claims, wherein the blowing agent comprises up to about 80% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene and up to about 20% by weight of cyclopentane. 8. The process of any one of the preceding embodiments, wherein the blowing agent consists essentially of Z-1,1,1,4,4,4-hexafluoro-2-butene and cyclopentane. 9. The process of any one of the preceding embodiments, wherein the blowing agent further comprises HFC-152a. 10. The process of embodiment 9, wherein the solubility of the blowing agent in the polymer is greater than the solubility of Z-1,1,1,4,4,4-hexafluoro-2-butene alone in the polymer. 11. The process of any one of embodiments 9 to 10, wherein the blowing agent comprises about 75% to about 10% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. 12. The process of any one of embodiments 9 to 10, wherein the blowing agent comprises about 50% to about 10% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. 13. The process of any one of embodiments 9-12, wherein the blowing agent comprises about 2% to about 45% by weight of cyclopentane. 14. The process of any one of embodiments 9-13, wherein the blowing agent comprises about 5% to about 90% by weight of HFC-152a. 15. The process of any one of embodiments 9 to 13, wherein the blowing agent comprises about 75% to 85% by weight of HFC-152a. 16. The process of any one of embodiments 9-15, wherein the blowing agent consists essentially of Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a. 17. The process of any one of the preceding embodiments, wherein the thermoplastic polymer is an alkenyl aromatic polymer. 18. The process of any one of the preceding embodiments, wherein the thermoplastic polymer is selected from the group consisting of polystyrene, polyethylene homopolymer, polyethylene copolymer, polypropylene homopolymer, polypropylene copolymer, acrylonitrile butadiene styrene, and styrene acrylonitrile copolymer, and blends thereof. 19. The process of any one of the preceding embodiments, wherein the thermoplastic polymer is selected from the group consisting of polystyrene homopolymer, polystyrene copolymer, styrene-acrylonitrile copolymer, and blends thereof. 20. The process of any one of the preceding embodiments, wherein the process is carried out at a pressure just below foaming of about 100 psi to about 5000 psi. 21. The process of any one of the preceding embodiments, wherein the process is carried out at a pressure just below foaming of about 1000 psi to about 2500 psi. 22. The process of any one of the preceding embodiments, further comprising extruding a thermoplastic polymer to form a thermoplastic polymer foam. 23. The process of embodiment 22, wherein the extrusion is carried out at a die temperature of about 100°C to about 150°C. 24. The process of embodiment 22, wherein the extrusion is carried out at a die temperature of about 110°C to about 140°C. 25. The process of embodiment 22, wherein the extrusion is carried out at a die temperature of about 120°C to about 130°C. 26. The process of any one of the preceding embodiments, wherein the polymer foam is a closed-cell polymer foam. 27. The process of any one of the preceding embodiments, wherein the polymer comprises at least 70% closed cells. 28. The process of any one of the preceding embodiments, wherein the polymer foam is a smooth-skin polymer foam. 29. The process of any one of the preceding embodiments, wherein the polymer foam is substantially free of blowholes. 30. The process of any one of embodiments 1-16-19-29, wherein the polymer is a polystyrene homopolymer. 31. The process of any one of the preceding embodiments, wherein the foamable composition further comprises a nucleating agent. 32. The process of embodiment 31, wherein the nucleating agent is selected from the group consisting of talc, graphite, and magnesium silicate. 33. The process of any one of the preceding embodiments, wherein the foamable composition further comprises a flame retardant. 34. The process of embodiment 33, wherein the flame retardant comprises a polymeric flame retardant or a halogenated flame retardant. 35. The process of embodiment 33, wherein the flame retardant is a brominated flame retardant or a chlorinated flame retardant. 36. The process of embodiment 33, wherein the flame retardant is PolyFR. 37. The process of any one of the preceding embodiments, wherein the foamable composition further comprises an infrared attenuating agent. 38. The process of any one of the preceding embodiments, wherein the blowing agent is from about 5 parts to about 25 parts per 100 parts by weight of the polymer. 39. The process of any one of the preceding embodiments, wherein the blowing agent is from about 7 parts to about 18 parts per 100 parts by weight of the polymer. 40. The present application further provides a thermoplastic polymer foam, the thermoplastic polymer foam comprising: (a) a thermoplastic polymer selected from the group consisting of polystyrene homopolymer, polystyrene copolymer, and styrene-acrylonitrile copolymer, or blends thereof; (b) a blowing agent comprising 95% by weight to 1% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene and 1% by weight to 95% by weight of cyclopentane; Includes. 41. The thermoplastic polymer foam of embodiment 40, wherein the blowing agent comprises about 75% to about 10% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. 42. The thermoplastic polymer foam of embodiment 40, wherein the blowing agent comprises about 50% to about 10% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. 43. The thermoplastic polymer foam of embodiment 40, wherein the blowing agent comprises about 25% to about 15% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. 44. The thermoplastic polymer foam of any one of embodiments 40-43, wherein the blowing agent comprises about 2% to about 45% by weight of cyclopentane. 45. The thermoplastic polymer foam of any one of embodiments 40-43, wherein the blowing agent comprises about 15% to about 25% by weight of cyclopentane. 46. ​​The thermoplastic polymer foam of embodiment 40, wherein the blowing agent comprises up to about 80% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene and up to about 20% by weight of cyclopentane. 47. The thermoplastic polymer foam of any one of embodiments 40-46, wherein the blowing agent consists essentially of Z-1,1,1,4,4,4-hexafluoro-2-butene and cyclopentane. 48. The thermoplastic polymer foam of embodiment 40, wherein the blowing agent further comprises HFC-152a. 49. The thermoplastic polymer foam of embodiment 48, wherein the blowing agent comprises about 75% to about 10% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. 50. The thermoplastic polymer foam of embodiment 48, wherein the blowing agent comprises about 50% to about 10% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene. 51. The thermoplastic polymer foam of any one of embodiments 48-50, wherein the blowing agent comprises about 2% to about 45% by weight of cyclopentane. 52. The thermoplastic polymer foam of any one of embodiments 48-51, wherein the blowing agent comprises about 5% to about 90% by weight of HFC-152a. 53. The thermoplastic polymer foam of any one of embodiments 48-51, wherein the blowing agent comprises about 75% to 85% by weight of HFC-152a. 54. The thermoplastic polymer foam of any one of embodiments 48-53, wherein the blowing agent consists essentially of Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a. 55. The polymer has a strength of approximately 64 kg / m according to ISO method 845-85. 3 55. The thermoplastic polymer foam of any one of embodiments 40-54, having a density of less than 56. The polymer has a strength of approximately 48 kg / m according to ISO method 845-85. 3 55. The thermoplastic polymer foam of any one of embodiments 40-54, having a density of less than 57. The foam is approximately 40 kg / m according to ISO method 845-85. 3 55. The thermoplastic polymer foam of any one of embodiments 40-54, having a density of less than 58. The polymer has a strength of approximately 35 kg / m according to ISO method 845-85. 3 55. The thermoplastic polymer foam of any one of embodiments 40-54, having a density of less than 59. The polymer has a strength of approximately 29 kg / m according to ISO method 845-85. 3 55. The thermoplastic polymer foam of any one of embodiments 40-54, having a density of less than 60. The polymer has a strength of approximately 25 kg / m according to ISO method 845-85. 3 55. The thermoplastic polymer foam of any one of embodiments 40-54, having a density of less than 61. The thermoplastic polymer foam of any one of embodiments 40-60, wherein the polymer has a melt flow rate of less than about 25 g / 10 min. 62. The thermoplastic polymer foam of any one of embodiments 40-61, which is a closed-cell polymer foam. 63. The thermoplastic polymer foam of any one of embodiments 40-62, which is a smooth-skin polymer foam. 64. The thermoplastic polymer foam of any one of embodiments 40 to 63, wherein the polymer foam is substantially free of blowholes. 65. The thermoplastic polymer foam of any one of embodiments 40-64, wherein the foam comprises at least 70% closed cells. 66. The thermoplastic polymer foam of any one of embodiments 40 to 65, wherein the average cell size of the foam is from about 1 micrometer to about 5,000 micrometers. 67. The thermoplastic polymer foam of any one of embodiments 40-66, wherein the average cell size of the foam is from about 10 micrometers to about 5,000 micrometers. 68. The thermoplastic polymer foam of any one of embodiments 40-66, wherein the average cell size of the foam is from about 100 micrometers to about 300 micrometers. 69. The thermoplastic polymer foam of any one of embodiments 40-68, wherein the foam is a polystyrene foam. 70. The thermoplastic polymer foam of any one of embodiments 40-68, wherein the foam is a styrene / acrylonitrile copolymer foam.

[0112] Although the present invention has been described in conjunction with its detailed description, it should be understood that the foregoing description is intended to illustrate, but not to limit, the scope of the invention as defined by the appended claims. Other aspects, advantages, and modifications are within the scope of the following claims. It should be understood by those skilled in the art to which the present invention pertains that any of the features described herein with respect to any particular aspect and / or embodiment of the present invention can be combined with any one or more of the other features of any other aspect and / or embodiment of the present invention described herein, with appropriate modifications to ensure compatibility of the combination. Such combinations are considered to be part of the invention contemplated by this disclosure.

Claims

1. 1. A process for preparing a thermoplastic polymer foam comprising: (a) providing a foamable composition comprising a thermoplastic polymer and a blowing agent, the blowing agent comprising 95% to 1% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene, 1% to 95% by weight of cyclopentane and HFC-152a; (b) expanding the foamable composition to produce the thermoplastic polymer foam; Including, The process wherein the thermoplastic polymer is selected from the group consisting of polystyrene homopolymer, polystyrene copolymer, styrene-acrylonitrile copolymer, and blends thereof.

2. 2. The process of claim 1, wherein the solubility of the blowing agent in the polymer is greater than the solubility of a mixture of Z-1,1,1,4,4,4-hexafluoro-2-butene and HFC-152a in the polymer.

3. 2. The process of claim 1, wherein the blowing agent comprises 50% to 10% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene.

4. 2. The process of claim 1, wherein the blowing agent comprises 5% to 90% by weight of HFC-152a.

5. 2. The process of claim 1, wherein the blowing agent comprises 35% to 45% by weight of HFC-152a.

6. 2. The process of claim 1, wherein the blowing agent consists of Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a.

7. 10. The process of claim 1, wherein the process is carried out at a pressure just below foaming of 750 psi to 2500 psi.

8. 10. The process of claim 1, further comprising extruding the thermoplastic polymer to form the thermoplastic polymer foam, wherein the extrusion is carried out at a die temperature of from 100°C to 150°C.

9. The process of claim 8, wherein the extrusion is carried out at a die temperature of from 120°C to 130°C.

10. The process of claim 1 , wherein the polymer foam is a closed-cell polymer foam.

11. 11. The process of claim 10, wherein the polymer foam is free of blowholes.

12. The process of claim 1 , wherein the foamable composition further comprises a nucleating agent.

13. The process of claim 1 , wherein the foamable composition further comprises a flame retardant.

14. The process of claim 1, wherein the blowing agent is from 1 part to 25 parts per 100 parts by weight of polymer.

15. (a) a thermoplastic polymer selected from the group consisting of polystyrene homopolymer, polystyrene copolymer, and styrene-acrylonitrile copolymer, or blends thereof; (b) a blowing agent comprising 95% by weight to 1% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene, 1% by weight to 95% by weight of cyclopentane and HFC-152a; 1. A thermoplastic polymer foam comprising:

16. 16. The thermoplastic polymer foam of claim 15, wherein the blowing agent comprises 50% to 10% by weight of Z-1,1,1,4,4,4-hexafluoro-2-butene.

17. 16. The thermoplastic polymer foam of claim 15, wherein the blowing agent comprises 2% to 45% by weight cyclopentane.

18. 16. The thermoplastic polymer foam of claim 15, wherein the blowing agent comprises 5% to 90% by weight of HFC-152a.

19. 16. The thermoplastic polymer foam of claim 15, wherein the blowing agent consists of Z-1,1,1,4,4,4-hexafluoro-2-butene, cyclopentane, and HFC-152a.

20. 16. The thermoplastic polymer foam of claim 15, wherein the polymer has a melt flow rate of less than 25 g / 10 min according to ASTM D 1238.

Citation Information

Patent Citations

  • Azeotrope and azeotropic compositions of Z-1,1,1,4,4,4-hexafluoro-2-butene

    JP2010526171A

  • Z-1,1,1,4,4,4-Hexafluoro-2-butene, trans-1,2-dichloroethylene, and azeotropic and azeotropic-like compositions of a third component.

    JP2012531495A

  • Composition and use of cis-1,1,1,4,4,4-hexafluoro-2-butene

    JP2013514450A