Method for producing long films containing poly(3-hydroxyalkanoate) resin

Heat treatment of poly(3-hydroxyalkanoate) resin films at specific temperature ranges addresses the brittle fracture issue, resulting in films with improved mechanical properties and transport stability.

JP7570857B2Active Publication Date: 2024-10-22KANEKA CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020153039
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-11
Publication Date
2024-10-22
Estimated Expiration
2040-09-11

AI Technical Summary

Technical Problem

Existing methods for producing poly(3-hydroxyalkanoate) resin films lack the ability to maintain excellent elastic modulus, yield strength, and elongation at break, particularly due to brittle fracture during storage and transport.

Method used

A heat treatment process is applied to unwound films at specific temperature ranges, specifically between the lowest DSC melting point temperature and 25°C lower than the DSC melting point with the highest heat, to prevent brittle fracture and improve mechanical properties.

Benefits of technology

The method produces films with enhanced elastic modulus, yield strength, and elongation at break, while preventing wrinkles and ensuring stability during transport.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570857000003
    Figure 0007570857000003
  • Figure 0007570857000001
    Figure 0007570857000001
  • Figure 0007570857000002
    Figure 0007570857000002
Patent Text Reader

Abstract

To provide a method for producing a long film containing poly (3-hydroxyalkanoate) resin.SOLUTION: The present invention discloses a method for producing a long film containing poly (3-hydroxyalkanoate) resin. In the process of rolling out the long film wound around a roll and conveying it to the next step, the rolled-out film is heated in a specific temperature range.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a long film containing a poly(3-hydroxyalkanoate) (hereinafter, sometimes referred to as "P3HA" or "P3HA-based resin")-based resin. [Background technology]

[0002] A large amount of petroleum-derived plastics are discarded every year, and the lack of landfill sites and environmental pollution caused by this large amount of waste are being raised as serious issues. In recent years, microplastics have also become a major problem in the marine environment.

[0003] Poly(3-hydroxyalkanoate) resins have excellent seawater degradability and are materials that can solve the environmental problems caused by discarded plastics. For example, the mechanical properties of poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), a type of poly(3-hydroxyalkanoate) resin, can be flexibly controlled by changing the composition ratio of 3-hydroxyhexanoate. In addition, it has high gas barrier properties among biodegradable resins and is resistant to hydrolysis, so it is expected to be used in a wide range of applications, including packaging materials.

[0004] Patent Document 1 discloses a polyester film containing a white pigment and having the highest peak top temperature of a specific cold crystallization peak and the peak top temperature of a specific minor endothermic peak in a DSC curve, and a method for producing the same. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2020-050876 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, there is room for improvement in the method for producing a long film containing a poly(3-hydroxyalkanoate) resin.

[0007] Therefore, an object of the present invention is to provide a method for producing a long film containing a poly(3-hydroxyalkanoate) resin, which has excellent elastic modulus and yield strength as well as excellent elongation at break. [Means for solving the problem]

[0008] As a result of extensive research to solve the above-mentioned problems, the inventors have discovered for the first time that, in the manufacturing process of a long film containing a poly(3-hydroxyalkanoate) resin, by subjecting the unwound film to heat treatment at a specific temperature, it is possible to produce a long film that is excellent in elastic modulus and yield strength as well as breaking elongation, and have thus completed the present invention.

[0009] Therefore, one aspect of the present invention is a method for producing a long film containing a poly(3-hydroxyalkanoate) resin, which includes a step of heat-treating the unwound film in a temperature range from (i) above to (ii) below in a process of unwinding the long film wound around a roll and transporting it to a next process: (i) the lowest DSC melting point temperature of the film, and (ii) a temperature 25°C lower than the DSC melting point temperature of the film with the greatest amount of heat. Effect of the Invention

[0010] According to one aspect of the present invention, there is provided a long film containing a poly(3-hydroxyalkanoate) resin, which is excellent in elastic modulus and yield strength as well as in breaking elongation. [Brief description of the drawings]

[0011] [Figure 1]FIG. 2 is a schematic diagram showing a differential scanning calorimeter (DSC) curve of a long film containing a P3HA resin according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] An embodiment of the present invention will be described in detail below. In this specification, unless otherwise specified, "A to B" representing a numerical range means "A or more, B or less." In addition, all documents described in this specification are incorporated herein by reference.

[0013] 1. Overview of the Invention The manufacturing method of a long film containing a poly(3-hydroxyalkanoate) resin according to one embodiment of the present invention (hereinafter referred to as "this manufacturing method") is characterized in that, in the process of unwinding the long film wound around a roll and transporting it to the next process, the unwound film is subjected to a heat treatment in a temperature range of the following (i) or higher and (ii) or lower: (i) the lowest DSC melting point temperature of the film, and (ii) a temperature 25°C lower than the DSC melting point temperature of the film with the greatest heat quantity.

[0014] In investigating the manufacturing process of a long film containing a poly(3-hydroxyalkanoate)-based resin, the present inventors have made the following discoveries: (i) a long film containing a poly(3-hydroxyalkanoate)-based resin has a certain degree of flexibility (breaking elongation) immediately after production, making it suitable for secondary processing; and (ii) on the other hand, if a long film containing a poly(3-hydroxyalkanoate)-based resin is stored for a certain period of time after production in a rolled-up state, there is a problem in that the long film is prone to brittle fracture during the process of transporting the long film to the next process.

[0015] As a result of further investigation, the present inventors presumed that the cause of the above problem was that the crystallization of the poly(3-hydroxyalkanoate) resin in the long film progressed during storage of the film, and as a result, when a minute scratch was given to the film, brittle fracture occurred rapidly. Up to now, there has been no known method for producing a long film containing a poly(3-hydroxyalkanoate) resin that has excellent brittle fracture resistance (breaking elongation) while maintaining mechanical properties (elastic modulus, yield strength, etc.).

[0016] Therefore, the inventors conducted intensive research to solve the above problems and discovered for the first time that by subjecting the unwound film to heat treatment at a specific temperature during the manufacturing process of the long film, it is possible to produce a long film that has excellent mechanical properties as well as excellent breaking elongation.

[0017] They also found that by setting the heat treatment temperature during the transport process within a specific temperature range, in addition to the mechanical properties and brittle fracture resistance, the occurrence of wrinkles in the long film can be prevented.

[0018] 2. Film manufacturing method This manufacturing method is a method for producing a long film containing a P3HA-based resin, and includes a step of subjecting the unwound film to heat treatment within a specified temperature range during the process of unwinding the long film wound around a roll and transporting it to the next process.

[0019] (P3HA resin) The long film in this manufacturing method contains a P3HA-based resin. A preferred example of such a resin is poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (P3HB3HH (hereinafter, also referred to as "PHBH")). For convenience of explanation, the following description will be mainly given using PHBH as a representative example.

[0020] In the present specification, the term "P3HA resin" refers to a polymer having the following formula (1): [-O-CHR-CH2-CO-] (1) (Wherein, R is C n H 2n+1 and n is an integer of 1 to 15. The term "alkyl group" refers to a polymer or copolymer comprising one or more types of units represented by the following formula:

[0021] The P3HA resin may be a poly(3-hydroxybutyrate) having only 3-hydroxybutyrate as a repeating unit, or a copolymer of 3-hydroxybutyrate and other hydroxyalkanoates. The P3HA resin may be a mixture of a homopolymer and one or more types of copolymers, or a mixture of two or more types of copolymers. The type of copolymerization is not particularly limited, and may be random copolymerization, alternating copolymerization, block copolymerization, graft copolymerization, or the like.

[0022] Examples of P3HA-based resins include poly(3-hydroxybutyrate) (P3HB), poly(3-hydroxybutyrate-co-3-hydroxypropionate) (P3HB3HP), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (P3HB3HH), poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (P3HB3HV), poly(3-hydroxybutyrate-co-4-hydroxybutyrate) (P3HB4 HB), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate) (P3HB3HO), poly(3-hydroxybutyrate-co-3-hydroxyoctadecanoate) (P3HB3HOD), poly(3-hydroxybutyrate-co-3-hydroxydecanoate) (P3HB3HD), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate) (P3HB3HV3HH), etc. are included. From the viewpoint of being able to adjust the melting point low and widen the processing range, PHBH, P3HB4HB, and P3HB3HP are preferred. Among them, PHBH and P3HB4HB are particularly preferred because they are easy to produce industrially. From the viewpoint of industrial productivity, in addition to the above, P3HB and P3HB3HV are also preferred.

[0023] The P3HA resin is preferably produced by a microorganism. The microorganism that produces the P3HA resin is not particularly limited as long as it is a microorganism capable of producing the P3HA resin. For example, the first PHBH-producing bacterium was Bacillus megaterium, discovered in 1925, and other natural microorganisms include Cupriavidus necator (formerly classified as Alcaligenes eutrophus and Ralstonia eutropha) and Alcaligenes latus. It is known that PHBH accumulates in the cells of these microorganisms.

[0024] Also, as producers of copolymers of hydroxybutyrate and other hydroxyalkanoates, Aeromonas caviae, which produces PHBH, and Alcaligenes eutrophus, which produces P3HB4HB, are known. In particular, for PHBH, in order to increase the productivity of PHBH, Alcaligenes eutrophus AC32 (FERM BP-6038) (T. Fukui, Y. Doi, J. Bateriol., 179, p4821-4830 (1997)) into which genes of PHBH synthesis enzyme group have been introduced is more preferable, and microbial cells in which these microorganisms are cultured under appropriate conditions and PHBH has been accumulated in the cells are used. In addition to the above, genetically modified microorganisms into which various P3HA synthesis-related genes have been introduced may be used according to the P3HA to be produced, or the culture conditions, including the type of substrate, may be optimized.

[0025] PHBH can also be produced by the method described in, for example, International Publication No. 2010 / 013483. Commercially available PHBH products include Kaneka Biodegradable Polymer PHBH (registered trademark) from Kaneka Corporation.

[0026] In one embodiment of the present invention, the composition ratio of the copolymerization components of PHBH is not particularly limited, but is preferably (3-hydroxybutyrate) / (3-hydroxyhexanoate)=99 / 1 to 90 / 10 (mol / mol), more preferably 98 / 2 to 91 / 9 (mol / mol), and even more preferably 97 / 3 to 92 / 8 (mol / mol). When (3-hydroxybutyrate) / (3-hydroxyhexanoate) is 99 / 1 (mol / mol) or less, sufficient flexibility is obtained, and when it is 90 / 10 (mol / mol) or more, good productivity is obtained.

[0027] The content of the P3HA resin in the long film is 70% by weight or more, and from the viewpoint of enhancing the seawater decomposability of the film, it is preferably 80% by weight or more, and more preferably 90% by weight or more. The upper limit of the content of the P3HA resin in the long film is not particularly limited, and may be 100% by weight.

[0028] In one embodiment of the present invention, the weight average molecular weight (hereinafter sometimes referred to as Mw) of the P3HA resin is not particularly limited, but from the viewpoint of molding processability, the weight average molecular weight is preferably 50,000 to 3,000,000, more preferably 100,000 to 2,500,000, and even more preferably 150,000 to 2,000,000. If the weight average molecular weight of the P3HA resin is less than 50,000, mechanical properties such as strength may be insufficient, and if it exceeds 3,000,000, molding processability may be poor.

[0029] The method for measuring the weight-average molecular weight of the P3HA-based resin is not particularly limited. For example, the weight-average molecular weight can be determined as a polystyrene-equivalent weight-average molecular weight by using chloroform as the mobile phase, a GPC system manufactured by Waters Corporation as the system, and Shodex K-804 (polystyrene gel) manufactured by Showa Denko K.K. as the column.

[0030] (Long film) In one embodiment of the present invention, the long film may contain, in addition to the P3HA resin, one or more biodegradable resins other than the P3HA resin, as long as the effects of the present invention are achieved. Examples of biodegradable resins other than the P3HA resin include polybutylene adipate terephthalate, polybutylene succinate adipate, polybutylene succinate, polybutylene succinate terephthalate, polybutylene succinate adipate terephthalate, polybutylene sebacate terephthalate, polybutylene azelate terephthalate, and polycaprolactone.

[0031] The content of biodegradable resins other than P3HA is preferably 30% by weight or less, and more preferably 10% by weight or less, from the viewpoints of physical properties, the degree of biomass plastic, etc. The lower limit is not particularly limited, and may be 0% by weight.

[0032] In one embodiment of the present invention, the long film may contain, in addition to the P3HA resin and the biodegradable resin other than the P3HA resin, additives that are commonly used in the art within the scope of the effects of the present invention. Examples of such additives include nucleating agents, lubricants, plasticizers, inorganic fillers, antioxidants, ultraviolet absorbers, colorants such as dyes and pigments, and antistatic agents. The additives may be one type or two or more types. The content of these additives can be appropriately set by a person skilled in the art depending on the purpose of use.

[0033] From the viewpoint of handling, the thickness of the long film obtained by the present production method is preferably from 15 to 100 μm, and more preferably from 20 to 60 μm.

[0034] The long film produced is a film used for continuous production, and is a wide and long film. From the viewpoint of film productivity, the width of such a long film is preferably 50 cm or more, more preferably 90 cm or more. The length of the film is preferably 1000 m or more, more preferably 2000 m or more.

[0035] The elastic modulus of the long film obtained by this production method is preferably 800 MPa or more, more preferably 850 MPa or more, and even more preferably 900 MPa or more from the viewpoint of transportability. Also, from the viewpoint of handling, it is preferably 2500 MPa or less, more preferably 2450 MPa or less, and even more preferably 2400 MPa or less. The elastic modulus of the long film is measured by the method described in the examples.

[0036] The yield strength of the long film obtained by this manufacturing method is preferably 10 MPa or more, more preferably 12 MPa or more, and even more preferably 15 MPa or more, from the viewpoint of resistance to tension during transportation. Also, from the viewpoint of secondary processing, it is preferably 60 MPa or less, more preferably 50 MPa or less, and even more preferably 40 MPa or less. The yield strength of the long film is measured by the method described in the Examples.

[0037] The breaking elongation of the long film obtained by the present production method is preferably 15% or more, more preferably 25% or more, and even more preferably 40% or more, from the viewpoint of fracture toughness. The upper limit is not particularly limited, but is, for example, 200% or less. The breaking elongation of the long film is measured by the method described in the Examples.

[0038] (Heat treatment process) In this manufacturing method, in the process of unwinding the long film wound around a roll and transporting it to the next process, the unwound film is subjected to a heat treatment within a predetermined temperature range.

[0039] When a long film wound around a roll is unwound, fine crystals may be present in the film. These fine crystals in the film may cause the film to break. Therefore, by subjecting the film to a heat treatment, the fine crystals in the film melt, resulting in a film that is less likely to break. The temperature ranges for the heat treatment in this manufacturing method are the following temperature ranges (i) and (ii): (i) The lowest DSC melting point temperature of the film (ii) A temperature 25° C. lower than the DSC melting point temperature of the film at which the heat quantity is greatest.

[0040] In this specification, the "lowest DSC melting point temperature" refers to the peak top temperature of the lowest-temperature melting point peak among the endothermic peaks present in the DSC curve. For example, in FIG. 1, the "lowest DSC melting point temperature" refers to point k, which is the peak top of the lowest-temperature DSC melting point peak Q.

[0041] On the other hand, when the degree of crystallinity of the fine crystals in the film is so low that no melting point peak appears on the DSC curve, but only a broad shoulder or a baseline shift appears, the "lowest DSC melting point temperature" refers to the midpoint temperature of the baseline shift.

[0042] In this specification, the "DSC melting point temperature with the largest calorific value" refers to the peak top temperature of the largest peak (main peak) among the endothermic peaks present in the DSC curve. For example, in FIG. 1, the "DSC melting point temperature with the largest calorific value" refers to point m, which is the peak top with the largest endothermic calorific value, in the DSC melting point peak R, which is the main peak.

[0043] By the heat treatment step of this manufacturing method, fine crystals of the P3HA resin in the "temperature range in which fine crystals exist" are removed from the film. In Figure 1, the "temperature range in which fine crystals exist" refers to the range of T.

[0044] In one embodiment of the present invention, the "lowest DSC melting point temperature" of (i) is preferably 50°C, more preferably 55°C, and even more preferably 60°C.

[0045] In one embodiment of the present invention, the "DSC melting point temperature at which the amount of heat is the largest" in (ii) is preferably 160° C., more preferably 155° C., even more preferably 150° C., and particularly preferably 140° C. Therefore, in one embodiment of the present invention, the "temperature 25° C. lower than the DSC melting point temperature at which the amount of heat is the largest in the film" in (ii) is preferably 135° C., more preferably 130° C., even more preferably 125° C., and particularly preferably 115° C. By setting (i) and (ii) within the above temperature ranges, fine crystals in the film can be sufficiently melted, and a long film excellent in mechanical properties and breaking elongation can be produced.

[0046] In the heat treatment, the heating device used to heat the film is not particularly limited as long as it can heat the film to the specific temperature. Examples of the heating device include a heating furnace, a heating roll, and a preheating chamber attached to a secondary processing facility. A heating furnace is preferable from the viewpoint of stabilizing the temperature of the film during the heat treatment.

[0047] As a method of heat treatment, the film may be heated by hot air, or may be heated by an infrared heater, etc. In addition, the film may be heated by using an auxiliary heat source such as an infrared heater and a heating roll in combination with supplying hot air.

[0048] The time for which the film is heat-treated in the temperature ranges (i) and (ii) is not particularly limited as long as it is a time that can sufficiently melt the fine crystals in the film, but it is, for example, 0.1 to 100 minutes, and from the viewpoint of productivity, 0.1 to 10 minutes is preferable.

[0049] (Heat shrinkage rate) From the viewpoint of dimensional stability, the heat shrinkage rate of the film before and after the above-mentioned heat treatment process is preferably 2.0% or less, more preferably 1.5% or less. The lower the heat shrinkage rate of the film, the better, and it may be 0%. The heat shrinkage rate of the film is measured by the method described in the examples.

[0050] (Transportation process) The above-mentioned heat treatment step is preferably carried out in a transport step in which the film is unwound from the roll and transported to the next step. The "transport step" refers to any time or period from when the film starts being unwound from the roll until it is provided to the next step. Therefore, the heat treatment step may be carried out, for example, at the same time when the film is unwound from the roll, or when the film unwound from the roll is transported to the next step. Preferably, the heat treatment step is carried out at the same time when the film is unwound from the roll. This allows the film to be given strength before being transported to the next step, and makes it possible to withstand impacts and the like during transport.

[0051] In one embodiment of the present invention, the stress applied to the film in the transport step is preferably 5 to 30 MPa, more preferably 5 to 20 MPa, and even more preferably 5 to 10 MPa. When the stress applied to the film is within this range, the film does not bend and no excessive tension is generated.

[0052] The film transport speed is not particularly limited, but is preferably 5 to 100 m / min, more preferably 5 to 80 m / min, and even more preferably 5 to 50 m / min. If the transport speed is within this range, the film can be sufficiently heat-treated, and fine crystals in the film can be sufficiently melted.

[0053] (Other processes) In one embodiment of the present invention, the manufacturing method may be a method for continuously manufacturing a film in a roll-to-roll manner. In one embodiment of the present invention, the manufacturing method may include other steps before and after the heat treatment. Such other steps are not particularly limited and may include any steps generally performed in the film manufacturing process. Before the heat treatment step, for example, there may be a step of molding the P3HA resin. The step of molding the P3HA resin is not particularly limited, but examples thereof include an extrusion molding step, an inflation molding step, a T-die molding step, and a calendar molding step. After the heat treatment step, for example, a printing step, a vapor deposition step, a lamination step, a bag making step, and the like may be included as the next step.

[0054] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention.

[0055] That is, one embodiment of the present invention is as follows. <1> A method for producing a long film containing a poly(3-hydroxyalkanoate)-based resin, comprising the steps of: In the process of unwinding the long film wound around the roll and transporting it to the next process, A method for producing a long film, comprising a step of subjecting the unwound film to a heat treatment in a temperature range of the following (i) or more and the following (ii) or less: (i) The lowest DSC melting point temperature of the film (ii) A temperature 25° C. lower than the DSC melting point temperature of the film at which the heat quantity is greatest. <2> The heat shrinkage rate of the film is 2.0% or less before and after the heat treatment step. <1> The manufacturing method described in <3> The poly(3-hydroxyalkanoate)-based resin is selected from the group consisting of poly(3-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxypropionate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate), poly(3-hydroxybutyrate-co-4-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate), poly(3-hydroxybutyrate-co-3-hydroxyoctadecanoate), poly(3-hydroxybutyrate-co-3-hydroxydecanoate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate), and combinations thereof. <1> or <2> The manufacturing method described in <4> the poly(3-hydroxyalkanoate) resin is poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (P3HB3HH); (3-hydroxybutyrate) / (3-hydroxyhexanoate)=99 / 1 to 90 / 10 (mol / mol); <1> ~ <3> 13. A method for producing a film according to any one of the preceding claims. <5> The temperature of (i) is 50°C. <1> ~ <4> 13. A method for producing a film according to any one of the preceding claims. <6> The temperature in (ii) is 130°C. <1> ~ <5> 13. A method for producing a film according to any one of the preceding claims. <7> The stress applied to the film during the transport process is 5 to 30 MPa. <1> ~ <6> 13. A method for producing a film according to any one of the preceding claims. <8> The thickness of the film is 15 to 100 μm. <1> ~ <7> 13. A method for producing a film according to any one of the preceding claims. EXAMPLES

[0056] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.

[0057] 〔material〕 (P3HA) The P3HA used to form the film was poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (hereinafter referred to as "PHBH-1"), which has a copolymerization component ratio of (3-hydroxybutyrate) / (3-hydroxyhexanoate) = 92.4 / 7.6 (mol / mol) and a weight-average molecular weight of 600,000.

[0058] In addition, poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (hereinafter referred to as "PHBH-2") was used as the P3HA constituting the film, with a composition ratio of copolymer components of (3-hydroxybutyrate) / (3-hydroxyhexanoate) = 94 / 6 (mol / mol) and a weight average molecular weight of 600,000.

[0059] [Measurement and evaluation methods] (DSC measurement) A 4 mg sample was weighed, and a DSC chart was obtained using a DSC6220 manufactured by Seiko Denshi Kogyo Co., Ltd. The scanning temperature range was 30 to 190° C., and the scanning speed was 10° C. / min.

[0060] (Heat shrinkage rate) The film was cut into a size of 10cm x 10cm, and the dimensions in the MD and TD directions were measured. Next, the film was heated at a specific temperature range for 1 minute, cooled at room temperature, and the dimensions in the MD and TD directions were measured again. The rate of change in each direction was calculated, and the average of the rates of change in the MD and TD directions was taken as the heat shrinkage rate of the film.

[0061] (Elasticity Modulus) The elastic modulus was obtained by conducting a tensile test in accordance with JIS K7127:1999 Plastics - Test method for tensile properties. The test piece shape was Type 5 and the tensile speed was 100 mm / min.

[0062] (yield strength) The yield strength was obtained using the same test method as above (elastic modulus).

[0063] (Elongation at break) The breaking elongation was obtained using the same test method as above (elastic modulus).

[0064] (wrinkle) A 5 cm line was drawn crosswise on the film, and the film was evaluated for streaks or waviness. 0 streaks or waves: Yes One or more streaks or waves: × [ Reference example 1, Working Example 2 ~5, Comparative Examples 1 and 2] 0.5 parts of an internal lubricant was added to 100 parts by mass of PHBH-1 and dry blended. The obtained resin material (resin mixture) was extrusion molded at an extrusion temperature of 160°C using an inflation molding machine to produce a film with a thickness of 30 μm.

[0065] Here, the produced film was subjected to DSC measurement to identify the melting point temperature, etc. The "lowest DSC melting point temperature" of the produced film was 54°C, and the "DSC melting point temperature with the largest amount of heat" was 136°C.

[0066] The film was heat-treated by heating it for 1 minute in a hot air drying oven. Reference example 1, Working Example 2 The heat treatment temperatures in Comparative Example 2 to 5 are as shown in Table 1. In Comparative Example 1, the film was not subjected to heat treatment.

[0067] Reference example 1, Working Example 2 The heat shrinkage rate, elastic modulus, yield strength, elongation at break, and wrinkles were measured and evaluated for each of the films of Examples 1 to 5 and Comparative Examples 1 and 2. The measurement results are shown in Table 1.

[0068] [Table 1]

[0069] As shown in Table 1, heat treatment was performed within a specified temperature range. Reference example 1, Working Example 2The films from 1 to 5 all had a thermal shrinkage rate of 2% or less before and after the heat treatment, and were excellent in elastic modulus, yield strength, and breaking elongation. Reference example 1, Working Example 2 No wrinkles were observed in the ~4 film.

[0070] On the other hand, the film of Comparative Example 2, which was heat-treated at a predetermined temperature or higher, had a high heat shrinkage rate of 3%. In Comparative Example 2, the elastic modulus, yield strength, elongation at break, and wrinkles could not be measured or evaluated because the film was partially melted. Furthermore, the film of Comparative Example 1, which was not heat-treated, had a small elongation at break.

[0071] [Examples 6 to 8, Comparative Examples 3 and 4] Except for using PHBH-2 instead of PHBH-1, Reference example 1, Working Example 2 〜5, the films were produced under the same conditions as in Comparative Examples 1 and 2.

[0072] Here, the produced film was subjected to DSC measurement to identify the melting point temperature, etc. The "lowest DSC melting point temperature" of the produced film was 60°C, and the "highest DSC melting point temperature with the greatest amount of heat" was 139°C.

[0073] The films were heat-treated by heating them for 1 minute in a hot air drying oven. The heat treatment temperatures in Examples 6 to 8 and Comparative Examples 3 and 4 are as shown in Table 1.

[0074] The heat shrinkage, elastic modulus, yield strength, elongation at break, and wrinkles were measured and evaluated for each of the films of Examples 6 to 8 and Comparative Examples 3 and 4. The measurement results are shown in Table 2.

[0075] [Table 2]

[0076] As shown in Table 2, the films of Examples 6 to 8, which were heat-treated within a predetermined temperature range, all had a heat shrinkage rate of 2% or less before and after the heat treatment, and were excellent in elastic modulus, yield strength, and breaking elongation. In addition, no wrinkles were observed in the films of Examples 6 to 8.

[0077] On the other hand, the films of Comparative Examples 3 and 4, which were heat-treated at a temperature lower than the specified temperature, had small breaking elongation. [Industrial Applicability]

[0078] INDUSTRIAL APPLICABILITY The present invention can be utilized in a method for producing a long film containing a poly(3-hydroxyalkanoate) resin, which has excellent elastic modulus and yield strength as well as excellent elongation at break.

Claims

1. A method for producing a long film containing a poly(3-hydroxyalkanoate)-based resin, comprising the steps of: In the process of unwinding the long film wound around the roll and transporting it to the next process, A method for producing a long film, comprising a step of subjecting the unwound film to a heat treatment at a temperature range of the following (i) temperature or more and 70° C. or more and the following (ii) temperature or less: (i) The lowest DSC melting point temperature of the film (ii) A temperature 25° C. lower than the DSC melting point temperature of the film at which the amount of heat is greatest.

2. The method according to claim 1 , wherein the heat shrinkage rate of the film is 2.0% or less before and after the heat treatment step.

3. 3. The method according to claim 1, wherein the poly(3-hydroxyalkanoate)-based resin is selected from the group consisting of poly(3-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxypropionate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate), poly(3-hydroxybutyrate-co-4-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate), poly(3-hydroxybutyrate-co-3-hydroxyoctadecanoate), poly(3-hydroxybutyrate-co-3-hydroxydecanoate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate), and combinations thereof.

4. the poly(3-hydroxyalkanoate)-based resin is poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (P3HB3HH); The method for producing a film according to any one of claims 1 to 3, wherein (3-hydroxybutyrate) / (3-hydroxyhexanoate)=99 / 1 to 90 / 10 (mol / mol).

5. A method for producing a film described in any one of claims 1 to 4, wherein the temperature of the heat treatment is in a temperature range below the temperature of (ii) and below 130°C.

6. The method for producing a film according to any one of claims 1 to 5, wherein a stress applied to the film during the transporting process is 5 to 30 MPa.

7. The method for producing a film according to any one of claims 1 to 6, wherein the film has a thickness of 15 to 100 µm.

Citation Information

Patent Citations

  • Biodegradable film and laminate

    JP1995188432A

  • Film comprising poly(3-hydroxybutanoic acid)

    JP1998176070A

  • Adhering heat-resistant wrapping film

    JP2000026625A

  • Manufacturing method of biodegradable film

    JP2006168159A

  • Biodegradable polyester film and production method thereof

    JP2013185139A