Polylactic acid resin piezoelectric film and its manufacturing method

The sequential biaxial stretching method aligns molecular orientation in a specific direction, overcoming limitations of existing techniques to produce a polylactic acid resin piezoelectric film with high piezoelectric constant and large area, suitable for applications requiring thin and efficient piezoelectric films.

JP7569193B2Active Publication Date: 2024-10-17SUNDIC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020171854
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-12
Publication Date
2024-10-17
Estimated Expiration
2040-10-12

AI Technical Summary

Technical Problem

Existing methods for producing polylactic acid resin piezoelectric films struggle to achieve high piezoelectric constants, large areas, and thin film thickness due to limitations in biaxial stretching techniques, particularly sequential biaxial stretching, which fail to align molecular orientation in a single direction effectively.

Method used

A sequential biaxial stretching method is employed, with controlled stretching ratios and temperatures in both longitudinal and transverse directions, aligning molecular orientation in a specific direction, resulting in a polylactic acid resin piezoelectric film with high piezoelectric constant, large area, and thin film capabilities.

Benefits of technology

The method produces a polylactic acid resin piezoelectric film with a piezoelectric constant of 3.0 pC/N or more, capable of being made into a large area and thin film with uniform molecular orientation, exhibiting high piezoelectricity and excellent thickness accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569193000002
    Figure 0007569193000002
  • Figure 0007569193000003
    Figure 0007569193000003
  • Figure 0007569193000004
    Figure 0007569193000004
Patent Text Reader

Abstract

To provide a polylactic resin piezoelectric film which contains a polylactic resin, has a molecule orientation direction aligned in one direction even when biaxially drawn, exhibits high piezoelectricity, and enables a large area and a thin film.SOLUTION: A polylactic resin piezoelectric film is a biaxially drawn film that contains a polylactic resin and is drawn in a film flow direction (MD direction) and a direction (TD direction) orthogonal to the flow direction (MD direction), in which an angle formed by a main axis direction of an orientation angle of the biaxially drawn film and the orthogonal direction (TD direction) is within 5° .SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polylactic acid resin piezoelectric film and a method for producing the same. [Background technology]

[0002] Polyvinylidene fluoride (PVDF) is well known as a polymer with piezoelectricity, and uniaxially stretched films of polyvinylidene fluoride are known to exhibit large piezoelectricity. However, in order to exhibit piezoelectricity, it is necessary to apply a voltage to the stretched film and perform a polarization poling process. In addition, since it also has pyroelectricity (electric charge is generated by temperature changes), it cannot be used inside machines or in places that generate heat from the human body. On the other hand, polylactic acid is a crystalline resin, and a uniaxially stretched film of polylactic acid, which has its molecules oriented in a certain direction by stretching and then heat-treated to cause oriented crystallization, exhibits piezoelectricity simply by applying shear stress along the molecular orientation direction. Polymeric piezoelectric materials using polylactic acid are known (see, for example, Patent Document 1). Piezoelectric films using polylactic acid do not require poling treatment, and have a high piezoelectric constant among organic piezoelectric materials. They also have other characteristics such as non-pyroelectricity, low dielectric constant, high transparency, and ease of processing, so their application to the market is anticipated. In order to realize piezoelectricity, it is important to align the molecules in a uniform direction. Various stretching methods for stretching a polymeric piezoelectric material are known in order to efficiently orient the polymer in the main stretching direction and obtain a piezoelectric film exhibiting high piezoelectric properties (see, for example, Patent Documents 2 to 5). In addition, although not intended for piezoelectric films, a method is known in which a polylactic acid-based resin sheet is sequentially biaxially stretched to produce a polylactic acid-based stretched sheet that can be used to mold secondary molded products with excellent transparency and heat resistance (see, for example, Patent Document 6). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 5-152638 [Patent Document 2] International Publication No. 2010 / 104196 [Patent Document 3] International Publication No. 2012 / 026494 [Patent Document 4] International Publication No. 2016 / 129400 [Patent Document 5] Patent No. 5313414 [Patent Document 6] JP 2019-26742 A Summary of the Invention [Problem to be solved by the invention]

[0004] In order to suitably use piezoelectric films in sensors that detect pressure on touch panels and the like, flexible touch panel displays, and the like, efforts are being made to improve the piezoelectric constant of piezoelectric films and to increase the area and thickness of piezoelectric films. However, when producing a piezoelectric film, if the solid-phase stretching in which stretching is performed under compressive stress as described in Patent Document 2 or the uniaxial stretching as described in Patent Documents 3 and 4 is used, the molecular chains of the polymeric piezoelectric material can be oriented in one direction and crystallized, and thus a piezoelectric film exhibiting high piezoelectric properties may be obtained. However, when these stretching methods are used, it is difficult to produce a wide width, and therefore it is not possible to efficiently produce a large-area piezoelectric film. In addition, Patent Document 5 describes biaxial stretching of a polymeric piezoelectric material, and lists simultaneous biaxial stretching and sequential biaxial stretching as examples of biaxial stretching. However, the examples in Patent Document 5 only list examples using the simultaneous biaxial stretching method, and there are no specific examples using the sequential biaxial stretching method. With the simultaneous biaxial stretching method described in Patent Document 5, wide-width production is difficult, and large-area piezoelectric films cannot be efficiently produced. On the other hand, the successive biaxial stretching method may be able to efficiently produce large-area films, but simply applying successive biaxial stretching to polymeric piezoelectric materials stretches them in two directions, lengthwise and widthwise, resulting in molecular orientation in two directions, making it impossible to obtain a film that exhibits sufficient piezoelectricity. The piezoelectric constant of piezoelectric films obtained by the successive biaxial stretching method is inferior to that of piezoelectric films obtained by uniaxial stretching, in which the molecular orientation is aligned in one direction. Patent Document 6 describes a method of sequentially biaxially stretching a polylactic acid resin sheet, but it is not possible to obtain a piezoelectric film in which the molecules are oriented in one direction and exhibit high piezoelectricity even if an attempt is made to produce a piezoelectric film using the sequential biaxial stretching method described in Patent Document 6. Further investigation was required to obtain a piezoelectric film in which the molecules are oriented in one direction and exhibit high piezoelectricity using the sequential biaxial stretching method.

[0005] Therefore, an object of the present invention is to provide a polylactic acid-based resin piezoelectric film that contains a polylactic acid-based resin, has molecular orientation aligned in one direction even after biaxial stretching, exhibits high piezoelectricity, and can be made large in area and thin in thickness. [Means for solving the problem]

[0006] As a result of extensive research to solve the above problems, the inventors have discovered that by using a sequential biaxial stretching method to obtain a polylactic acid-based resin piezoelectric film and specifying the stretching ratios for longitudinal and transverse stretching in the sequential biaxial stretching method and the temperatures during longitudinal and transverse stretching, it is possible to produce a polylactic acid-based resin piezoelectric film in which the molecules are oriented in a certain direction, and as a result, it is possible to obtain a polylactic acid-based resin piezoelectric film that exhibits a high piezoelectric constant equivalent to that of a piezoelectric film obtained by a uniaxial stretching method and that can be made large in area and thin in thickness, thereby completing the present invention.

[0007] That is, the present invention includes the following aspects. [1] Contains polylactic acid resin, It is a biaxially stretched film stretched in the machine direction (MD) of the film and in the direction perpendicular to the machine direction (TD), A polylactic acid-based resin piezoelectric film, in which the angle between the main axis direction of the biaxially stretched film and the orthogonal direction (TD direction) is within 5°. [2] The average value of in-plane orientation birefringence measured at multiple points in the perpendicular direction (TD direction) of the polylactic acid-based resin piezoelectric film is 1×10 -2 The polylactic acid resin piezoelectric film according to [1], [3] The polylactic acid-based resin piezoelectric film according to [1] or [2], wherein the polylactic acid-based resin piezoelectric film has a piezoelectric constant d14 of 3.0 pC / N or more. [4] The method for producing a polylactic acid-based stretched sheet according to any one of [1] to [3], wherein the polylactic acid-based resin piezoelectric film has a crystallinity Wc calculated by the following formula (I) of 40% or more. Wc [%] = ΔHm / ΔH0 × 100 (I) ΔHm: Melting enthalpy measured by DSC [J / g] ΔH0: Enthalpy of complete crystallization of polylactic acid 93 [J / g] [5] A step (A) of melt-extruding a polylactic acid-based resin into a thin film to obtain a film; After the step (A), a step (B) of stretching the film in the machine direction (MD) of the film; After step (B), a step (C) of stretching the film in a direction perpendicular to the machine direction (MD), A method for producing a polylactic acid-based resin piezoelectric film, comprising, after step (C), a step (D) of heat-treating the film to crystallize it, The stretching temperature (T MD ) is 130 to 250 ° C., The stretching ratio (X MD ) is more than twice as large, The stretching temperature (T TD ) is 55 to 80°C, The stretching ratio (X TD ) is the stretching ratio in the machine direction (MD direction) (X MD ) is more than twice as large as A method for producing a polylactic acid resin piezoelectric film. [6] The method for producing a polylactic acid resin piezoelectric film according to [5], wherein the temperature of the heat treatment in the step (D) is 100 to 160°C. [7] The stretching temperature (T MD ) is 180 to 250° C. [8] The stretching ratio (X TD ) is 4 to 6 times. Effect of the Invention

[0008] The present invention can provide a polylactic acid-based resin piezoelectric film that contains a polylactic acid-based resin, has molecules oriented in one direction even after biaxial stretching, exhibits high piezoelectricity, and can be made large in area and thin in thickness. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic diagram showing an example of the configuration of a stretching device used when a film is longitudinally stretched by using the sequential biaxial stretching method. [Diagram 2] FIG. 2 is a schematic diagram showing an example of the configuration of a stretching device used when a film is stretched laterally by using the successive biaxial stretching method. [Diagram 3] FIG. 3 is a graph showing the measurement results of the orientation angle between the principal axis direction and the orthogonal direction (TD direction) in the polylactic acid resin piezoelectric film obtained in Example 1. [Figure 4] FIG. 4 is a graph showing the measurement results of the orientation angle between the principal axis direction and the orthogonal direction (TD direction) in the polylactic acid resin piezoelectric film obtained in Example 2. [Diagram 5] FIG. 5 is a graph showing the measurement results of the orientation angle between the principal axis direction and the orthogonal direction (TD direction) in the polylactic acid resin piezoelectric film obtained in Example 3. [Figure 6] FIG. 6 is a graph showing the measurement results of the orientation angle between the principal axis direction and the orthogonal direction (TD direction) in the polylactic acid resin piezoelectric film obtained in Comparative Example 1. [Figure 7] FIG. 7 is a graph showing the measurement results of the orientation angle between the principal axis direction and the orthogonal direction (TD direction) in the polylactic acid resin piezoelectric film obtained in Comparative Example 2. [Figure 8] FIG. 8 is a graph showing the measurement results of the orientation angle between the principal axis direction and the orthogonal direction (TD direction) in the polylactic acid resin piezoelectric film obtained in Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below. Note that the following description of the constituent elements is merely an example for explaining the present invention, and the present invention is not limited to the contents thereof.

[0011] (Polylactic acid resin piezoelectric film) The polylactic acid-based resin piezoelectric film of the present invention contains a polylactic acid-based resin. The polylactic acid-based resin piezoelectric film of the present invention may contain other components, such as known resins typified by polyethylene resins and polystyrene resins, inorganic fillers such as hydroxyapatite, and known crystal nucleating agents, in addition to the polylactic acid-based resin, as long as the effects of the present invention are not impaired. The polylactic acid resin piezoelectric film of the present invention is a biaxially stretched film stretched in the machine direction (MD) of the film and in a direction perpendicular to the machine direction (TD). Film formation by biaxial stretching is performed by stretching in two directions: the machine direction (MD), which is parallel to the film's running direction, and the direction perpendicular to the machine direction (TD). Here, the "machine direction (MD) of the film" can also be rephrased as the "longitudinal direction of the film" or the "longitudinal direction of the film." Additionally, the "orthogonal direction (TD) of the film" can also be rephrased as the "width direction of the film" or the "transverse direction of the film."

[0012] In the polylactic acid resin piezoelectric film of the present invention, the angle between the main axis direction and the orthogonal direction (TD direction) of the orientation angle of the biaxially stretched film is within 5°. According to the polylactic acid-based resin piezoelectric film of the present invention, the main axis direction of the orientation angle can be aligned to the orthogonal direction (TD direction), that is, the molecular orientation direction can be aligned in one direction that is orthogonal to the film (TD direction). In the present invention, the main axis direction of the orientation angle can be aligned to the orthogonal direction (TD direction), so the main axis direction of the orientation angle and the orthogonal direction (TD direction) are parallel, and the angle between the main axis direction of the orientation angle and the orthogonal direction (TD direction) is 0°, but considering measurement errors such as the measuring instrument and the accuracy of cutting out the sample for measurement, the angle is specified to be within 5°. However, if it is within 5°, the main axis direction of the orientation angle and the orthogonal direction (TD direction) can be considered to be aligned in the same direction, and the orientation direction of the molecules can be said to be aligned in one direction, the orthogonal direction (TD direction) of the film.

[0013] The main axis direction of the orientation angle refers to the direction in which the refractive index on the film is the largest, and is measured by an optical method. Specifically, the value measured by a retardation measuring device KOBRA series manufactured by Oji Scientific Instruments Co., Ltd. can be used. In the present invention, the flow direction of the film (so-called film longitudinal direction) means, in the case of a biaxially oriented polylactic acid resin piezoelectric film on a roll, that the winding direction of the roll corresponds to the flow direction of the film, and the width direction of the roll corresponds to the perpendicular direction of the film (so-called film width direction).

[0014] [Orientation angle measurement] The principal axis direction of the orientation angle can be measured using the "KOBRA 21D" model manufactured by Oji Scientific Instruments.

[0015] The polylactic acid-based resin piezoelectric film of the present invention, in which the molecular orientation is aligned in a certain direction, can be produced by using a sequential biaxial stretching method in which the stretching ratios in the machine direction (MD) and the orthogonal direction (TD) of the film, and the temperatures during stretching in the machine direction (MD) and the orthogonal direction (TD) are within specific ranges; a detailed description of the method for producing a polylactic acid-based resin piezoelectric film using the sequential biaxial stretching method will be given later. The polylactic acid-based resin piezoelectric film of the present invention can be obtained using a sequential biaxial stretching method, and therefore can be made large in area. Furthermore, since the polylactic acid-based resin piezoelectric film of the present invention is formed with neatly aligned molecular orientation in a certain direction, it exhibits sufficient piezoelectricity and can be made thin.

[0016] <Polylactic acid resin> The polylactic acid resin used in the present invention is a polymer containing 85% by mass or more of lactic acid monomer units, and may contain 95% by mass or more of lactic acid monomer units, or may contain 98% by mass or more of lactic acid monomer units. The polylactic acid resin refers to "polylactic acid," "a copolymer of L-lactic acid or D-lactic acid with a copolymerizable polyfunctional compound," or a mixture of both. "Polylactic acid" is a polymer in which lactic acid is polymerized through ester bonds and linked together into a long chain, and it is known that it can be produced by the lactide method via lactide, or by the direct polymerization method in which lactic acid is heated under reduced pressure in a solvent and polymerized while removing water. "Polylactic acid" includes homopolymers of L-lactic acid, homopolymers of D-lactic acid, block copolymers containing at least one polymer of L-lactic acid and D-lactic acid, and graft copolymers containing at least one polymer of L-lactic acid and D-lactic acid.

[0017] Examples of the "copolymerizable polyfunctional compound" include hydroxycarboxylic acids such as glycolic acid, dimethylglycolic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 2-hydroxypropanoic acid, 3-hydroxypropanoic acid, 2-hydroxyvaleric acid, 3-hydroxyvaleric acid, 4-hydroxyvaleric acid, 5-hydroxyvaleric acid, 2-hydroxycaproic acid, 3-hydroxycaproic acid, 4-hydroxycaproic acid, 5-hydroxycaproic acid, 6-hydroxycaproic acid, 6-hydroxymethylcaproic acid, and mandelic acid; cyclic esters such as glycolide, β-methyl-δ-valerolactone, γ-valerolactone, and ε-caprolactone; oxalic acid, malonic acid, succinic acid, glutaric acid, and adipic acid. Examples of the polyvalent carboxylic acids include polycarboxylic acids such as polyacid, pimelic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, and terephthalic acid, and their anhydrides; polyhydric alcohols such as ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, 3-methyl-1,5-pentanediol, neopentyl glycol, tetramethylene glycol, and 1,4-hexanedimethanol; polysaccharides such as cellulose; and aminocarboxylic acids such as α-amino acids.

[0018] The above-mentioned "copolymer of lactic acid and a copolymerizable polyfunctional compound" includes a block copolymer or a graft copolymer having a polylactic acid sequence capable of forming a helical crystal.

[0019] Polylactic acid-based resins can be produced, for example, by a method of directly dehydrating and condensing lactic acid, as described in JP-A-59-096123 and JP-A-7-033861, or by a method of ring-opening polymerization using lactide, a cyclic dimer of lactic acid, as described in U.S. Pat. Nos. 2,668,182 and 4,057,357.

[0020] The weight average molecular weight (Mw) of the polylactic acid resin is preferably 50,000 to 1,000,000.

[0021] <Other ingredients> <<Inorganic filler>> For example, in order to make the polymeric piezoelectric material into a transparent film suppressing the generation of voids such as air bubbles, inorganic fillers such as hydroxyapatite may be nano-dispersed in the polylactic acid resin piezoelectric material, but nano-dispersing the inorganic filler requires a large amount of energy to break down the agglomerates, and if the filler is not nano-dispersed, the transparency of the film may decrease. When the polylactic acid resin piezoelectric material contains an inorganic filler, the content of the inorganic filler relative to the total mass of the polylactic acid resin piezoelectric material is preferably less than 1 mass%. In addition, when the polylactic acid-based resin piezoelectric material contains components other than polylactic acid-based resin, the content of the components other than polylactic acid-based resin is preferably 20 mass % or less, and more preferably 10 mass % or less, of the total mass of the polylactic acid-based resin piezoelectric material.

[0022] <<Crystallization accelerator (crystal nucleating agent)>> The crystallization promoter is not particularly limited as long as it has the effect of promoting crystallization, but it is preferable to select a substance having a crystal structure with a lattice spacing close to that of the crystal lattice of polylactic acid, because the closer the lattice spacing, the more effective the substance is as a nucleating agent. Examples of the organic substances include zinc phenylsulfonate, melamine polyphosphate, melamine cyanurate, zinc phenylphosphonate, calcium phenylphosphonate, and magnesium phenylphosphonate, and inorganic substances such as talc and clay. Among them, zinc phenylphosphonate is preferred because it has a lattice spacing similar to that of polylactic acid and can provide a good crystal formation promoting effect. The crystallization promoter used can be a commercially available one. Specific examples include zinc phenylphosphonate; Ecopromote (manufactured by Nissan Chemical Industries, Ltd.). The content of the crystal nucleating agent is usually 0.01 to 1.0 part by mass, and preferably 0.01 to 0.5 part by mass, based on 100 parts by mass of the polylactic acid resin. From the viewpoint of transparency, it is preferable that the polylactic acid-based resin piezoelectric material does not contain any components other than the polylactic acid-based resin.

[0023] <Characteristics of polylactic acid resin piezoelectric film> The average value of birefringence of the in-plane orientation of the polylactic acid-based resin piezoelectric film of the present invention measured at multiple points in the perpendicular direction (TD direction) is 1×10 -2 A larger value is preferred. The piezoelectric constant d14 of the polylactic acid resin piezoelectric film of the present invention is preferably 3.0 pC / N or more. The degree of crystallinity Wc of the polylactic acid resin piezoelectric film of the present invention, calculated by the following formula (I), is preferably 40% or more. Wc [%] = ΔHm / ΔH0 × 100 (I) ΔHm: Melting enthalpy measured by DSC [J / g] ΔH0: Enthalpy of complete crystallization of polylactic acid 93 [J / g]

[0024] <<Birefringence of polylactic acid-based piezoelectric film>> As described above, the average birefringence of the polylactic acid-based resin piezoelectric film of the present invention is 1×10 -2 Greater than. The polylactic acid resin piezoelectric film of the present invention has uniform molecular orientation, and therefore can exhibit such a high birefringence value. Here, "average value of in-plane orientation birefringence measured at multiple points in the perpendicular direction (TD direction)" refers to the average value of multiple in-plane orientation birefringence measured when multiple measurement points are set evenly in the perpendicular direction (TD direction) to the sheet flow direction (MD direction) except for the clipped portions at both ends, and light is incident perpendicularly to the film surface at those measurement points to measure the in-plane orientation birefringence.

[0025] [Method of measuring birefringence] Using the "KOBRA 21D" model manufactured by Oji Scientific Instruments, birefringence Δn can be measured in the orthogonal direction (TD) to the width direction of the film. The birefringence is measured at a plurality of points at predetermined intervals in the orthogonal direction (TD direction) of the polylactic acid-based resin piezoelectric film, and the average value is calculated.

[0026] <<Piezoelectric constant d14 of polylactic acid-based resin piezoelectric film>> The piezoelectric property of the polylactic acid-based resin piezoelectric film can be evaluated, for example, by measuring the piezoelectric constant d14 of the polylactic acid-based resin piezoelectric film. As described above, the piezoelectric constant d14 of the polylactic acid resin piezoelectric film of the present invention is 3.0 pC / N or more. The piezoelectric constant d14 is a constant that represents the piezoelectric performance, and the larger the value of the piezoelectric constant d14, the higher the piezoelectricity. The piezoelectric constant d14 can be determined, for example, by using the stress-charge method described below, by applying stress to a film cut out along the orientation direction and measuring the amount of charge generated.

[0027] [Method for measuring piezoelectric constant d14] A test piece is prepared by cutting a polylactic acid-based resin piezoelectric film at a position 100 mm from the center and end in the orthogonal direction (also called TD direction or width direction) to a direction at an angle of 45 mm to the molecular orientation direction (TD direction in this invention) and a direction at an angle of 25 mm to the 45° direction to prepare a test piece. Next, electrodes are prepared on both sides of the film of the test piece using a sputtering device. From the test piece film with electrodes formed on both sides, cut 20 mm in the direction at 45° to the TD direction and 10 mm in the direction perpendicular to the 45° direction to obtain a rectangular film sample for piezoelectric constant measurement. The piezoelectric constant d14 of the obtained sample is measured using a piezo reader (LPF02) manufactured by Lead Techno Corporation, with a tensile stress of 1 N and a force of 0.25 N being applied as measurement conditions.

[0028] <<Other characteristics of polylactic acid resin piezoelectric film>> The haze of the polylactic acid resin piezoelectric film is preferably 0.1-10, and more preferably 0.1-5. The haze can be measured in accordance with JIS-K7136, for example, by using a HAZE METER NDH-4000 manufactured by Nippon Denshoku Industries Co., Ltd. for a polylactic acid-based resin piezoelectric film having a thickness of 0.05 mm.

[0029] The polylactic acid resin piezoelectric film of the present invention is a piezoelectric film in which the molecular orientation is aligned in a certain direction (TD direction) despite being biaxially stretched, and exhibits the above-mentioned characteristics, resulting in an excellent piezoelectric film with high piezoelectricity. The polylactic acid resin piezoelectric film of the present invention can be obtained using a sequential biaxial stretching method, so that it is a piezoelectric film that can be easily made large in area, has high thickness accuracy without thickness unevenness, and can easily be made thin to 50 μm or less.

[0030] (Method of manufacturing polylactic acid resin piezoelectric film) The method for producing a polylactic acid-based resin piezoelectric film of the present invention includes the steps of: (I) A step (A) of melt-extruding a polylactic acid-based resin into a thin film to obtain a film; (II) after step (A), a step (B) of stretching the film in the machine direction (MD) of the film; (III) after step (B), a step (C) of stretching the film in a direction perpendicular to the machine direction (MD), (IV) after step (C), a step (D) of heat treating the film to crystallize it; Includes. The method for producing a polylactic acid-based resin piezoelectric film of the present invention includes the steps of: The stretching temperature (T MD ) is 130 to 250 ° C., The stretch ratio (X MD ) is more than twice as large, The stretching temperature (T TD ) is 55 to 80°C, The stretching ratio (X TD ) is the stretch ratio in the machine direction (MD direction) (X MD ) is more than twice as much.

[0031] By including all of the above steps (I) to (IV) and further specifying in steps (B) and (C) the stretching ratios for stretching in the machine direction (MD) and the orthogonal direction (TD) of the film, as well as the temperatures during stretching in the machine direction (MD) and the orthogonal direction (TD), within specific ranges, it is possible to produce a polylactic acid-based resin piezoelectric film in which the molecules are oriented in a certain direction. Each step will be described in detail below.

[0032] <(I) Process (A)> In step (A), a polylactic acid resin is melt-extruded into a thin film to form a film.

[0033] <(II) Process (B)> In the step (B), the film formed in the step (A) is stretched in the machine direction (MD) of the film. The stretching temperature (T MD ) is 130 to 250°C. The stretch ratio (X MD ) is more than twice as high. The stretching temperature (T MD The stretching temperature (T MD ) is more preferably a high temperature of about 200°C, more preferably 180 to 250°C, even more preferably 190 to 250°C, and particularly preferably 200 to 240°C. In the present invention, the stretching temperature (T MDThe temperature of 130 to 250°C in the above table indicates the film temperature (temperature applied to the film). For example, when the heating device is in direct contact with the film, the temperature of the heating device can be interpreted as the film temperature (temperature applied to the film). On the other hand, when the heating device and the film are separated, the temperature of the heating device does not necessarily become the film temperature. For example, when stretching a film in the machine direction (MD direction) using the stretching device shown in FIG. 1 used in the following examples, in order to make the film temperature 130 to 250°C, it is recommended to set the infrared heater (IR heater) to about 140 to 260°C. When stretching in the machine direction (MD), the means for heat-treating the film is not limited to the above-mentioned infrared heater (IR heater). For example, if the roll that transports the film in the machine direction itself has a heating function, the roll having the heating function may be used. The film may be heated by using an infrared heater (IR heater) in combination with a roll heating means.

[0034] <(III) Process (C)> In step (C), the film stretched in the machine direction (MD) in step (B) is stretched in a direction (TD) perpendicular to the machine direction (MD). The stretching temperature (T TD ) is 55 to 80 degrees Celsius. The stretching ratio (X TD ) is the stretch ratio in the machine direction (MD direction) (X MD In other words, the stretch ratio in the machine direction (MD) (X MD ) is 2 times or more, so the stretch ratio in the machine direction (MD) is 2 times or more compared to the stretch ratio in the perpendicular direction (TD) (X TD ), which is more than four times higher. For example, the stretch ratio in the MD direction (X MD When the stretch ratio in the TD direction (X TD ) is 4 times or more, and the stretch ratio in the MD direction (X MDWhen the stretch ratio in the TD direction (X TD ) is more than six times higher. Stretching ratio in TD direction (X TD ) is preferably 4 to 9 times, more preferably 4 to 8 times, and even more preferably 4 to 7 times.

[0035] In this way, in the present invention, the stretching ratio in the MD direction (X MD ) is stretched in the MD direction at a stretch ratio of 2 times or more, and then the stretch ratio in the TD direction (X TD ) is the stretching ratio in the MD direction (X MD ), i.e., four or more times, and the temperature during stretching in the MD direction is set to a high temperature of 130 to 250°C, and the temperature during stretching in the TD direction is set to 55 to 80°C. This makes it possible to align the molecular orientation in a certain direction (TD direction) despite the fact that the film is stretched in two axes.

[0036] The stretching temperature (T TD ) is the stretching temperature (T MD ) is important. The stretching temperature (T TD ) is preferably 65 to 80°C, and more preferably 70 to 75°C. The above stretching temperature (T TD The temperature of 55 to 80°C in the drawing indicates the film temperature (temperature applied to the film). For example, when a film is stretched in the MD direction using the stretching device shown in Figure 2 used in the following examples, the temperature of the stretching zone of the tenter is set to 55 to 80°C.

[0037] <(IV) Process (D)> In step (D), the film stretched in the orthogonal direction (TD) in step (C) is heat-treated to crystallize it. In the step (D), the heat treatment temperature is preferably 100 to 160°C. The heat treatment step in step (D) is carried out in order to crystallize the polylactic acid-based resin and to orient and crystallize the polylactic acid-based resin film. Here, the "heat treatment" step can also be called a "thermal setting" step or an "annealing" step. The heat treatment temperature of 100 to 160°C indicates the film temperature (temperature applied to the film). For example, after stretching the film in the MD direction using the stretching device shown in Fig. 2 used in the following examples, the temperature of the heat fixing zone of the tenter is set to 100 to 160°C as the heat treatment step. If the heat treatment temperature in step (D) is too high, the film thickness precision deteriorates, so it is preferable to set the temperature between 100° C. and 160° C., which is the melting point or lower, taking into consideration the crystallization temperature. The heat treatment time in step (D) is preferably from 1 second to 10 minutes, and more preferably from 1 second to 5 minutes. EXAMPLES

[0038] The present invention will be described in more detail below with reference to examples, but the scope of the present invention is not limited to these examples.

[0039] Example 1 As the polylactic acid resin, Nature Works' polylactic acid resin 4032D (D content = 1.4%) was used. A polylactic acid resin was extruded into a film shape from a 300 mm wide T-die at 230°C using a single screw extruder with a diameter of φ50 mm. The extruded film was quenched with a cooling roll at about 40°C to obtain an unstretched film. The obtained film was preheated with a temperature-controlled roll at about 60°C, and an infrared heater (IR heater) was installed at a height of 25 mm from the film. While adjusting the temperature of the infrared heater to 220°C so that the film temperature was 210°C, the film was stretched 2.0 times in the film flow direction (MD direction) due to the difference in peripheral speed between the rolls. The film width at this point was 220 mm. FIG. 1 shows a schematic diagram of a stretching device used for performing such longitudinal stretching in the machine direction. In FIG. 1, reference numeral 1 denotes a nip roll, reference numeral 2 denotes a low-speed roll, reference numeral 3 denotes a high-speed roll, reference numeral 4 denotes an IR heater, and reference numeral 5 denotes the machine direction (MD) of the film. Next, in the tenter, both ends of the film were held with clips in the direction perpendicular (TD) to the film flow direction (MD), the tenter's preheating / stretching zone was set to 70°C, and the film was stretched 4.5 times (tenter entrance width 190 mm, exit width 855 mm), and the film was treated at 130°C for 20 seconds in the heat treatment (heat setting) process. After that, the clip-held portions on both ends of the film were removed at the tenter exit, yielding a film with an effective width of 750 mm and a thickness of 50 μm. FIG. 2 shows a schematic diagram of a stretching device used for performing the transverse stretching in the orthogonal direction. In FIG. 2, reference numeral 11 denotes a tenter entrance, reference numeral 12 denotes a preheating zone, reference numeral 13 denotes a stretching zone, reference numeral 14 denotes a heat setting zone, reference numeral 15 denotes a tenter exit (TD direction), and reference numeral 16 denotes the machine direction (MD direction) of the film.

[0040] [Measurement of piezoelectric constant d14] The obtained polylactic acid-based resin piezoelectric film was cut at a position 100 mm from the center and end in the transverse direction (TD direction, also called the width direction) to prepare a test piece, with a length of 45 mm at a 45° angle to the molecular orientation direction (TD direction) and a length of 25 mm at a right angle to the 45° angle direction. Next, electrodes were prepared on both sides of the film of the test piece using a sputtering device. A rectangular film was cut from the test piece film with electrodes formed on both sides in a direction at 45° to the TD direction and in a direction perpendicular to the 45° direction to obtain a sample for measuring the piezoelectric constant. The piezoelectric constant d14 of the obtained sample was measured using a Piezo Reader (LPF02) manufactured by Lead Techno Corporation. The piezoelectric constant d14 of the piezoelectric film obtained in Example 1 was 7.4 pC / N.

[0041] [Measurement of birefringence and orientation angle] The birefringence Δn of the obtained piezoelectric film was measured at 25 mm intervals (30 points) in the TD direction (width direction) of the film using KOBRA21D manufactured by Oji Scientific Instruments Co., Ltd. In addition, the angle between the TD direction (width direction) and the principal axis direction of the orientation angle (such angle is also called the "principal axis angle in the width direction") was measured at 25 mm intervals (30 points) in the TD direction (width direction) of the film using KOBRA21D manufactured by Oji Scientific Instruments Co., Ltd. The average value of the birefringence Δn in the width direction of the piezoelectric film obtained in Example 1 was 0.021. The average value of the principal axis angle in the width direction of the piezoelectric film obtained in Example 1 was 4.1, and the principal axis direction of the orientation angle was 5° or less with respect to the TD direction (width direction).

[0042] [Hayes] The haze of the obtained piezoelectric film was measured using a haze measuring device, Haze Meter NDH-4000, manufactured by Nippon Denshoku Industries Co., Ltd.

[0043] [Film thickness] The obtained piezoelectric film was measured using a digital indicator (U-30A manufactured by Sony Magnescale Corp.).

[0044] The results of various measurements on the polylactic acid resin piezoelectric film obtained in Example 1 are shown in Table 1 below. FIG 3 shows the measurement results of the angle between the main axis direction and the orthogonal direction (TD direction) (such angle is also called the main axis angle) of the orientation angle of the polylactic acid-based resin piezoelectric film obtained in Example 1. In the graph of FIG 3, the results of two measurements are shown by a solid line and a dotted line, respectively. As shown in FIG 3, the average value of the angle between the main axis direction and the TD direction of the orientation angle of the polylactic acid-based resin piezoelectric film obtained in Example 1 was within 5°.

[0045] (Examples 2 to 3) A polylactic acid resin piezoelectric film was produced in the same manner as in Example 1, except that the stretching conditions in Example 1 were changed as shown in Table 1. The results of various measurements on the polylactic acid resin piezoelectric films obtained in Examples 2 and 3 are shown in Table 1 below. 4 and 5 show the measurement results of the orientation angle between the principal axis direction and the orthogonal direction (TD direction) in the polylactic acid resin piezoelectric films obtained in Examples 2 and 3, respectively.

[0046] (Comparative Examples 1 to 3) A polylactic acid resin piezoelectric film was produced in the same manner as in Example 1, except that the stretching conditions in Example 1 were changed as shown in Table 1. The results of various measurements on the polylactic acid resin piezoelectric films obtained in Comparative Examples 1 to 3 are shown in Table 1 below. 6 to 8 show the measurement results of the orientation angle between the principal axis direction and the orthogonal direction (TD direction) in the polylactic acid resin piezoelectric films obtained in Comparative Examples 1 to 3, respectively.

[0047] [Table 1]

[0048] From the above examples, it was confirmed that the polylactic acid resin piezoelectric film of the present invention has molecules oriented in one direction, exhibits high piezoelectricity, has good thickness accuracy, and can be made large in area and thin in thickness.

Claims

1. A step (A) of melt-extruding a polylactic acid-based resin into a thin film to obtain a film; After the step (A), a step (B) of stretching the film in the machine direction (MD) of the film; A method for producing a polylactic acid-based resin piezoelectric film, comprising, after step (B), a step (C) of stretching the film in a direction (TD direction) perpendicular to the machine direction (MD direction), A stretching temperature (TTD) for stretching in the orthogonal direction (TD direction) in the step (C) is set lower than a stretching temperature (TMD) for stretching in the machine direction (MD direction) in the step (B); The method for producing a polylactic acid based resin piezoelectric film, wherein the stretching ratio (X TD ) in the orthogonal direction (TD) in the step (C) is equal to or greater than twice the stretching ratio (X MD ) in the machine direction (MD).

2. The method for producing a polylactic acid based resin piezoelectric film according to claim 1 , further comprising, after step (C), a step (D) of heat treating the film to crystallize it.

3. The stretching temperature (T MD ) is 130 to 250° C., The stretching ratio (X MD ) is more than twice as large, The stretching temperature (T TD ) is 55 to 80° C., The stretching ratio (X TD ) is the stretching ratio in the machine direction (MD direction) (X MD ) is more than twice as much as A method for producing the polylactic acid resin piezoelectric film according to claim 1 or 2.

4. 3. The method for producing a polylactic acid based resin piezoelectric film according to claim 2, wherein the temperature of the heat treatment in the step (D) is 100 to 160° C.

5. The stretching temperature (T MD 5. The method for producing a polylactic acid based resin piezoelectric film according to claim 3, wherein the temperature is 180 to 250° C.

6. The stretching ratio (X TD 6. The method for producing a polylactic acid based resin piezoelectric film according to claim 3, wherein the ratio of the thickness of the piezoelectric film to the thickness of the piezoelectric film is 4 to 6 times.

Citation Information

Patent Citations

  • Improved silver halide color photographic photosensitive material

    JP1978013414A

  • High polymer piezo-electric material

    JP1993152638A

  • Uniaxially oriented film for piezoelectric laminate

    JP2017075332A

  • Production method of polylactic acid oriented sheet, polylactic acid oriented sheet, and production method of secondary molded product

    JP2019026742A

  • Piezoelectric polymer material, process for producing same, and piezoelectric element

    WO2010104196A1