Resin composition for injection molding and injection molded article

A biodegradable resin blend of poly(3-hydroxyalkanoate) and polylactic acid with controlled molecular weights and additives addresses heat resistance and burr issues, enhancing the quality and sustainability of injection molded products.

JP7569311B2Active Publication Date: 2024-10-17KANEKA CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021520645
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-17
Filing Date
2020-04-07
Publication Date
2024-10-17
Estimated Expiration
2040-04-07

AI Technical Summary

Technical Problem

Existing biodegradable resin compositions, particularly those based on polylactic acid, suffer from insufficient heat resistance and burr formation during injection molding, which can compromise the quality and appearance of molded products.

Method used

A resin composition comprising a blend of poly(3-hydroxyalkanoate) resin with a specific molecular weight range and polylactic acid, along with optional inorganic fillers and additives, is used to enhance heat resistance and reduce burr formation.

Benefits of technology

The composition achieves high heat resistance and minimizes burr occurrence in injection molded articles, improving product quality and environmental sustainability by using biodegradable materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569311000001
    Figure 0007569311000001
  • Figure 0007569311000002
    Figure 0007569311000002
Patent Text Reader

Abstract

This resin composition for injection molding contains a resin component and optionally, an inorganic filler. The resin component contains a poly(3-hydroxyalkanoate)-based resin and a polylactic acid. The content of the polylactic acid is 20 to 50 parts by weight with respect to 100 parts by weight of the total of the poly(3-hydroxyalkanoate)-based resin and the polylactic acid. The content of the inorganic filler is 0 to 40 parts by weight with respect to 100 parts by weight of the total of the poly(3-hydroxyalkanoate)-based resin and the polylactic acid. The weight average molecular weight of the poly(3-hydroxyalkanoate)-based resin is 150,000 to 350,000.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition for injection molding and an injection molded article. [Background technology]

[0002] A large amount of petroleum-derived plastics are discarded every year, and the lack of landfill sites and environmental pollution caused by this large amount of waste are being raised as serious issues. For this reason, biodegradable plastics that are decomposed by the action of microorganisms in the environment, landfill sites, and compost are attracting attention. Development of biodegradable plastics is being promoted with the aim of a wide range of applications, such as agricultural, forestry, and fishery materials used in the environment, food containers, packaging materials, sanitary products, and garbage bags that are difficult to recover and reuse after use.

[0003] Among these, polylactic acid and poly(3-hydroxyalkanoate) resins are attracting attention from the viewpoint of reducing or fixing carbon dioxide gas emissions (carbon neutrality).

[0004] Patent Document 1 discloses a resin composition containing 55 to 75 parts by weight of polylactic acid, 25 to 45 parts by weight of a poly(3-hydroxyalkanoate) resin (the total amount of both resins is 100 parts by weight), 0.05 to 20 parts by weight of pentaerythritol, and 10 to 40 parts by weight of a silicate, which is intended to improve the heat resistance, which is a drawback of polylactic acid, as well as to improve processability in injection molding and extrusion molding. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2016 / 114128 Summary of the Invention [Problem to be solved by the invention]

[0006] In Patent Document 1, the polylactic acid is contained at a high ratio relative to the total amount of the resin components, so the heat resistance of the obtained molded body is not sufficiently high. In order to improve the heat resistance, it is possible to reduce the blending ratio of polylactic acid, but in that case, as described in Comparative Example 6 of the document, there is a problem that burrs are generated in the injection molded body.

[0007] Here, burrs are formed when molten resin penetrates into gaps that exist in the mating parts of the cavity part of an injection molding die (e.g., parting line parts, insert parts, sliding parts of slide cores, etc.), and are formed on the surface of the produced injection molded article along the places where the mating parts were located, and can cause problems in terms of the appearance of the injection molded article.

[0008] In view of the above-mentioned current situation, an object of the present invention is to provide a resin composition for injection molding which is composed of a biodegradable resin component, has high heat resistance, and is capable of forming an injection molded article in which the generation of burrs is suppressed. [Means for solving the problem]

[0009] As a result of extensive research into solving the above-mentioned problems, the inventors discovered that high heat resistance can be achieved by reducing the blending ratio of polylactic acid and increasing the blending ratio of poly(3-hydroxyalkanoate) resin, while using a poly(3-hydroxyalkanoate) resin with a molecular weight within a specified range, thereby suppressing burrs in injection-molded articles, and thus completed the present invention.

[0010] That is, the present invention relates to a resin composition for injection molding containing a resin component and, optionally, an inorganic filler, wherein the resin component contains a poly(3-hydroxyalkanoate)-based resin and polylactic acid, the content of the polylactic acid is 20 parts by weight or more and 50 parts by weight or less per 100 parts by weight of the total of the poly(3-hydroxyalkanoate)-based resin and the polylactic acid, the content of the inorganic filler is 0 parts by weight or more and 40 parts by weight or less per 100 parts by weight of the total of the poly(3-hydroxyalkanoate)-based resin and the polylactic acid, and the weight average molecular weight of the poly(3-hydroxyalkanoate)-based resin is 150,000 to 350,000. Preferably, the poly(3-hydroxyalkanoate)-based resin is one or more selected from the group consisting of poly(3-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), and poly(3-hydroxybutyrate-co-4-hydroxybutyrate). Preferably, the poly(3-hydroxyalkanoate)-based resin includes poly(3-hydroxybutyrate-co-3-hydroxyhexanoate). Preferably, the weight-average molecular weight of the poly(3-hydroxyalkanoate)-based resin is 200,000 to 300,000. Preferably, the content of the inorganic filler is 5 parts by weight or more and 40 parts by weight or less per 100 parts by weight of the total of the poly(3-hydroxyalkanoate) resin and the polylactic acid. Preferably, the inorganic filler is a silicate. Preferably, the silicate is one or more selected from the group consisting of talc, mica, kaolinite, montmorillonite, and smectite. Preferably, the resin composition for injection molding further contains a crystallization nucleating agent. The present invention also relates to an injection-molded article made from the above-mentioned resin composition for injection molding, and also to a method for producing the injection-molded article, comprising the steps of heating and melting the resin composition for injection molding, injecting the composition into a mold, and then cooling and solidifying the composition. Effect of the Invention

[0011] According to the present invention, it is possible to provide a resin composition for injection molding which is composed of a biodegradable resin component and is capable of forming an injection molded article having high heat resistance and suppressing the generation of burrs. The resin composition for injection molding according to a preferred embodiment of the present invention has an advantage that it can solve the environmental problem caused by the dumping of plastics into the ocean, since the main material of the resin component is a poly(3-hydroxyalkanoate)-based resin which is degradable in seawater. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of the present invention will be described, however, the present invention is not limited to the following embodiment.

[0013] The resin composition according to the present invention is a resin composition used for producing a molded article by injection molding. The resin composition contains at least a poly(3-hydroxyalkanoate) resin and a polylactic acid as resin components. In addition to the resin components, the resin composition may contain an inorganic filler or may not contain an inorganic filler.

[0014] [Poly(3-hydroxyalkanoate) resin] The poly(3-hydroxyalkanoate) resin (abbreviated as P3HA) constituting the main resin component of the resin composition for injection molding is a polymer containing a 3-hydroxyalkanoate structural unit (monomer unit). One type of poly(3-hydroxyalkanoate) resin may be used, or two or more types of poly(3-hydroxyalkanoate) resins may be used in combination.

[0015] The poly(3-hydroxyalkanoate) resin preferably contains 3-hydroxyalkanoate structural units in an amount of 50 mol% or more, more preferably 60 mol% or more, and even more preferably 70 mol% or more of the total structural units. The poly(3-hydroxyalkanoate) resin may contain only one or more types of 3-hydroxyalkanoate structural units as structural units, or may contain other structural units (e.g., 4-hydroxyalkanoate structural units, etc.) in addition to one or more types of 3-hydroxyalkanoate structural units.

[0016] Specifically, the 3-hydroxyalkanoate structural unit is preferably a structural unit represented by the following general formula (1). [-CHR-CH2-CO-O-] (1)

[0017] In the general formula (1), R is C p H 2p+1 where p is an integer of 1 to 15. Examples of R include linear or branched alkyl groups such as methyl, ethyl, propyl, methylpropyl, butyl, isobutyl, t-butyl, pentyl, and hexyl. p is preferably 1 to 10, and more preferably 1 to 8.

[0018] As the poly(3-hydroxyalkanoate)-based resin, a poly(3-hydroxyalkanoate)-based resin produced from a microorganism is particularly preferred. In the poly(3-hydroxyalkanoate)-based resin produced from a microorganism, all of the 3-hydroxyalkanoate structural units are contained as (R)-3-hydroxyalkanoate structural units.

[0019] The poly(3-hydroxyalkanoate) resin preferably contains 3-hydroxybutyrate (hereinafter, sometimes referred to as 3HB) structural units. In particular, it is preferable that all of the 3-hydroxybutyrate structural units are (R)-3-hydroxybutyrate structural units.

[0020] Specific examples of poly(3-hydroxyalkanoate) resins include poly(3-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxypropionate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (abbreviation: P3HB3HV), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-3-hydroxyhexanoate), and poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (abbreviation: P3HB3HH). , poly(3-hydroxybutyrate-co-3-hydroxyheptanoate), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate), poly(3-hydroxybutyrate-co-3-hydroxynonanoate), poly(3-hydroxybutyrate-co-3-hydroxydecanoate), poly(3-hydroxybutyrate-co-3-hydroxyundecanoate), poly(3-hydroxybutyrate-co-4-hydroxybutyrate) (abbreviation: P3HB4HB), and the like.

[0021] Particularly from the viewpoint of processability, mechanical properties, and the like, the poly(3-hydroxyalkanoate)-based resin preferably contains one or more selected from the group consisting of poly(3-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), and poly(3-hydroxybutyrate-co-4-hydroxybutyrate), more preferably contains poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) and / or poly(3-hydroxybutyrate-co-4-hydroxybutyrate), and even more preferably contains poly(3-hydroxybutyrate-co-3-hydroxyhexanoate).

[0022] When the poly(3-hydroxyalkanoate) resin constituting the resin composition for injection molding contains a resin containing a 3-hydroxybutyrate structural unit, the average content ratio of 3-hydroxybutyrate and other monomers in the entire poly(3-hydroxyalkanoate) resin is preferably 3-hydroxybutyrate / other monomers=99 / 1 to 70 / 30 (mol% / mol%), more preferably 98 / 2 to 85 / 15 (mol% / mol%), and even more preferably 97 / 3 to 93 / 7 (mol% / mol%). When the 3-hydroxybutyrate ratio is 99 mol% or less, sufficient mechanical properties tend to be easily obtained. In addition, when the 3-hydroxybutyrate ratio is 70% or more, the crystallization speed of the resin is fast and a practical solidification speed tends to be obtained.

[0023] Examples of other monomers include hydroxyalkenoates such as 3-hydroxyhexanoate (hereinafter sometimes referred to as 3HH) and 4-hydroxybutyrate (hereinafter sometimes referred to as 4HB).

[0024] The average content ratio of each monomer in the entire poly(3-hydroxyalkanoate) resin can be determined by a method known to those skilled in the art, for example, the method described in paragraph

[0047] of WO 2013 / 147139. The average content ratio means the molar ratio of 3-hydroxybutyrate and other monomers contained in the entire poly(3-hydroxyalkanoate) resin, and when the poly(3-hydroxyalkanoate) resin is a mixture of two or more poly(3-hydroxyalkanoate) resins, it means the molar ratio of each monomer contained in the entire mixture.

[0025] In order to suppress the generation of burrs in the injection molded article, a poly(3-hydroxyalkanoate)-based resin having a weight-average molecular weight within a predetermined range is used. The weight-average molecular weight of the poly(3-hydroxyalkanoate)-based resin is 150,000 to 350,000. If the weight-average molecular weight is less than 150,000, the molded article is difficult to release from the mold after injection molding, the molded article is easily broken, or the mechanical strength of the molded article may decrease. On the other hand, if the weight-average molecular weight exceeds 350,000, burrs are easily formed in the injection molded article. By setting the weight-average molecular weight of the poly(3-hydroxyalkanoate)-based resin to 350,000 or less, the generation of burrs can be effectively suppressed. By lowering the molecular weight of the resin, the melt viscosity when the resin is melted decreases, and therefore the injection pressure required for performing injection molding can be reduced. As a result, it is considered that the intrusion of the molten resin into the gap present in the mating portion of the cavity portion of the mold can be suppressed, and the generation of burrs can be suppressed. The weight average molecular weight is preferably from 200,000 to 350,000, and more preferably from 200,000 to 300,000.

[0026] Furthermore, when the poly(3-hydroxyalkanoate) resin is composed of a mixture of two or more poly(3-hydroxyalkanoate) resins, the weight average molecular weight of each poly(3-hydroxyalkanoate) resin is not particularly limited as long as the weight average molecular weight measured for the entire mixture of poly(3-hydroxyalkanoate) resins satisfies the above range.

[0027] The weight-average molecular weight of the poly(3-hydroxyalkanoate) resin can be measured in terms of polystyrene by gel permeation chromatography using a chloroform solution. As the column for the gel permeation chromatography, a column suitable for measuring the weight-average molecular weight may be used.

[0028] The method for producing the poly(3-hydroxyalkanoate) resin is not particularly limited, and may be a production method by chemical synthesis or a production method using a microorganism. Among them, a production method using a microorganism is preferable. A known method can be applied to the production method using a microorganism. For example, Aeromonas caviae, which produces P3HB3HV and P3HB3HH, and Alcaligenes eutrophus, which produces P3HB4HB, are known as bacteria that produce copolymers of 3-hydroxybutyrate and other hydroxyalkanoates. In particular, with regard to P3HB3HH, in order to increase the productivity of P3HB3HH, it is more preferable to use Alcaligenes eutrophus AC32 (FERM BP-6038) (T. Fukui, Y. Doi, J. Bateriol., 179, pp. 4821-4830 (1997)) or the like, into which genes of P3HA synthase group have been introduced, and these microorganisms are cultured under appropriate conditions to accumulate P3HB3HH in the cells, and microbial cells are used. In addition to the above, genetically modified microorganisms into which various poly(3-hydroxyalkanoate) resin synthesis-related genes have been introduced may be used according to the poly(3-hydroxyalkanoate) resin to be produced, or the culture conditions, including the type of substrate, may be optimized.

[0029] [Polylactic acid] Polylactic acid is a polyester with lactic acid as a constituent monomer. Conventionally known polylactic acid can be used, and any of L-lactic acid homopolymer, D-lactic acid homopolymer, L-lactic acid and D-lactic acid copolymer, and polymer blends thereof can be used. The ratio of L- and D-isomers constituting polylactic acid is not particularly limited. Polylactic acid may be either crystalline or amorphous, but amorphous polylactic acid can be preferably used from the viewpoint of processability. Amorphous polylactic acid refers to polylactic acid in which only the glass transition point (Tg), which is the temperature at which the physical properties of the amorphous part change significantly, is observed in thermal analysis such as differential scanning calorimetry (DSC), and the melting point (Tcc), which is the temperature at which the crystalline part begins to flow, is not observed.

[0030] The raw material for producing polylactic acid is not particularly limited, and can be L-lactic acid, D-lactic acid, DL-lactic acid, or a mixture thereof, or L-lactide, D-lactide, meso-lactide, or a mixture thereof, etc. The method for producing polylactic acid is not particularly limited, and can be a known method such as a dehydration condensation polymerization method or a ring-opening polymerization method.

[0031] The molecular weight of polylactic acid is not particularly limited as long as it can be used in injection molding, but the weight average molecular weight is preferably 50,000 to 300,000, and more preferably 100,000 to 250,000, in terms of excellent balance between physical properties and processability of the molded product. The weight average molecular weight of polylactic acid is measured using gel permeation chromatography (GPC) using a chloroform solution and converted into polystyrene. The column used in the GPC may be a column appropriate for measuring the molecular weight.

[0032] Commercially available polylactic acid can be used, and examples of such commercially available products include "Ingeo" (registered trademark) from NatureWorks and "REVODE" (registered trademark) from Zhejiang Haizheng Biomaterials, but are not limited thereto.

[0033] The amount of the polylactic acid is 20 parts by weight or more and 50 parts by weight or less, preferably 21 parts by weight or more and less than 49 parts by weight, based on 100 parts by weight of the total of the poly(3-hydroxyalkanoate) resin and the polylactic acid. If the amount of the polylactic acid is less than 20 parts by weight, it may be difficult to sufficiently suppress the occurrence of burrs in the injection molded article. If the amount of the polylactic acid is more than 50 parts by weight, the heat resistance may decrease.

[0034] The resin composition for injection molding may contain other resins in addition to the poly(3-hydroxyalkanoate) resin and any polylactic acid, as long as the effects of the invention are not impaired. Examples of such other resins include aliphatic polyester resins such as polybutylene succinate adipate, polybutylene succinate, and polycaprolactone, and aliphatic aromatic polyester resins such as polybutylene adipate terephthalate, polybutylene sebate terephthalate, and polybutylene azelate terephthalate. Only one type of other resin may be contained, or two or more types may be contained.

[0035] The content of the other resin is not particularly limited, but is preferably 30 parts by weight or less, more preferably 20 parts by weight or less, relative to 100 parts by weight of the total of the poly(3-hydroxyalkanoate) resin and the polylactic acid. The lower limit of the content of the other resin is not particularly limited, and may be 0 part by weight.

[0036] [Inorganic filler] The resin composition for injection molding can form an injection molded article in which the generation of burrs is suppressed without containing an inorganic filler, but from the viewpoint of improving the strength of the injection molded article, it is preferable that the resin composition for injection molding contains an inorganic filler.

[0037] The inorganic filler is not particularly limited as long as it is an inorganic filler that can be added to a resin material for injection molding, and examples thereof include silica-based inorganic fillers such as quartz, fumed silica, silicic anhydride, fused silica, crystalline silica, amorphous silica, fillers obtained by condensing alkoxysilanes, and ultrafine amorphous silica, alumina, zircon, iron oxide, zinc oxide, titanium oxide, silicon nitride, boron nitride, aluminum nitride, silicon carbide, glass, silicone rubber, silicone resin, titanium oxide, carbon fiber, mica, graphite, carbon black, ferrite, graphite, diatomaceous earth, clay, clay, talc, calcium carbonate, manganese carbonate, magnesium carbonate, barium sulfate, and silver powder. These may be used alone or in combination of two or more.

[0038] The inorganic filler may be surface-treated to improve dispersibility in the resin composition for injection molding. Examples of the treatment agent used for the surface treatment include higher fatty acids, silane coupling agents, titanate coupling agents, sol-gel coating agents, and resin coating agents.

[0039] The water content of the inorganic filler is preferably 0.01 to 10%, more preferably 0.01 to 5%, and even more preferably 0.01 to 1%, in order to easily suppress hydrolysis of the poly(3-hydroxyalkanoate) resin and polylactic acid. The water content can be determined in accordance with JIS-K5101.

[0040] The average particle size of the inorganic filler is preferably 0.1 to 100 μm, more preferably 0.1 to 50 μm, in order to provide excellent properties and processability of the resin composition for injection molding. The average particle size can be measured using a laser diffraction / scattering device such as "Microtrac MT3100II" manufactured by Nikkiso Co., Ltd.

[0041] Among inorganic fillers, inorganic fillers belonging to silicates are preferred because they can improve heat resistance and processability. Furthermore, among silicates, one or more selected from the group consisting of talc, mica, kaolinite, montmorillonite, and smectite are preferred because they have a large effect of improving the mechanical strength of the injection molded body, have a small particle size distribution, and are less likely to impair surface smoothness and mold transferability. Two or more silicates may be used in combination, and in that case, the type and use ratio of the silicate can be appropriately adjusted.

[0042] Examples of the talc include general-purpose talc and surface-treated talc. Specific examples include "Microace" (registered trademark) from Nippon Talc Co., Ltd., "Talcan Powder" (registered trademark) from Hayashi Kasei Co., Ltd., and talc manufactured by Takehara Chemical Industry Co., Ltd. and Maruo Calcium Co., Ltd.

[0043] Examples of the mica include wet-ground mica and dry-ground mica, and specific examples include mica manufactured by Yamaguchi Mica Co., Ltd. and Keiwa Rozai Co., Ltd.

[0044] Examples of the kaolinite include dry kaolin, calcined kaolin, wet kaolin, etc., and specific examples include "TRANSLINK" (registered trademark), "ASP" (registered trademark), "SANTINTONE" (registered trademark), and "ULTREX" (registered trademark) manufactured by Hayashi Kasei Corporation, and kaolinite manufactured by Keiwa Rozai Co., Ltd.

[0045] The amount of the inorganic filler is 0 to 40 parts by weight per 100 parts by weight of the total of the poly(3-hydroxyalkanoate) resin and the polylactic acid. The inorganic filler does not have to be added, but adding an inorganic filler has the advantage of improving the strength of the injection molded article. When an inorganic filler is added, the amount is preferably 5 to 35 parts by weight, more preferably 10 to 30 parts by weight. If the amount of the inorganic filler exceeds 40 parts by weight, the flowability may decrease.

[0046] (Additives) The resin composition for injection molding may contain additives other than inorganic fillers, as long as the effects of the invention are not impaired. Examples of additives that can be used depending on the purpose include crystallization nucleating agents, lubricants, plasticizers, antistatic agents, flame retardants, conductive agents, heat insulating agents, crosslinking agents, antioxidants, ultraviolet absorbers, colorants, organic fillers, and hydrolysis inhibitors. Additives having biodegradability are particularly preferred.

[0047] Examples of the crystallization nucleating agent include pentaerythritol, orotic acid, aspartame, cyanuric acid, glycine, zinc phenylphosphonate, and boron nitride. Among them, pentaerythritol is preferred because it is particularly effective in promoting the crystallization of poly(3-hydroxyalkanoate) resin. The amount of the crystallization nucleating agent used is not particularly limited, but is preferably 0.1 to 10 parts by weight, more preferably 0.5 to 8.5 parts by weight, and even more preferably 0.7 to 6 parts by weight, relative to 100 parts by weight of poly(3-hydroxyalkanoate) resin. The crystallization nucleating agent may be used alone or in combination of two or more kinds, and the mixing ratio can be appropriately adjusted depending on the purpose.

[0048] Examples of the lubricant include behenamide, oleamide, erucamide, stearamide, palmitamide, N-stearylbehenamide, N-stearylerucamide, ethylenebisstearamide, ethylenebisoleamide, ethylenebiserucamide, ethylenebislauramide, ethylenebiscapricamide, p-phenylenebisstearamide, and polycondensates of ethylenediamine, stearic acid, and sebacic acid. Among them, behenamide and erucamide are preferred because of their particularly excellent lubricant effect on poly(3-hydroxyalkanoate)-based resins. The amount of the lubricant used is not particularly limited, but is preferably 0.01 to 5 parts by weight, more preferably 0.05 to 3 parts by weight, and even more preferably 0.1 to 1.5 parts by weight, relative to 100 parts by weight of poly(3-hydroxyalkanoate)-based resin. In addition, the lubricant may be used alone or in combination of two or more kinds, and the mixing ratio can be appropriately adjusted depending on the purpose.

[0049] Examples of the plasticizer include glycerin ester compounds, citrate compounds, sebacic acid ester compounds, adipate compounds, polyether ester compounds, benzoic acid ester compounds, phthalic acid ester compounds, isosorbide ester compounds, polycaprolactone compounds, and dibasic acid ester compounds. Among them, glycerin ester compounds, citrate compounds, sebacic acid ester compounds, and dibasic acid ester compounds are preferred because of their particularly excellent plasticizing effect on poly(3-hydroxyalkanoate) resins. Examples of the glycerin ester compounds include glycerin diacetomonolaurate and the like. Examples of the citrate compounds include acetyl tributyl citrate and the like. Examples of the sebacic acid ester compounds include dibutyl sebacate and the like. Examples of the dibasic acid ester compounds include benzyl methyl diethylene glycol adipate and the like. The amount of the plasticizer used is not particularly limited, but is preferably 1 to 20 parts by weight, more preferably 2 to 15 parts by weight, and even more preferably 3 to 10 parts by weight, per 100 parts by weight of the total of the poly(3-hydroxyalkanoate) resin and the polylactic acid. In addition, the plasticizer may be used alone or in combination of two or more kinds, and the mixing ratio can be appropriately adjusted depending on the purpose.

[0050] [Manufacturing method of injection molded products] Hereinafter, a method for producing an injection molded article made from the above-mentioned resin composition for injection molding will be specifically described.

[0051] First, a poly(3-hydroxyalkanoate) resin, any polylactic acid, any inorganic filler, and other components are added as necessary, and melt-kneaded using an extruder, kneader, Banbury mixer, roll, or the like to prepare a resin composition, which is extruded into a strand shape and then cut to obtain pellets having a particle shape such as a cylindrical shape, an elliptical cylindrical shape, a spherical shape, a cubic shape, a rectangular parallelepiped shape, etc. The prepared pellets are desirably thoroughly dried at 40 to 80°C to remove moisture, and then subjected to injection molding.

[0052] The temperature at which the melt kneading is carried out cannot be generally defined because it depends on the melting point, melt viscosity, etc. of the resin used, but the resin temperature of the melt kneaded product at the die outlet is preferably 160 to 200° C., more preferably 165 to 195° C., and even more preferably 170 to 190° C. If the resin temperature of the melt kneaded product is less than 160° C., the resin components containing the poly(3-hydroxyalkanoate) resin may not melt, and if it exceeds 200° C., the resin components containing the poly(3-hydroxyalkanoate) resin may be thermally decomposed.

[0053] Next, the prepared pellets can be subjected to injection molding to form an injection molded article. Injection molding refers to a method in which a heated and melted resin composition is injected into a mold, the resin composition is cooled and solidified in the mold, the mold is opened, and the molded article is released to obtain a molded article. As the injection molding method, in addition to the injection molding method generally adopted when molding a thermoplastic resin, injection molding methods such as a gas-assisted molding method and an injection compression molding method can be adopted. In addition, an in-mold molding method, a gas press molding method, a two-color molding method, a sandwich molding method, a PUSH-PULL method, a SCORIM method, etc. can also be adopted. However, the injection molding method that can be used is not limited to the above methods.

[0054] The temperature at which the resin composition is melted during injection molding is, for example, preferably 160 to 200° C., and more preferably 170 to 190° C. The temperature at which the resin composition is cooled by a mold after injection is, for example, preferably 25 to 55° C., and more preferably 30 to 50° C.

[0055] The obtained injection molded article has high heat resistance and good appearance because the generation of burrs is suppressed, and the effort of removing burrs in post-processing can be omitted or simplified. In addition, since the resin component is mainly composed of poly(3-hydroxyalkanoate) resin, it has seawater degradability, which can solve the environmental problem caused by the dumping of plastics into the ocean.

[0056] The uses of the injection molded articles are not particularly limited, but examples thereof include tableware, agricultural materials, office automation parts, home appliance parts, automotive parts, daily necessities, stationery, bottle molded products, extruded sheets, and irregular extrusion products. EXAMPLES

[0057] The present invention will be specifically described below with reference to examples, but the technical scope of the present invention is not limited to these examples.

[0058] (Method of measuring weight average molecular weight) The weight average molecular weight of the poly(3-hydroxyalkanoate) resin was measured by first dissolving the poly(3-hydroxyalkanoate) resin in chloroform and heating the resin in a hot water bath at 60° C. for 0.5 hours, filtering the soluble matter through a disposable PTFE filter having a pore size of 0.45 μm, and then subjecting the filtrate to GPC measurement under the following conditions. GPC measuring device: Hitachi RI monitor (L-3000) Columns: Showa Denko KG (1 column), K-806L (2 columns) Sample concentration: 3mg / ml Free solution: Chloroform solution Free liquid flow rate: 1.0ml / min Sample injection volume: 100 μL Analysis time: 30 minutes Standard sample: Standard polystyrene

[0059] (A) Poly(3-hydroxyalkanoate) resin: The following was used. P3HA-1: The one obtained in Production Example 1 was used. <Production Example 1> The KNK-005 strain (see U.S. Patent No. 7,384,766) was used for the culture production. The composition of the seed culture medium was 1 w / v% Meat-extract, 1 w / v% Bacto-Tryptone, 0.2 w / v% Yeast-extract, 0.9 w / v% Na2HPO4·12H2O, and 0.15 w / v% KH2PO4 (pH 6.8).

[0060] The composition of the preculture medium was 1.1w / v% Na2HPO4·12H2O, 0.19w / v% KH2PO4, 1.29w / v% (NH4)2SO4, 0.1w / v% MgSO4·7H2O, 0.5v / v% trace metal salt solution (1.6w / v% FeCl3·6H2O, 1w / v% CaCl2·2H2O, 0.02w / v% CoCl2·6H2O, 0.016w / v% CuSO4·5H2O, 0.012w / v% NiCl2·6H2O dissolved in 0.1N hydrochloric acid). Palm oil was added as a carbon source at a concentration of 10g / L.

[0061] The composition of the P3HA production medium was 0.385 w / v% Na2HPO4·12H2O, 0.067 w / v% KH2PO4, 0.291 w / v% (NH4)2SO4, 0.1 w / v% MgSO4·7H2O, 0.5 v / v% trace metal salt solution (1.6 w / v% FeCl3·6H2O, 1 w / v% CaCl2·2H2O, 0.02 w / v% CoCl2·6H2O, 0.016 w / v% CuSO4·5H2O, and 0.012 w / v% NiCl2·6H2O dissolved in 0.1 N hydrochloric acid), and 0.05 w / v% BIOSPUREX200K (antifoaming agent: manufactured by Cognis Japan).

[0062] First, glycerol stock (50μl) of KNK-005 strain was inoculated into a seed medium (10ml) and cultured for 24 hours to perform seed culture. Next, the seed culture liquid was inoculated at 1.0v / v% into a 3L jar fermenter (Marubishi Bioengineering MDL-300 type) containing 1.8L of preculture medium. The operating conditions were a culture temperature of 33°C, agitation speed of 500rpm, and aeration rate of 1.8L / min, and the preculture was performed for 28 hours while controlling the pH between 6.7 and 6.8. A 14% aqueous solution of ammonium hydroxide was used for pH control.

[0063] Next, the preculture solution was inoculated at 1.0 v / v% into a 10 L jar fermenter (Marubishi Bioengineering MDS-1000 model) containing 6 L of production medium. The operating conditions were a culture temperature of 28°C, an agitation speed of 400 rpm, and an aeration rate of 6.0 L / min, and the pH was controlled between 6.7 and 6.8. A 14% aqueous solution of ammonium hydroxide was used for pH control. Palm oil was used as the carbon source. Cultivation was continued for 64 hours, and after completion of the cultivation, the cells were collected by centrifugation, washed with methanol, freeze-dried, and the dry cell weight was measured.

[0064] 100 ml of chloroform was added to 1 g of the dried cells obtained, and the mixture was stirred at room temperature for 24 hours to extract the P3HA from the cells. The cell residue was filtered, and then concentrated to a total volume of 30 ml using an evaporator. 90 ml of hexane was gradually added, and the mixture was left for 1 hour with gentle stirring. The precipitated P3HA was filtered, and then vacuum dried at 50°C for 3 hours to obtain P3HA.

[0065] The 3HH composition of the obtained P3HA was measured by gas chromatography as follows. 2 ml of sulfuric acid-methanol mixture (15:85) and 2 ml of chloroform were added to 20 mg of dried P3HA, sealed, and heated at 100°C for 140 minutes to obtain methyl ester of P3HA decomposition product. After cooling, 1.5 g of sodium bicarbonate was gradually added to neutralize it and left until the generation of carbon dioxide gas stopped. 4 ml of diisopropyl ether was added and mixed well, then centrifuged, and the monomer unit composition of the polyester decomposition product in the supernatant was analyzed by capillary gas chromatography. A gas chromatograph made by Shimadzu Corporation GC-17A and a capillary column made by GL Science Co., Ltd. NEUTRA BOND-1 (column length 25 m, column inner diameter 0.25 mm, liquid film thickness 0.4 μm) were used. He was used as the carrier gas, the column inlet pressure was 100 kPa, and 1 μl of the sample was injected. The temperature conditions were as follows: the initial temperature was 100, the temperature was raised from 200° C. to 200° C. at a rate of 8° C. / min, and the temperature was then raised from 200 to 290° C. at a rate of 30° C. / min. Analysis under the above conditions revealed that the compound was P3HA, poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (abbreviation: P3HB3HH), as shown in chemical formula (1).

[0066] After the cultivation, P3HB3HH was obtained from the culture medium by the method described in International Publication No. 2010 / 067543. The weight average molecular weight measured by GPC was 220,000. The 3-hydroxyhexanate (3HH) composition was 4.6 mol%.

[0067] P3HA-2: The one obtained in Production Example 2 was used. <Production Example 2> Except for using palm kernel oil as the carbon source, P3HB3HH was obtained in the same manner as in Production Example 1. The weight-average molecular weight was 430,000, and the 3HH composition was 5.8 mol%.

[0068] P3HA-3: The one obtained in Production Example 3 was used. <Production Example 3> P3HA-2 was hydrolyzed using a pressure cooker (HASTEST PC-422R5E) to obtain P3HB3HH with a weight-average molecular weight of 320,000. The hydrolysis conditions were a treatment time of 4 hours and a pressure of 1 kgf / cm. 2 The temperature was 120°C and the humidity was 100%.

[0069] P3HA-4: The one obtained in Production Example 4 was used.

[0070] <Production Example 4> P3HA-2 was hydrolyzed using a pressure cooker (HASTEST PC-422R5E) to obtain P3HB3HH with a weight-average molecular weight of 110,000. The hydrolysis conditions were a treatment time of 12 hours and a pressure of 1 kgf / cm. 2 The temperature was 120°C and the humidity was 100%.

[0071] P3HA-5: The one obtained in Production Example 5 was used. <Production Example 5> KNK-005 ΔphaZ1::Plac-phaC described in Example 11 of WO 2015 / 146195 ReA mixture containing P3HB3HH and P3HB was produced using the ΔphaZ2,6 strain in the same manner as in Example 1 of the International Publication, except that palm kernel oil was used as the carbon source. The weight-average molecular weight was 260,000, and the 3HH composition was 6.8 mol%.

[0072] Other substances used in the examples and comparative examples are listed below. (B) Polylactic acid: The following was used. PLA-1: NatureWorks Ingeo 3251D PLA-2: NatureWorks Ingeo 10361D

[0073] (C) Inorganic filler: talc (Microace K-1 manufactured by Nippon Talc Co., Ltd.) (D) Pentaerythritol: NeuRizer P, manufactured by Nippon Synthetic Chemical Industry Co., Ltd.

[0074] <Examples 1 to 24 and Comparative Examples 1 to 5> (Production of polyester resin composition) (A) Poly(3-hydroxyalkanoate) resin of the type shown in Table 1, (B) polylactic acid, and (C) talc as an inorganic filler, and further (D) pentaerythritol as a crystallization nucleating agent were melt-kneaded at a set temperature of 160 to 180°C and a screw rotation speed of 100 rpm using a co-rotating intermeshing type twin screw extruder (Toshiba Machine Co., Ltd.: TEM-26SS) in the blending ratio shown in Table 1 (the blending ratio in the table indicates parts by weight), to obtain a polyester resin composition. At this time, the resin temperature was 152°C. The resin temperature was measured directly on the molten resin coming out of the die using a K-type thermocouple. The polyester resin composition was taken out of the die in the form of a strand and cut into pellets. The obtained pellets were dehumidified and dried at 60°C to remove moisture.

[0075] (Injection molding: Making ISO dumbbells for measuring physical properties) Using the obtained pellets of the polyester resin composition as a raw material, an injection molding machine (Toyo Machinery & Metals: Si-100IV) was used to mold dumbbell test pieces conforming to the ISO3167 standard with a cylinder temperature setting of 120 to 165°C and a mold temperature setting of 45°C (mold temperature).

[0076] (Heat resistance) The dumbbell test pieces obtained by injection molding were cut into bar-shaped test pieces, which were then stored for one month at 23°C and 50% humidity, after which the deflection temperature under load (abbreviated as DTUL) was measured in accordance with ISO 751-1. The higher the deflection temperature under load, the better the heat resistance.

[0077] (Flexural modulus) The dumbbell test pieces obtained by injection molding were cut into bar-shaped test pieces, which were then stored for one month at 23°C and 50% humidity. After that, a bending test was carried out in accordance with ISO178 to measure the bending modulus.

[0078] (Practical usability) The obtained dumbbell test pieces were immersed in water at 80°C for 5 minutes, and visually observed for changes in shape (distortion, bending, breakage) to evaluate their practical usability as cutlery. ○: No deformation is observed and it can be used practically △: Slight changes, but can be used depending on the object of use ×: Broken in hot water, cannot be used.

[0079] (Burr evaluation method) The obtained polyester resin composition pellets were used as a raw material and molded using an injection molding machine (Toyo Machinery & Metals: Si-30IV) with the cylinder temperature set at 120 to 165°C and the mold temperature set at 45°C. The procedure was as follows: first, a spiral flow mold was used to determine the injection pressure required to flow the specified flow length (170 mm), then a burr evaluation mold was used to produce a molded body for burr evaluation at the aforementioned injection pressure, and the burrs were quantified on the molded body.

[0080] (Confirmation of flow length using a spiral flow mold) The flow length of the resin was measured using a spiral flow mold (gate φ6 mm, thickness 1.5 mm, width 10 mm). At this time, a flow length of 170 mm was assumed to be a state in which a large number of molded products (15 to 20 pieces) could be obtained. The flow length was confirmed from the spiral molded product, and the injection pressure at that time was recorded.

[0081] (Molding using a burr evaluation mold) The mold used for burr evaluation was a mold capable of molding a disk with a diameter of 50 mm and a thickness of 2 mm and a direct gate (φ5 mm). A molded body for burr evaluation was produced using the injection pressure required to flow a flow length of 170 mm confirmed with the spiral flow mold.

[0082] (Bali rating) The mating surface (parting line) between the dies of the molded product for burr evaluation was observed under a microscope, and the length of the burr was quantitatively measured. A burr length of 30 μm or less was considered to be acceptable.

[0083] (Mold releasability) In injection molding, the molten resin composition is poured into a mold and then cooled. After cooling, the mold is opened. When removing the molded product from the movable surface of the mold, an ejector pin is used to push out and remove the molded product. When the molded product was not deformed or damaged, it was evaluated as ◯, and when it was deformed or damaged, it was evaluated as ×.

[0084] [Table 1-1]

[0085] [Table 1-2]

[0086] From Table 1, the following can be seen. In Examples 1 to 24, injection molding was performed using a resin composition in which a poly(3-hydroxyalkanoate)-based resin was the main resin component, the content of polylactic acid was 50% by weight or less of the resin component, and the weight-average molecular weight of the poly(3-hydroxyalkanoate)-based resin was in the range of 150,000 to 350,000, and the obtained injection-molded body had high heat resistance and a small amount of burrs of 30 μm or less. On the other hand, in Comparative Examples 1 to 3, the content of polylactic acid was zero, and the amount of burrs was large, 30 μm or more. In Comparative Example 4, the weight-average molecular weight of the poly(3-hydroxyalkanoate)-based resin was low at 110,000, and the mold releasability during injection molding was poor, and an injection-molded body could not be obtained. In Comparative Examples 5 to 7, the weight-average molecular weight of the poly(3-hydroxyalkanoate)-based resin was high at 430,000, and regardless of the blending ratio of polylactic acid, the amount of burrs was very large, 100 μm or more. Among them, Comparative Example 7 had a drawback in that the blending ratio of polylactic acid was high and the heat resistance was low.In addition, Comparative Examples 8 and 9 were injection molded using only polylactic acid without using poly(3-hydroxyalkanoate) resin, and the amount of burrs was high at 30 μm or more, and the heat resistance was also extremely low.

Claims

1. A resin composition for injection molding comprising a resin component and, optionally, an inorganic filler, The resin component contains a poly(3-hydroxyalkanoate) resin and a polylactic acid, the content of the polylactic acid is 20 parts by weight or more and 50 parts by weight or less per 100 parts by weight of the total of the poly(3-hydroxyalkanoate) resin and the polylactic acid, the content of the inorganic filler is 0 parts by weight or more and 40 parts by weight or less with respect to 100 parts by weight of the total of the poly(3-hydroxyalkanoate) resin and the polylactic acid, the poly(3-hydroxyalkanoate)-based resin is one or more selected from the group consisting of poly(3-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), and poly(3-hydroxybutyrate-co-4-hydroxybutyrate); The poly(3-hydroxyalkanoate) resin has a weight average molecular weight of 150,000 to 300,000.

2. 2. The injection molding resin composition according to claim 1, wherein the poly(3-hydroxyalkanoate)-based resin comprises poly(3-hydroxybutyrate-co-3-hydroxyhexanoate).

3. 3. The resin composition for injection molding according to claim 1, wherein the poly(3-hydroxyalkanoate) resin has a weight average molecular weight of 200,000 to 300,000.

4. The resin composition for injection molding according to any one of claims 1 to 3, wherein the content of the inorganic filler is 5 parts by weight or more and 40 parts by weight or less per 100 parts by weight of the total of the poly(3-hydroxyalkanoate) resin and the polylactic acid.

5. The resin composition for injection molding according to any one of claims 1 to 4, wherein the inorganic filler is a silicate.

6. 6. The resin composition for injection molding according to claim 5, wherein the silicate is at least one selected from the group consisting of talc, mica, kaolinite, montmorillonite, and smectite.

7. The resin composition for injection molding according to any one of claims 1 to 6, further comprising a crystallization nucleating agent.

8. An injection molded article made from the resin composition for injection molding according to any one of claims 1 to 7.

9. A method for producing an injection molded article, comprising the steps of heating and melting the resin composition for injection molding according to any one of claims 1 to 7, injecting the composition into a mold, and then cooling and solidifying the composition.

Citation Information

Patent Citations

  • Resin composition, method for producing the resin composition and injection molded article

    JP2005232229A

  • Resin composition

    JP2005232230A

  • Resin composition and method for producing resin composition

    JP2005232231A

  • Copolymer resin composition, molded article, and method of producing the copolymer resin composition

    JP2012087207A

  • Aliphatic polyester resin composition

    JP2013057039A