Process for forming polylactide-based expanded bead foams
The described process for producing expanded PLA beads with controlled crystallization and expansion addresses the challenges of high expansion and consistent processing, resulting in high expansion rates and improved mechanical properties for PLA bead foams.
Patent Information
- Application Number
- JP2021507448
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-08-31
- Filing Date
- 2019-08-21
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2039-08-21
AI Technical Summary
Existing methods face challenges in producing expanded polylactide (PLA) bead foams with high expansion coefficients and consistent processing, leading to defects and inadequate mechanical properties due to difficulties in maintaining foaming conditions and sintering without bead collapse.
A process involving pressurizing unfoamed PLA resin beads with carbon dioxide at low temperatures, followed by partial crystallization and controlled expansion to form beads with a blend of PLA stereocomplex and homocrystals, allowing for high expansion rates and improved sintering characteristics.
The process achieves high expansion rates with low density PLA beads, enabling consistent sintering and reduced defects in molded articles, with wide processing tolerances and improved mechanical properties.
Smart Images

Figure 0007569305000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for forming polylactide (PLA) based expanded bead foams. [Background technology]
[0002] Bead foam is used to make lightweight plastic articles that are difficult to manufacture using other methods such as foam extrusion and injection molding. Unlike the extrusion and injection molding processes, the bead foam process has few constraints regarding the shape of the product and can produce foams with very low densities.
[0003] Bead foam products are made by forming polymer beads that are impregnated with a blowing agent and then partially or fully expanded. Expanded beads are made by pouring the beads into a mold and heating them to soften their surfaces sufficiently to fuse ("sinter") them together to form a single mass.
[0004] PLA has thus far shown limited suitability for use in bead foaming processes. There are two main problems. The first is that of insufficient expansion. It has proven difficult to produce expanded PLA beads at the low densities seen when using other polymers such as polystyrene and polypropylene. The other main problem is that of processing. The expansion conditions need to be maintained within strict limits that are difficult to maintain consistently on an industrial production line. It has proven very difficult to obtain good sintering when producing PLA bead foams without collapsing the beads. The resulting foamed products often have defects and inadequate mechanical properties.
[0005] US Patent Application Publication No. 2016 / 003990 and US Patent No. 9,023,470 describe attempts to improve PLA bead foam processing. In these processes, the expanded PLA bead foam has a crystalline structure characterized by two melting ranges whose peaks are separated by about 5° C. to 25° C. in a DSC (differential scanning calorimetry) thermogram. This leads to some improvements, but processing options during sintering remain scarce.
[0006] US Patent No. 9,206,296 describes an attempt to solve the processing problem by using PLA beads with a core-shell structure, but this does not represent a practical solution since the core-shell bead structure is difficult and expensive to produce.
[0007] Xue et al., in J. Cellular Plastics 2018, vol 54(1), 113-119, describes a method for producing microporous sheet foams from a mixture of poly-L-lactic acid (PLLA) and poly-D-lactic acid (PDLA). In this process, a sheet with low crystallinity is made from a blend of PLLA and PDLA. The sheet is saturated with carbon dioxide at 0°C and superatmospheric pressure. The carbon dioxide saturated sheet is depressurized while cooling to avoid expansion. The sheet is then expanded by immersion in a liquid bath at 90°C to 160°C. This process reaches a volume expansion ratio of up to about 25, but the value is still less than desired. Since the starting material is a sheet rather than a bead, no subsequent shaping is performed. Summary of the Invention [Problem to be solved by the invention]
[0008] What is desired is a process for producing expanded PLA bead foams that is characterized by being economical and producing high expansion rates and foams in which the expanded beads are well sintered and therefore have good mechanical properties. [Means for solving the problem]
[0009] The present invention provides a process for making expanded PLA beads, comprising: (a) pressurizing unexpanded beads of a PLA resin blend having a crystallinity of 10 J / g or less as measured by DSC with carbon dioxide to superatmospheric pressure while maintaining a temperature of 40° C. or less; (b) heating the pressed unexpanded beads to a temperature of 90° C. to 160° C. to at least partially crystallize the PLA resin blend to form unexpanded beads saturated with carbon dioxide and partially crystallized; and thereafter (c) applying a pressure reduction to the unexpanded beads saturated with carbon dioxide to at least partially vaporize the carbon dioxide and expand the beads; and then (d) cooling the expanded beads to less than 40° C. simultaneously with and / or after step (c). Equipped with PLA resin blends include: i) a first PLA polymer containing at least 88% L-lactide units, based on the total weight of the first PLA polymer; ii) a second PLA polymer containing at least 88% D-lactide units, based on the total weight of the second PLA polymer; Including, The process wherein the first PLA copolymer and the second PLA copolymer are present in the PLA resin blend in a weight ratio of 75:25 to 98:2 or 25:75 to 2:98.
[0010] The process is suitable for industrial applications and provides a high expansion rate of the beads. Thus, the resulting expanded PLA foam has a low density. Another advantage of the present invention is that all the expansion processes can be carried out in a single manufacturing vessel.
[0011] In a second aspect, the present invention is an expanded PLA bead made by the process described above.
[0012] In a third embodiment, the expanded PLA beads include a blend of PLA resins of the present invention, the expanded PLA beads having a viscosity of 0.025 to 0.35 g / cm 3 Density and 0.5~1500mm 3 and the PLA resin blend contains PLA stereocomplex crystals having a crystal melting peak temperature of 200 to 240°C and PLA homocrystals having a melting peak temperature of 140 to 180°C.
[0013] The present invention is also a method of producing a molded article comprising introducing the expanded PLA beads of the second or third aspect into a mold, sintering, and optionally further expanding the expanded PLA beads to form a molded article. The molding process is characterized by a wide processing latitude, which simplifies the work steps and reduces defects. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The expanded bead resin beads for producing the foam in this invention are made from a PLA resin blend, which is formed from at least two starting PLA resins, a first PLA resin and a second PLA resin.
[0015] For purposes of this invention, PLA resin contains at least 90% by weight, such as at least 95% or at least 98% by weight, lactide (-OC(CH3)-C(O)-) repeat units. These polymers are readily produced by polymerizing lactic acid or, more preferably, by polymerizing lactide.
[0016] The first PLA resin is a PLLA polymer containing at least 88% L-lactide units based on the total weight of the first PLA copolymer. The first PLA resin may contain at least 92%, at least 95%, at least 97%, at least 98%, or at least 99% L-lactide units on the same basis. The first PLA resin may contain up to 100% L-lactide units. The remaining weight of the PLLA polymer, if present, may be D-lactide units. The first PLA resin may be a mixture of two or more polymers having the aforementioned proportions of L-lactide units.
[0017] The second PLA resin is a PDLA polymer containing at least 88% D-lactide units based on the total weight of the first PLA copolymer. The second PLA resin may contain at least 92%, at least 95%, at least 97%, at least 98%, or at least 99% D-lactide units on the same basis. The second PLA resin may contain up to 100% D-lactide units. The remaining weight of the PDLA polymer, if present, may be L-lactide units. The second PLA resin may be a mixture of two or more polymers having the aforementioned proportions of D-lactide units.
[0018] The first and second PLA resins may each have a sufficiently high molecular weight for melt processing applications. Number average molecular weights in the range of 20,000 to 150,000 g / mole as measured by gel permeation chromatography against polystyrene standards are generally suitable, although somewhat higher or lower values may be used in some circumstances. The molecular weights of the high D and high L starting resins may be similar to each other (e.g., the difference in number average molecular weights is no more than 20,000 g / mole).
[0019] The first PLA copolymer and the second PLA copolymer are present in the PLA resin blend in a weight ratio of 75:25 to 98:2 or 25:75 to 2:98. Preferred weight ratios are 80:20 to 95:5 and 20:80 to 95:5.
[0020] The starting unexpanded beads are conveniently made by melt blending a first PLA resin with a second PLA resin. A melt of the two resins is preferably formed at a temperature above the peak melting temperature of the PLA stereocomplex crystals (about 200°C to 240°C). The melt is solidified by cooling and is simultaneously or subsequently formed into particles. The cooling step is preferably carried out by rapidly lowering the temperature of the melt blend from above the melting temperature of the stereocomplex to below the glass transition temperature of PLA (about 60°C) to minimize crystallization during the cooling process. The PLA blend in the particles preferably has a crystallinity of 10 J / g or less by DSC until they are pressurized with carbon dioxide. DSC measurements are performed at a temperature ramp from 0°C to 270°C at a rate of 50°C / min.
[0021] A preferred method of forming beads from the PLA resin blend is to extrude the molten blended resin into strands that are chopped to length when cooled and solidified or to length after cooling and solidification. However, for purposes of the present invention, the beads are not necessarily spherical. They may be, for example, cylindrical, ellipsoidal, or other shapes. If cylindrical, the cross-section of the beads may be circular, oval, polygonal, or irregular. It is desirable for the beads to have an aspect ratio (ratio of longest orthogonal dimension to shortest orthogonal dimension) of 5 or less, particularly 2.5 or less, or 1.5 or less, since the aspect ratio promotes good packing and certain property enhancements in the final product.
[0022] The diameter of the strands and the length of the chopped particles may be, for example, 0.2 to 3 mm, in particular at least 0.5 mm, and up to 2 mm, or up to 1.5 mm, respectively. The diameter for the purposes of the present invention is the diameter of a circle having the same cross-sectional area as the strands. The strands can be extruded into a cooling bath, such as a water bath or other liquid bath, to rapidly cool and solidify before their temperature drops below the glass transition temperature, to avoid significant crystallization. A suitable bath temperature is up to 40° C., or up to 30° C.
[0023] The starting particles are unfoamed before being pressurized with carbon dioxide in step a) of the process.
[0024] In step a), the PLA resin blend particles are pressurized with carbon dioxide. This step is carried out by contacting the PLA resin beads with carbon dioxide under conditions including superatmospheric pressure and a temperature of 40° C. or less. The pressure is preferably at least 1 MPa gauge, and may be, for example, at least 3 MPa gauge, at least 4 MPa gauge, or at least 5 MPa gauge. The pressure may be, for example, up to 10 MPa gauge or up to 8 MPa gauge. The temperature may be, for example, at least −20° C. or at least 0° C., and may be up to, for example, 30° C. Particularly preferred temperatures are between 15° C. and 30° C. The pressurization step usually takes up to 10 minutes.
[0025] Once the beads are pressurized, they are heated under superatmospheric pressure to a temperature of 90°C to 160°C to at least partially crystallize the PLA resin blend without expanding the beads (step (b)). This heating step may be carried out in a hot fluid as described below. The superatmospheric pressure may be the same as in pressurization step a). The beads may be kept within this temperature range for at least 5 minutes or at least 10 minutes and for example up to 60 minutes, up to 30 minutes, or up to 20 minutes. A preferred temperature is 110°C to 140°C, and a particularly preferred temperature is 120°C to 135°C. This step (b) produces unexpanded resin beads saturated with carbon dioxide and partially crystallized.
[0026] Two types of crystals form during the partial crystallization step (b). PLA stereocomplex crystals form when PLLA and PDLA are crystallized together to form a 31-helix conformation. PLA stereocomplex crystals have a melting peak temperature (measured by DSC) of about 200-240°C. Additionally, PLA homocrystals form when either PLLA or PDLA (usually one is present in excess in the PLA resin blend) crystallizes with itself. PLA homocrystals are characterized by a melting peak temperature of about 140-180°C. As a result of the formation of these two types of crystals during the partial crystallization step, the partially crystallized particles exhibit two melting peak temperatures separated by about 20°C-100°C, and preferably 40-75°C.
[0027] The degree of crystallization occurring during the partial crystallization step may be, for example, 5% to 50% of the total weight of the PLA resin blend in the particles. Preferred amounts are, on the same basis, 10% to 35% or 15% to 30%. The degree of crystallization is determined by measuring the enthalpy of fusion of the PLA stereocomplex and the PLA homocrystals in weighed samples using DSC. A fully crystallized PLA stereocomplex is defined as having 124 J / g of stereocomplex crystals and a fully crystallized PLA homopolymer is defined as having 93 J / g of PLA homocrystals, measured in each case by DSC. The degree of crystallization in the sample is therefore calculated as follows:
number
[0028] PLA stereocomplex crystallinity can refer to the total crystallinity in the particles after the partial crystallization step, for example, 5% to 90%, 10% to 80%, 10% to 50%, or 10% to 25%, as measured using DSC.
[0029] The pressure during the partial pressurization step is sufficient to avoid the particles expanding until partial crystallinity occurs in the particles as described above. The pressures described for the saturation step a) are preferred.
[0030] Step (b) produces unexpanded beads that are partially crystallized and saturated with carbon dioxide, having a temperature between 90° C. and 160° C. In step (c), these beads are depressurized. The pressure is reduced so that the carbon dioxide injected into the beads at least partially vaporizes and expands the beads. The pressure may be reduced in the depressurization step, for example, to below 500 kPa absolute, below 250 kPa absolute, or below 101 kPa absolute. The depressurization is desirably rapid, such as over a period of 0.1 to 5 seconds.
[0031] The reduction in pressure and evaporation of the carbon dioxide causes the beads to expand. The beads may expand to at least four times their original (before expansion) volume. However, an advantage of the present invention is that much larger expansions are easily obtained. In some embodiments, the beads can expand to at least 20 times, at least 30 times, at least 35 times, or even at least 40 times their original volume. The density of the beads after expansion can be, for example, 0.025 to 0.35 g / cm. 3 In a preferred embodiment, the expanded beads have a viscosity of 0.025 to 0.05 g / cm 3 , especially 0.025~0.04g / cm 3 has a density of
[0032] Due to stretch crystallization, some additional crystallization may occur during the expansion step.
[0033] In step (d), the beads are cooled simultaneously with and / or after the expansion step to below 40°C, preferably below 30°C, to solidify the beads and create a tack-free surface that prevents the beads from sticking prematurely.
[0034] Steps (a)-(c) can be carried out in any vessel capable of being pressurized to the required pressure, and for step (b) in any vessel capable of withstanding the required temperature. Although different equipment can be used for the various steps, it is preferred to carry out at least steps (a)-(c), and preferably each of steps (a)-(d), in a single vessel. An autoclave or other pressure vessel is suitable.
[0035] Steps (a)-(c) may be performed while the beads are suspended in a thermal fluid, which may be, for example, water, an alkylene or polyalkylene glycol, silicone oil, or other material that is liquid under the temperature and pressure conditions of the various steps. Step (d) may also be performed with the beads suspended in the thermal fluid.
[0036] In a preferred process, the starting unexpanded beads are suspended in a hot fluid in a vessel. The vessel is pressurized with carbon dioxide to saturate the beads, and then the beads, still in the vessel, are heated to partially crystallize the PLA resin blend in the beads. A depressurization step is similarly performed in the same vessel by releasing the pressure.
[0037] The expanded beads, such as the partially crystallized beads, are characterized as having both PLA stereocomplex crystals having a peak melting temperature of 200-240° C. and PLA homocrystals having a peak melting temperature of about 140-180° C. The degree of crystallization of the expanded beads may also be, for example, 5%-35% of the total weight of the PLA resin blend in the particle.
[0038] The expanded beads are suitable for making molded articles in a bead molding process. In such a process, the expanded beads are introduced into a mold, the inner walls of which define the size and shape of the part to be produced. The expanded beads are heated to soften their surfaces so that adjacent beads join together to form a single molded body. Further expansion of the beads may occur during the molding step. For example, it may be desirable to only partially expand the beads in step (c) above, so that further expansion of the beads can occur during the molding process.
[0039] Bead molding can be carried out, for example, in a steam chest molding machine. In such an apparatus, expanded or partially expanded beads are introduced into a mold located in a steam chest. High pressure steam is introduced into the steam chest to heat and soften the surfaces of the beads, thereby causing adjacent beads to fuse together.
[0040] An advantage of the present invention is the wide processing latitude afforded by the use of expanded beads made according to the present invention. Previously, bead forming of expanded PLA beads was difficult because the steam temperature had to be controlled within precise limits. Because steam temperature varies with its pressure, precise temperature control requires careful control of steam pressure, which is difficult to achieve using industrial scale equipment.
[0041] A fairly wide temperature range (and consequently a wide variation in vapor pressure) can be tolerated with the present invention. The greater processing latitude is believed to be due, at least in part, to the presence of two different types of crystals that form in the PLA resin blend and the wide separation of their respective melting temperatures. Since molding can be carried out at any intermediate temperature, strict temperature control is less important and the beads are easier to mold.
[0042] The expanded beads can be used to make foams such as cups, plates, coolers and other insulation, buoys and other flotation devices, shock absorbing devices such as automobile bumper components, and the like.
[0043] The following examples are offered to illustrate the invention but are not intended to limit its scope. All parts and percentages are by weight unless otherwise specified. EXAMPLES
[0044] Examples 1 and 2 and Comparative Sample A 85% PLLA resin containing 95.5% L-lactide units and 4.5% D-lactide units and having a relative viscosity of about 4 g / dL is melt blended with 15% PDLA having a weight average molecular weight of 70,000 g / mol (GPC, polystyrene equivalent) to produce PLA Blend 1. Pellets of the starting resin are melted to the melting temperature in a twin screw extruder and extruded through a strand die into a water bath where the strands are immediately quenched to a temperature below 40° C. The strands are chopped into spherical beads having a diameter of about 1-2 mm.
[0045] PLA Blend 2 is prepared using the same procedure but with a weight ratio of 95% PLLA and 5% PDLA.
[0046] PLA Blend 1 is expanded to produce Example 1. PLA Blend 2 is expanded to produce Example 2. Pellets of PLLA are expanded to produce Comparative Sample A.
[0047] In each case, the beads are expanded as follows: A 1 L autoclave is filled with 800 mL of room temperature water. 20 g of beads and 1 g of suspending aid are added. The autoclave is sealed and pressurized to 6 MPa gauge with carbon dioxide at room temperature. The contents of the sealed autoclave are then heated to 123-135°C and held at that temperature for 15 minutes to saturate the beads with carbon dioxide and partially crystallize them. The autoclave is then depressurized to atmospheric pressure over a few seconds. Depressurization is accompanied by cooling to room temperature.
[0048] In Example 1, the beads expand 4-5 times their original volume. In Example 2, the beads expand to about 40 times their original volume. SEM micrographs of the foamed Examples 1 and 2 reveal a regular cell structure. Comparative Sample A expands to 4-5 times its original volume. It has a fairly irregular cell structure characterized by many large cells.
[0049] DSC thermograms of the expanded beads are taken. Example 1 is found to contain both PLA stereocomplex crystals (about 34 J / g) and PLLA homocrystals at about 7.7 J / g. The total crystallinity is about 36%.
[0050] Example 2 is found to contain about 4 J / g PLA stereocomplex crystals and about 21 J / g PLLA homocrystals. The total crystallinity is about 26%.
[0051] Comparative sample A contains only PLA homocrystals. The total crystallinity is about 17%.
[0052] Examples 1 and 2 sinter easily in a steam chest press at temperatures ranging from about 150°C to 200°C to produce compacts, whereas Comparative Sample A is difficult to mold as small variations in pressure and temperature result in a product with molded part defects.
Claims
1. 1. A method for making an expanded poly(lactide) bead foam, comprising the steps of: (a) pressurizing unexpanded beads of a PLA resin blend having a crystallinity of 10 J / g or less as measured by differential scanning calorimetry with carbon dioxide to superatmospheric pressure while maintaining a temperature of 40° C. or less; (b) heating the pressed unexpanded beads to a temperature of from 90° C. to 160° C. to at least partially crystallize the PLA resin blend to form carbon dioxide saturated partially crystallized unexpanded beads; and thereafter (c) subjecting the carbon dioxide saturated and partially crystallized unexpanded beads to a pressure reduction to at least partially vaporize the carbon dioxide to produce expanded beads; and then (d) cooling the expanded beads to less than 40° C. simultaneously with and / or after step (c). Equipped with The PLA resin blend comprises: i) a first PLA copolymer, the first PLA copolymer containing at least 88% L-lactide units based on the total weight of the first PLA copolymer; ii) a second PLA copolymer containing at least 88% D-lactide units based on the total weight of the second PLA copolymer; Includes The method wherein said first PLA copolymer and said second PLA copolymer are present in said PLA resin blend in a weight ratio of from 75:25 to 98:
2.
2. 1. A method for making an expanded poly(lactide) bead foam, comprising the steps of: (a) pressurizing unexpanded beads of a PLA resin blend having a crystallinity of 10 J / g or less as measured by differential scanning calorimetry with carbon dioxide to superatmospheric pressure while maintaining a temperature of 40° C. or less; (b) heating the pressed unexpanded beads to a temperature of from 90° C. to 160° C. to at least partially crystallize the PLA resin blend to form carbon dioxide saturated partially crystallized unexpanded beads; and thereafter (c) subjecting the carbon dioxide saturated and partially crystallized unexpanded beads to a pressure reduction to at least partially vaporize the carbon dioxide to produce expanded beads; and then (d) cooling the expanded beads to less than 40° C. simultaneously with and / or after step (c). Equipped with The PLA resin blend comprises: i) a first PLA copolymer, the first PLA copolymer containing at least 88% L-lactide units based on the total weight of the first PLA copolymer; ii) a second PLA copolymer containing at least 88% D-lactide units based on the total weight of the second PLA copolymer; Includes The method wherein said first PLA copolymer and said second PLA copolymer are present in said PLA resin blend in a weight ratio of from 25:75 to 2:
98.
3. The method of claim 1 or 2, wherein the first PLA copolymer contains at least 92% L-lactide units and the second PLA copolymer contains at least 92% D-lactide units.
4. The method of any one of claims 1 to 3, wherein the first PLA copolymer contains at least 95% L-lactide units and the second PLA copolymer contains at least 95% D-lactide units.
5. 5. The method of any one of claims 1 to 4, wherein the superatmospheric pressure in step (a) and the superatmospheric pressure in step (b) are each between 3 MPa gauge and 10 MPa gauge.
6. The method according to any one of claims 1 to 5, wherein the temperature in step (b) is from 110°C to 140°C.
7. The method according to any one of claims 1 to 6, wherein in step (b), the pressed unexpanded beads are maintained at a temperature of from 110°C to 140°C for a period of from 5 to 30 minutes.
8. 8. The method of any one of claims 1 to 7, wherein the carbon dioxide saturated, partially crystallized unexpanded beads formed in step (b) have a degree of crystallinity of from 10% to 35%, based on the total weight of the PLA resin blend in the carbon dioxide saturated, partially crystallized unexpanded beads, as measured by DSC.
9. The method according to any one of claims 1 to 8, wherein PLA stereocomplex crystals and PLA homocrystals form during step (b).
10. 10. The method of claim 9, wherein the PLA stereocomplex crystals constitute 10% to 50% of the combined weight of the PLA stereocomplex crystals and the PLA homocrystals.
11. The method of any one of claims 1, 3 to 10, wherein the first PLA copolymer and the second PLA copolymer are present in the PLA resin blend in a weight ratio of from 85:15 to 98:
2.
12. The method of any one of claims 2 to 10, wherein the first PLA copolymer and the second PLA copolymer are present in the PLA resin blend in a weight ratio of from 15:85 to 2:98.
Citation Information
Patent Citations
Polylactic acid foamed particle and molded product of the polylactic acid foamed particle
JP2004083890A
Foamable polylactic acid resin particle, polylactic acid foamed particle, and polylactic acid foamed particle molded article
JP2006233192A
Method for producing polylactic acid resin foamed particle for in-mold expansion molding
JP2009235170A
Manufacturing of polylactic acid foam using liquid carbon dioxide
JP2015531415A
Impregnated polymer granules, processes for preparation and polymer products thereof
WO2013181705A1