Method for producing ion-exchanged glass, mixture for ion exchange, and apparatus for producing ion-exchanged glass
By using alkali metal silicates to manage ion concentration in molten salt during ion exchange, the method addresses productivity and equipment corrosion issues, ensuring high-quality ion exchange glass production.
Patent Information
- Application Number
- JP2020184443
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-05-25
- Filing Date
- 2020-11-04
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2040-11-04
AI Technical Summary
The accumulation of eluted ions in molten salt during ion exchange treatment leads to increased concentration, reducing productivity and causing equipment corrosion and defects in ion exchange glass products.
Incorporating an alkali metal silicate with a larger ionic radius than the eluted ions into the molten salt, along with a controlled addition based on stress measurements, to maintain ion balance and prevent equipment corrosion.
This approach maintains product quality and productivity by stabilizing ion exchange conditions, preventing equipment deterioration and reducing defects in ion exchange glass.
Smart Images

Figure 0007569007000003 
Figure 0007569007000004 
Figure 0007569007000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing ion-exchanged glass, an apparatus for producing ion-exchanged glass, and a mixture for ion exchange. [Background technology]
[0002] In recent years, chemically strengthened glass that has been ion-exchanged has been used for the cover glass of display devices. Such ion-exchange treatment is generally performed by immersing glass in a molten salt and exchanging ions in the glass and ions in the molten salt, which have different ionic radii. For example, ion-exchange treatment is performed by dissolving Li ions in the glass into the molten salt and introducing Na ions or K ions in the molten salt into the glass, or by dissolving Na ions in the glass into the molten salt and introducing K ions in the molten salt into the glass.
[0003] In the mass production process of ion-exchanged glass, such an ion exchange process is repeatedly performed on multiple lots of glass using the same molten salt. As a result, ions eluted from the glass (hereinafter referred to as eluted ions) gradually accumulate in the molten salt, and the concentration of the eluted ions in the molten salt gradually increases. If the concentration of the eluted ions becomes excessively high, the above-mentioned ion exchange process becomes difficult to proceed, resulting in a problem of reduced productivity.
[0004] In order to solve such problems, a technique for adjusting the concentration of eluted ions by adding a phosphate to the molten salt has been developed (for example, Patent Document 1). In the technique disclosed in Patent Document 1, an alkali metal phosphate such as Na3PO4 or K3PO4 is added to the molten salt, and the phosphate absorbs the eluted ions in the molten salt, thereby suppressing an increase in the concentration of eluted ions in the molten salt. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] US Patent Application Publication No. 2018 / 0362399 Summary of the Invention [Problem to be solved by the invention]
[0006] However, when phosphate is added as in Patent Document 1, there is a problem that metals constituting equipment such as the molten salt tank and the jig for holding the glass are corroded by the phosphate, which makes the production equipment more susceptible to deterioration. In addition, there is a risk that the corroded metal will adhere to the glass, causing defects in the ion-exchanged glass products produced.
[0007] An object of the present invention is to provide a method for producing ion-exchanged glass, a mixture for ion exchange, and an apparatus for producing ion-exchanged glass, which are capable of maintaining product quality, i.e., high productivity, while preventing deterioration of production equipment. [Means for solving the problem]
[0008] The method for producing ion-exchanged glass according to the present invention comprises a step of immersing a part or the whole of ion-exchange glass containing an alkali metal component in an ion-exchange mixture to perform ion exchange treatment, and is characterized in that the ion-exchange mixture contains a molten salt and an alkali metal silicate as an additive, and the alkali metal silicate contains an alkali metal component that is ion-exchangeable with an alkali metal component that dissolves from the ion-exchange glass into the molten salt during ion exchange.
[0009] In the method for producing ion-exchanged glass according to the present invention, it is preferable that the alkali metal silicate contains an alkali metal component having a larger ionic radius than the alkali metal component eluted from the ion-exchange glass into the molten salt during ion exchange treatment, the alkali metal component eluted from the ion-exchange glass into the molten salt during ion exchange treatment is Li ion, and the alkali metal silicate contains at least one type selected from Na2SiO3, Na4SiO4, Na2Si2O5, and Na2Si4O9.
[0010] In the method for producing ion-exchanged glass according to the present invention, it is preferable that the glass for ion exchange is an alkali aluminosilicate glass containing 1.0 mol % or more of Li2O as a composition, and the molten salt contains one or more selected from NaNO3 and KNO3.
[0011] In the method for producing ion-exchanged glass according to the present invention, it is preferable that the alkali metal component eluted from the ion-exchange glass into the molten salt during ion exchange treatment is Na ion, and the alkali metal silicate contains at least one selected from K2SiO3, K4SiO4, K2Si2O5, and K2Si4O9.
[0012] In the method for producing ion-exchanged glass according to the present invention, it is preferable that the alkali metal component eluted from the ion-exchange glass into the molten salt during the ion exchange treatment is Na ion, and the alkali metal silicate contains at least one selected from Li2SiO3, Li4SiO4, Li2Si2O5, and Li2Si4O9.
[0013] In the method for producing ion-exchanged glass according to the present invention, it is preferable that the glass for ion exchange is an alkali aluminosilicate glass containing 1.0 mol % or more of Na2O as a composition, and the molten salt contains KNO3.
[0014] In the method for producing ion-exchanged glass according to the present invention, the alkali metal silicate is preferably a powdered alkali metal silicate crystal.
[0015] In the method for producing ion-exchanged glass according to the present invention, the powdered alkali metal silicate preferably has an average particle size D50 of 10 to 1000 μm.
[0016] The method for producing ion-exchanged glass according to the present invention preferably further comprises the step of stirring the molten salt after adding the alkali metal silicate to the molten salt.
[0017] In the method for producing ion-exchanged glass according to the present invention, the amount of alkali metal silicate added is preferably 0.1 to 30 parts by mass relative to 100 parts by mass of the molten salt.
[0018] In the method for producing ion-exchanged glass according to the present invention, it is preferable to further include a step of performing the ion exchange treatment multiple times by successively immersing a plurality of different lots of ion-exchange glass in a molten salt, and measuring the stress characteristics of the ion-exchanged glass obtained after the ion exchange treatment of a predetermined lot of ion-exchanged glass, and a step of determining whether or not to add an alkali metal silicate to the molten salt depending on the measurement results of the stress characteristics.
[0019] In the method for producing ion-exchanged glass according to the present invention, it is preferable that, as a stress characteristic, the surface compressive stress of glass is measured, and if the surface compressive stress is less than a predetermined threshold value, an alkali metal silicate is added to the molten salt and then ion exchange of a next lot of ion-exchangeable glass is performed, and if the surface compressive stress is equal to or greater than the predetermined threshold value, an alkali metal silicate is not added to the molten salt and ion exchange of a next lot of ion-exchangeable glass is performed.
[0020] The ion exchange mixture of the present invention is a glass ion exchange mixture containing a molten salt and an additive, and preferably contains one or more molten salts selected from NaNO3 and KNO3, and an alkali metal silicate as an additive.
[0021] The mixture for ion exchange according to the present invention preferably contains 0.1 to 30 parts by mass of an alkali metal silicate as an additive, based on 100 parts by mass of the molten salt.
[0022] In the mixture for ion exchange according to the present invention, the alkali metal silicate is a powdery crystalline material, and it is preferable that the alkali metal silicate contains at least one selected from Na2SiO3, Na4SiO4, Na2Si2O5, and Na2Si4O9.
[0023] In the ion exchange mixture according to the present invention, the alkali metal silicate is a powdery crystalline material, and the alkali metal silicate preferably contains at least one selected from Li2SiO3, Li4SiO4, Li2Si2O5, and Li2Si4O9.
[0024] The ion-exchanged glass manufacturing apparatus according to the present invention comprises any one of the above-mentioned ion exchange mixtures and a storage tank for storing the ion exchange mixture, and at least a part of the contact surface of the storage tank with the ion exchange mixture is made of metal.
[0025] The ion-exchanged glass manufacturing apparatus according to the present invention preferably further comprises a jig that holds the ion-exchange glass and is immersed in the ion-exchange mixture, and the surface of the jig that comes into contact with the ion-exchange mixture is preferably made of metal.
[0026] In the ion-exchanged glass manufacturing apparatus according to the present invention, the metal is preferably stainless steel.
[0027] A method for producing ion-exchanged glass according to the present invention includes a step of immersing a part or the whole of ion-exchange glass containing NaO as a glass composition in an ion-exchange mixture to perform ion exchange treatment, and is characterized in that the ion-exchange mixture contains a molten salt and a lithium salt as an additive. Effect of the Invention
[0028] According to the present invention, deterioration of production equipment and deterioration of product quality can be suppressed compared to the conventional techniques. [Brief description of the drawings]
[0029] [Figure 1] 1 is a schematic view of an apparatus for producing ion-exchanged glass according to a first embodiment of the present invention. [Diagram 2] 1 is a flowchart outlining a method for producing ion-exchanged glass according to a first embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] (First embodiment) Hereinafter, a method for producing ion-exchanged glass, an apparatus for producing ion-exchanged glass, and a mixture for ion exchange according to a first embodiment of the present invention will be described.
[0031] 1 is a schematic diagram of an apparatus for producing ion-exchanged glass according to a first embodiment of the present invention. The apparatus for producing ion-exchanged glass 1 is a processing apparatus for subjecting glass G1 for ion exchange treatment to obtain ion-exchanged glass GX. The apparatus for producing ion-exchanged glass 1 includes a mixture for ion exchange 10, a container 11, and a jig 12.
[0032] The mixture for ion exchange 10 is a treatment agent that, upon contact with the glass for ion exchange G1, performs ion exchange with components in the glass for ion exchange G1. The mixture for ion exchange 10 contains a molten salt 101 and an additive 102.
[0033] The molten salt 101 is a salt containing a component in the ion-exchange glass G1 and an ion-exchangeable component, and is typically an alkali nitrate. Examples of the alkali nitrate include NaNO3, KNO3, LiNO3, etc., which can be used alone or in combination. In this embodiment, a mixed salt of NaNO3 and KNO3 is used. The mixing ratio of NaNO3 and KNO3 may be determined arbitrarily, but may be, for example, 5 to 95% NaNO3 and 5 to 95% KNO3, preferably 30 to 80% NaNO3 and 20 to 70% KNO3, and more preferably 50 to 70% NaNO3 and 30 to 50% KNO3, in mass %.
[0034] The additive 102 is a substance containing an alkali metal component that is ion-exchangeable with the alkali metal component eluted from the ion-exchange glass G1 into the molten salt 101 during the ion exchange process, and is a metal salt containing a monovalent metal component different from the eluted ions. In the present embodiment, the additive 102 can use, as the alkali metal salt, for example, an alkali metal silicate containing an alkali metal component having an ionic radius larger than that of the alkali metal component eluted from the ion-exchange glass G1 into the molten salt 101.
[0035] The type of alkali metal silicate added as the additive 102 is preferably appropriately selected according to the alkali metal component eluted from the ion-exchange glass G1 into the molten salt 101. In the present first embodiment, a case will be described in which the ion-exchange glass G1 is a lithium aluminosilicate glass, and the alkali metal component eluted into the molten salt 101 is Li ion. In this case, the alkali metal silicate is preferably sodium silicate. The sodium silicate includes at least one selected from Na2SiO3 (sodium metasilicate), Na4SiO4, Na2Si2O5, and Na2Si4O9. The sodium silicate is preferably anhydrous, but may be a hydrate. With this configuration, Li ions eluted into the molten salt 101 are ion-exchanged with Na ions contained in the alkali metal silicate, and an increase in the concentration of Li ions in the molten salt 101 can be suppressed.
[0036] The alkali metal silicate is preferably a crystalline substance. Furthermore, the alkali metal silicate is preferably a powdered alkali metal silicate crystalline substance. The alkali metal salt crystalline substance is preferably in a powdered state at the time of addition to the molten salt, but may be in a powdered state by pulverizing in the molten salt after addition to the molten salt. The average particle size D50 of the powder is preferably 10 to 1000 μm. In order to improve the ion exchangeability with the alkali metal component eluted from the ion exchange glass, the average particle size D50 of the powder is more preferably 900 μm or less, 800 μm or less, 700 μm or less, 500 μm or less, or 450 μm or less. In order to prevent dust before addition, the average particle size D50 of the powder is more preferably 20 μm or more, 50 μm or more, 100 μm or more, 150 μm or more, 200 μm or more, or 250 μm or more.
[0037] The amount of additive 102 to be added to molten salt 101, i.e., the amount of alkali metal salt, is preferably measured and added so that the amount of alkali metal salt is 0.1 to 30 parts by mass when molten salt 101 is taken as 100 parts by mass. The amount of alkali metal salt added is more preferably 1 to 30 parts by mass, 2 to 25 parts by mass, 3 to 20 parts by mass, or 4 to 15 parts by mass. If the amount of additive 102 added is too small, a sufficient ion adjustment effect cannot be obtained, and if the amount added is too excessive, there is a concern that the cost of the additive will increase.
[0038] In the first embodiment, potassium silicate may be used as the alkali metal silicate instead of sodium silicate or in combination with sodium silicate. Potassium silicate includes at least one selected from K2SiO3, K4SiO4, K2Si2O5, and K2Si4O9. Potassium silicate is preferably anhydrous, but may be a hydrate.
[0039] The storage tank 11 is a tank that stores the mixture for ion exchange 10. At least a part of the surface of the storage tank 11 that comes into contact with the mixture for ion exchange 10 is made of metal. In the first embodiment, the inner surface 11S of the storage tank 11 is made of stainless steel. Note that the storage tank 11 preferably further includes an opening for inserting and removing the jig 12 and the glass for ion exchange G1, and a lid for covering the opening (not shown).
[0040] The jig 12 is a member that holds the ion-exchange glass G1. During ion exchange processing, the jig 12 is immersed in the ion-exchange mixture 10 in the storage tank 11 while holding the ion-exchange glass G1. At least a part of the contact surface of the jig 12 with the ion-exchange mixture 10 is made of metal. In the first embodiment, the entire jig 12 is made of stainless steel. The jig 12 is carried in and out of the storage tank 11 by a carrier device (not shown).
[0041] The glass for ion exchange G1 is a glass article before ion exchange treatment that is to be the target of ion exchange treatment. In the present first embodiment, the glass for ion exchange G1 is exemplified as a rectangular plate. The plate thickness of the glass for ion exchange G1 is, for example, 2.0 mm or less, more preferably 1.0 mm or less, and further preferably 0.3 mm to 0.9 mm. The length of the glass for ion exchange G1 is, for example, 5 mm to 5000 mm, 15 mm to 1000 mm, 30 mm to 500 mm, 50 mm to 300 mm, or 70 mm to 200 mm, and the width of the glass for ion exchange G1 is, for example, 1 mm to 4000 mm, 10 mm to 1000 mm, 30 mm to 500 mm, 40 mm to 300 mm, or 50 mm to 150 mm.
[0042] As described above, in the first embodiment, the ion exchange glass G1 is an alkali aluminosilicate glass, and for example, the glass composition preferably contains, in mass %, 40% to 70% SiO2, 10% to 30% Al2O3, 0% to 3% B2O3, 5% to 25% Na2O, 0% to 5.5% K2O, 0.1% to 10% Li2O, 0% to 5.5% MgO, and 52% to 10% P2O.
[0043] Na2O is an ion exchange component, and is a component that reduces high-temperature viscosity and improves melting and moldability. Na2O is also a component that improves devitrification resistance and reaction devitrification resistance with a shaped refractory, especially an alumina refractory. If the content of Na2O is too low, the melting property decreases, the thermal expansion coefficient decreases too much, and the ion exchange rate tends to decrease. Therefore, the preferable lower limit range of Na2O is 5% or more, 7% or more, 8% or more, 8.5% or more, 9% or more, 9.5% or more, 10% or more, 11% or more, 12% or more, and particularly 12.5% or more by mass. On the other hand, if the content of Na2O is too high, the phase separation occurrence viscosity tends to decrease. In addition, acid resistance may decrease, and the glass composition may lack a component balance, resulting in a decrease in devitrification resistance. Therefore, a suitable upper limit range of Na2O is 25% or less, 22% or less, 20% or less, 19.5% or less, 19% or less, 18% or less, 17% or less, 16.5% or less, 16% or less, 15.5% or less, particularly 15% or less.
[0044] K2O is a component that reduces high-temperature viscosity and improves melting and moldability. It is also a component that improves devitrification resistance and increases Vickers hardness. However, if the content of K2O is too high, the phase separation viscosity is likely to decrease. In addition, acid resistance decreases, and the glass composition loses its component balance, which tends to decrease devitrification resistance. Therefore, the preferred lower limit range of K2O is, in mass%, 0% or more, 0.01% or more, 0.02% or more, 0.1% or more, 0.5% or more, 1% or more, 1.5% or more, 2% or more, 2.5% or more, 3% or more, particularly 3.5% or more, and the preferred upper limit range is 5.5% or less, 5% or less, particularly less than 4.5%.
[0045] Li2O is an ion exchange component, and also a component that reduces high-temperature viscosity and improves melting and moldability. It also increases Young's modulus. Li2O is also a component that dissolves during ion exchange treatment and deteriorates the ion exchange solution. Therefore, the preferred lower limit range of Li2O is, in mass%, 0.1% or more, 0.5% or more, 1.0% or more, 1.5% or more, 2.0% or more, particularly 2.5% or more, and the preferred upper limit range is 10% or less, 8% or less, 5% or less, 4.5% or less, 4.0% or less, particularly less than 3.5%.
[0046] The above-mentioned ion exchange glass G1 can be prepared, for example, as follows.
[0047] First, glass raw materials prepared to obtain the above glass composition are charged into a continuous melting furnace, heated and melted at 1500°C to 1600°C, clarified, and then fed into a forming device, where they are formed into a plate shape or the like by an overflow downdraw method, and slowly cooled, thereby producing glass G1 for ion exchange. Note that various forming methods can be adopted in addition to the overflow downdraw method. For example, forming methods such as a float method, a downdraw method (slot down method, redraw method, etc.), a roll-out method, and a press method can be adopted.
[0048] After or simultaneously with forming the glass for ion exchange G1, it may be subjected to bending as required. In addition, it may be subjected to cutting, drilling, surface polishing, chamfering, edge polishing, etching, etc. as required.
[0049] A description will now be given of a method for producing ion-exchanged glass using the above-mentioned ion-exchanged glass producing apparatus 1. Fig. 2 is a flow chart showing an outline of the method for producing ion-exchanged glass according to the first embodiment of the present invention.
[0050] First, as shown in Fig. 2, a molten salt preparation process is performed (step S1). Specifically, first, NaNO3 and KNO3 are mixed and heated to melt inside the containing layer 11 to prepare a molten salt 101.
[0051] Next, an ion exchange treatment step is performed (step S2). Specifically, a plurality of sheets of glass G1 for ion exchange are held in a jig 12 as one lot and immersed in molten salt 101. Conditions such as the temperature of the molten salt and the immersion time in the ion exchange treatment may be determined arbitrarily, but the temperature of the molten salt is, for example, 350°C to 500°C, preferably 360°C to 470°C, 360°C to 450°C, 360°C to 430°C, or 360°C to 410°C. The immersion time is, for example, 0.1 to 30 hours, preferably 0.2 to 20 hours, 0.3 to 15 hours, 0.4 to 10 hours, or 0.5 to 5 hours. By subjecting the glass G1 for ion exchange treatment to ion exchange treatment, an ion exchange glass GX is obtained.
[0052] When the ion exchange process for one lot is completed, the next lot of glass for ion exchange G1 is subjected to the ion exchange process, and the ion exchange process is repeatedly performed until the ion exchange process for a predetermined number of lots is completed (NO in step S3).
[0053] On the other hand, when the ion exchange of a predetermined number of lots is completed (YES in step S3), the stress characteristics of the ion-exchanged glass GX obtained in the last ion exchange process are measured. Specifically, the surface compressive stress CS of the ion-exchanged glass GX is measured using a stress measuring device.
[0054] In the present invention, the stress characteristics can be measured using a known stress measurement method and a known stress measurement device. For example, the stress characteristics can be measured using a surface stress meter FSM-6000LE or SLP-1000 manufactured by Orihara Seisakusho Co., Ltd. alone or in combination.
[0055] After the stress characteristic measurement is completed, it is determined whether the stress characteristic is less than a predetermined threshold value (step S5). The threshold value may be set arbitrarily depending on the product specifications and the measuring device, and can be set to any value within the range of, for example, 300 to 1000 MPa. Specifically, in the first embodiment, it is determined whether the value of the surface compressive stress CS is less than 400 MPa, for example. More preferably, when the value of the surface compressive stress CS of the first lot of ion-exchanged glass GX is taken as 100%, it is preferable to set the threshold value to a compressive stress value that is 75 to 85% of that value.
[0056] If the stress characteristic is equal to or greater than the predetermined threshold value (NO in step S5), the ion exchange process for the next lot is carried out, and the processes from step S2 to step S5 described above are repeated.
[0057] On the other hand, if the stress characteristic is less than the predetermined threshold value (YES in step S5), an addition process is performed to add an alkali metal silicate as an additive 102 to the molten salt 101 (step S6). By this addition process, the ion exchange mixture 10 according to the present invention is formed inside the storage tank 11.
[0058] In step S6, it is preferable to stir the molten salt 101 after adding the additive 102 to the molten salt 101. The stirring can be performed by inserting a stick, a paddle, or the like into the storage tank 11 and operating it manually or automatically by a machine. After stirring, the next process may be performed in a state in which the additive is dispersed in the molten salt 101, or the process may wait until the additive 101 settles on the inner bottom of the storage tank 11.
[0059] After completing the addition process of step S6, the process of step S2 is performed on the next lot of ion-exchange glass G1, and the above-mentioned process is repeated. Note that after the process of step S6, a waiting period of a predetermined time may be provided until the adjustment of the ion concentration by the additive 102 progresses to a certain extent, and then the process of step S2 may be started. The waiting time before starting step S2 after the process of step S6 may be arbitrarily set, and may be, for example, 1 minute or more, 5 minutes or more, 10 minutes or more, 30 minutes or more, 1 hour to 24 hours, or 1 hour to 12 hours.
[0060] According to the method for producing ion-exchanged glass according to the first embodiment described above, the ion balance of the molten salt 101 can be adjusted to an appropriate state by adding an alkali metal silicate as the additive 102 to the molten salt 101 to form the ion exchange mixture 10. Furthermore, by adding an alkali metal silicate as the additive 102, corrosion of the container vessel 11 and the jig 12 can be suppressed. Therefore, the stress characteristics of the obtained ion-exchanged glass GX can be stabilized.
[0061] Moreover, according to the method for producing ion-exchanged glass in the first embodiment, by adding additive 102 at an appropriate timing, excessive addition of additive 102 can be prevented, and the ion balance of molten salt 101 can be more appropriately adjusted.
[0062] In the method for producing ion-exchanged glass according to the first embodiment, the surface compressive stress CS is measured as a stress characteristic, and the necessity of performing the addition treatment is determined based on the magnitude of the value of the surface compressive stress CS. However, the above-mentioned treatment may be performed based on other stress characteristics. For example, the depth DOC of the compressive stress layer may be measured in step S4, and it may be determined in step S5 whether the depth of the compressive stress layer is less than a predetermined threshold value. In this case, the threshold value of the depth DOC of the compressive stress layer may be set to an arbitrary value within a range of, for example, 50 to 150 μm. In addition, the threshold value of the depth DOC of the compressive stress layer may be set based on a ratio according to the thickness of the glass G1 for ion exchange. In this case, the threshold value of the depth DOC of the compressive stress layer may be set to an arbitrary value within a range of, for example, 10% to 25% of the thickness of the glass G1 for ion exchange.
[0063] In the above-described first embodiment of the method for producing ion-exchanged glass, a so-called sampling inspection is performed for each predetermined number of lots, but a measurement step may be performed each time each lot of ion-exchanged glass G1 is subjected to ion exchange treatment. In this case, the determination step in step S3 may be omitted. By performing such a process, the addition step in step S6 can be performed at an appropriate timing, and the outflow of defective products can be more appropriately suppressed.
[0064] In the method for producing ion-exchanged glass according to the first embodiment, the processes of steps S4 and S5 may be omitted. That is, the addition process of step S6 may be performed when the ion-exchange process for a predetermined number of lots is completed (YES in step S3). For example, in cases where the degree of deterioration of the molten salt 101 or the degree of deterioration in the properties of the ion-exchanged glass GX can be predicted based on the number of lots, the number of steps S4 and S5 can be reduced and production efficiency can be improved by adopting such a process.
[0065] In the method for producing ion-exchanged glass according to the first embodiment, after the molten salt preparation step of step S1 and before the ion exchange treatment of step S2, the addition treatment of step S6 may be performed so that production can be started in a state in which additive 102 has been added to molten salt 101 in advance.
[0066] Second embodiment In the above-mentioned first embodiment, the case where the increase in the Li ion concentration eluted in the molten salt is suppressed has been described as an example, but the present invention can also be applied to the adjustment of other ion concentrations. For example, the case where the increase in the Na ion concentration eluted in the molten salt is suppressed can be applied as in the following second embodiment. Note that, in the following, differences from the first embodiment will be described, and explanations of other configurations will be omitted as they are the same as those of the first embodiment.
[0067] The ion-exchange glass G2 according to the second embodiment of the present invention is an alkali aluminosilicate glass containing Na2O as a glass composition and not containing Li2O. More specifically, the ion-exchange glass G2 is a glass containing, for example, 40% to 70% SiO2, 10% to 30% Al2O3, 0% to 3% B2O3, 5% to 25% Na2O, 0% to 5.5% K2O, 0% to 5.5% MgO, and 52% to 10% P2O as a glass composition by mass%, and not containing Li2O. In the present invention, not containing Li2O means that the content of Li2 is less than 0.1 mass%.
[0068] Na2O is an ion exchange component, and is a component that reduces high-temperature viscosity and improves melting and moldability. Na2O is also a component that improves devitrification resistance and reaction devitrification resistance with a shaped refractory, especially an alumina refractory. If the content of Na2O is too low, the melting property decreases, the thermal expansion coefficient decreases too much, and the ion exchange rate tends to decrease. Therefore, the preferable lower limit range of Na2O is 5% or more, 7% or more, 8% or more, 8.5% or more, 9% or more, 9.5% or more, 10% or more, 11% or more, 12% or more, and particularly 12.5% or more by mass. On the other hand, if the content of Na2O is too high, the phase separation occurrence viscosity tends to decrease. In addition, acid resistance may decrease, and the glass composition may lack a component balance, resulting in a decrease in devitrification resistance. Therefore, a suitable upper limit range of Na2O is 25% or less, 22% or less, 20% or less, 19.5% or less, 19% or less, 18% or less, 17% or less, 16.5% or less, 16% or less, 15.5% or less, particularly 15% or less.
[0069] K2O is a component that reduces high-temperature viscosity and improves melting and moldability. It is also a component that improves devitrification resistance and increases Vickers hardness. However, if the content of K2O is too high, the phase separation viscosity is likely to decrease. In addition, acid resistance decreases, and the glass composition loses its component balance, which tends to decrease devitrification resistance. Therefore, the preferred lower limit range of K2O is, in mass%, 0% or more, 0.01% or more, 0.02% or more, 0.1% or more, 0.5% or more, 1% or more, 1.5% or more, 2% or more, 2.5% or more, 3% or more, particularly 3.5% or more, and the preferred upper limit range is 5.5% or less, 5% or less, particularly less than 4.5%.
[0070] In the second embodiment, the alkali metal silicate as an additive contained in the mixture for ion exchange is preferably potassium silicate. The potassium silicate includes at least one selected from K2SiO3, K4SiO4, K2Si2O5, and K2Si4O9. With this configuration, Na ions dissolved in the molten salt are ion-exchanged with K ions contained in the alkali metal silicate, and an increase in the concentration of Na ions in the molten salt can be suppressed.
[0071] It is particularly effective to add potassium silicate to a molten salt mainly composed of KNO3. The molten salt 101 mainly composed of KNO3 contains, for example, 80-100% KNO3 and 0-20% NaNO3+LiNO3 by mass%, preferably 90-99.9% KNO3, 0.1-10% NaNO3+LiNO3, and more preferably 98.5-99.8% KNO3, and 0.2-1.5% NaNO3+LiNO3. In such a molten salt mainly composed of KNO3, Na ions are easily eluted from the glass and the Na ion concentration in the molten salt increases, so the increase in concentration can be effectively suppressed by adding the above-mentioned potassium silicate.
[0072] Third embodiment In the second embodiment, the case where potassium silicate is used as the additive contained in the mixture for ion exchange has been described, but in order to suppress an increase in the Na ion concentration of the molten salt, a lithium salt may be used as the additive. That is, a metal salt containing a metal component with an ionic radius smaller than that of the eluted ions may be used as the additive.
[0073] The lithium salt is, for example, a lithium silicate, and includes at least one selected from Li2SiO3 (lithium metasilicate), Li4SiO4, Li2Si2O5, and Li2Si4O9.
[0074] The lithium salt may be a lithium phosphate. The lithium phosphate includes at least one selected from Li3PO4 (trilithium phosphate), Li2HPO4, and LiH2PO4. The lithium silicate and the lithium phosphate may be used alone or in combination.
[0075] In the third embodiment, the same ion-exchange glass and molten salt as those described in the first and second embodiments can be used under the same conditions.
[0076] (Fourth embodiment) The ion-exchanged glass GX obtained as in the first embodiment may be subjected to an additional ion-exchange treatment. That is, the ion-exchange treatment (step S2) shown in FIG. 2 may be used as the first-stage ion-exchange treatment, and a second-stage ion-exchange treatment (not shown) may be further performed. In the second-stage ion-exchange treatment, it is preferable to separately prepare and use a molten salt (referred to as the second molten salt) having a higher KNO3 mixing ratio than the molten salt 101 (referred to as the first molten salt) used in the first-stage ion-exchange treatment, more preferably the KNO3 mixing ratio is 90 mass% or more, and more preferably the molten salt composition described in the second embodiment can be used. According to such a treatment, a deep compressive stress layer is formed in the first-stage ion-exchange treatment in the ion-exchanged glass GX, and a high surface compressive stress CS can be imparted in the second-stage ion-exchange treatment. In the second-stage ion-exchange treatment, it is preferable to adjust the composition of the molten salt, the treatment temperature, the treatment time, etc. so that the surface compressive stress CS of the ion-exchanged glass GX is 700 MPa or more.
[0077] Moreover, potassium silicate or lithium salt may be added to the second molten salt used in the above-mentioned second-stage ion exchange treatment, as in the methods shown in the second and third embodiments. With this configuration, an excessive increase in the Na ion concentration in the second molten salt can be suppressed.
[0078] Also, sodium silicate may be added to the second molten salt in the same manner as in the first embodiment. If the glass surface is left in a state where lithium salt is attached by the first ion exchange treatment, and the glass is immersed in the second molten salt in this state to perform the second ion exchange treatment, the Li ion concentration may increase in the second molten salt, which may inhibit the ion exchange. However, by adding sodium silicate to the second molten salt as described above, the increase in the Li ion concentration in the second molten salt can be suppressed.
[0079] In each of the above embodiments, the ion-exchange glass G1 and the ion-exchange glass GX are exemplified as being rectangular plates, but are not limited to rectangular plates and can be applied to any shape, such as bent plates, disks, tubes, containers, and spheres.
[0080] In addition, in each of the above embodiments, the ion exchange treatment is mainly intended to improve the strength of the glass, and the ion exchange glass GX is chemically strengthened glass. However, the present invention may be applied to ion exchange treatments for other purposes, such as ion exchange treatments for adjusting the refractive index of optical components such as lenses, or for surface treatment of glass for medical use.
[0081] The alkali metal silicate used as the additive 102 may be a mixture of potassium silicate, sodium silicate, and lithium silicate. For example, when a plurality of types of alkali metal ions are eluted from the ion exchange glass G1, the concentrations of the alkali metal ions in the molten salt 101 can be suitably adjusted by mixing a plurality of types of alkali metal silicates according to the number of types of eluted alkali metal ions.
[0082] In addition, in each of the above embodiments, stainless steel is used for the storage tank 11 and the jig 12, but any known type of stainless steel such as austenitic stainless steel or ferritic stainless steel may be used as the stainless steel. In addition, the storage tank 11 and the jig 12 may be made of any metal that is corrosion-resistant to the molten salt 101, other than stainless steel. EXAMPLES
[0083] The method for producing ion-exchanged glass and the mixture for ion exchange according to the present invention will be described below with reference to examples. Note that the following examples are merely illustrative and the present invention is not limited to the following examples in any way.
[0084] The samples were prepared as follows: First, ion-exchange glass G1 was prepared, which had a glass composition, by mass percent, of 51.6% SiO2, 27.9% Al2O3, 0.3% B2O3, 0.6% K2O, 7.5% Na2O, 3.3% Li2O, 0.3% MgO, 58.4% P2O, and 0.1% SnO2.
[0085] Specifically, glass raw materials were prepared so as to obtain the above composition, and melted in a platinum pot at 1600° C. for 21 hours. Thereafter, the obtained molten glass was formed into a plate having a thickness of 0.7 mm by flow-down-drawing from a refractory molded body.
[0086] Next, the above-mentioned glass for ion exchange was subjected to an ion exchange treatment by immersing it in a mixture for ion exchange having the composition shown in Table 1, No. 1 to 6, under the temperature and time conditions shown in Table 1. In Table 1, No. 1 to 3 are examples of the present invention, and No. 4 to 6 are comparative examples.
[0087] The ion exchange mixtures Nos. 1, 2, and 4 were prepared by mixing LiNO3 into the molten salt to simulate the molten salt with an increased Li-ion concentration after repeated ion exchange treatment. On the other hand, the ion exchange mixtures Nos. 3, 5, and 6 were fresh molten salts that did not contain Li ions.
[0088] Na2SiO3 was added as an additive to the ion exchange mixtures according to Nos. 1 to 3. On the other hand, no additive was added to the ion exchange mixtures according to Nos. 4 and 6 for comparison. Na3PO4 was added as an additive to the ion exchange mixture according to No. 5 for comparison. In Table 1, the amount of additive added is expressed in parts by mass when the molten salt is taken as 100 parts by mass.
[0089] In order to evaluate the metal corrosiveness, plate-shaped metal test pieces made of SUS304, SUS316, and SUS430, each having a thickness of 1.0 mm, a width of 20 mm, and a length of 50 mm, were immersed in the ion exchange mixtures Nos. 3 and 5, respectively.
[0090] The properties of the thus obtained ion-exchange mixture and ion-exchange glass are shown in Table 1.
[0091] [Table 1]
[0092] The surface compressive stress CS in Table 1 is a value measured using a surface stress meter FSM-6000LE manufactured by Orihara Seisakusho Co., Ltd.
[0093] The amount of metal corrosion in Table 1 indicates the amount of change in weight of each metal sample piece after immersion in the ion exchange mixture relative to the weight before immersion.
[0094] Comparative Example 4, in which the molten salt had a high Li ion concentration and contained no additives, showed a significantly lower surface compressive stress value CS of the ion-exchanged glass than Comparative Example 6, in which the molten salt contained no Li ions.
[0095] On the other hand, it was confirmed that in both Examples 1 and 2 containing Na2SiO3 as an additive, the decrease in the surface compressive stress value CS of the ion-exchanged glass was suppressed compared to Comparative Example 4 containing no additive.
[0096] In addition, in Comparative Example No. 5, in which Na3PO4 was added as an additive, a weight loss was observed for each metal sample immersed, and the occurrence of metal corrosion was confirmed. On the other hand, in the metal samples of Example No. 3, in which Na2SiO3 was added as an additive, no weight loss was observed, and it was confirmed that metal corrosion was suppressed. EXAMPLES
[0097] In the following examples, the effect of suppressing an increase in the Na ion concentration in the molten salt by adding a lithium salt was verified. In Table 2, No. 7 is an example of the present invention, No. 8 is a reference example, and No. 9 is a comparative example.
[0098] First, the molten salts having the compositions shown in Nos. 7 to 9 in Table 2 were adjusted to the temperatures shown in Table 1. The molten salts according to Nos. 7 to 9 were adjusted by mixing NaNO3 into the molten salt in order to simulate a molten salt with an increased Na ion concentration after repeated ion exchange treatment.
[0099] Next, each additive shown in Table 2 was added to each molten salt to prepare an ion exchange mixture. Li2SiO3 was added as an additive to the ion exchange mixture related to No. 7. Li3PO4 was added as an additive to the ion exchange mixture related to No. 8. On the other hand, no additive was added to the ion exchange mixture related to No. 9 for comparison. In Table 2, the amount of additive added is expressed in parts by mass when the molten salt is taken as 100 parts by mass.
[0100] Next, the Li ion concentration and the Na ion concentration of the ion exchange mixture were measured after the time shown in Table 2 had elapsed from the time of adding the additives. More specifically, about 10 g of the supernatant liquid without precipitate was collected from each molten salt, and the Li ion and Na ion concentrations were quantitatively analyzed by atomic absorption spectrometry.
[0101] [Table 2]
[0102] According to the above measurement results, in the ion exchange mixture of Example No. 7, the Na ion concentration was lower than in Comparative Example No. 9 containing no additive, and the effect of suppressing an increase in the Na ion concentration was recognized. [Industrial Applicability]
[0103] The method for producing ion-exchanged glass, the apparatus for producing ion-exchanged glass, and the mixture for ion exchange of the present invention can be used in the production of ion-exchanged glass used in, for example, smartphones, mobile phones, tablet computers, personal computers, digital cameras, touch panel displays, cover glasses of other display devices, in-vehicle panels, magnetic disks, and the like. [Explanation of symbols]
[0104] 1. Ion exchange glass manufacturing equipment 10 Ion exchange mixture 11 Containment tank 12 Jig 101 Molten Salt 102 Additives G1, G2 Ion exchange glass GX Ion Exchange Glass
Claims
1. A method for producing ion-exchanged glass, comprising a step of immersing a part or whole of ion-exchangeable glass containing an alkali metal component in a mixture for ion exchange to perform ion exchange treatment, The ion exchange mixture includes a molten salt and an alkali metal silicate, the alkali metal silicate contains an alkali metal component that is ion-exchangeable with an alkali metal component eluted from the ion-exchange glass into the molten salt during the ion exchange treatment, an alkali metal component eluted from the ion-exchange glass into the molten salt during the ion exchange treatment is a Na ion; A method for producing ion-exchanged glass, wherein the alkali metal silicate contains at least one selected from the group consisting of Li 2 SiO 3 , Li 4 SiO 4 , Li 2 Si 2 O 5 and Li 2 Si 4 O 9 .
2. The ion exchange glass has a composition of Na 2 The glass is an alkali aluminosilicate glass containing 1.0 mol % or more of O, The molten salt is KNO 3 The method for producing ion-exchanged glass according to claim 1 , comprising:
3. 3. The method for producing ion-exchanged glass according to claim 1, wherein the alkali metal silicate is a powdered alkali metal silicate crystal.
4. 4. The method for producing ion-exchanged glass according to claim 3, wherein the powdered alkali metal silicate has an average particle size D50 of 10 to 1000 μm.
5. The method for producing ion-exchanged glass according to claim 3 , further comprising the step of stirring the molten salt after adding the alkali metal silicate to the molten salt.
6. 6. The method for producing ion-exchanged glass according to claim 1, wherein the amount of the alkali metal silicate added is 0.1 to 30 parts by mass relative to 100 parts by mass of the molten salt.
7. performing the ion exchange treatment a plurality of times by sequentially immersing a plurality of different lots of the glass for ion exchange in the mixture for ion exchange; a step of measuring stress characteristics of the ion-exchanged glass obtained in the final ion-exchange treatment after the ion-exchange treatment of a predetermined number of lots of the glass for ion-exchange; 7. The method for producing ion-exchanged glass according to claim 1, further comprising the step of determining whether or not to add the alkali metal silicate to the molten salt depending on a result of the measurement of the stress characteristics.
8. As the stress characteristic, a surface compressive stress of the ion-exchanged glass is measured; if the surface compressive stress is less than a predetermined threshold value, adding the alkali metal silicate to the molten salt and then performing ion exchange of a next lot of the glass for ion exchange; when the surface compressive stress is equal to or greater than a predetermined threshold value, the alkali metal silicate is not added to the molten salt, and a next lot of the glass for ion exchange is subjected to ion exchange. The method for producing the ion-exchanged glass according to claim 7 .
9. A mixture for ion exchange comprising a molten salt and an additive, The molten salt is NaNO 3 and K.N.O. 3 One or more selected from The additive includes an alkali metal silicate, The alkali metal silicate is a powdered alkali metal silicate crystal, The mixture for ion exchange, wherein the alkali metal silicate comprises at least one selected from the group consisting of Li 2 SiO 3 , Li 4 SiO 4 , Li 2 Si 2 O 5 , and Li 2 Si 4 O 9 .
10. 10. The ion exchange mixture according to claim 9, comprising 0.1 to 30 parts by mass of an alkali metal silicate as the additive, based on 100 parts by mass of the molten salt.
11. A mixture for ion exchange according to claim 9 or 10, a storage tank for storing the ion exchange mixture; At least a part of the surface of the container that comes into contact with the mixture for ion exchange is made of metal.
12. A jig for holding ion-exchange glass and for being immersed in the ion-exchange mixture, The apparatus for producing ion-exchanged glass according to claim 11, wherein a surface of the jig in contact with the mixture for ion exchange is made of metal.
13. The ion-exchanged glass manufacturing apparatus according to claim 11 or 12, wherein the metal is stainless steel.
Citation Information
Patent Citations
Molten salt for glass chemistry toughening and chemical toughening method using the same
CN101328026A
Process for preparing magnetic disk substrate of chemically strengthened glass
CN1305965A
JP1972-050849B
Methods for regenerating lithium-enriched salt baths
US20180362399A1
Method of removing ion from salt bath by ion exchange regeneration
US3441398A