Ammonia and Ammonium Hydroxide Stabilizers for Paraformaldehyde
Ammonia and ammonium hydroxide stabilize paraformaldehyde by inhibiting chain growth and alcohol end-capping, addressing the short shelf life and stickiness issues, ensuring extended shelf life and easy handling.
Patent Information
- Application Number
- JP2021510036
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-09-28
- Filing Date
- 2019-09-05
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2039-09-05
AI Technical Summary
Paraformaldehyde exhibits a short shelf life due to solubility decrease and insoluble matter formation over time, which is exacerbated by the use of traditional stabilizers that make it sticky and difficult to handle.
Using ammonia and/or ammonium hydroxide as stabilizers to inhibit chain growth and alcohol end-capping of paraformaldehyde, maintaining its solubility and preventing stickiness, thereby extending shelf life and enabling easy handling and transportation.
Ammonia and ammonium hydroxide stabilize paraformaldehyde, reducing insoluble matter formation and maintaining transportability, thus extending shelf life and ensuring easy handling without stickiness.
Smart Images

Figure 0007569306000002 
Figure 0007569306000001
Abstract
Description
[Technical field]
[0001] This disclosure relates to improving the shelf life, handling, and transportation of paraformaldehyde. [Background technology]
[0002]
[0002] Paraformaldehyde is a solid form of formaldehyde that is greater than 80%. Typically, the formaldehyde concentration ranges from 90% to 96%. Paraformaldehyde is a poly(oxymethylene) glycol, HO--(CH2O) n --H (n = 8-100). Generally, paraformaldehyde is produced by concentrating a hot aqueous solution of formaldehyde under reduced pressure. Upon cooling, the resulting solution solidifies into prills for storage and / or transportation.
[0003]
[0003] Paraformaldehyde, immediately after preparation, has good solubility in water and in organic solvents such as butanol. It dissolves readily in water or alcohols by hydrolysis or depolymerization to produce methylene glycol or formal. However, its solubility in water and solvents decreases over time, or upon storage at temperatures generally above about 35°C. This change in solubility is probably due to changes in molecular weight (or the value of n) and end-capping of the paraformaldehyde chain with methanol. The solubility and reactivity of paraformaldehyde decrease with increasing molecular weight.
[0004] The presence of methanol in the reaction mixture also leads to the formation of insolubles. The insolubles are typically paraformaldehyde end-capped with an alcohol to form ethers. These high molecular weight ethers are insoluble in any solution unless they contain a strong acid. Paraformaldehyde typically contains insolubles at a concentration of about 10 ppm to 20 ppm. As paraformaldehyde is stored over time, small amounts of alcohol in the prill react with the paraformaldehyde to form more insolubles. For example, after storage at ambient temperature, the concentration of insolubles can exceed 100 ppm, and in some cases even exceed 350 ppm in the presence of high concentrations of methanol. The industry standard for the amount of insolubles that is acceptable is less than 100 ppm. Thus, the shelf life of paraformaldehyde is very short.
[0005]
[0005] Many stabilizers and inhibitors have been proposed to alleviate this problem. For example, amines such as hexaethylamine and triethylamine have been used. It is believed that the stabilizers slow down the chain growth and slow down the endcapping of the paraformaldehyde, thus reducing the formation of insolubles over time. However, the stabilizers also increase the stickiness of the prills, making them very difficult to manufacture and handle.
[0006]
[0006] The following drawings are included to illustrate certain aspects of the embodiments and should not be considered as exclusive embodiments. The disclosed subject matter is capable of considerable modification, permutations, combinations and equivalents in form and function, as will occur to those skilled in the art having the benefit of this disclosure. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 shows a diagram of an apparatus that simulates a quenching vessel. Summary of the Invention
[0008]
[0008] This disclosure relates to improving the shelf life, handling, and transportation of paraformaldehyde using ammonia and / or ammonium hydroxide as stabilizers. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009]
[0009] As used herein, the term "prills" refers to pellets or small solid pellets. The final paraformaldehyde may be in the form of flakes, chunks, granules, etc., depending on the method of solidification and drying of the paraformaldehyde. As used herein, the final paraformaldehyde is described in the form of "solidified (or solidified) paraformaldehyde," which may be in any suitable solidified form, including, but not limited to, prills, flakes, chunks, granules, etc.
[0010]
[0010] At low concentrations, hydrocarbylamines can stabilize the solidified paraformaldehyde without making it sticky. However, the concentration of hydrocarbylamines is not high enough to appreciably extend the shelf life of the solidified paraformaldehyde. At high concentrations, hydrocarbylamines can make the solidified paraformaldehyde too sticky to be transported by conventional means such as compressed air.
[0011] It has been discovered that ammonia and / or ammonium hydroxide can be used as a stabilizer for paraformaldehyde to produce solidified paraformaldehyde that is not tacky and has a long shelf life because it can be used in high concentrations. Urea can be used as a source of ammonia by mixing the urea with water and heating.
[0012] Without being limited by theory, ammonia and / or ammonium hydroxide react with the paraformaldehyde chain ends to form crystalline oximes and also neutralize any acid catalyst, both of which effectively inhibit chain growth and alcohol end-capping of the solidified paraformaldehyde.
[0013]
[0013] In general, the production of solidified paraformaldehyde involves heating a formaldehyde solution containing 30 wt% or more of formaldehyde (e.g., about 30 wt% to 90 wt% formaldehyde) to a temperature of about 70°C to about 130°C, preferably about 80°C to about 100°C. The formaldehyde solution is held at this temperature for about 0.1 hours to about 3 hours, preferably about 20 minutes to about 40 minutes, more preferably about 20 minutes to about 30 minutes. This is often called aging. During aging, formaldehyde polymerizes to form paraformaldehyde. Once the aging process is complete, the paraformaldehyde product is solidified. Specifically for prilling, the paraformaldehyde is passed through a nozzle to form prills, which are then dropped into a countercurrent gas in a prilling tower. This causes the paraformaldehyde to solidify. Polymerization reactions can still occur during the solidification of the paraformaldehyde. Optionally, the solidified paraformaldehyde is transferred to a quenching vessel and further cooled, typically using compressed air. The solidified paraformaldehyde can be dried at a temperature of about ambient temperature to about 150°C, preferably about 50°C to about 100°C, for about 15 minutes to about 20 hours, preferably about 1 hour to about 2 hours. Polymerization reactions can still occur during the drying of the solidified paraformaldehyde. The solidified paraformaldehyde is then stored or transported to a customer. Handling and transportation of the solidified paraformaldehyde within the plant or to and from storage is typically performed using compressed air. The use of ammonia and / or ammonium hydroxide stabilizers does not make the solidified paraformaldehyde sticky like other amine stabilizers, so handling and transportation of the solidified paraformaldehyde is essentially the same as untreated solidified paraformaldehyde. Ammonia and / or ammonium hydroxide stabilizers can be incorporated into any part of the production or storage of paraformaldehyde.
[0014]
[0014] An exemplary embodiment of the present disclosure includes heating a formaldehyde solution containing 30 wt% or more formaldehyde and about 50 ppm to about 1000 ppm, preferably 100 ppm to 500 ppm, more preferably 150 ppm to 250 ppm of ammonia and / or ammonium hydroxide stabilizer to a temperature in the range of about 70°C to about 130°C; aging the formaldehyde solution for a time sufficient for the formaldehyde to polymerize and form paraformaldehyde; and solidifying the paraformaldehyde (e.g., passing the paraformaldehyde through a nozzle to form prills which then fall into a countercurrent gas in a prilling tower for further polymerization and solidification). The method can also further include drying the solidified paraformaldehyde.
[0015]
[0015] Another exemplary embodiment of the present disclosure includes heating a formaldehyde solution containing 30 wt% or more of formaldehyde to a temperature in the range of about 70°C to about 130°C; aging the formaldehyde solution in the presence of about 50 ppm to about 1000 ppm, preferably 100 ppm to 500 ppm, more preferably 150 ppm to 250 ppm of ammonia and / or ammonium hydroxide stabilizer for a time sufficient for the formaldehyde to polymerize to form paraformaldehyde; and solidifying the paraformaldehyde (e.g., passing the paraformaldehyde through a nozzle to form prills, which are then dropped into a countercurrent gas in a prilling tower for further polymerization and solidification). The method can also further include drying the solidified paraformaldehyde.
[0016]
[0016] Yet another exemplary embodiment of the present disclosure includes heating a formaldehyde solution containing 30 wt% or more of formaldehyde to a temperature in the range of about 70°C to about 130°C; aging the formaldehyde solution for a time sufficient for the formaldehyde to polymerize to form paraformaldehyde; and solidifying the paraformaldehyde in a prilling tower (e.g., passing the paraformaldehyde through a nozzle to form prills that fall into a countercurrent gas) in the presence of a gas containing about 10 ppm to about 1000 ppm, preferably 25 ppm to 500 ppm, more preferably 50 ppm to 150 ppm of ammonia and / or ammonium hydroxide stabilizer, for further polymerization and solidification. The method can also further include drying the solidified paraformaldehyde.
[0017]
[0017] Another exemplary embodiment of the present disclosure includes heating a formaldehyde solution containing 30 wt % or more formaldehyde to a temperature in the range of about 70°C to about 130°C; aging the formaldehyde solution for a time sufficient for the formaldehyde to polymerize to form paraformaldehyde; solidifying the paraformaldehyde (e.g., passing the paraformaldehyde through a nozzle to form prills which are then dropped into a countercurrent gas flow in a prilling tower for further polymerization and solidification); drying the solidified paraformaldehyde; and exposing the solidified paraformaldehyde during and / or after drying to a gas containing about 10 ppm to about 1000 ppm, preferably 25 ppm to 500 ppm, and more preferably 50 ppm to 150 ppm of ammonia and / or ammonium hydroxide stabilizer.
[0018]
[0018] Another exemplary embodiment of the present disclosure includes heating a formaldehyde solution containing 30 wt % or more formaldehyde to a temperature in the range of about 70°C to about 130°C; aging the formaldehyde solution for a time sufficient for the formaldehyde to polymerize to form paraformaldehyde; solidifying the paraformaldehyde (e.g., passing the paraformaldehyde through a nozzle to form prills which are then dropped into a countercurrent gas flow in a prilling tower for further polymerization and solidification); drying the solidified paraformaldehyde; transporting the solidified paraformaldehyde to a storage facility; and exposing the solidified paraformaldehyde during transport or in the storage facility to a gas containing about 10 ppm to about 1000 ppm, preferably 25 ppm to 500 ppm, and more preferably 50 ppm to 150 ppm of ammonia and / or ammonium hydroxide stabilizer.
[0019]
[0019] Combinations of the foregoing methods can be used. For example, ammonia and / or ammonium hydroxide stabilizers can be used in one or more of the heating, aging, solidifying, drying, or storing steps. If more than one step involves exposure to ammonia and / or ammonium hydroxide stabilizers, each step can use a lower concentration of ammonia and / or ammonium hydroxide stabilizers.
[0020] In each of the foregoing embodiments, urea can be used as the source of ammonia and / or ammonium hydroxide stabilizer.
[0021] In each of the foregoing embodiments, the formaldehyde solution can contain 30 wt% or more formaldehyde (eg, about 30 wt%-90 wt% formaldehyde), preferably about 35 wt%-75 wt% formaldehyde, and more preferably about 36 wt%-50 wt% formaldehyde.
[0021]
[0022] In each of the foregoing embodiments, the formaldehyde solution can be heated to a temperature of about 70°C to about 130°C, preferably about 80°C to about 100°C.
[0023] In each of the above-mentioned embodiments, the formaldehyde solution can be held (aged) at a temperature of about 70°C to about 130°C, preferably about 80°C to about 100°C, for about 0.1 hours to about 3 hours, preferably about 20 minutes to about 40 minutes, and more preferably about 20 minutes to about 30 minutes.
[0022]
[0024] In each of the aforementioned embodiments, the solidified paraformaldehyde can be dried at a temperature of about ambient temperature to about 150° C., preferably about 50° C. to about 100° C., for about 15 minutes to about 20 hours, preferably about 1 hour to about 2 hours.
[0023]
[0025] Exposing the solidified paraformaldehyde to an ammonia and / or ammonium hydroxide stabilizer at any time between formation and storage, including during formation and storage, can include exposing the solidified paraformaldehyde to a gas containing about 10 ppm to about 1000 ppm, preferably 25 ppm to 500 ppm, and more preferably 50 ppm to 150 ppm of the ammonia and / or ammonium hydroxide stabilizer. The ammonia and / or ammonium hydroxide stabilizer may be diluted in a carrier gas. Examples of carrier gases include, but are not limited to, air, oxygen, nitrogen, carbon dioxide, argon, and the like, and any combination thereof.
[0024]
[0026] In each of the foregoing aspects, the formaldehyde solution may further include an acid or base catalyst, examples of which include, but are not limited to, formic acid, boric acid, sodium tetraborate, oxalic acid, and any combination thereof.
[0025]
[0027] In each of the foregoing embodiments, the formaldehyde solution, paraformaldehyde, and solidified paraformaldehyde may be free of organic amines. As used herein, the term "organic amine" includes low molecular weight compounds (less than 500 g / mol, preferably less than 300 g / mol) composed of carbon, hydrogen, nitrogen, and optionally oxygen. Examples of organic amines include, but are not limited to, methylamine, ethylamine, n-propylamine, n-butylamine, iso-butylamine, tert-butylamine, dimethylamine, diethylamine, di-n-propylamine, di-iso-propylamine, dibutylamine, triethylamine, and triethanolamine, hexamethylenetetramine, 2-ethylhexylamine, 2-aminopropanediol, hexylamine, ethanolamine, mixed C 20 Amine, Mixed C 10 amine, cyclohexylamine, 1,2-dimethoxypropanamine, triethylamine, ethanolamine, 1-amino-1,3-propanediol, 1-aminopentane, 2-methyloxypropylamine, and any combination thereof.
[0026]
[0028] In each of the foregoing embodiments, the method further includes storing the solidified paraformaldehyde at between ambient temperature and 50° C. for greater than 30 days (e.g., between 30 days and 1 year or more) without increasing the insoluble matter concentration in the solidified paraformaldehyde by more than about 150 ppm, preferably about 120 ppm, and more preferably about 100 ppm.
[0027]
[0029] An additional embodiment of the present disclosure is a paraformaldehyde composition comprising about 1 ppm to about 100 ppm, preferably about 5 ppm to about 50 ppm, and more preferably about 10 ppm to about 25 ppm of an ammonia and / or ammonium hydroxide stabilizer, and about 80 wt% to about 99.9 wt%, preferably about 90 wt% to about 99.9 wt%, and more preferably about 95 wt% to about 99.9 wt% paraformaldehyde.
[0028]
[0030] The paraformaldehyde composition may also contain about 1 ppm to about 200 ppm, preferably about 5 ppm to about 100 ppm, and more preferably about 10 ppm to about 50 ppm of insoluble matter.
[0029]
[0031] In each of the foregoing paraformaldehyde composition embodiments, the paraformaldehyde composition can further include an acid or base catalyst. Examples of catalysts include, but are not limited to, formic acid, boric acid, sodium tetraborate, oxalic acid, and any combination thereof.
[0030]
[0032] The source of the ammonia and / or ammonium hydroxide stabilizer is urea. In each of the above paraformaldehyde composition embodiments, the paraformaldehyde composition may be free of organic amines. Examples of organic amines include, but are not limited to, methylamine, ethylamine, n-propylamine, n-butylamine, iso-butylamine, tertbutylamine, dimethylamine, diethylamine, di-n-propylamine, di-iso-propylamine, dibutylamine, triethylamine, and triethanolamine, hexamethylenetetramine, 2-ethylhexylamine, 2-aminopropanediol, hexylamine, ethanolamine, mixed C 20 Amine, Mixed C 10 amine, cyclohexylamine, 1,2-dimethoxypropanamine, triethylamine, ethanolamine, 1-amino-1,3-propanediol, 1-aminopentane, 2-methyloxypropylamine, and any combination thereof.
[0031]
[0033] For each of the paraformaldehyde composition embodiments described above, the solidified paraformaldehyde can be in the form of prills, flakes, chunks, granules, and the like.
[0034] An exemplary embodiment of the invention is a method that includes heating a formaldehyde solution containing 30 wt % or more formaldehyde to a temperature in the range of about 70° C. to about 130° C.; aging the formaldehyde solution for a time sufficient for the formaldehyde to polymerize to form paraformaldehyde; solidifying the paraformaldehyde; and contacting the formaldehyde solution before and / or during heating, the formaldehyde solution during the aging, the paraformaldehyde, and / or the solidified paraformaldehyde with an ammonia and / or ammonium hydroxide stabilizer. Optionally, the method may include one or more of the following:Element 1: the formaldehyde solution during heating further comprises about 50 ppm to about 1000 ppm of an ammonia and / or ammonium hydroxide stabilizer; Element 2: the formaldehyde solution during aging further comprises about 50 ppm to about 1000 ppm of an ammonia and / or ammonium hydroxide stabilizer; Element 3: solidifying the paraformaldehyde comprises contacting the paraformaldehyde with a gas comprising about 10 ppm to about 1000 ppm of an ammonia and / or ammonium hydroxide stabilizer; Element 4: the method further comprises drying the solidified paraformaldehyde; Element 5: Element 4 and the method further comprises exposing the solidified paraformaldehyde during and / or after drying to a gas comprising about 10 ppm to about 1000 ppm of an ammonia and / or ammonium hydroxide stabilizer; Element 6: Element 4 or 5 and the method further comprises exposing the solidified paraformaldehyde to a gas comprising about 10 ppm to about 1000 ppm of an ammonia and / or ammonium hydroxide stabilizer. and transporting the solidified paraformaldehyde to a storage facility; element 7: element 6 and the method further comprising exposing the solidified paraformaldehyde during transport and / or in the storage facility to a gas comprising from about 10 ppm to about 1000 ppm of an ammonia and / or ammonium hydroxide stabilizer; element 8: element 6 or 7 and the method further comprising storing the solidified paraformaldehyde at from ambient temperature to about 50° C. for longer than 30 days and maintaining an insoluble matter concentration in the solidified paraformaldehyde at less than about 150 ppm; element 9: the aging of the formaldehyde solution is from about 0.1 hours to about 3 hours; element 10: an organic amine is not included in the method; element 11: the method further comprises transporting the solidified paraformaldehyde to a storage facility; element 12: the aging of the formaldehyde solution is from 70° C. to 130° C.; and element 13: the source of the ammonia and / or ammonium hydroxide stabilizer is urea. Examples of combinations include, but are not limited to, combinations of elements 1, 4, and 11; combinations of elements 2, 4, and 11; combinations of elements 3, 4, and 11; combinations of elements 4, 5, and 11; combinations of elements 4, 6, and 7 (and optionally 8); combinations of elements 1, 4, 6, and 8; combinations of elements 2, 4, 6, and 8; combinations of elements 3, 4, 6, and 8; combinations of two or more of elements 1, 2, 3, 4, and 5 (optionally further combining elements 6 and 7); and combinations of elements 9, 12, and / or 13 with any of the foregoing.
[0032]
[0035] Another exemplary embodiment of the invention includes exposing the solidified paraformaldehyde to a gas containing about 10 ppm to about 1000 ppm of an ammonia and / or ammonium hydroxide stabilizer. Optionally, the solidified paraformaldehyde is free of organic amines and / or the source of the ammonia and / or ammonium hydroxide stabilizer is urea.
[0033]
[0036] Yet another exemplary embodiment of the present invention is solidified paraformaldehyde comprising about 1 ppm to about 100 ppm of ammonia and / or ammonium hydroxide stabilizer; and about 80 wt % to about 99.9 wt % paraformaldehyde. Optionally, the solidified paraformaldehyde can include one or more of the following: element 14: the solidified paraformaldehyde is free of organic amines; element 15: the solidified paraformaldehyde further comprises less than 150 ppm of insoluble matter; and element 16: the solidified paraformaldehyde is in the form of prills, flakes, chunks, or granules.
[0034]
[0037] Unless otherwise indicated, all numerical values expressing quantities of ingredients, properties such as molecular weight, reaction conditions, and the like used in the specification and appended claims are to be understood as being modified in all instances by the term "about." Accordingly, unless indicated to the contrary, the numerical parameters set forth in the following specification and appended claims are approximations that may vary depending upon the desired properties sought to be obtained by embodiments of the present invention. At the very least, and not as an attempt to limit the application of the doctrine of equivalents to the scope of the claims, each numerical parameter should be construed in light of at least the number of reported significant digits and by applying ordinary rounding techniques.
[0035]
[0038] One or more exemplary embodiments incorporating aspects of the invention disclosed herein are presented herein. For clarity, not all features of a physical implementation are described or shown in this application. It should be understood that in developing a physical embodiment incorporating aspects of the invention, numerous implementation-specific decisions must be made to achieve the developer's goals, including compliance with system-related, business-related, government-related and other constraints that vary from implementation to implementation and from time to time. Although the developer's efforts are time-consuming, such efforts are nevertheless routine for those of ordinary skill in the art having the benefit of this disclosure.
[0036]
[0039] Although compositions and methods are described herein in terms of "comprising" various components or steps, the compositions and methods may also "consist essentially of" or "consist of" various components and steps.
[0037]
[0040] In order to facilitate a better understanding of the aspects of the present invention, the following examples of preferred or representative embodiments are presented. The following examples should not be read in any way as limiting or defining the scope of the invention. EXAMPLES
[0038]
[0041] Example 1. An apparatus 100 according to Figure 1 was used to simulate a quenching vessel. The apparatus 100 includes a dryer tube 102 (2.5 inch (6.35 cm) radius, 11 inch (27.94 cm) height) with a perforated plate 104 located 1.75 inches (4.445 cm) from the bottom, a gas inlet 106 between the bottom of the dryer tube 102 and the perforated plate 104, and a vent 108 at the top of the dryer tube 102. Additionally, a thermocouple 110 extends through the top of the dryer tube 102 and above the perforated plate to measure the temperature within the dryer tube 102. The gas inlet 106 is fluidly connected to a source 112 of ammonia and / or ammonium hydroxide stabilizer (e.g., a tank of ammonia, a tank of ammonia in air dilution, an aqueous solution of urea, an ammonium hydroxide solution, etc.). As used herein, when two components are described as being fluidly connected, there is hardware connecting the two components such that fluid can pass from one component to the other, which may be two or more components including lines, pipes, tubes, pumps, connectors, heat exchangers, valves, etc.
[0039]
[0042] A heat exchanger 114 is located between the source 112 of ammonia and / or ammonium hydroxide stabilizer and is used to heat the ammonia and / or ammonium hydroxide stabilizer before it is introduced into the dryer tubes 102. Optionally, gas (e.g., plant air) can be taken through line 116 to combine with the ammonia and / or ammonium hydroxide stabilizer to dilute the ammonia and / or ammonium hydroxide stabilizer to a desired concentration.
[0040]
[0043] In this example, 350 grams of paraformaldehyde prills were added to the dryer tube 102. This resulted in the height of the prills reaching 2.5 inches (6.35 cm) from the top of the dryer tube 102. A tank of 100 ppm ammonia in air was used as the source of ammonia and / or ammonium hydroxide stabilizer 112. The heat exchanger 114 was set at 200° F. (93.3° C.). The 100 ppm ammonia in air was passed through the apparatus 100 at 30 standard cubic feet per minute (0.85 cubic meters per minute). This resulted in the prills forming a fluidized bed within the dryer tube 102. The fact that the prills maintained a fluidized bed indicates that the ammonia and / or ammonium hydroxide stabilizer did not make the prills too sticky for transport.
[0041]
[0044] The same experiment was performed, except that ethylhexylamine was used as the stabilizer. The prills became too sticky in the dryer tube 102 and would not fluidize.
[0045] Example 2. In a full-scale plant, paraformaldehyde prills were exposed to various concentrations of ammonium hydroxide in a prilling tower. More specifically, a 19% aqueous solution of ammonium hydroxide was heated to about 90°C. The resulting steam was passed through the prilling tower. Optionally, the steam was diluted with plant air. The prills were then aged at 50°C for 4 days, simulating 6 months of aging under normal storage conditions (about 23°C to 38°C). The amount of insoluble matter after aging is shown in Table 1, where the control was prills that were not exposed to ammonium hydroxide.
[0042] [Table 1]
[0043]
[0046] In no case did the prills become sticky and were easily transported by standard methods and equipment.
[0047] These examples demonstrate that the use of ammonia and / or ammonium hydroxide stabilizers can be used to maintain low levels of insoluble matter in the solidified paraformaldehyde during storage, preserving the ability to be handled and transported by conventional means.
[0044]
[0048] Thus, the present invention is well adapted to attain the ends and advantages mentioned as well as those inherent therein. The specific embodiments disclosed above are illustrative only, as the invention may be modified and practiced in different but equivalent manners apparent to those skilled in the art having the benefit of the teachings herein. Furthermore, no limitations are intended to the details of construction or design shown herein, other than as set forth in the following claims. It is therefore evident that the specific exemplary embodiments disclosed above may be altered, combined or modified and all such variations are considered to be within the scope and spirit of the invention. The invention illustratively disclosed herein may suitably be practiced in the absence of any element not specifically disclosed herein and / or any optional element disclosed herein. The compositions and methods may be "comprising" various components or steps. Although described in terms of, "containing," or "including," the compositions and methods may also "consist essentially of" or "consist of" various components and steps. All numerical values and ranges disclosed above are subject to some variation. Whenever a numerical range with a lower and upper limit is disclosed, any numerical value falling within that range and any encompassing range is specifically disclosed. In particular, any value range disclosed herein (in the form of "from about a to about b," or equivalently, "from approximately a to b," or equivalently, "from approximately a to b") is understood to set forth any numerical value or range encompassed within the broader range of values. Additionally, the terms in the claims have their plain and ordinary meaning unless expressly and unambiguously defined by the patentee. Additionally, the indefinite articles "a" or "an," as used in the claims, are defined herein to mean one or more of the element to which they refer. The claims as filed are set forth below. [Claim 1] Heating a formaldehyde solution containing 30 wt % or more of formaldehyde to a temperature in the range of about 70°C to about 130°C; Aging the formaldehyde solution for a period of time sufficient for the formaldehyde to polymerize to form paraformaldehyde; solidifying the paraformaldehyde; and Contacting the formaldehyde solution before and / or during heating, the formaldehyde solution during aging, the paraformaldehyde, and / or the solidified paraformaldehyde with an ammonia and / or ammonium hydroxide stabilizer. The method includes: [Claim 2] 10. The method of claim 1, wherein the formaldehyde solution during heating further comprises about 50 ppm to about 1000 ppm of ammonia and / or ammonium hydroxide stabilizer. [Claim 3] 3. The method of claim 1 or 2, wherein the formaldehyde solution during aging further comprises about 50 ppm to about 1000 ppm of ammonia and / or ammonium hydroxide stabilizer. [Claim 4] 4. The method of claim 1, wherein solidifying the paraformaldehyde comprises contacting the paraformaldehyde with a gas comprising from about 10 ppm to about 1000 ppm of an ammonia and / or ammonium hydroxide stabilizer. [Claim 5] 5. The method according to claim 1, further comprising drying the solidified paraformaldehyde. [Claim 6] 6. The method of claim 5, further comprising exposing the solidified paraformaldehyde during and / or after drying to a gas comprising about 10 ppm to about 1000 ppm of an ammonia and / or ammonium hydroxide stabilizer. [Claim 7] 7. The method of claim 5 or 6, further comprising transporting the solidified paraformaldehyde to a storage facility. [Claim 8] 8. The method of claim 7, further comprising exposing the solidified paraformaldehyde during transport or in a storage facility to a gas comprising about 10 ppm to about 1000 ppm of an ammonia and / or ammonium hydroxide stabilizer. [Claim 9] 9. The method of claim 7 or 8, further comprising storing the solidified paraformaldehyde at ambient temperature to about 50° C. for more than 30 days and maintaining an insoluble matter concentration in the solidified paraformaldehyde at less than about 150 ppm. [Claim 10] 10. The method according to claim 1, wherein the formaldehyde solution is aged for about 0.1 hour to about 3 hours. [Claim 11] 11. The method according to claim 1, wherein the formaldehyde solution is aged at 70°C to 130°C. [Claim 12] 12. The method according to any one of claims 1 to 11, wherein the method does not include an organic amine. [Claim 13] The method of any one of claims 1 to 12, further comprising transporting the solidified paraformaldehyde to a storage facility. 2. The method according to any one of claims 1 to 11. [Claim 14] 14. The method of any one of claims 1 to 13, wherein the source of ammonia and / or ammonium hydroxide stabilizer is urea. [Claim 15] A method comprising exposing the solidified paraformaldehyde to a gas comprising about 10 ppm to about 1000 ppm of an ammonia and / or ammonium hydroxide stabilizer. [Claim 16] 16. The method of claim 15, wherein the solidified paraformaldehyde does not contain organic amines. [Claim 17] 17. The method of claim 15 or 16, wherein the source of ammonia and / or ammonium hydroxide stabilizer is urea. [Claim 18] 18. The method of claim 15, further comprising storing the solidified paraformaldehyde at ambient temperature to about 50° C. for more than 30 days and maintaining an insoluble matter concentration in the solidified paraformaldehyde at less than about 150 ppm. [Explanation of symbols]
[0045] 100 devices 102 Dryer tube 104 Perforated plate 106 Gas inlet 108 Vent 110 Thermocouple 112 Source of ammonia and / or ammonium hydroxide stabilizer 114 Heat exchanger 116 Line
Claims
1. heating a formaldehyde solution containing 30 wt % or more formaldehyde and 50 ppm to 1000 ppm ammonia and / or ammonium hydroxide stabilizer to a temperature in the range of 70° C. to 130° C.; Aging the formaldehyde solution for a period of time sufficient for the formaldehyde to polymerize to form paraformaldehyde; The paraformaldehyde is solidified. The method includes:
2. 10. The method of claim 1, further comprising drying the solidified paraformaldehyde.
3. 3. The method of claim 2, further comprising exposing the solidified paraformaldehyde during and / or after drying to a gas containing 10 ppm to 1000 ppm of ammonia and / or ammonium hydroxide stabilizer.
4. 4. The method of claim 2 or 3, further comprising transporting the solidified paraformaldehyde to a storage facility.
5. 5. The method of claim 4, further comprising exposing the solidified paraformaldehyde during transportation or in the storage facility to a gas containing 10 ppm to 1000 ppm of ammonia and / or ammonium hydroxide stabilizer.
6. 6. The method of claim 4 or 5, further comprising storing the solidified paraformaldehyde at ambient temperature to 50° C. for more than 30 days and maintaining an insoluble matter concentration in the solidified paraformaldehyde below 150 ppm.
7. 7. The method according to claim 1, wherein the formaldehyde solution is aged for 0.1 to 3 hours.
2. The method according to claim 1.
8. The process according to any one of claims 1 to 7, wherein the maturation of the formaldehyde solution is carried out at 70°C to 130°C.
9. The method according to any one of claims 1 to 8, wherein no organic amine is included in the method.
10. 10. The method of any one of claims 1 to 9, further comprising transporting the solidified paraformaldehyde to a storage facility.
11. The method of any one of claims 1 to 10, wherein the source of ammonia and / or ammonium hydroxide stabilizer is urea.
12. heating a formaldehyde solution containing 30 wt % or more of formaldehyde to a temperature in the range of 70° C. to 130° C.; aging the formaldehyde solution in the presence of 50 ppm to 1000 ppm of ammonia and / or ammonium hydroxide stabilizer for a time sufficient for the formaldehyde to polymerize to form paraformaldehyde; The paraformaldehyde is solidified. The method includes:
13. The solidified paraformaldehyde is dried, and Exposing the solidified paraformaldehyde during and / or after drying to a gas containing 10 ppm to 1000 ppm of ammonia and / or ammonium hydroxide stabilizer. The method of claim 12 further comprising:
14. 13. The method of claim 12, wherein an organic amine is not included in the method.
Citation Information
Patent Citations
Preparation of paraformaldehyde
JP1979122214A
Method of manufacture for paraformaldehyde prills
US4550213A