Weyl antiferromagnetic powder and thermoelectric conversion element using same
Weyl antiferromagnetic powders with controlled particle sizes enhance the coercive force of thermoelectric conversion elements, addressing the low coercive force issue in existing antiferromagnetic materials.
Patent Information
- Application Number
- JP2020044763
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-13
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-03-13
AI Technical Summary
Thermoelectric conversion elements using antiferromagnetic materials like Mn3Sn exhibit low coercive force, hindering practical applications.
Utilizing Weyl antiferromagnetic powders with controlled particle sizes, primarily composed of Mn3X compounds (X = Sn, Ge, Ga, Pt, Ir, Rh) and a D019 crystal structure, to enhance coercive force.
The Weyl antiferromagnetic powders significantly improve the coercive force of thermoelectric conversion elements, enabling practical industrial use.
Smart Images

Figure 0007570816000002 
Figure 0007570816000003 
Figure 0007570816000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a Weyl antiferromagnetic powder having high coercivity, and a thermoelectric conversion element using the same. [Background technology]
[0002] In recent years, research into thermoelectric conversion elements that utilize the anomalous Nernst effect has been progressing. The anomalous Nernst effect is a phenomenon in which, when a heat flow perpendicular to the magnetization is applied to a spontaneously magnetized magnetic material, an electromotive force is generated in a direction perpendicular to both the magnetization and the heat flow. The anomalous Nernst effect allows current to be extracted in a direction perpendicular to the heat flow, which is an advantage over the Seebeck effect in that it allows the construction of a thin sheet-shaped thermoelectric conversion device. For example, Patent Document 1 shows a thermoelectric generation device that uses an FePt film.
[0003] Since the anomalous Nernst effect is a phenomenon based on the spontaneous magnetization of a magnetic material, it was commonly believed that the magnetic material required a ferromagnetic material. However, it was discovered that some intermetallic compounds, such as Mn3Sn, exhibit the anomalous Nernst effect even though they are antiferromagnetic. Patent Document 2 shows an example in which a single crystal of Mn3Sn was produced by the Bridgman method, a heat flow was applied parallel to the [0 1 -1 0] direction of the Mn3Sn crystal, and an external magnetic field was applied parallel to the a-axis [2 -1 -1 0] direction, and the electromotive force per unit temperature was measured. According to this, hysteresis was observed in the electromotive force when the external magnetic field was changed, and the anomalous Nernst effect was confirmed, in which a voltage was generated even when the external magnetic field was zero. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2014-72256 A [Patent Document 2] JP 2017-84854 A Summary of the Invention [Problem to be solved by the invention]
[0005] The anomalous Nernst effect using single crystals of Mn3Sn disclosed in Patent Document 2 is due to an "antiferromagnet" in which the spins are aligned in opposite directions. Therefore, it is said that the "leakage magnetic field" can be suppressed significantly more than in thermoelectric conversion devices using "ferromagnets" in which the spins are aligned in the same direction. However, since the thermoelectric conversion element obtained by the method shown in Patent Document 2 has a small coercive force, it is desirable to improve the coercive force in order to put thermoelectric conversion devices into practical use.
[0006] An object of the present invention is to provide a highly practical technique useful for obtaining a thermoelectric conversion element having a large coercive force. [Means for solving the problem]
[0007] A magnetic material that has a band structure with Weyl points created by magnetism is called a "Weyl magnet." A Weyl magnet that is an antiferromagnetic material, such as Mn3Sn, is called a "Weyl antiferromagnet."
[0008] In order to achieve the above object, the present invention provides a powder composed of particles mainly composed of a Weyl antiferromagnet, which has a cumulative 50% particle diameter D 50 1~150μm, cumulative 90% particle size D 90 A Weyl antiferromagnetic powder is provided having a particle size of 250 μm or less.
[0009] As the Weyl antiferromagnet, one or more intermetallic compounds whose composition formula is Mn3X (where X is a metal element) and whose crystal structure is an ordered lattice of the D019 structure can be applied. The element X can be, for example, one or more elements selected from Sn, Ge, Ga, Pt, Ir, and Rh. More specifically, Mn3Sn, Mn3Ge, Mn3Ga, Mn3Pt, Mn3Ir, Mn3Rh, etc. can be exemplified.
[0010] The present invention also provides a thermoelectric conversion element using the above-mentioned Weyl antiferromagnetic powder. Effect of the Invention
[0011] According to the present invention, it is possible to obtain a thermoelectric conversion element having a large coercive force. Since the magnetic material used in the thermoelectric conversion element is in the form of a powder, it is easy to put the element into industrial use. [Brief description of the drawings]
[0012] [Figure 1] A photograph showing the appearance of a Mn3Sn alloy ingot. [Diagram 2] X-ray diffraction pattern of a powder sample prepared from a sample approximately halfway along the height of a Mn3Sn alloy ingot. [Diagram 3] Reference X-ray diffraction patterns for pure materials of metallic Mn, Mn oxides and Mn-Sn intermetallic compounds. [Figure 4] 4 is a particle size distribution curve of the Mn3Sn crystal powder used in Examples 1 to 3. [Diagram 5] 4 is a magnetization curve of a sintered body using the powder of Example 1. [Figure 6] 4 is a magnetization curve of a sintered body using the powder of Example 2. [Figure 7] FIG. 2 is a schematic diagram showing the attachment positions of the terminals for power measurement and the probes for temperature measurement, as well as the directions of heat flow and magnetic field application, for the samples for Nernst effect measurement in Examples 1 to 3. [Figure 8] 1 is a graph showing the relationship between an external magnetic field and the magnetic field reversal component ΔSANE of the Nernst coefficient SANE for a sintered body using the powder of Example 2. [Figure 9] FIG. 1 is a schematic diagram showing the configuration of a powder production apparatus using a gas atomization method. [Figure 10] 4 is a magnetization curve of a sintered body using the powder of Example 3. [Figure 11] 1 is a graph showing the relationship between an external magnetic field and the magnetic field reversal component ΔSANE of the Nernst coefficient SANE for a sintered body using the powder of Example 3. [Figure 12]4 is a magnetization curve of a sintered body using the pulverized sample of Comparative Example 1. [Figure 13] 1 is a graph showing the relationship between the external magnetic field and the magnetic field reversal component ΔSANE of the Nernst coefficient SANE for the polycrystalline body cut from the ingot of Comparative Example 1. [Figure 14] 4 is a magnetization curve of the single crystal of Comparative Example 2. [Figure 15] 1 is a graph showing the relationship between the external magnetic field and the magnetic field reversal component ΔSANE of the Nernst coefficient SANE for the single crystal of Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] As a result of their research, the inventors discovered that a thermoelectric conversion element with high coercivity can be obtained by using powder of a Weyl antiferromagnet. They also found that a powder with a small average particle size and a particle size distribution with a small proportion of coarse particles is extremely effective in improving the coercivity. In the particle size distribution based on volume measured by the laser diffraction / scattering method, the cumulative 50% particle size D 50 1~150μm, cumulative 90% particle size D 90 Thermoelectric conversion elements made of Weyl antiferromagnetic powder with a cumulative 50% particle diameter D of 250 μm or less show a remarkable improvement in coercivity compared to thermoelectric conversion elements made of single crystals of Weyl antiferromagnetic material. 50 1~30μm, cumulative 90% particle size D 90 When fine Weyl antiferromagnetic powder having a particle size of 50 μm or less is used, an even more excellent effect of improving the coercive force can be obtained.
[0014] A relatively simple method for producing the powder is to crush an ingot of a melted Weyl antiferromagnet into fine powder. The crushed powder can be classified using a mesh filter or the like to obtain a cumulative 50% particle diameter D 50 1~150μm, cumulative 90% particle size D 90It is possible to obtain a Weyl antiferromagnet powder with a particle size distribution adjusted to 250 μm or less. As a method for producing finer powder, for example, a gas atomization method can be applied in which an inert gas is blown in a vacuum onto droplets of molten metal adjusted to the chemical composition of the Weyl antiferromagnet, and the molten metal is directly solidified into fine particles. With this method, the cumulative 50% particle diameter D 50 1~30μm, cumulative 90% particle size D 90 It is possible to produce fine Weyl magnetic powder with a particle size of 50 μm or less.
[0015] To make a thermoelectric conversion element using powder, it is necessary to form a conductor so that the powder particles can maintain contact with each other. Methods for forming the conductor include firing the green compact at a temperature lower than the melting point, and applying a conductive paint containing the powder to form a conductive film.
[0016] As the Weyl antiferromagnet, for example, an intermetallic compound whose composition formula is Mn3X (where X is a metal element) and whose crystal structure is an ordered lattice of the D019 structure can be applied. The molar ratio of Mn to element X is stoichiometrically 3:1, but in reality, there may be some variation from the strict stoichiometric ratio within the range in which the D019 crystal structure can be maintained. In this specification, the compound represented by the composition formula Mn3X includes those within the above-mentioned range of variation.
[0017] Examples of the Weyl antiferromagnet represented by the composition formula Mn3X include intermetallic compounds such as Mn3Sn, Mn3Ge, Mn3Ga, Mn3Pt, Mn3Ir, and Mn3Rh. One of these may be used alone, or two or more may be mixed and used. When two or more intermetallic compounds of Weyl antiferromagnets are mixed and used, a method of preparing powders composed of particles mainly composed of each intermetallic compound and blending the powders is envisioned.
[0018] The particles constituting the Weyl antiferromagnet powder of the present invention may contain a different phase in addition to the intermetallic compound phase exhibiting Weyl antiferromagnetism, as long as it is possible to construct a thermoelectric conversion element that exhibits antiferromagnetism in the intended temperature range of the thermoelectric conversion element and that exhibits the anomalous Nernst effect in that temperature range. That is, the present invention targets powders composed of particles whose main component is a Weyl antiferromagnet. The proportion of the main component intermetallic compound phase exhibiting Weyl antiferromagnetism (substance represented by the composition formula Mn3X) in the particles is preferably 50 mass% or more. In particular, it is more preferable that the remainder excluding the main component intermetallic compound phase exhibiting Weyl antiferromagnetism is unavoidable impurities.
[0019] In general, in Mn-X alloys (where X means a metal element capable of forming the compound Mn3X), the compound Mn3X exists stably in a single phase in a certain composition range close to the Mn3X composition. For example, in the case of Mn-Sn alloys, it has been confirmed that Mn3Sn exists stably in a single phase when the molar ratio of Mn:Sn is in the range of 3.02:0.98 to 3.15:0.85. However, when actually melting an ingot of an Mn-X alloy, even if it is melted with a feed composition in a range in which the compound Mn3X can exist in a single phase, a different phase other than the Mn3X phase may be generated during the solidification process and may be mixed into a part of the ingot. Therefore, it is effective to adjust the blending of the raw materials (feed composition) so that powder particles in a composition range in which Mn3X exists stably in a single phase are obtained according to the manufacturing method, in order to obtain a powder consisting mainly of the compound Mn3X and the remainder consisting of unavoidable impurities, that is, a powder substantially composed of a single Mn3X phase.
[0020] The operating temperature range of a thermoelectric conversion element can be assumed to be, for example, from -270°C to 680°C, depending on the type of Mn3X. In the case of Mn3Sn, the anomalous Nernst effect is said to be manifested in the range of -223°C (50K) to 157°C (430K).
[0021] Below, we will show an example of an experiment in which magnetization and the Nernst effect were investigated using Mn3Sn-based Weyl antiferromagnetic powder. EXAMPLES
[0022] [Example 1] (Preparation of Mn3Sn alloy ingot) The raw materials, metallic Mn and metallic Sn, were weighed out so that the molar ratio was Mn:Sn = 3.07:0.93, and placed in a 50 ml alumina crucible. The total mass of the raw materials was approximately 120 g. This crucible was placed in an electric furnace, and in an Ar gas atmosphere, the temperature was raised from room temperature to 1200°C over 5 hours, and then held at 1200°C for 24 hours. After that, the raw materials were melted and solidified using a heat pattern that cooled them to near room temperature over 5 hours, and an ingot of Mn3Sn alloy was obtained. Figure 1 shows an example of an external view of the ingot.
[0023] Samples were cut out from the ingot at four height positions: near the top of the ingot in the height direction (vertical direction at the time of solidification), near 1 / 4 position in the height direction from the top, near 1 / 2 position in the height direction from the top, and near the bottom. In all cases, the sampling position in the horizontal direction of the ingot as viewed in the vertical direction at the time of solidification was the center. Each sample was crushed to obtain a powder sample for X-ray diffraction. X-ray diffraction patterns of the powder samples at each position were measured using an X-ray diffractometer (Rigaku Corporation; Smartlab) under the conditions of Cu-Kα, tube voltage 40 kV, and tube current 100 mA.
[0024] Figure 2 shows an example of an X-ray diffraction pattern for a powder sample prepared from a sample at about 1 / 2 the height direction. Figure 3 shows the reference X-ray diffraction patterns for pure materials of metallic Mn, Mn oxide, and Mn-Sn intermetallic compounds. No impurity peaks were observed except for a small amount of MnO observed near the top of the ingot. In addition, when samples cut from various parts of the ingot were analyzed by an EDX (energy dispersive X-ray analyzer) attached to an SEM (scanning electron microscope), a small amount of Mn3Sn2 phase was detected. The average composition of the other parts was Mn:Sn = 3.03:0.97 in molar ratio. From the above analysis results, it was confirmed that the above-mentioned melting method can produce an ingot consisting of Mn3Sn phase and a small amount of a different phase. It is considered that the amount of the different phase in the ingot is small enough not to inhibit the physical properties brought about by the Weyl antiferromagnetism of the Mn3Sn phase. Therefore, the ingot obtained by this method may be referred to below as a "Mn3Sn crystal ingot." Also, the powder derived from the ingot may be referred to as a "Mn3Sn crystal powder."
[0025] (Powder preparation) The Mn3Sn crystal ingot (mass approximately 200 g) produced by the above method was crushed on an anvil placed in a bag to make small pieces of about 5 mm. 197 g of the small pieces were collected from the bag and crushed with a hammer mill (manufactured by Sansho Industry Co., Ltd.; hammer crusher NH-34S, screen opening: 0.7 mm) to obtain 163 g of coarse powder of Mn3Sn crystal. All operations from the above-mentioned small pieces to the crushing were carried out under a nitrogen atmosphere. The oxygen concentration in the nitrogen atmosphere was measured to be 0.2% or less using a high-concentration oxygen concentration meter (manufactured by Ichinohe Jiko Co., Ltd.; Oxy-medi, model number OXY-1-M).
[0026] The particle size distribution of this Mn3Sn crystal powder was measured by the volumetric method using a laser diffraction / scattering method with a dry laser diffraction particle size distribution analyzer HELOS&RODOS (manufactured by Japan Laser Co., Ltd.) and a lens with a focal length of 200 mm. The particle size distribution curve is shown in Figure 4 (the same applies to Examples 2 and 3 described later). The cumulative 10% particle diameter D 10is 27.3μm, cumulative 50% particle diameter D 50 is 100.7μm, cumulative 90% particle diameter D 90 was 227.7 μm.
[0027] (Preparation of sintered body using powder) 3 g of the above Mn3Sn crystal powder was placed in a cylinder of a cylindrical graphite cell with an inner diameter of 10 mm, and a load of 4.5 kN was applied by upper and lower pistons, and the powder was heated in a discharge plasma sintering apparatus under a vacuum atmosphere of about 1 Pa to obtain a cylindrical sintered body with a diameter of 10 mm and a height of about 7 mm. The heating temperature was 500°C, the heating holding time was 30 minutes, and the 4.5 kN load was maintained during the heating holding time.
[0028] (Measurement of magnetic properties) From the above sintered body, several cubic samples with a side length of 2 mm were cut out, and the magnetic properties of the samples were measured at 300 K using a SQUID (Super Quantum Interference Device) magnetometer as follows. That is, the temperature of the sample was set to 300 K, and a maximum magnetic field of 3 T (30,000 Oe) was applied using a superconducting magnet attached to the SQUID magnetometer. Then, during the magnetic field sweep process from 3 T to -3 T and from -3 T to 3 T, the magnetic field was fixed at each measurement point, and the magnetization (μ B The magnetization curve is shown in Figure 5. The coercive force was approximately 0.25 T (2500 Oe).
[0029] [Example 2] Powder was produced using an ingot of Mn3Sn alloy produced in the same manner as in Example 1. In this example, small pieces of about 5 mm crushed in the same manner as in Example 1 were fed into a sample mill (SK-M10 type, manufactured by Kyoritsu Riko Co., Ltd.) and crushed for 30 seconds in a nitrogen atmosphere to produce powder with a smaller average particle size than in Example 1. All of the above operations from crushing to crushing were carried out in a nitrogen atmosphere. The oxygen concentration in the nitrogen atmosphere was 0.2% or less, the same as in Example 1. The cumulative 10% particle size D of the powder obtained in this example was 10 is 9.6μm, cumulative 50% particle diameter D 50 is 50.1μm, cumulative 90% particle diameter D90 The particle size distribution curve is shown in FIG.
[0030] This powder was used to prepare a sintered body in the same manner as in Example 1. A number of cubic samples with sides of 2 mm were cut out from the sintered body, and the magnetic properties were measured in the same manner as in Example 1. The magnetization curves are shown in Figure 6.
[0031] (Measurement of the Nernst effect) A rectangular parallelepiped sample measuring 1.5 mm x 1.5 mm x 7 mm was cut out from the above-mentioned fired body. Terminals for measuring electromotive force and a probe for measuring temperature were attached to this sample, and a magnetic field was applied while a heat flow was generated in the longitudinal direction of the sample in a physical property measurement system (PPMS) manufactured by Quantum Design, and the electromotive force as a thermoelectric conversion element was measured. Figure 7 shows the attachment positions of the terminals for measuring electromotive force and the probe for measuring temperature, and the directions of the heat flow and magnetic field. Electromotive force measurement terminals 2a and 2b were attached to the center positions of the opposing sides of sample 1 with conductive epoxy adhesive, respectively, so that the voltage (V) generated between the two terminals could be measured with a voltmeter. This voltage is generated by the anomalous Nernst effect, so V ANE The temperature is displayed as "T1 / T2". Two temperature measurement probes were attached to the top surface of sample 1 with conductive epoxy adhesive at two points spaced 5 mm apart in the longitudinal direction, making it possible to monitor the temperature difference ΔT between the temperatures T1 (K) and T2 (K) at the two points. One longitudinal end face of sample 1 was heated by a resistance heater and the other end face was connected to a heat bath, so that one longitudinal end face was heated by a resistance heater and the other end face was connected to the heat bath and cooled, forming a temperature gradient in the longitudinal direction of the sample. The black arrow (4) in the figure indicates the direction of heat flow in the sample. After temperatures T1 and T2 had stabilized, a magnetic field was applied to the sample and a voltage V ANE The magnetic field was swept between 3T and -3T and between -3T and 3T. The Nernst coefficient S was calculated using the following formula (1): ANE (μV / K) was calculated. S ANE (μV / K)=V ANE(V) / 1.5(mm) / [(T1-T2)(K) / 5.0(mm)] …(1)
[0032] Figure 8 shows the Nernst coefficient ΔS ANE The measurement results of the Nernst coefficient S due to the magnetic field are shown here. ANE In order to clearly show the reversal magnetic field, the Nernst coefficient S ANE The magnetic field reversal component of the Nernst coefficient S at zero magnetic field ANE (approximately 0.3μV / K) normalized value ΔS ANE (The same applies to Figures 11, 13, and 15 described below.) As can be seen from Figure 8, the Nernst effect occurs even in zero magnetic field. In other words, the anomalous Nernst effect appears, and an electromotive force is generated by temperature difference alone. Although Mn3Sn is an antiferromagnetic material, the anomalous Nernst effect appears, which is thought to be due to the creation of a virtual magnetic field caused by the material being a Weyl magnet. The coercive force of the thermoelectric conversion element using the Weyl antiferromagnetic powder of this example is approximately 0.25 T (2500 Oe). This is evaluated as a practical coercive force that can withstand use inside general electronic devices and around automobile engines.
[0033] [Example 3] (Powder preparation) In this example, powder was produced directly from molten Mn3Sn alloy by gas atomization. Figure 9 shows a schematic diagram of the powder production apparatus using gas atomization. Powder was produced as follows. The raw materials, metal Mn and metal Sn, were weighed out so that the molar ratio was Mn:Sn = 3.07:0.93, and placed in a CP crucible (porous alumina) with a hole at the bottom and set in a high-frequency induction heating device. The chamber was evacuated and then filled with Ar gas. The hole at the bottom of the crucible was blocked by a stopper rod. The raw materials were melted by high-frequency induction heating and held at 1450°C for 40 minutes, after which the stopper rod was raised and the molten alloy was dripped from the hole at the bottom of the crucible into the lower space in the chamber. Ar gas was sprayed onto the molten metal in the lower space to turn the droplets into fine particles and rapidly cool and solidify them, obtaining alloy powder (atomized powder).
[0034] The obtained alloy powder was subjected to X-ray diffraction and EDX analysis in the same manner as above, and the results showed that the powder was composed of particles consisting of almost a single phase of Mn3Sn, with an average composition of Mn:Sn = 3.02:0.98 in molar ratio. Therefore, this powder can also be called "Mn3Sn crystal powder" as above. The particle size distribution of this Mn3Sn crystal powder was measured by the method shown in Example 1. The particle size distribution curve is shown in Figure 4. The cumulative 10% particle diameter D of the powder obtained in this example was 10 is 4.8μm, cumulative 50% particle diameter D 50 is 15.2μm, cumulative 90% particle diameter D 90 was 31.9 μm.
[0035] This powder was used to prepare a sintered body in the same manner as in Example 1. From the sintered body, multiple cubic samples with a side length of 2 mm were cut out, and the magnetic properties were measured in the same manner as in Example 1. The magnetization curves are shown in FIG. 10. Furthermore, rectangular parallelepiped samples of 1.5 mm×1.5 mm×7 mm were cut out from the above sintered body, and the Nernst effect was measured in the same manner as in Example 2. The Nernst coefficient ΔS ANE The measurement results are shown below. The coercive force of the thermoelectric conversion element using the Weyl antiferromagnet powder of this example was about 0.5 T (5000 Oe), which was higher than those of Examples 1 and 2. It was found that the atomization of the Weyl antiferromagnet powder is extremely effective in improving the coercive force of the thermoelectric conversion element using the powder. The mechanism by which the coercive force is improved by using such a finely-divided Weyl antiferromagnet has not been fully elucidated at present, but it is speculated that the contribution of pinning the magnetic domain wall increases as the particle diameter approaches the size at which a single magnetic domain is formed.
[0036] [Comparative Example 1] Powder was produced using an ingot of Mn3Sn alloy produced by the same method as in Example 1. In this example, small pieces of about 5 mm crushed by the same method as in Example 1 were manually crushed in an alumina mortar. The crushed material obtained was sieved with a sieve with a mesh size of 200 μm. 68% of the crushed material remained on the sieve by mass. For this crushed material sample, a particle size distribution measurement was attempted using a dry laser diffraction particle size distribution measurement device as in Example 1, but since the particle diameter of the sample was coarse, the measurement was over the range of a lens with a focal length of 200 mm, and the particle size distribution could not be measured.
[0037] Using the above pulverized sample, a sintered body was produced in the same manner as in Example 1. From the sintered body, multiple cubic samples with a side length of 2 mm were cut out, and the magnetic properties were measured in the same manner as in Example 1. The magnetization curve is shown in FIG. 12. In addition, a rectangular parallelepiped sample (polycrystalline body) of 1.5 mm×1.5 mm×7 mm was cut out directly from the above ingot. At that time, the rectangular parallelepiped sample was taken from a part of the ingot where defects such as shrinkage cavities were not observed, so that the longitudinal direction of the sample coincided with the horizontal direction at the time of solidification of the ingot. The Nernst effect was examined using this rectangular parallelepiped sample in the same manner as in Example 1. The Nernst coefficient ΔS ANE The measurement results are shown below. The coercive force of the thermoelectric conversion element using the Weyl antiferromagnet of this example was approximately 0.05 T (500 Oe), which was significantly lower than that of the example using the powder of the Weyl antiferromagnet. With such a low coercive force, there is a risk of demagnetization due to the magnetic field near permanent magnets or magnetic components, making it difficult to construct a highly reliable thermoelectric conversion element.
[0038] [Comparative Example 2] An ingot of Mn3Sn alloy prepared by the same method as in Example 1 was melted, and a single crystal of Mn3Sn was prepared by the Bridgman method. The maximum temperature of the Bridgman furnace was 1080°C, and the sample was moved at a speed of 1.5 mm / h. The composition of the obtained single crystal was analyzed by ICP-AES, and the molar ratio was Mn:Sn=3.06:0.94.
[0039] From this single crystal, multiple cubic samples with a side length of 2 mm were cut out, and magnetic measurements were performed in the same manner as in Example 1. In this case, the direction of application of the external magnetic field was made to coincide with the [2-1-10] direction of the Mn3Sn crystal. Figure 14 shows the magnetization curve. Furthermore, from the above single crystal, a rectangular sample of 1.5 mm x 1.5 mm x 7 mm was cut out, and the Nernst effect was examined in the same manner as in Example 1. In this case, the direction of the heat flow (the longitudinal direction of the rectangular sample) was made to coincide with the [0 1-10] direction of the Mn3Sn crystal, and the direction of application of the external magnetic field was made to coincide with the [2-1-10] direction of the Mn3Sn crystal. Figure 15 shows the Nernst coefficient ΔS ANE The coercive force of the thermoelectric conversion element using the Weyl antiferromagnetic single crystal of this example was less than 0.01 T (100 Oe). The coercive force was significantly lower than that of the example using the Weyl antiferromagnetic powder.
[0040] [Table 1] [Explanation of symbols]
[0041] 1. Sample for measuring the Nernst effect 2a, 2b Electromotive force measurement terminal 31, 32 Temperature measurement position 4. Heat flow direction in the sample 5. Magnetic Field Direction
Claims
1. A powder composed of particles mainly composed of Weyl antiferromagnets, and in a volume-based particle size distribution measured by a laser diffraction / scattering method, the cumulative 50% particle diameter D 50 is 1 to 150 μm, cumulative 90% particle diameter D 90 A Weyl antiferromagnetic powder having a particle size of 250 μm or less.
2. The Weyl antiferromagnet has the composition formula Mn 3 2. The Weyl antiferromagnetic powder according to claim 1, which is an intermetallic compound having a D019 structure represented by X, where X is a metal element.
3. The Weyl antiferromagnet has the chemical formula Mn 3 2. The Weyl antiferromagnetic powder according to claim 1, which is a compound represented by X, where X is one or more elements selected from the group consisting of Sn, Ge, Ga, Pt, Ir and Rh.
4. The Weyl antiferromagnet is Mn 3 Sn, Mn 3 Ge, Mn 3 Ga, Mn 3 Pt, Mn 3 Ir, Mn 3 2. The Weyl antiferromagnetic powder according to claim 1, which is one or more compounds selected from Rh.
5. A thermoelectric conversion element using the Weyl antiferromagnetic powder according to any one of claims 1 to 4.
Citation Information
Patent Citations
Magnetic powder
JP1999335702A
Magnetic material and its manufacturing method
JP2006332155A
Thermoelectric generation device
JP2014072256A
Thermoelectric conversion device