Manufacturing method of superabsorbent resin
By crosslinking and chopping hydrogel polymers with a carboxylic acid additive and using alternating air flows, the method addresses issues of warping and efficiency in superabsorbent resin production, achieving superior drying and physical properties.
Patent Information
- Application Number
- JP2023504422
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-12-06
- Filing Date
- 2021-12-07
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-12-07
AI Technical Summary
The production of superabsorbent resins faces challenges such as the generation of fine powder, increased energy usage, and warping during the drying process due to cohesive forces, which affect the physical properties and efficiency of the final product.
A method involving the crosslinking of a water-soluble ethylenically unsaturated monomer with an internal crosslinking agent, mixing with a carboxylic acid additive, and chopping the hydrogel polymer into pieces, followed by drying with alternating up-flow and down-flow air at specific temperatures to control particle size and reduce agglomeration.
This method effectively suppresses warping and enhances drying efficiency, resulting in superabsorbent resins with improved physical properties and reduced fine powder generation.
Smart Images

Figure 0007570758000023 
Figure 0007570758000024 
Figure 0007570758000001
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of priority based on Korean Patent Application No. 10-2020-0169708 filed on December 7, 2020, and Korean Patent Application No. 10-2021-0173196 filed on December 6, 2021, and all contents disclosed in the documents of said Korean patent applications are incorporated herein by reference.
[0002] The present invention relates to a method for producing a superabsorbent polymer, and more specifically, to a method for producing a superabsorbent polymer that achieves excellent drying efficiency and thereby effectively suppresses the occurrence of warping of the resin. [Background technology]
[0003] Super absorbent polymer (SAP) is a synthetic polymeric substance that has the ability to absorb 500 to 1,000 times its own weight in water, and each developer has a different name for it, such as SAM (Super Absorbency Material), AGM (Absorbent Gel Material), etc. Such super absorbent polymers first came into practical use as sanitary products, and are now widely used as soil water retention agents for horticulture, water stoppers for civil engineering and construction, seedling sheets, freshness preserving agents in the food distribution field, and materials for packs.
[0004] Such superabsorbent polymers are widely used in the field of sanitary materials, such as diapers and sanitary napkins. In the sanitary materials, the superabsorbent polymers are generally contained in a state of being spread in the pulp. However, in recent years, efforts have been made to provide sanitary materials, such as diapers, with thinner thicknesses, and as part of these efforts, the pulp content has been reduced, or even going a step further, the development of so-called pulpless diapers, which do not use pulp at all, has been actively promoted.
[0005] In this way, in the case of sanitary materials in which the pulp content is reduced or no pulp is used, it is inevitable that the superabsorbent polymer is contained at a relatively high ratio, and the superabsorbent polymer particles are contained in the sanitary materials as multiple layers. In order for the overall superabsorbent polymer particles contained in multiple layers to more efficiently absorb a large amount of liquid such as urine, the superabsorbent polymer basically needs to exhibit not only high water absorption performance but also a fast water absorption speed.
[0006] On the other hand, such a superabsorbent resin is generally manufactured by polymerizing a monomer to produce a hydrogel polymer containing a large amount of water, and then drying the hydrogel polymer and pulverizing it into resin particles having a desired particle size. However, when the hydrogel polymer is dried and then pulverized, a large amount of fine powder is generated, which deteriorates the physical properties of the final superabsorbent resin.
[0007] In order to reuse such fine powder, it is common to mix the fine powder with water, coagulate the powder, produce a fine regranulated powder, and then feed the fine regranulated powder produced through processes such as drying, pulverization, and classification. However, the water used in this process increases energy consumption during the drying process, and increases the load on the equipment, which can reduce the productivity of the superabsorbent resin.
[0008] Furthermore, during the manufacturing process of the superabsorbent resin, the polymerized hydrogel polymer has the property of agglomerating with itself, and when it is manufactured into agglomerated fine particles, the cohesive force increases, which causes a problem that the drying process performed later is not performed well. Specifically, such a drying process is usually performed by applying hot air using a belt dryer equipped with a perforated plate, but the void ratio in the drying layer is significantly reduced due to the increase in the cohesive force of the hydrogel polymer, and this causes a high differential pressure of the hot air, which causes the outer periphery of the drying layer to warp, making it difficult to dry a large amount of material.
[0009] In other words, if the wet rate is high or the dried product is warped, it is difficult to achieve the desired physical properties of the product, resulting in defects. Therefore, there is a continuous demand for development of a technology to improve drying efficiency without such problems. Summary of the Invention [Problem to be solved by the invention]
[0010] Therefore, the present invention provides a method for producing a superabsorbent polymer, which involves cutting a polymerized hydrogel polymer with a specific additive and then drying the resulting product under specific conditions, thereby easily controlling the particle size to a desired range without generating a large amount of fine powder, exhibiting excellent drying efficiency and effectively suppressing warping of the dried product even when the drying amount is large, thereby improving the physical properties of the superabsorbent polymer finally produced. [Means for solving the problem]
[0011] In order to solve the above problems, the present invention provides a step of cross-linking and polymerizing a water-soluble ethylenically unsaturated monomer having at least a partially neutralized acidic group in the presence of an internal cross-linking agent and a polymerization initiator to form a hydrogel polymer; preparing a mixture containing chopped hydrogel polymer by mixing the hydrogel polymer with a carboxylic acid additive and then chopping the mixture; and and drying the chopped mixture by alternately blowing upflow air at 120°C to 210°C and downflow air at 120°C to 210°C to form a base resin powder. The total time for supplying the downward airflow is longer than the total time for supplying the upward airflow. A method for producing a superabsorbent resin is provided. Effect of the Invention
[0012] According to the method for producing the superabsorbent polymer of the present invention, the polymerized hydrogel polymer is mixed with a carboxylic acid additive and then chopped, thereby making it possible to control the particle size to a desired range without aggregation between hydrogel polymer particles, and thus simplifying the grinding process leading to coarse grinding and fine grinding after the drying process, and significantly reducing the amount of fine powder generated during the process. In addition, by adjusting the drying conditions after chopping to a specific range, excellent drying efficiency is achieved, and warping of the dried product can be effectively suppressed even if the drying amount is large. Finally, the superabsorbent polymer produced as described above can achieve excellent physical properties. [Brief description of the drawings]
[0013] [Figure 1] 4 is a cross-sectional photograph of dried products produced according to an embodiment of the present invention and a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention.
[0015] The singular expression includes the plural expression unless the context clearly indicates otherwise. It should be understood that, in this specification, the terms "comprise", "comprise", "have" and the like are intended to specify the presence of embodied features, steps, components, or combinations thereof, and do not preclude the possibility of the presence or addition of one or more other features, steps, components, or combinations thereof.
[0016] The terms first, second, third, etc. are used to describe various elements, and such terms are used only to distinguish one element from another.
[0017] Although the present invention can be implemented in various forms through various modifications, specific embodiments are described in detail below, but it is to be understood that this is not intended to limit the present invention to the specific disclosed embodiments, and that the present invention includes all modifications, equivalents, and alternatives falling within the spirit and technical scope of the present invention.
[0018] The term "polymer" or "polymeric polymer" used herein means a state in which a water-soluble ethylenically unsaturated monomer is polymerized, and may include any range of water content or particle size. Among the above polymers, a polymer having a water content (water content) of about 40% by weight or more in a state after polymerization and before drying may be called a hydrogel polymer, and particles of such a hydrogel polymer that have been crushed and dried may be called a crosslinked polymer.
[0019] In addition, the term "super absorbent resin powder" refers to a particulate substance containing a crosslinked polymer obtained by polymerizing a water-soluble ethylenically unsaturated monomer containing acidic groups and at least a portion of the acidic groups being neutralized, and crosslinking the water-soluble ethylenically unsaturated monomer with an internal crosslinking agent.
[0020] Furthermore, the term "super absorbent polymer" refers, depending on the context, to a crosslinked polymer obtained by polymerizing a water-soluble ethylenically unsaturated monomer containing an acidic group and at least a portion of the acidic group being neutralized, or to a powder-like base resin consisting of super absorbent polymer particles obtained by pulverizing the crosslinked polymer, or to a crosslinked polymer or base resin that has been subjected to an additional process, such as surface crosslinking, fine powder regranulation, drying, pulverization, classification, etc., to be made into a state suitable for commercialization.
[0021] In addition, the term "crosslinked polymer" means a product crosslinked and polymerized in the presence of the water-soluble ethylenically unsaturated monomer and an internal crosslinking agent, and the term "base resin powder" means a material containing such a crosslinked polymer.
[0022] A method for producing a superabsorbent resin according to one embodiment of the present invention includes the steps of: cross-linking and polymerizing a water-soluble ethylenically unsaturated monomer having at least a partially neutralized acidic group in the presence of an internal cross-linking agent and a polymerization initiator to form a hydrogel polymer; mixing the hydrogel polymer with a carboxylic acid additive and then chopping the mixture to produce a mixture containing chopped hydrogel polymer; and drying the chopped mixture by alternately introducing up-flow at 120°C to 210°C and down-flow at 120°C to 210°C to form a base resin powder, wherein the total introduction time of the down-flow is longer than the total introduction time of the up-flow.
[0023] In order to produce superabsorbent resin particles with a desired particle size during the manufacturing process of superabsorbent resin, the polymerized hydrogel polymer is crushed (or chopped) and dried, but when the hydrogel polymer is manufactured into fine particles, the cohesive force increases, which makes it difficult to dry in the subsequent drying process, resulting in an increase in the amount of energy used in the drying process. In addition, because re-agglomeration occurs, a long period of coarse crushing and fine crushing is required after the drying process to achieve the desired particle size, and there is a problem that the amount of fine powder generated increases significantly in the additional crushing process.
[0024] Specifically, this drying process is usually carried out by applying hot air using a belt dryer equipped with a perforated plate, but the void ratio in the drying layer is significantly reduced due to the increase in the cohesive force of the hydrogel polymer, which causes the hot air pressure difference to increase, resulting in the problem of warping of the outer periphery of the dried product. Also, when there is a large amount of dried product, the inside of the dried product is not dried sufficiently, and the drying efficiency is significantly reduced.
[0025] Therefore, the inventors have found that by chopping the hydrogel polymer in the presence of a specific carboxylic acid additive, it is possible to control the hydrogel particles to have a desired particle size without agglomeration, and a long additional grinding process after drying is not necessary, thereby significantly reducing the amount of fine powder generated. In addition, the inventors have found that by drying the chopped mixture, in which the cohesive force is reduced by mixing the additive, under specific conditions, excellent drying efficiency can be achieved and the occurrence of warping of the dried product can be effectively suppressed even if the drying amount is large, and have completed the present invention.
[0026] Meanwhile, the carboxylic acid additive has both hydrophobic and hydrophilic functional groups. Since the water-soluble ethylenically unsaturated monomer contains an acid group (-COOH) and / or a neutralized acid group (-COO-), the surface of the hydrogel polymer produced by polymerization has a large amount of hydrophilic moieties due to the acid group (-COOH) and / or the neutralized acid group (-COO-) that remain uninvolved in the polymerization. Therefore, when the additive is mixed with the hydrogel polymer, the hydrophilic functional group of the additive is adsorbed to at least a part of the hydrophilic moieties present on the surface of the hydrogel polymer, and the surface of the polymer to which the additive is adsorbed is hydrophobic due to the hydrophobic functional group located at the other end of the additive. This can suppress the aggregation between the resin particles.
[0027] Hereinafter, each step of the manufacturing method will be described in detail.
[0028] (Polymerization stage) A method for preparing a superabsorbent resin according to an embodiment of the present invention includes a step of cross-linking and polymerizing a water-soluble ethylenically unsaturated monomer having at least a partially neutralized acidic group in the presence of an internal cross-linking agent and a polymerization initiator to form a hydrogel polymer.
[0029] Specifically, the process is a step of thermally or photopolymerizing a monomer composition containing a monomer mixture and a polymerization initiator in the presence of an internal crosslinking agent to form a hydrogel polymer.
[0030] The water-soluble ethylenically unsaturated monomer may be any monomer commonly used in the manufacture of superabsorbent resins. As a non-limiting example, the water-soluble ethylenically unsaturated monomer may be a compound represented by the following formula 2:
[0031] [Chemical formula 2] R1-COOM 1
[0032] In the above Chemical Formula 2, R1 is an alkyl group having 2 to 5 carbon atoms and containing an unsaturated bond, M 1 is a hydrogen atom, a monovalent or divalent metal, an ammonium group, or an organic amine salt.
[0033] Preferably, the monomer may be one or more selected from the group consisting of acrylic acid, methacrylic acid, and monovalent metal salts, divalent metal salts, ammonium salts, and organic amine salts of these acids. In this way, when acrylic acid or a salt thereof is used as the water-soluble ethylenically unsaturated monomer, it is advantageous to obtain a highly water-absorbent resin having improved water absorption. In addition, the monomer may be at least one selected from the group consisting of anionic monomers and salts thereof, such as maleic anhydride, fumaric acid, crotonic acid, itaconic acid, 2-acryloylethanesulfonic acid, 2-methacryloylethanesulfonic acid, 2-(meth)acryloylpropanesulfonic acid, or 2-(meth)acrylamido-2-methylpropanesulfonic acid; nonionic hydrophilic monomers, such as (meth)acrylamide, N-substituted (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, or polyethylene glycol (meth)acrylate; and amino group-containing unsaturated monomers, such as (N,N)-dimethylaminoethyl (meth)acrylate or (N,N)-dimethylaminopropyl (meth)acrylamide, and quaternized products thereof.
[0034] Here, the water-soluble ethylenically unsaturated monomer has an acidic group, and at least a part of the acidic group is partially neutralized using the neutralizing solution of the present invention described above.
[0035] At this time, the neutralization degree of the monomer may be 40 to 95 mol%, or 40 to 80 mol%, or 45 to 75 mol%, as described above. The range of the neutralization degree varies depending on the final properties, but if the neutralization degree is too high, the neutralized monomer precipitates and polymerization is difficult to proceed smoothly, and conversely, if the neutralization degree is too low, the water absorption of the polymer is greatly reduced and the polymer may exhibit properties similar to elastic rubber, which are difficult to handle.
[0036] The term "internal crosslinking agent" used in this specification is used to distinguish it from the "surface crosslinking agent" for crosslinking the surface of the base resin, and plays a role in crosslinking and polymerizing the unsaturated bonds of the water-soluble ethylenically unsaturated monomers described above. The crosslinking in this step is performed regardless of the surface or the inside, but the surface of the superabsorbent resin particles finally produced by the surface crosslinking process of the base resin described below has a structure crosslinked by the surface crosslinking agent, and the inside has a structure crosslinked by the internal crosslinking agent.
[0037] Non-limiting examples of the internal crosslinking agent include N,N'-methylenebisacrylamide, trimethylolpropane tri(meth)acrylate, ethylene glycol di(meth)acrylate, polyethylene glycol (meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol (meth)acrylate, butanediol di(meth)acrylate, butylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, dipentaerythritol pentaacrylate, glycerin tri(meth)acrylate, pentaerythritol tetraacrylate, triarylamine, ethylene glycol diglycidyl ether, propylene glycol, glycerin, and ethylene carbonate, which may be used alone or in combination. The internal crosslinking agent is not limited thereto. Of these, ethylene glycol diglycidyl ether is preferably used.
[0038] The internal crosslinking agent can be used in an amount of 0.01 to 5 parts by weight based on 100 parts by weight of the water-soluble ethylenically unsaturated monomer. For example, the internal crosslinking agent can be used in an amount of 0.01 parts by weight or more, 0.05 parts by weight or more, 0.1 parts by weight or more, or 0.45 parts by weight or more and 5 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, 1 part by weight or less, or 0.7 parts by weight or less based on 100 parts by weight of the water-soluble ethylenically unsaturated monomer. If the content of the upper internal crosslinking agent is too low, crosslinking does not occur sufficiently, making it difficult to achieve strength above an appropriate level, and if the content of the upper internal crosslinking agent is too high, the internal crosslinking density increases, making it difficult to achieve the desired water retention ability.
[0039] The monomer composition also contains a polymerization initiator that is commonly used in the manufacture of superabsorbent resins. As a non-limiting example, the polymerization initiator may be a thermal polymerization initiator or a photopolymerization initiator, depending on the polymerization method. However, even in the photopolymerization method, a certain amount of heat is generated by irradiation with ultraviolet light, and a certain amount of heat is generated by the progress of the polymerization reaction, which is an exothermic reaction, so a thermal polymerization initiator is additionally included.
[0040] The photopolymerization initiator may be, for example, one or more compounds selected from the group consisting of benzoin ether, dialkyl acetophenone, hydroxyl alkyl ketone, phenyl glyoxylate, benzyl dimethyl ketal, acyl phosphine, and α-aminoketone. Specific examples of acylphosphine include diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, and ethyl(2,4,6-trimethylbenzoyl)phenylphosphinate. More various photoinitiators are described in detail in "UV Coatings: Basics, Recent Developments and New Application" (Elsevier, 2007), p. 115, by Reinhold Schwalm, and are not limited to the above-mentioned examples.
[0041] The thermal polymerization initiator may be one or more compounds selected from the group consisting of persulfate initiators, azo initiators, hydrogen peroxide, and ascorbic acid.Specific examples of persulfate initiators include sodium persulfate (Na2S2O8), potassium persulfate (K2S2O8), and ammonium persulfate ((NH4)2S2O8). Examples of azo initiators include 2,2-azobis(2-amidinopropane) dihydrochloride, 2,2-azobis-(N,N-dimethylene)isobutyramidine dihydrochloride, 2-(carbamoylazo)isobutylonitrile, 2,2-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 4,4-azobis-(4-cyanovaleric acid), and 4,4-azobis-(4-cyanovaleric acid). Examples of thermal polymerization initiators include aryl ethers such as aryl ethers, aryl ethers, and aryl ethers with aryl groups. More various thermal polymerization initiators are disclosed in "Principle of Polymerization" by Odian (Wiley, 1981), page 203, which can be referred to.
[0042] The polymerization initiator is added at a concentration of 0.001 to 1 part by weight per 100 parts by weight of the water-soluble ethylenically unsaturated monomer. That is, if the concentration of the polymerization initiator is too low, the polymerization rate is slowed down and a large amount of residual monomer may be extracted in the final product, which is not preferable. On the other hand, if the concentration of the polymerization initiator is too high, the polymer chain forming the network is shortened, the content of water-soluble components is increased, and the physical properties of the resin, such as the pressurized water absorption capacity, may be reduced, which is not preferable.
[0043] In addition, the monomer composition may further contain additives such as a thickener, a plasticizer, a storage stabilizer, and an antioxidant, if necessary.
[0044] The foaming agent plays a role in increasing the surface area by forming pores in the hydrogel polymer as the foaming occurs during polymerization. The foaming agent may be a carbonate, for example, sodium bicarbonate, sodium carbonate, potassium bicarbonate, potassium carbonate, calcium bicarbonate, calcium carbonate, magnesium bicarbonate, or magnesium carbonate.
[0045] Commercial blowing agents that can be used include, but are not limited to, encapsulated blowing agent F-36D.
[0046] In addition, the foaming agent is preferably used in an amount of 1500 ppmw or less based on the weight of the water-soluble ethylenically unsaturated monomer. If the amount of foaming agent used exceeds 1500 ppmw, the number of pores increases excessively, the gel strength of the superabsorbent resin decreases, and the density decreases, which may cause problems in distribution and storage. In addition, the foaming agent is preferably used in an amount of 500 ppmw or more, or 1000 ppmw or more based on the weight of the water-soluble ethylenically unsaturated monomer.
[0047] In addition, the surfactant induces uniform dispersion of the foaming agent, and prevents the gel strength and density from decreasing due to uniform foaming during foaming. It is preferable to use an anionic surfactant as the surfactant. Specifically, the surfactant is SO3 -The compound containing an anion and represented by the following chemical formula 3 can be used.
[0048] [Chemical formula 3] R-SO3Na
[0049] In the above Chemical Formula 3, R is an alkyl group having 8 to 16 carbon atoms.
[0050] In addition, the surfactant is preferably used in an amount of 300 ppmw or less based on the weight of the water-soluble ethylenically unsaturated monomer. If the amount of the surfactant used exceeds 300 ppmw, the content of the surfactant in the superabsorbent resin increases, which is not preferable. Furthermore, the surfactant is preferably used in an amount of 100 ppmw or more, or 150 ppmw or more based on the weight of the water-soluble ethylenically unsaturated monomer.
[0051] The monomer composition is prepared in the form of a solution in which raw materials such as the water-soluble ethylenically unsaturated monomer, the polymerization initiator, and the internal crosslinking agent are dissolved in a solvent.
[0052] The solvent that can be used at this time is not limited in composition as long as it can dissolve the above-mentioned raw materials. For example, the solvent can be water, ethanol, ethylene glycol, diethylene glycol, triethylene glycol, 1,4-butanediol, propylene glycol, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, methyl ethyl ketone, acetone, methyl amyl ketone, cyclohexanone, cyclopentanone, diethylene glycol monomethyl ether, diethylene glycol ethyl ether, toluene, xylene, butyrolactone, carbitol, methyl cellosolve acetate, N,N-dimethylacetamide, or a mixture thereof.
[0053] The formation of the hydrogel polymer by polymerization of the monomer composition may be carried out by a conventional polymerization method, and the process is not particularly limited. As a non-limiting example, the polymerization method is largely divided into thermal polymerization and photopolymerization depending on the type of polymerization energy source, and the thermal polymerization is carried out in a reactor having a stirring shaft such as a kneader, and the photopolymerization is carried out in a reactor equipped with a movable conveyor belt.
[0054] As an example, the monomer composition is introduced into a reactor such as a kneader equipped with an agitator shaft, and hot air is supplied thereto or the reactor is heated to thermally polymerize the monomer composition, thereby obtaining a hydrogel polymer. At this time, depending on the type of the agitator shaft equipped in the reactor, the hydrogel polymer discharged from the outlet of the reactor is obtained as particles of several millimeters to several centimeters in size. Specifically, the obtained hydrogel polymer is obtained in various forms depending on the concentration of the monomer composition injected and the injection speed, and generally, a hydrogel polymer having a (weight average) particle size of 2 to 50 mm is obtained.
[0055] As another example, when the photopolymerization of the monomer composition is carried out in a reactor equipped with a movable conveyor belt, a sheet-like hydrogel polymer is obtained. In this case, the thickness of the sheet varies depending on the concentration and injection speed of the monomer composition to be injected, but it is generally preferable to adjust the thickness to 0.5 to 10 cm in order to ensure the production speed while allowing the entire sheet to be polymerized uniformly.
[0056] The water content of the hydrogel polymer obtained by such a method may be 40% to 80% by weight. Meanwhile, throughout this specification, the term "water content" refers to the water content relative to the weight of the entire hydrogel polymer, and means the weight of the hydrogel polymer minus the weight of the polymer in a dry state. Specifically, it is defined as a value calculated by measuring the weight loss due to evaporation of water in the polymer during the process of drying by increasing the temperature of the polymer by infrared heating. At this time, the drying conditions are a method of increasing the temperature from room temperature to 180°C and then maintaining it at 180°C, and the total drying time is set to 20 minutes, including 5 minutes for the temperature increase step, and the water content is measured.
[0057] (Cutting stage) Next, the hydrogel polymer is mixed with a carboxylic acid additive and then chopped to prepare a mixture containing chopped hydrogel polymer.
[0058] When a hydrogel polymer having a strong cohesive force is mixed with the carboxylic acid additive of the present invention and then chopped, it is possible to produce a particle group having a desired particle size without the phenomenon of aggregation of the crushed particles, which makes it unnecessary to perform an additional crushing process after drying and reduces the generation of fine powder. In addition, by controlling the subsequent drying process within a specific range, excellent drying efficiency can be achieved and the occurrence of warping of the dried product can be effectively suppressed even if the drying amount is large.
[0059] The carboxylic acid additive may be at least one selected from the group consisting of carboxylic acids represented by the above Chemical Formula 1 and metal salts thereof:
[0060] [ka]
[0061] In the above Chemical Formula 1, A is an alkyl group having 5 to 21 carbon atoms; B1 is -OCO-, -COO-, or -COOCH(R1)COO-; B2 is -CH2-, -CH2CH2-, -CH(R2)-, -CH=CH-, or -C≡C-; wherein R1 and R2 are each independently an alkyl group having 1 to 4 carbon atoms; n is an integer from 1 to 3, C is a carboxyl group.
[0062] Specifically, the carboxylic acid additive is at least one selected from the group consisting of a carboxylic acid represented by Chemical Formula 1, an alkali metal salt of a carboxylic acid represented by Chemical Formula 1, and an alkaline earth metal salt of a carboxylic acid represented by Chemical Formula 1. More specifically, the carboxylic acid additive is one of a carboxylic acid represented by Chemical Formula 1, an alkali metal salt of a carboxylic acid represented by Chemical Formula 1, and an alkaline earth metal salt of a carboxylic acid represented by Chemical Formula 1.
[0063] In the formula 1, A is a hydrophobic moiety and may be a linear or branched alkyl group having 5 to 21 carbon atoms, but it is more advantageous in terms of suppressing aggregation of pulverized particles and improving dispersibility when A is an alkyl group having a linear structure. If A is an alkyl group having less than 5 carbon atoms, there is a problem that the chain length is short and aggregation of pulverized particles is not effectively controlled, and if A is an alkyl group having more than 21 carbon atoms, there is a problem that the mobility of the additive is reduced and it may not be effectively mixed into the hydrogel polymer, and there is a problem that the unit price of the composition becomes high due to the increase in the cost of the additive.
[0064] Specifically, in the above Chemical Formula 1, A may be a linear alkyl having 5 to 21 carbon atoms, that is, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decanyl, n-undecanyl, n-dodecanyl, n-tridecanyl, n-tetradecanyl, n-pentadecanyl, n-hexadecanyl, n-heptadecanyl, n-octadecanyl, n-nonadecanyl, n-icosanyl, or n-heptacosanyl.
[0065] More specifically, A may be a linear alkyl having 6 to 18 carbon atoms. For example, A is -CH 13 , -C 11 H 23 , -C 12 H 25 , -C 17 H 35 , or -C 18 H 37 may be also possible.
[0066] In addition, in the above formula 1, the (B1-B2) portion plays a role in improving the adsorption performance to the polymer surface, which may be insufficient due to the C portion alone. When B2 has 3 or more carbon atoms, the distance between the B1 portion and the C portion becomes large, and the adsorption performance to the hydrogel polymer may decrease.
[0067] In this case, R1 and R2 may each independently be a linear or branched alkyl having 1 to 4 carbon atoms, more specifically, R1 and R2 may each independently be methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, or tert-butyl, but from the viewpoint of the additive being adsorbed to the superabsorbent resin particles, it is advantageous that the molecular structure of the additive is not bulky, so that R1 and R2 may all be methyl.
[0068] In addition, in the above formula 1, n may be 1, 2 or 3. More specifically, n, which means the number of (B1-B2), is preferably 1 in consideration of the fact that the (B1-B2) portion is intended to reinforce the adsorption performance for the C portion and the molecular length for the carboxylic acid additive to be effectively adsorbed to the hydrogel polymer.
[0069] Specifically, in the above Chemical Formula 1, B1 is
[0070] [ka]
[0071] where * is a bond site to an adjacent atom.
[0072] For example, B1 is
[0073] [ka]
[0074] may be also possible.
[0075] Further, in the above Chemical Formula 1, B2 is
[0076] [ka]
[0077] In this case, B2 may be represented by the following formula: where * is a bonding site with an adjacent atom. In this case, B2 may be represented by the following formula:
[0078] [ka]
[0079] It is preferable that:
[0080] In addition, in the formula 1, the C portion is a hydrophilic portion and is a carboxyl group (COOH). However, when the carboxylic acid additive is a salt, the C portion is a carboxylate group (COO - ).
[0081] In other words, the carboxylic acid additive may be a compound represented by the following formula 1a:
[0082] [ka]
[0083] In the above formula 1a, M is H + , a monovalent cation of an alkali metal, or a divalent cation of an alkaline earth metal, k is M is H + or 1 for monovalent cations of alkali metals, or 2 for divalent cations of alkaline earth metals, The explanations for A, B1, B2 and n are as defined in Chemical Formula 1 above.
[0084] More specifically, when the carboxylic acid additive is an alkali metal salt of a carboxylic acid represented by the above formula 1, the additive is represented by the following formula 1':
[0085] [ka]
[0086] In the above Chemical Formula 1', M1 is an alkali metal, for example sodium or potassium; The explanations for A, B1, B2 and n are as defined in Chemical Formula 1 above.
[0087] In addition, when the carboxylic acid-based additive is an alkaline earth metal salt of a carboxylic acid represented by the above Chemical Formula 1, the additive is represented by the following Chemical Formula 1″:
[0088] [ka]
[0089] In the above formula 1", M2 is an alkaline earth metal, for example, calcium; The explanations for A, B1, B2 and n are as defined in Chemical Formula 1 above.
[0090] As an example, the carboxylic acid additive may be any one of the carboxylic acids selected from the group consisting of:
[0091] [ka] [ka]
[0092] Alternatively, the carboxylic acid additive may be any one of the alkali metal salts selected from the group consisting of:
[0093] [ka] [ka]
[0094] In the above, Each M1 is independently an alkali metal.
[0095] Alternatively, the carboxylic acid additive may be any one of the alkaline earth metal salts selected from the group consisting of:
[0096] [ka] [ka]
[0097] In the above, Each M2 is independently an alkaline earth metal.
[0098] For example, the carboxylic acid additive may be any one of the compounds represented by the following chemical formulas 1-1 to 1-7, but is not limited thereto:
[0099] [ka]
[0100] Meanwhile, the base resin powder produced by subjecting the chopped mixture containing the chopped hydrogel polymer to a subsequent drying process may further contain, in addition to the carboxylic acid additive, a compound formed by decomposing the ester bond of B1 during the drying process after the additive is pulverized together with the hydrogel polymer.
[0101] Specifically, when the additive is a compound in which n is 1 and B1 is --OCO--, the base resin powder may further contain an alcohol having an A-OH structure and a compound having an HOOC-B2-C structure.
[0102] In addition, when the additive is a compound in which n is 1 and B1 is -COO-, the superabsorbent polymer composition may further contain a carboxylic acid having an A-COOH structure and a compound having an HO-B2-C structure.
[0103] Furthermore, when the additive is a compound in which n is 1 and B1 is -COOCH(R1)COO-, the base resin powder may further contain a carboxylic acid having an A-COOH structure and a compound having an HOCH(R1)COO-B2-C structure.
[0104] In this way, since the base resin powder further contains a compound formed by decomposition of the ester bond in the additive molecule, the mobility of the additive is increased, and the phenomenon of re-agglomeration after pulverization can be further prevented.
[0105] At this time, the carboxylic acid additive is contained in an amount of 100 ppmw to 5,000 ppmw relative to the hydrogel polymer. Preferably, the amount is 500 ppmw to 4,500 ppmw, or 1,000 ppmw to 4,000 ppmw, 1,500 ppmw to 4,000 ppmw, or 3,000 ppmw to 4,000 ppmw. If the amount of the additive is too low, the aggregation control effect of the additive is small, it is not easy to crush to a desired particle size, and water-soluble components may increase due to excessive kneading during the chopping process. If the amount of the additive is too high, the carboxylic acid additive may remain on the particle surface, reducing the surface tension and decreasing the initial water absorption rate of the superabsorbent resin.
[0106] The method for mixing such a carboxylic acid-based additive with the hydrogel polymer is not particularly limited as long as it can uniformly mix the additive with the hydrogel polymer, and any method can be appropriately adopted and used.
[0107] For example, the additive may be mixed in a state of solution dissolved in a solvent, specifically, water, and the solution may be prepared by mixing the additive and the hydrogel polymer in a reaction vessel, by putting the hydrogel polymer in a mixer and injecting the solution, or by continuously supplying the hydrogel polymer and the solution to a continuously operated mixer and mixing them.
[0108] The step of roughly pulverizing the mixture of the carboxylic acid-based additive and the hydrogel polymer may be performed by extruding the hydrogel polymer into an outlet having holes with an average diameter of 1 mm to 5 mm.
[0109] Specifically, a meat chopper can be used, and the meat chopper includes a chopping module including a perforated plate having holes with an average diameter of 1 mm to 5 mm. A plurality of perforated plates are used. The pulverization is considered to be performed by extruding the hydrogel polymer mixed with the additives so that the hydrogel polymer can be pulverized while passing through the holes of the perforated plate. In this case, an extruder can be used to extrude the hydrogel polymer, for example, a single or multiple screw type extruder. The chopping process can be performed at a discharge speed of 50 Hz to 8,000 Hz.
[0110] In this case, the average particle size (D50) of the chopped hydrogel polymer is about 0.5 mm to 4 mm. When the hydrogel polymer is formed into fine particles having a small particle size as described above, the hydrogel polymer usually aggregates with each other due to its high water content. However, by using the carboxylic acid additive of the present invention, such a problem does not occur.
[0111] Meanwhile, in the present invention, the average particle size "Dn" means the particle size or particle diameter at the n% point of the cumulative distribution of the number of particles according to the particle size. That is, D50 indicates the particle size at the 50% point of the cumulative distribution of the number of particles according to the particle size, D90 indicates the particle size at the 90% point of the cumulative distribution of the number of particles according to the particle size, and D10 indicates the particle size at the 10% point of the cumulative distribution of the number of particles according to the particle size. The Dn can be measured using a laser diffraction method or the like. Specifically, the powder to be measured is dispersed in a dispersion medium, and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500) to measure the difference in the diffraction pattern according to the particle size when the particles pass through a laser beam, and the particle size distribution is calculated. D10, D50, and D90 can be measured by calculating the particle sizes at the 10%, 50%, and 90% points of the cumulative distribution of the number of particles according to the particle size in the measuring device.
[0112] Meanwhile, at least a part of the carboxylic acid additive contained in the chopped mixture may be present on the surface of the hydrogel polymer particles. As mentioned above, "at least a part of the additive is present on the surface of the hydrogel polymer" means that at least a part of the additive is adsorbed or bonded to the surface of the hydrogel polymer particles. This is because the carboxylic acid additive is not added during the polymerization process of the water-soluble ethylenically unsaturated monomer, but is added after the formation of the polymer, and the phenomenon of re-aggregation between the hydrogel polymer particles can be suppressed compared to when the additive is added during the polymerization process and the additive is present inside the polymer.
[0113] (Drying stage) Next, the mixture containing the chopped hydrogel polymer is dried by alternately blowing upflow at 120°C to 210°C and downflow at 120°C to 210°C to form a base resin powder.
[0114] The upflow means that hot air is blown upward from below onto the object to be dried, and the downflow means that hot air is blown downward from above onto the object to be dried. In other words, the upflow and downflow mean that the hot air flows in opposite directions. The angle of the direction can be changed depending on the conditions of the hot air dryer used, but the angle difference between the directions of the upflow and downflow is usually considered to be 180°±5°.
[0115] In the drying, the number of times that the upward and downward winds are blown is not particularly limited, and they can be blown alternately several times as long as the blowing time of the downward wind is longer than that of the upward wind, based on the total blowing time of each. When blown several times, the total blowing time of each of the upward and downward winds is calculated based on the total of these blowing times.
[0116] The drying is performed in a fixed-bed type, which refers to a method in which the material to be dried is placed on a base such as a perforated plate through which air can pass, and hot air passes from bottom to top to dry the material. Specifically, the drying is performed using a ventilated belt dryer equipped with a perforated plate. Specifically, the chopped mixture to be dried is placed on a perforated plate, and thus, upward airflow means that airflow is applied from below to above the perforated plate, and downward airflow means that airflow is applied from above to below the chopped mixture placed on the perforated plate.
[0117] At this time, by making the total time of the downward wind longer than the total time of the upward wind, excellent drying efficiency and suppression of warping of the resin can be achieved. Even if fine hydrogel polymer particles are formed in the above-mentioned chopping stage, the dried material does not aggregate by using a carboxyl-based additive in combination, and further, by making the total time of the downward wind longer, it is possible to effectively suppress warping of the outer periphery of the object to be dried, and thus it is possible to achieve the desired drying efficiency even when there are many objects to be dried.
[0118] On the other hand, if the upward airflow is applied for a long time, the outer periphery of the container may warp, and the inside of the container may not be sufficiently dried, resulting in a significant decrease in drying efficiency.
[0119] The temperature of the hot air in the drying step is 120°C to 210°C, but if it is performed at less than 120°C, it is difficult to dry to the desired extent, and if it exceeds 210°C, the polymer may deteriorate. Preferably, it is performed at 160°C to 180°C.
[0120] The total execution time of the drying step is not particularly limited as long as the time for supplying the downward air is longer than the time for supplying the upward air, but is, for example, 10 minutes to 2 hours, preferably 30 minutes to 40 minutes. When it is performed within the above range, it is preferable because the desired drying efficiency can be achieved.
[0121] The hot air drying is carried out by introducing hot air having a linear velocity of 0.5 m / s to 3.0 m / s, 0.7 m / s to 2.5 m / s, or 0.85 m / s to 2.0 m / s. When the above speed range is satisfied, the object to be dried can be dried uniformly to the inside, which is preferable. When the linear velocity is less than 0.5 m / s, it is difficult for the hot air to reach the inside of the object to be dried, and when it exceeds 3.0 m / s, the object to be dried may be scattered inside the dryer.
[0122] Preferably, the total time for supplying the upward air may be 1% to 25% of the drying time, and when the time for supplying the upward air is controlled within the above range, even if a large amount of fine hydrogel polymer particles is contained, a uniform and excellent drying efficiency can be achieved without the occurrence of warping of the outer layer. Most preferably, the total time for supplying the upward air is 1% to 12% of the drying time.
[0123] On the other hand, if the total time of the upward airflow is less than 1%, the uniformity of the drying efficiency is slightly reduced, and if it exceeds 25%, the occurrence of warping of the drying layer cannot be effectively controlled, and the drying efficiency may be reduced.
[0124] In one embodiment of the invention, the moisture content of the base resin powder produced through the drying process under the above conditions is less than 8 wt%. The "moisture content" is the amount of moisture relative to the weight of the base resin powder to be measured, and refers to the weight of the base resin powder minus the weight of the polymer in a dry state. Specifically, it is defined as a value calculated by measuring the weight loss due to evaporation of moisture in the base resin powder during the process of drying by increasing the temperature of the polymer by infrared heating.
[0125] The moisture content is one of the indicators showing the degree of drying efficiency, and is preferably 0.01 wt% to 7 wt%, or 0.01 wt% to 5 wt%. A method for measuring the moisture content of the base resin powder will be described in more detail in the experimental examples described later.
[0126] (Crushing and classification stage) In one embodiment of the invention, the method may further include, after the drying step, grinding and classifying the dried base resin powder.
[0127] As described above, the base resin powder obtained by drying the mixture with reduced cohesive force under specific conditions has a significantly low occurrence of re-agglomeration between particles, and can be easily pulverized with low pulverization energy to produce a base resin powder having a desired particle size. In other words, after the drying step, the pulverization step is reduced (coarse pulverization can be omitted and only fine pulverization can be carried out), and a step of classifying the pulverized product can be used to obtain a base resin powder having a desired particle size.
[0128] In one embodiment of the invention, the wet ratio of the base resin powder produced through the above process is less than 15%.
[0129] The non-drying rate indicates the degree of drying of crumb-shaped powder, which is relatively large and difficult to dry in the base resin powder, and is one of the indicators of drying efficiency.
[0130] Specifically, it means the mass ratio of powder that cannot be sieved after classifying the base resin powder with a 4 mesh sieve according to ASTM E11 for 10 minutes or more, and the particles that cannot be sieved after the process of classifying with a 4 mesh sieve for 10 minutes or more mean that the particles were not dried sufficiently and re-agglomerated due to internal moisture. In fact, the moisture content of the powder that cannot be sieved after classifying with a 4 mesh sieve for 10 minutes or more is 10% or more.
[0131] The smaller the wet ratio, the better, and the lower limit of the wet ratio is theoretically 0. It is preferably 0.1% to 13%, 0.1% to 10%, or 0.5% to 5%. The method for measuring the wet ratio of the base resin powder will be described in more detail in the experimental examples described later.
[0132] (Surface cross-linking stage) Next, the method for producing a superabsorbent resin according to one embodiment of the present invention further includes a step of heat-treating the base resin powder in the presence of a surface cross-linking agent to surface-cross-link at least a portion of the surface of the base resin powder to produce a superabsorbent resin.
[0133] The surface cross-linking step induces a cross-linking reaction on the surface of the base resin powder in the presence of a surface cross-linking agent, and the unsaturated bonds of the water-soluble ethylenically unsaturated monomer remaining on the surface without being cross-linked are cross-linked by the surface cross-linking agent to form a superabsorbent resin with a high surface cross-linking density.
[0134] Specifically, a surface cross-linked layer is formed in a heat treatment process due to the presence of a surface cross-linking agent, and the heat treatment process increases the surface cross-linking density, i.e., the external cross-linking density, while the internal cross-linking density remains unchanged. Thus, the superabsorbent resin having a surface cross-linked layer thus produced has a structure in which the external cross-linking density is higher than the internal cross-linking density.
[0135] In the surface cross-linking step, a surface cross-linking agent composition containing an alcohol-based solvent and water in addition to a surface cross-linking agent may be used.
[0136] Meanwhile, the surface cross-linking agent contained in the surface cross-linking agent composition can be any surface cross-linking agent used in the manufacture of existing superabsorbent resins without any particular limitations. For example, the surface cross-linking agent can include one or more polyols selected from the group consisting of ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, 1,2-hexanediol, 1,3-hexanediol, 2-methyl-1,3-propanediol, 2,5-hexanediol, 2-methyl-1,3-pentanediol, 2-methyl-2,4-pentanediol, tripropylene glycol and glycerol; one or more carbonate-based compounds selected from the group consisting of ethylene carbonate and propylene carbonate; epoxy compounds such as ethylene glycol diglycidyl ether; oxazoline compounds such as oxazolidinone; polyamine compounds; mono-, di- or polyoxazolidinone compounds; or cyclic urea compounds; etc. Preferably, the same internal crosslinking agent as described above can be used, for example, a diglycidyl ether compound of an alkylene glycol such as ethylene glycol diglycidyl ether can be used.
[0137] Such a surface cross-linking agent can be used in an amount of 0.001 to 2 parts by weight per 100 parts by weight of the base resin powder. Preferably, the amount is 0.005 parts by weight or more, 0.01 parts by weight or more, or 0.02 parts by weight or more and 0.5 parts by weight or less, or 0.3 parts by weight or less. By adjusting the content range of the surface cross-linking agent to the above-mentioned range, a highly water-absorbent resin exhibiting various physical properties such as excellent water absorption performance and liquid permeability can be produced.
[0138] Meanwhile, the surface crosslinking agent is added to the base resin powder in the form of a surface crosslinking agent composition containing the surface crosslinking agent, and the method of adding such a surface crosslinking agent composition is not particularly limited in its constitution. For example, a method of putting the surface crosslinking agent composition and the base resin powder in a reaction tank and mixing them, a method of spraying the surface crosslinking agent composition on the base resin powder, a method of continuously supplying the base resin powder and the surface crosslinking agent composition to a continuously operating mixer, and the like can be used.
[0139] The surface crosslinking agent composition may further include water and / or a hydrophilic organic solvent as a medium. This has the advantage that the surface crosslinking agent can be uniformly dispersed on the base resin powder. At this time, the content of water and the hydrophilic organic solvent can be adjusted and applied in an addition ratio relative to 100 parts by weight of the base resin powder in order to induce uniform dissolution / dispersion of the surface crosslinking agent and prevent the agglomeration phenomenon of the base resin powder, while optimizing the surface penetration depth of the surface crosslinking agent.
[0140] The surface cross-linking step can be carried out by heat treatment for 30 minutes or more at a temperature of 110° C. to 200° C., or 110° C. to 150° C. More specifically, the surface cross-linking reaction can be carried out by heat treatment at the maximum reaction temperature, which is the above-mentioned temperature, for 30 to 80 minutes, or 40 to 70 minutes.
[0141] By satisfying such surface cross-linking step conditions (particularly, the temperature rise conditions and the reaction conditions at the maximum reaction temperature), a highly water-absorbent resin that appropriately satisfies physical properties such as excellent pressurized liquid permeability can be produced.
[0142] The temperature raising means for the surface crosslinking reaction is not particularly limited. Heating can be performed by supplying a heat medium or directly supplying a heat source. At this time, the type of heat medium that can be used can be a heated fluid such as steam, hot air, hot oil, etc., but is not limited thereto, and the temperature of the heat medium to be supplied can be appropriately selected in consideration of the means of the heat medium, the heating rate, and the target temperature of the heat raising. On the other hand, examples of the heat source to be directly supplied include heating by electricity and heating by gas, but are not limited to the above examples.
[0143] Meanwhile, in the method for producing a superabsorbent resin according to an embodiment of the present invention, various polyvalent metal salts, such as aluminum salts, such as aluminum sulfate, may be further used during surface cross-linking in order to further improve liquid permeability, etc. Such polyvalent metal salts are contained on the surface cross-linked layer of the finally produced superabsorbent resin.
[0144] Meanwhile, the superabsorbent resin produced according to one embodiment of the present invention may have a particle size of 150 to 850 μm. More specifically, at least 95% by weight of the base resin powder and the superabsorbent resin containing the base resin powder may have a particle size of 150 to 850 μm, and may contain 50% by weight or more of particles having a particle size of 300 to 600 μm, and the amount of fine powder having a particle size of less than 150 μm is less than 3% by weight.
[0145] The superabsorbent polymer produced by the method for producing a superabsorbent polymer according to the embodiment described above has excellent other physical properties, and has excellent drying efficiency, which effectively suppresses warping of the outer shell, thereby improving the quality of the final product.
[0146] Specifically, the superabsorbent resin may have a centrifugation retention capacity (CRC) according to EDENA method WSP241.2 of 26 g / g or more, preferably 28 g / g or more, 30 g / g or more, or 50 g / g or less, 45 g / g or less, 40 g / g or less, or 35 g / g or less. A specific method for measuring the centrifugation retention capacity will be described in more detail in the experimental examples.
[0147] Specifically, the superabsorbent polymer may have a water absorbency under pressure (AUP) of 24 g / g or more at 0.3 psi according to EDANA method WSP242.3, and may preferably have an AUP of 26 g / g or more, 27 g / g or more, or 50 g / g or less, 40 g / g or less, 35 g / g or less, or 30 g / g or less. A specific method for measuring the water absorbency under pressure will be described in more detail in the experimental examples.
[0148] The functions and effects of the present invention will be described in more detail below through specific examples of the present invention, however, these examples are merely presented as examples of the present invention and do not define the scope of the invention.
[0149] [Example] <Production of superabsorbent resin> Example 1 (Stage 1) In a 3L glass vessel equipped with a stirrer and a thermometer, 100g (1.388mol) of acrylic acid, 0.001g of internal crosslinking agent polyethylene glycol diacrylate (Mn=508) and 0.24g of ethylene glycol diglycidyl ether, 0.008g of photopolymerization initiator diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, 0.125g of thermal polymerization initiator sodium persulfate, 123.5g of 32% caustic soda solution, 0.1g of encapsulated foaming agent (F-36D) and 0.02g of sodium dodecyl sulfate (SDS) aqueous solution were mixed with 66.0g of water at room temperature (25±1℃) to prepare a monomer composition with a total solid content of 42.0wt% (neutralization degree of acrylic acid: 70mol%).
[0150] Thereafter, the monomer composition was supplied at a rate of 500 to 2000 mL / min onto a conveyor belt having a width of 10 cm and a length of 2 m, which rotated at a speed of 50 cm / min. 2 The polymerization reaction was allowed to proceed for 60 seconds by irradiating the mixture with ultraviolet light having an intensity of 100 nm to obtain a sheet-like hydrogel polymer having a water content of 50% by weight.
[0151] (Stage 2) Next, an aqueous solution containing sodium stearoyl-2-lactylate (Almax-6900, Irsinwells) represented by the following chemical formula A-1 as a carboxylic acid additive (0.4 parts by weight of the carboxylic acid additive per 100 parts by weight of the hydrogel polymer) was mixed with the sheet-shaped hydrogel polymer obtained by the polymerization reaction by coating, and then chopped using a meat chopper with a hole diameter of 3 mm to produce a mixture containing chopped hydrogel particles. The chopped hydrogel particles had an average particle size (D50) of about 3.66 mm. The water content of the hydrogel polymer contained in the chopped mixture was 46% by weight:
[0152] [ka]
[0153] (Stage 3) Then, 1,000 g of the shredded mixture was placed in a belt dryer equipped with a 200 mm wide, 200 mm long, 1 mm perforated plate that allows airflow to be transferred up and down. The shredded mixture was placed on top of the perforated plate, and first, 160°C upward air flowing from the bottom to the top of the perforated plate was applied at a linear velocity of 0.93 m / s for 8 minutes 18 seconds, and then 160°C downward air flowing at a linear velocity of 0.93 m / s for 24 minutes 42 seconds to dry the mixture, producing a base resin powder.
[0154] (Stage 4) Next, the base resin powder was classified using a standard mesh sieve according to ASTM standards to obtain a base resin powder having a particle size of 150 to 850 μm.
[0155] A surface crosslinking agent composition (4.8 parts by weight of water, 5.0 parts by weight of methanol, 0.03 parts by weight of ethylene glycol diglycidyl ether, 0.01 parts by weight of silica Aerosil 200) was mixed with 100 parts by weight of the base resin powder, and the surface crosslinking reaction was allowed to proceed for 30 minutes at 140° C. After the surface crosslinking step, the superabsorbent resin was classified with a standard mesh sieve according to the ASTM standard so as to have a particle size of 150 μm to 850 μm.
[0156] Examples 2 to 6 and Comparative Examples 1 to 5 A highly water-absorbent resin containing a base resin powder was produced in the same manner as in Example 1, except that the conditions in the chopping step and drying step were changed as shown in Table 1 below.
[0157] [Table 1]
[0158] <Experimental Example 1: Evaluation of base resin powder> The properties of the base resin powders produced in the above Examples and Comparative Examples were evaluated by the following methods. The results are shown in Table 2.
[0159] (1) Wetness rate evaluation For the base resin powders produced in the above Examples and Comparative Examples after drying and before surface crosslinking, the base resin powder sample (A1) was classified for 10 minutes using a 4 mesh sieve according to ASTM E11 to obtain a powder sample (A2) that could not be sieved, relative to the initial weight A'1 (g) of the base resin powder sample (A1), and the ratio of the weight A'2 (g) of the powder sample that could not be sieved was measured.
[0160] [Formula] Undried rate (wt%)={[A'2(g)] / A'1(g)}×100
[0161] (2) Moisture content evaluation For the base resin powders produced in the Examples and Comparative Examples after drying and before surface crosslinking, samples having particle sizes of 150 to 850 μm were taken from the base resin powder, and the weight loss due to water evaporation in the base resin powder sample during the drying process was measured.
[0162] Specifically, the base resin powder sample had an initial weight H0 (g) and was heated at 180° C. for 40 minutes by infrared heating, after which its weight H1 (g) was measured, and the moisture content was calculated using the following formula 2.
[0163] [Formula 2] Moisture content (wt%)={[H0(g)-H1(g)] / H0(g)}×100
[0164] (3) Warpage evaluation The degree of warping of the cross section of the dried product of the base resin powders produced in Example 4 and Comparative Example 1 after drying and before surface crosslinking was evaluated according to the following evaluation criteria, and the results are shown in Table 2 below. Also, a cross-sectional photograph of the dried product after the drying step is shown in Fig. 1. Fig. 1(a) is a cross-sectional photograph of the dried product after the drying step in Example 4, and Fig. 1(b) is a cross-sectional photograph of the dried product after the drying step in Comparative Example 6.
[0165] <Evaluation criteria for warpage> ○: When the thickness of the center of the dried product is compared to the outer periphery and the surface is lifted by 10% or more. △: The thickness of the center of the dried product is compared to the thickness of the outer periphery, and the lifting occurs by 5% to 10%. X: When the outer periphery of the dried product is raised by less than 5% compared to the thickness of the center of the dried product
[0166] <Experimental Example 2: Evaluation of superabsorbent resin> The properties of the surface-crosslinked superabsorbent resins prepared in the above Examples and Comparative Examples were evaluated by the following methods. The results are shown in Table 2.
[0167] Unless otherwise indicated, all of the following physical property evaluations were performed at constant temperature and humidity (23±1°C, relative humidity 50±10%), and saline or salt water refers to a 0.9 wt% sodium chloride (NaCl) aqueous solution.
[0168] (1)Centrifuge Retention Capacity (CRC) The water retention capacity of each resin composition in terms of the water absorption capacity under no load was measured according to the European Disposables and Nonwovens Association (EDANA) standard EDANA WSP241.3.
[0169] Specifically, the superabsorbent resin obtained in each of the examples and comparative examples was classified using a sieve of #30-50 to obtain a resin. Such resin W0(g) (about 0.2g) was evenly placed in a nonwoven fabric envelope, sealed, and then immersed in physiological saline (0.9% by weight) at room temperature. After 30 minutes, the envelope was centrifuged at 250G for 3 minutes to remove water, and the mass W2(g) of the envelope was measured. The same procedure was performed without using the resin, and the mass W1(g) at that time was measured.
[0170] The obtained masses were used to calculate the CRC (g / g) according to the following formula 3.
[0171] [Formula 3] CRC(g / g)={[W2(g)-W1(g)] / W0(g)}-1
[0172] (2) Absorbency under Pressure (AUP) The water absorption capacity of the superabsorbent resins of the above Examples and Comparative Examples at a pressure of 0.3 psi was measured by EDANA method WSP242.3.
[0173] First, when measuring the pressurized water absorption capacity, the resin-classified powder used in the CRC measurement was used.
[0174] Specifically, a stainless steel wire net of 400 mesh was attached to the bottom of a plastic cylinder with an inner diameter of 25 mm. Under conditions of room temperature and humidity of 50%, the water-absorbent resin composition W0(g) (0.16 g) was uniformly spread on the wire net, and a piston capable of uniformly applying a load of 0.3 psi thereon was slightly smaller than the outer diameter of 25 mm, had no gap with the inner wall of the cylinder, and was designed not to hinder the up and down movement. At this time, the weight W3(g) of the device was measured.
[0175] A glass filter with a diameter of 90 mm and a thickness of 5 mm was placed inside a petroleum dish with a diameter of 150 mm, and physiological saline consisting of 0.9% by weight sodium chloride was placed at the same level as the upper surface of the glass filter. A sheet of filter paper with a diameter of 90 mm was placed on top of the glass filter. The measuring device was placed on the filter paper and the liquid was absorbed under a load for one hour. After one hour, the measuring device was lifted and its weight W4 (g) was measured.
[0176] The obtained masses were used to calculate the water absorption capacity under pressure (g / g) according to the following formula 4.
[0177] [Formula 4] AUP(g / g)=[W4(g)-W3(g)] / W0(g)
[0178] [Table 2]
[0179] As can be seen from the data in Table 2, in the examples of the manufacturing method of the present invention, a specific additive is added when the hydrogel polymer is chopped and the drying process conditions are adjusted to control the aggregation of the hydrogel polymer, and the base resin powder exhibits excellent drying efficiency and effectively prevents warping of the dried product even if the drying amount is large in the drying process. It was also confirmed that the superabsorbent resin manufactured by this method achieves excellent water absorption properties.
[0180] On the other hand, when the additive of the present invention is not used, it is difficult to control the particle size range of the hydrogel particles due to re-agglomeration, and when chopping is performed using a 3 mm chopper as in the examples, the re-agglomeration rate of the particles is high, causing the chopper to stop operating, making it difficult to proceed with the experiment.
[0181] Therefore, in the case of Comparative Examples 1 to 3, the additive of the present application was not used, and a chopping process was performed using a 16 mm chopper, and it was confirmed that it was difficult to control the occurrence of warping in the dried product. In addition, in Comparative Examples 1 to 3, the drying amount (feed input amount) was increased, and it was confirmed that the drying efficiency rapidly decreased due to the increase in the drying amount compared to Examples 5 and 6, in which the drying amount was increased.
[0182] In Comparative Example 4, the additive of the present invention was not used and the material was chopped using an 8 mm chopper. It was confirmed that the re-agglomeration rate was high and a large amount of crumbs were formed during the drying process. As a result, it was confirmed that the CRC property of the final water absorbent resin was significantly decreased compared to the Examples.
[0183] In the case of Comparative Examples 5 and 6, in which the additives of the present invention were used but the drying process was beyond the scope of the present invention, it was confirmed that the drying efficiency was reduced, and in particular, the dried product was warped. As a result, it was confirmed that the CRC properties of the finally produced water absorbent resin were significantly reduced compared to the Examples.
[0184] On the other hand, in the case of some comparative examples, a CRC value similar to that of the examples was achieved depending on the moisture content of the base resin. However, in these cases, it was confirmed that there were problems such as difficulty in controlling the particle size due to re-agglomeration of the hydrous gel and a decrease in drying efficiency due to an increase in the drying amount (feed input amount).
Claims
1. A step of cross-linking and polymerizing a water-soluble ethylenically unsaturated monomer having at least a partially neutralized acidic group in the presence of an internal cross-linking agent and a polymerization initiator to form a hydrogel polymer; A step of mixing the hydrogel polymer with a carboxylic acid additive and then chopping the mixture to prepare a mixture containing chopped hydrogel polymer; and drying the mixture by alternately applying upflow at 120°C to 210°C and downflow at 120°C to 210°C to form a base resin powder; The total time for supplying the downward airflow is longer than the total time for supplying the upward airflow, The carboxylic acid additive is at least one selected from the group consisting of carboxylic acids and salts thereof represented by the following formula 1: Manufacturing method of superabsorbent polymer: [Formula 1] In the above Chemical Formula 1, A is an alkyl group having 5 to 21 carbon atoms; B 1 is —OCO—, —COO—, or —COOCH(R 1 )COO—; B 2 is —CH 2 —, —CH 2 CH 2 —, —CH(R 2 )—, —CH═CH—, or —C≡C—; wherein R 1 and R 2 are each independently an alkyl group having 1 to 4 carbon atoms; n is an integer from 1 to 3, C is a carboxyl group.
2. The average particle size (D50) of the chopped hydrogel polymer is 0.5 mm to 4 mm. A method for producing the highly water-absorbent resin according to claim 1.
3. In the above Chemical Formula 1, A is -C 6 H 13 , -C 11 H 23 , -C 12 H 25, -C 17 H 35 , or -C 18 H 37 That is, A method for producing the highly water-absorbent resin according to claim 1 or 2.
4. In the above Chemical Formula 1, B 1 teeth, [Case 2] and Here, * is a bonding site with an adjacent atom. A method for producing the highly water-absorbent resin according to any one of claims 1 to 3.
5. In the above Chemical Formula 1, B 2 teeth, [C3] and Here, * is a bonding site with an adjacent atom. A method for producing the highly water-absorbent resin according to any one of claims 1 to 4.
6. The carboxylic acid additive is at least one selected from the group consisting of a carboxylic acid represented by Chemical Formula 1, an alkali metal salt thereof, and an alkaline earth metal salt thereof. A method for producing the highly water-absorbent resin according to any one of claims 1 to 5.
7. The carboxylic acid additive is any one of the compounds represented by the following chemical formulas 1-1 to 1-7: A method for producing the superabsorbent polymer according to any one of claims 1 to 6: [C4]
8. The carboxylic acid additive is mixed in an amount of 100 ppmw to 5,000 ppmw relative to the hydrogel polymer. A method for producing the highly water-absorbent resin according to any one of claims 1 to 7.
9. The drying is performed with the total input time of the upward air being 1% to 25% of the total drying time. A method for producing the highly water-absorbent resin according to any one of claims 1 to 8.
10. The drying is performed in a fixed type. A method for producing the highly water-absorbent resin according to any one of claims 1 to 9.
11. The chopping is performed by extruding the hydrogel polymer into an outlet having holes with an average diameter of 1 mm to 5 mm. A method for producing the highly water-absorbent resin according to any one of claims 1 to 10.
12. The base resin powder is classified using a 4 mesh sieve according to ASTM E11 for 10 minutes or more, and then the wet ratio, defined as the mass ratio of the powder that cannot be sieved, is less than 14 wt %. A method for producing the superabsorbent resin according to any one of claims 1 to 11.
13. The moisture content of the base resin powder is less than 8 wt %. A method for producing the highly water-absorbent resin according to any one of claims 1 to 12.
14. The base resin powder is further crushed and classified. A method for producing the highly water-absorbent resin according to any one of claims 1 to 13.
15. The method further includes a step of heat-treating the base resin powder in the presence of a surface cross-linking agent to surface-cross-link at least a portion of the surface of the base resin powder to produce a highly water-absorbent resin. A method for producing the superabsorbent resin according to any one of claims 1 to 14.
16. The superabsorbent resin has a centrifugal retention capacity (CRC) according to EDENA method WSP241.2 of 26 g / g or more. A method for producing the highly water-absorbent resin according to claim 15.
17. The superabsorbent resin has an absorbency under pressure (AUP) of 24 g / g or more at 0.3 psi according to EDANA method WSP242.3; A method for producing the highly water-absorbent resin according to claim 15 or 16.
Citation Information
Patent Citations
Preparation method of water-absorbing resin
JP2001213914A
Method for producing water-absorbent polymer
JP2008534707A
Water-absorbing resin
JP2015101597A
Method for producing porous superabsorbent resin and porous superabsorbent resin
JP2019519663A
Process and apparatus for producing water-absorbable resin of polyacrylic acid (SALT) type
WO2012144595A1