Expandable polystyrene resin particles

By incorporating specific additives and surface features into expandable polystyrene resin particles, the issues of excessive softening, powder exfoliation, and blocking are mitigated, resulting in efficient and high-quality foamed molded products.

JP7569206B2Active Publication Date: 2024-10-17KANEKA CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020191338
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-18
Publication Date
2024-10-17
Estimated Expiration
2040-11-18

AI Technical Summary

Technical Problem

Conventional methods for producing expandable polystyrene resin particles result in excessive softening during molding, leading to powder exfoliation and blocking issues, while also extending the molding cycle.

Method used

The use of polystyrene as a base resin with specific additives such as fatty acid metal salts, methylphenyl silicone, and stearic acid triglyceride, along with controlled surface cracks and blowing agents, helps maintain the softening point and prevents powder exfoliation and blocking, while shortening the molding cycle.

Benefits of technology

The solution effectively suppresses powder exfoliation and blocking, maintains the resin's softening point, and reduces the molding cycle without excessive softening, ensuring high-quality foamed molded products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569206000001
    Figure 0007569206000001
  • Figure 0007569206000002
    Figure 0007569206000002
Patent Text Reader

Abstract

To provide expandable polystyrene resin particles which are prevented from blocking with exfoliation of powder suppressed and have a reduced molding cycle without excessively lowering a softening temperature of the resin.SOLUTION: Expandable polystyrene resin particles comprise, relative to 100 pts.wt. of an expandable polystyrene resin particle main body containing polystyrene as a base resin and 0.01 pt.wt or more to less than 0.50 pt.wt. of a plasticizer relative to 100 pts.wt of the base resin, 0.14 to 0.45 pt.wt of a fatty acid metal salt, 0.03 to 0.06 pt.wt. of methylphenylsilicone, and 0.03 to 0.20 pt.wt. of stearic acid triglyceride derived from hydrogenated soybean oil, which are added on a surface of the expandable polystyrene resin particle main body, where a particle diameter is 0.45 to 1.00 mm.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to expandable polystyrene-based resin particles. [Background technology]

[0002] Expandable polystyrene resin particles are relatively inexpensive, can be expanded using steam or other methods without the need for special methods, and provide excellent cushioning and insulation properties, making them a socially useful material.

[0003] The expandable polystyrene-based resin particles are produced, for example, by a method of impregnating polystyrene-based resin particles with a blowing agent (i.e., a volatile aliphatic hydrocarbon that only slightly swells the particles, such as butane, pentane, etc.) in an aqueous suspension. The expandable polystyrene-based resin particles produced in this manner are used as a raw material for producing foamed molded articles.

[0004] The method for industrially and economically producing a foamed molded article is as follows. Expandable polystyrene resin particles are made into pre-expanded particles by steam or the like. The pre-expanded particles are filled into a closed mold having a desired shape and a large number of small holes drilled in the wall surface. A heating medium such as steam is ejected from the small holes in the mold to heat the pre-expanded particles to a temperature above their softening point, causing them to fuse together. After that, the particles are cooled and removed from the mold to produce a foamed molded article of the desired shape.

[0005] In recent years, the growing interest in environmental issues has led to an increased demand for energy saving, and there is a demand for expandable polystyrene resin particles that can be expanded with a small amount of steam. As a technology for satisfying such market demands, for example, Patent Document 1 discloses a technology in which butyl acrylate is copolymerized with styrene to lower the softening point of the resin, thereby enabling low-pressure molding and reducing the amount of steam.

[0006] In Patent Document 2, the softening point of the resin is lowered by using a plasticizer, and methylphenyl silicone oil is applied to the surface of the expandable resin particles, thereby enabling low-pressure molding, and even during low-pressure molding, the pre-expanded particles are sufficiently fused together, making it possible to produce a foamed molded product with sufficient mechanical properties such as bending strength. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2019-65074 A [Patent Document 2] JP2007-246705A Summary of the Invention [Problem to be solved by the invention]

[0008] However, the above-mentioned conventional techniques have room for improvement. Specifically, in the conventional techniques described in Patent Documents 1 and 2, the softening point of the resin is lowered to achieve low-pressure molding and shorten the molding cycle. However, there is a problem in that the resin is excessively softened during molding.

[0009] An object of the present invention is to provide expandable polystyrene-based resin particles which can suppress powder peeling, prevent blocking, and shorten the molding cycle without excessively lowering the softening point of the resin. [Means for solving the problem]

[0010] The present inventors have conducted intensive research aimed at solving the above problems and have completed the present invention. That is, the present invention relates to the following [1] to [4]. [1] Expandable polystyrene-based resin particles having a particle diameter of 0.45 to 1.00 mm, the particles being formed by adding, to a surface of the expandable polystyrene-based resin particle body, 0.14 to 0.45 parts by weight of a fatty acid metal salt, 0.03 to 0.06 parts by weight of methylphenyl silicone, and 0.03 to 0.20 parts by weight of stearate triglyceride derived from hydrogenated soybean oil, per 100 parts by weight of expandable polystyrene-based resin particle body, which contains 0.01 part by weight or more and less than 0.50 part by weight of a plasticizer relative to 100 parts by weight of the base resin, and the particle diameter of the expandable polystyrene-based resin particles being 0.45 to 1.00 mm. [2] The expandable polystyrene-based resin particle according to [1], wherein the expandable polystyrene-based resin particle body has surface cracks on its surface, and the average number of intersecting cracks per 100 μm of straight line on the surface of the expandable polystyrene-based resin particle body is 4 / 100 μm to 15 / 100 μm. [3] The expandable polystyrene-based resin particles according to [1] or [2], containing 2.0 to 7.0 parts by weight of a foaming agent per 100 parts by weight of the expandable polystyrene-based resin particles, the foaming agent including an aliphatic hydrocarbon having 3 to 5 carbon atoms. [4] The expandable polystyrene-based resin particles according to any one of [1] to [3], containing 0.5 to 2.5 parts by weight of a foaming assistant having a boiling point of 50 to 90°C per 100 parts by weight of the expandable polystyrene-based resin particles. [5] Expanded particles obtained by expanding the expandable polystyrene-based resin particles according to any one of [1] to [4]. [6] A foamed molded article obtained by molding the foamed beads described in [5]. Effect of the Invention

[0011] According to the present invention, expandable polystyrene-based resin particles can be obtained which prevent blocking while suppressing peeling of powder and shortens the molding cycle without excessively lowering the softening point of the resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to each configuration described below, and various modifications are possible within the scope of the claims. In addition, embodiments and / or examples obtained by appropriately combining technical means disclosed in different embodiments and / or examples are also included in the technical scope of the present invention. In addition, unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more (including A and larger than A) and B or less (including B and smaller than B)".

[0013] As a result of intensive research by the present inventors, it was found that the above-mentioned Patent Documents 1 and 2 have the following problems. Specifically, in the methods disclosed in Patent Documents 1 and 2, the softening point of the resin is lowered by copolymerizing a type of monomer that significantly lowers the softening point of the base resin as a monomer constituting the base resin (polymer) or by incorporating a large amount of plasticizer into the resin. Here, when a foamed molded product is produced by in-mold foaming, the molding cycle described below is usually repeated continuously, so that the same mold is used repeatedly and continuously. Then, when a foamed molded product is produced using the expandable polystyrene-based resin particles produced by the methods disclosed in Patent Documents 1 and 2, the external additives and the resin itself peeled off from the expandable polystyrene-based resin particles may adhere to the slits of the mold and cause the slits to become clogged, so that the mold must be cleaned at least periodically. In addition, there is a risk that the resin, etc., adhered to the slits of the mold may damage the foamed molded product, thereby impairing the surface beauty of the foamed molded product.

[0014] The present inventor has completed the present invention in order to solve such problems.

[0015] The present invention relates to expandable polystyrene-based resin particles having an expandable polystyrene-based resin particle body containing 0.01 to 0.50 parts by weight of a plasticizer relative to 100 parts by weight of the base resin, with 0.15 to 0.45 parts by weight of a fatty acid metal salt, 0.03 to 0.06 parts by weight of methylphenyl silicone, and 0.03 to 0.20 parts by weight of stearate triglyceride derived from hydrogenated soybean oil being added to the surface of the expandable polystyrene-based resin particle body relative to 100 parts by weight of the expandable polystyrene-based resin particle body, and with a particle diameter of 0.45 to 1.00 mm. With such a constitution, the expandable polystyrene-based resin particles of the present invention can suppress peeling of the powder, prevent blocking, and shorten the molding cycle without excessively lowering the softening point of the resin. In this specification, "resin" means all components constituting the expandable polystyrene resin particle body (i.e., all components contained in the expandable polystyrene resin particle body). In this specification, the molding cycle refers to the time from the start of clamping the mold to the point at which the foamed molded body is removed from the mold. Specifically, the manufacturing process of the foamed molded body includes (1) a process in which the mold is closed from an open state, (2) a process in which pre-expanded particles are introduced into the closed mold, (3) a process in which steam is blown in to perform molding, (4) a process in which the heated molded body is cooled in the mold, and (5) a process in which the mold is opened and the molded body is released from the mold, and the molding cycle refers to the time required to perform (1) to (5) continuously. In this specification, the foamed particles may be referred to as pre-expanded particles.

[0016] The base resin constituting the expandable polystyrene-based resin particles in the present invention is polystyrene obtained by polymerizing one or more of the monomers described below. Monomers used in producing polystyrene include styrene and styrene derivatives such as α-methylstyrene, paramethylstyrene, t-butylstyrene, and chlorostyrene, and styrene homopolymers are preferred.

[0017] The expandable polystyrene resin particles in the present invention have a particle diameter of 0.45 mm to 1.00 mm. If it is less than 0.45 mm, the fusion property decreases. If it exceeds 1.00 mm, the molding cycle is extended. In the present invention, the particle diameter of the expandable polystyrene resin particles and the particle diameter of the expandable polystyrene resin particle body are equivalent, so in this specification, the particle diameter of the expandable polystyrene resin particle body is regarded as the particle diameter of the expandable polystyrene resin particles.

[0018] The plasticizer in the present invention is, for example, a liquid having a boiling point exceeding 90° C., such as aliphatic hydrocarbons of C7 or more, such as heptane and octane, aromatic hydrocarbons, such as toluene and xylene, diisobutyl adipate, dioctyl adipate, dibutyl sebacate, glycerin tristearate, glycerin tricaprylate, coconut oil, palm oil, rapeseed oil, etc. Coconut oil is more preferable from the viewpoint of affinity with polystyrene.

[0019] The amount of the plasticizer used in the present invention is 0.01 to 0.50 parts by weight based on 100 parts by weight of polystyrene. It is preferably 0.10 to 0.50 parts by weight, and more preferably 0.20 to 0.45 parts by weight. If the amount of the plasticizer used is less than 0.01 parts by weight, the fusion rate of the foamed molded article decreases. If it exceeds 0.50 parts by weight, the effect of suppressing slit clogging tends to be impaired.

[0020] Examples of the fatty acid metal salt in the present invention include zinc stearate, calcium stearate, magnesium stearate, aluminum stearate, zinc oleate, magnesium oleate, zinc laurate, calcium laurate, and the like. From the viewpoints of affinity with polystyrene and melting point, the metal stearates are preferred, and further, zinc stearate is more preferred since a good molded product can be obtained.

[0021] The amount of fatty acid metal salt used in the present invention is 0.14 to 0.45 parts by weight, preferably 0.15 to 0.30 parts by weight, based on 100 parts by weight of expandable polystyrene resin particles. If the amount of fatty acid metal salt used is less than 0.14 parts by weight, blocking during pre-expansion cannot be suppressed. If it exceeds 0.45 parts by weight, the amount of powder peeling increases and tends to inhibit fusion during molding.

[0022] In the present invention, the stearate triglyceride is stearate triglyceride (CAS: 8016-70-4) derived from hydrogenated soybean oil, and acts as an external additive to shorten the cooling time during molding. The stearate triglyceride derived from hydrogenated soybean oil is characterized by having no hydroxyl group in the stearate triglyceride molecule.

[0023] Stearic acid triglyceride is easily melted at room temperature and has poor handling properties, so it may be used in combination with other powdered external additives.

[0024] The amount of stearate triglyceride added in the present invention is 0.03 to 0.20 parts by weight, preferably 0.03 to 0.15 parts by weight, based on 100 parts by weight of expandable polystyrene resin particles. If the amount is less than 0.03 parts by weight, the molding cycle cannot be sufficiently improved, and if it exceeds 0.20 parts by weight, the fusion rate decreases.

[0025] The methylphenyl silicone of the present invention is preferably a polysiloxane having a structure represented by general formula (1).

[0026] [ka] General formula (1)

[0027] In the methylphenylpolysiloxane represented by the above general formula (1), Me represents a methyl group, and Ph represents a phenyl group. Furthermore, m and n in the repeating units are any natural numbers (1, 2, 3, etc.). The methylphenylpolysiloxane represented by the general formula (1) used in the present invention may be one in which the dimethyl moieties and diphenyl moieties are randomly bonded, or one in which they are regularly arranged.

[0028] In the present invention, the amount of methylphenyl silicone added is 0.03 to 0.06 parts by weight. If it is less than 0.03 parts by weight, the amount of powder peeling increases, and if it exceeds 0.06 parts by weight, the fusion rate decreases.

[0029] The expandable polystyrene-based resin particles of the present invention may further contain external additives and additives such as a fusion promoter and an antistatic agent within a range that does not impair the effects of the present invention.

[0030] The expandable polystyrene-based resin particles of the present invention may contain additives such as a foaming agent, a foaming assistant, a nucleating agent, a flame retardant, and a flame retardant assistant, within the range that does not impair the effects of the present invention.

[0031] The content of the foaming agent in the foaming agent polystyrene resin particles in the present invention is preferably 2.0 to 7.0 parts by weight, more preferably 3.0 to 6.0 parts by weight, based on 100 parts by weight of the expandable polystyrene resin particles. If it is less than 2.0 parts by weight, the fusion rate decreases, and if it exceeds 7.0 parts by weight, the molding cycle becomes longer.

[0032] The blowing agent used in the present invention is, for example, a gas or liquid having a boiling point of less than 50° C., such as aliphatic hydrocarbons such as propane, butane, and pentane, alicyclic hydrocarbons such as cyclobutane and cyclopentane, and halogenated hydrocarbons such as methyl chloride, dichlorodifluoromethane, and dichlorotetrafluoroethane. These blowing agents may be used alone or in combination of two or more. Among these blowing agents, butane is preferred because of its good blowing power.

[0033] The content of the foaming assistant in the expandable polystyrene resin particles in the present invention is preferably 0.5 to 2.5 parts by weight per 100 parts by weight of the expandable polystyrene resin particles. If it is less than 0.5 parts by weight, the fusion rate decreases, and if it exceeds 2.5 parts by weight, the molding cycle becomes longer.

[0034] The foaming assistant used in the present invention is, for example, a liquid having a boiling point of 50° C. or more and 90° C. or less, such as hexane or cyclohexane. These foaming assistants may be used alone or in combination of two or more. Among these foaming assistants, cyclohexane is preferred because of its good foaming power.

[0035] Examples of the nucleating agent used in the present invention include methyl methacrylate copolymers, polyethylene wax, talc, fatty acid bisamides, ethylene-vinyl acetate copolymers, etc. Specific examples of fatty acid bisamides include methylene bisstearylamide, ethylene bisstearylamide, hexamethylene bispalmitic acid amide, ethylene bisoleic acid amide, etc. These nucleating agents may be used alone or in combination of two or more.

[0036] The expandable polystyrene-based resin particle body in the present invention has surface cracks, which are cracks exposed on the surface of the expandable polystyrene-based resin particle, in a photograph obtained by observing the surface of the expandable polystyrene-based resin particle at a magnification of 1000 times using a scanning electron microscope (hereinafter sometimes referred to as "SEM") with an acceleration voltage of 10 kV. When four parallel straight lines are drawn at 10 μm intervals on the photograph having the surface cracks and the number of unit intersection cracks, which is the number of surface cracks intersecting with each straight line per 100 μm, is calculated, the average number of unit intersection cracks, which is the average number of unit intersection cracks of the obtained four straight lines, is preferably 4 / 100 μm to 15 / 100 μm. More preferably, it is 4 / 100 μm to 13 / 100 μm, and particularly preferably 5 / 100 μm to 12 / 100 μm.

[0037] If the average number of intersecting cracks is less than 4 / 100μm, the dispersion of the blowing agent is suppressed, the gaps between the particles are not easily filled, and the surface properties tend to deteriorate.If the number exceeds 15 / 100μm, the dispersion of the blowing agent is too high, so the gaps between the particles on the surface of the molded product are not easily filled, and the fusion properties tend to deteriorate.

[0038] The average chord length of the cells in the cross section of the foam can be controlled by the amount of nucleating agent: more nucleating agent will decrease the average chord length, and less nucleating agent will increase the average chord length.

[0039] The flame retardant and flame retardant aid contained in the present invention may be any known and commonly used one. Specific examples of the flame retardant include halogenated aliphatic hydrocarbon compounds such as hexabromocyclododecane, tetrabromobutane, and hexabromocyclohexane, brominated phenols such as tetrabromobisphenol A, tetrabromobisphenol F, and 2,4,6-tribromophenol, tetrabromobisphenol A-bis(2,3-dibromopropyl ether), tetrabromobisphenol A-bis(2,3-dibromo-2-methylpropyl ether), and tetrabromobisphenol A-dibromopropyl ether. Examples of the flame retardant include brominated phenol derivatives such as lysidyl ether and 2,2-bis[4'(2",3"-dibromoalkoxy)-3',5'-dibromophenyl]-propane, brominated styrene-butadiene block copolymers, brominated random styrene-butadiene copolymers, and brominated styrene-butadiene graft copolymers, etc., brominated butadiene-vinyl aromatic hydrocarbon copolymers (for example, EMERALD3000 manufactured by Chemtura or those disclosed in JP-T-2009-516019). These flame retardants may be used alone or in combination of two or more.

[0040] Specific examples of the flame retardant auxiliary include initiators such as cumene hydroperoxide, dicumyl peroxide, t-butyl hydroperoxide, and 2,3-dimethyl-2,3-diphenylbutane.

[0041] The expandable polystyrene-based resin particles of the present invention are pre-expanded and then heated to expand to form a foamed molded article.

[0042] As a pre-expansion method, for example, a conventional method can be used, such as using a cylindrical pre-expansion device to heat with steam or the like to cause expansion.

[0043] The method for foaming the pre-expanded particles may be, for example, a conventional method such as the so-called in-mold foaming method, in which the pre-expanded particles are filled into a mold and heated by blowing in steam or the like to obtain a foamed molded article. EXAMPLES

[0044] Examples and comparative examples are given below, but the present invention is not limited thereto. Measurement and evaluation methods were carried out as follows.

[0045] <Measurement of foaming agent and foaming assistant content> Equipment: Shimadzu GC-14B Column: PEG-20M 25% Chromosorb W 60 / 80 (3.0m x 3.0mm I.D.) Column temperature: 110℃ Detector (FID) temperature: 170℃ 1.0 g of expandable polystyrene resin particles was dissolved in 20 ml of dichloromethane, and 0.005 g of an internal standard solution (cyclopentanol) was added. The obtained expandable polystyrene resin particle solution was subjected to gas chromatography analysis under the above-mentioned conditions to measure the contents of the blowing agent and the blowing assistant.

[0046] <Measurement of external additive peeling rate> Equipment: Retsch AS2000 control Mesh: SUS mesh (opening: 250μm, 60 mesh, φ200mm) 600 g of expandable polystyrene resin particles were weighed out and sieved on an automatic sieve for 2 minutes. The powder that fell through the mesh was collected (if resin was mixed in, it was removed), and the weight was measured to determine the amount of peeling. The peeling rate was calculated using the following formula, with a value of 5% by weight or less being considered acceptable. Peeling rate [%] = Amount of powder passing through the sieve [g] / Total amount of external additives added [g] × 100

[0047] <Average number of intersecting cracks on the surface of expandable polystyrene resin particles> Equipment: JSM-6060LV manufactured by JEOL Voltage applied: 10kV Working distance: 19mm Vacuum degree: SEI Magnification: 1000x On a photograph obtained by observing the surface of the expandable polystyrene resin particle body with a scanning electron microscope (SEM) at a magnification of 1000 times, four parallel straight lines were drawn at 10 μm intervals so that a straight line parallel to the long side direction of the photograph crossed the short side of the photograph, and the number of surface cracks intersecting each line (100 μm long) was counted. Note that in the measurement, not only cracks crossing the straight lines but also cracks tangent to the straight lines were counted as intersecting cracks. The average number of surface cracks intersecting with four straight lines per 100 μm was calculated as the average number of intersecting cracks in one particle. Furthermore, the average number in the bodies of five expandable polystyrene resin particles was taken as the average number of intersecting cracks in the present invention.

[0048] <Blocking evaluation> Expandable polystyrene resin particles were put into a pre-expanding machine with an agitator (Daika Kogyo, BHP-301) and expanded by heating with 0.1 MPa steam, obtaining pre-expanded particles with an apparent expansion ratio of 55 times. Blocking was measured by stopping the crusher when the pre-expanded particles were discharged, passing the pre-expanded particles through a mesh with 1 cm openings, collecting and measuring the weight of the particles, and calculating the ratio of the pre-expanded particles recovered to the resin put in. A blocking amount of less than 1% by weight was considered acceptable.

[0049] The amount of blocking was evaluated according to the following three levels. ◎: Less than 0.1% by weight 〇: 0.1% by weight or more and less than 1.0% by weight ×: 1.0% by weight or more

[0050] <Moldability and molding cycle evaluation> (1) Molding cycle evaluation Using a molding machine [FOAMSTAR TH-90VM II], the pre-expanded particles produced by the method described in <Blocking evaluation> were filled into a box-shaped mold measuring 502 mm in length, 360 mm in width, 106 mm in height, and 21 mm in bottom thickness. Using water vapor as a heating medium, molding was performed in the mold at a steam source pressure of 0.58 MPa. After water cooling for 7 seconds, vacuum cooling was performed. When the surface pressure reached 0.3 MPa or less, vacuum cooling was terminated, and a box-shaped foamed molded product was obtained. At this time, the time taken from the time the pre-expanded particles were filled into the mold to the time the foamed molded body was discharged (the foamed molded body was released from the mold) was defined as the "total cycle time," and the time taken from the time the vacuum cooling started to the time the vacuum cooling ended was defined as the "cooling time."

[0051] The foamed molded article obtained by the above-mentioned method was dried at room temperature for 24 hours, and then the following moldability evaluation was carried out. (2) Evaluation of adhesion of foam molded products The obtained foamed molded article was broken, and the broken surface was observed to determine the proportion of particles that had broken, rather than the particle interfaces. Those in which 80% or more had fused were deemed to have passed the test. (3) Surface property evaluation of foamed molded products The surface condition of the foamed molded article was evaluated by visual observation. A higher value indicates a beautiful surface condition with fewer gaps between particles, and a score of 4 or more out of 5 was considered to be acceptable.

[0052] 5: I can't find any gaps 4: There are some gaps, but they are barely noticeable. 3: There are some gaps here and there, but overall it is acceptable 2: Gaps are noticeable 1: Many gaps

[0053] The external additives used in the examples are listed below. Methylphenyl silicone Methylphenyl polysiloxane, Viscosity (25℃) 400mm 2 / s, refractive index (25°C) 1.505 (Shin-Etsu Silicone Co., Ltd., KF-54)

[0054] Fatty acid metal salt: Zinc stearate (Zinc Stearate GF-200: NOF Corp.)

[0055] Stearic acid triglyceride: Melting point 67 degrees (Rikemal VT-50, manufactured by Riken Vitamin Co., Ltd., stearic acid triglyceride derived from hydrogenated soybean oil)

[0056] Others: Castor oil, melting point 84 degrees (Castarwax, NOF Corp., hydroxystearic acid triglyceride derived from hydrogenated castor oil)

[0057] Example 1 <Production of Expandable Polystyrene-Based Resin Particles> In a 6-liter autoclave equipped with a stirrer, 88 parts by weight of pure water, 0.156 parts by weight of tricalcium phosphate, 0.01 parts by weight of sodium dodecyl diphenyl ether disulfonate, 0.05 parts by weight of polyethylene wax, 0.21 parts by weight of benzoyl peroxide and 0.21 parts by weight of 1,1-bis(t-butylperoxy)cyclohexane as initiators, and 0.4 parts by weight of coconut oil as a plasticizer were charged. Then, while stirring at 250 rpm, 100 parts by weight of styrene monomer was charged, and the temperature was raised to 98°C. After 1 hour and 30 minutes, 0.10 parts by weight of tricalcium phosphate was added. The mixture was then held at 98°C for 2 hours and 30 minutes to obtain polystyrene resin particles. Next, 2.1 parts by weight of cyclohexane as a foaming assistant and 7 parts by weight of normal rich butane as a foaming agent were pressed into the autoclave, and the temperature was raised again to 120° C. After that, the mixture was kept at 120° C. for 2 hours, cooled to room temperature, and the polymerized slurry was taken out from the autoclave. The polymerized slurry taken out was washed and dehydrated to obtain expandable resin particles. <Production of expandable polystyrene-based resin particles having surface cracks> 100 parts by weight of the expandable resin particles obtained by the method described in <Production of Expandable Polystyrene-Based Resin Particles> were mixed and stirred to uniformly coat the resin particle surfaces with 0.03 parts by weight of polyoxyethylene cetyl ether (P-208, manufactured by NOF Corp.) in a 3% by weight aqueous solution. After that, the water was dried using an airflow dryer, and the particles were heated at 50°C for 20 minutes in a box-type ventilation dryer (manufactured by Tanaka Chemical Machinery Co., Ltd.), and then a sieve with a specified mesh size was used to obtain expandable polystyrene-based resin particle bodies having surface cracks with particle diameters of 0.60 to 1.00 mm.

[0058] <Production of Expandable Polystyrene-Based Resin Particles> In a polyethylene bag containing the expandable polystyrene resin particle body having surface cracks, 0.05 parts by weight of methylphenyl silicone (KF-54) was added to 100 parts by weight of the expandable polystyrene resin particle body, and the bag was shaken about 100 times to coat the particles evenly. Next, 0.15 parts by weight of zinc stearate and 0.038 parts by weight of triglyceride stearate were added, and the bag was shaken about 100 times to coat the particles evenly, to obtain expandable polystyrene resin particles.

[0059] The expandable polystyrene-based resin particles thus obtained were used to carry out the above-mentioned evaluations on the expandable polystyrene-based resin particles, pre-expanded particles, and foamed molded articles. The results are shown in Table 1.

[0060] (Examples 2 and 3, Comparative Examples 1 to 6) Expandable polystyrene resin particles, pre-expanded particles, and foamed molded articles were obtained and evaluated in the same manner as in Example 1, except that the amounts of plasticizer, foaming agent, foaming assistant, polyoxyethylene cetyl ether (NOF Corporation, P-208), methylphenyl silicone (KF-54), zinc stearate, and stearate triglyceride, the range of particle size, and the average number of cross cracks were changed as shown in Table 1. Note that the castor hardened oil in Comparative Example 2 was added to the polyethylene bag containing the expandable polystyrene resin particle bodies at the same time as the zinc stearate, and was allowed to coat the surfaces of the expandable polystyrene resin particle bodies. [Table 1]

Claims

1. For 100 parts by weight of expandable polystyrene-based resin particle bodies containing polystyrene as a base resin and 0.01 part by weight or more and less than 0.50 part by weight of a plasticizer relative to 100 parts by weight of the base resin, 0.14 to 0.45 parts by weight of fatty acid metal salt, 0.03 to 0.06 parts by weight of methylphenyl silicone, 0.03 to 0.20 parts by weight of stearic acid triglyceride derived from hydrogenated soybean oil is added to the surface of the expandable polystyrene-based resin particle body, The particle size is 0.45 to 1.00 mm, the expandable polystyrene-based resin particle body has surface cracks on its surface, The expandable polystyrene-based resin particles have an average number of intersecting cracks per 100 μm of straight line on the surface of the expandable polystyrene-based resin particle body, which is 4 / 100 μm to 15 / 100 μm.

2. The foam contains 2.0 to 7.0 parts by weight of a foaming agent relative to 100 parts by weight of the expandable polystyrene-based resin particles, 2. The expandable polystyrene-based resin particles according to claim 1, wherein the foaming agent contains an aliphatic hydrocarbon having 3 to 5 carbon atoms.

3. 3. The expandable polystyrene-based resin particles according to claim 1, further comprising 0.5 to 2.5 parts by weight of a foaming assistant having a boiling point of 50 to 90° C. per 100 parts by weight of the expandable polystyrene-based resin particles.

4. 4. Expanded beads obtained by expanding the expandable polystyrene-based resin beads according to claim 1.

5. A foamed molded article obtained by molding the foamed beads according to claim 4.

Citation Information

Patent Citations

  • Foamable styrenic resin particle and method for producing styrenic resin foamed molded article

    JP2007246705A

  • Foamable polystyrene resin particle for middle-low ratio expansion molding, foamed particle, expansion molded product and manufacturing method for expansion molded product

    JP2013023565A

  • Expandable thermoplastic resin particle

    JP2015108040A

  • Foamable polystyrene resin particle

    JP2018119109A

  • Expandable polystyrene resin particle, polystyrene pre-expanded particle, and foam molding

    JP2019065074A