Resin composition, cured resin, and fiber-reinforced resin

The resin composition with manganese (III)-coordinated complexes and specific ratios enhances transesterification reactions, addressing slow stress relaxation in dynamic covalent bonds, thereby improving stress relief and crack resistance in resin products.

JP7570892B2Active Publication Date: 2024-10-22HITACHI LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020187091
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-10
Publication Date
2024-10-22
Estimated Expiration
2040-11-10

AI Technical Summary

Technical Problem

Existing resin compositions using dynamic covalent bonds, such as those described in Patent Document 1, suffer from slow stress relaxation times when subjected to stress, which prolongs the time required for stress relief and crack suppression.

Method used

A resin composition comprising an epoxy compound with multiple epoxy groups, an acid anhydride, and a complex where manganese (III) is coordinated with an organic ligand, with specific ratios to enhance the transesterification reaction and reduce stress relaxation time.

Benefits of technology

The composition allows for a significant reduction in stress relaxation time, enabling faster stress relief and improved crack resistance and repairability in cured resin products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570892000003
    Figure 0007570892000003
  • Figure 0007570892000004
    Figure 0007570892000004
  • Figure 0007570892000001
    Figure 0007570892000001
Patent Text Reader

Abstract

To provide a resin composition capable of shortening the stress relaxation time, a resin cured product, and a fiber-reinforced resin.SOLUTION: A resin composition includes an epoxy compound having two or more epoxy groups in each molecule, an acid anhydride, and a complex in which an organic ligand is coordinated to manganese (III). A resin cured product includes a resin having an ester group and a hydroxyl group, and a complex in which an organic ligand is coordinated to manganese (III). A fiber-reinforced resin 101 includes a resin 1 having an ester group and a hydroxyl group, fibers 2 impregnated with at least the resin, and a complex 3 in which an organic ligand is coordinated to manganese (III).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a resin composition, a cured resin, and a fiber-reinforced resin. [Background technology]

[0002] In recent years, interest in resin compositions using dynamic covalent bonds has been growing. Dynamic covalent bonds are covalent bonds that can be reversibly dissociated and bonded by external stimuli such as heat and light, and attempts have been made to incorporate these bonds into the network structure of resins. In the cured resin obtained by curing the resin composition, the network structure changes due to the dynamic covalent bonds, so when stress such as distortion occurs in the cured resin, it is expected that the stress will be relieved and cracks will be suppressed.

[0003] By utilizing such "dynamic" covalent bonds, it becomes possible to form supramolecules and construct polymers that were previously impossible. What is particularly noteworthy is that since the bonds involved are covalent bonds, the bonds formed are much stronger than weak bonds such as hydrogen bonds found in conventional supramolecules and their polymers, and utilizing this can be an important means of constructing novel structures. The technology described in Patent Document 1 is known as a technology related to resin compositions using dynamic covalent bonds.

[0004] The technology of Patent Document 1 relates to a thermosetting resin capable of being thermally deformed and a thermosetting composite material containing the same. The composition is obtained by contacting at least one curing agent selected from an acid anhydride with at least one thermosetting resin precursor in the presence of at least one transesterification catalyst. The thermosetting resin precursor contains hydroxyl groups and / or epoxy groups, and optionally ester groups. The total molar amount of the transesterification catalyst is 5-25% of the total molar amount of hydroxyl groups and epoxy groups contained in the thermosetting precursor. The technology of Patent Document 1 also relates to a method for processing the material, a method for producing the material, and a method for recycling the material. The technology of Patent Document 1 also relates to a new solid form of the thermosetting resin and the composition used in carrying out the method. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2014-503670 (particularly the abstract) Summary of the Invention [Problem to be solved by the invention]

[0006] Patent Document 1 describes zinc acetylacetonate as a suitable transesterification catalyst (paragraph 0094). However, as described in detail below, when zinc acetylacetonate is used, the rate of bond recombination is slow, so that the time required for stress to be relaxed when stress is applied (stress relaxation time) becomes long. An object of the present disclosure is to provide a resin composition, a cured resin, and a fiber-reinforced resin that are capable of shortening the stress relaxation time. [Means for solving the problem]

[0007] The resin composition of the present disclosure includes an epoxy compound having two or more epoxy groups in the molecule, an acid anhydride, and a complex in which an organic ligand is coordinated to manganese (III). The content of the complex is 5 mol % or more and 30 mol % or less based on the epoxy group. Other solutions are described later in the description of the embodiment.

[0008] According to the present disclosure, it is possible to provide a resin composition, a cured resin, and a fiber-reinforced resin that are capable of shortening the stress relaxation time. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic diagram of a fiber reinforced resin according to the present disclosure. [Diagram 2] 1 is a graph showing stress relaxation times in Examples 1 to 6 and Comparative Examples 1 and 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, a form for carrying out the present disclosure (referred to as an embodiment) will be described with reference to the drawings as appropriate. In the following description of one embodiment, other embodiments applicable to the one embodiment will also be described as appropriate. The present disclosure is not limited to the following one embodiment, and different embodiments can be combined with each other or modified as desired without significantly impairing the effects of the present disclosure. In addition, the same symbols will be used for the same components, and duplicated descriptions will be omitted. Furthermore, parts having the same functions will be given the same names. The contents shown are merely schematic, and for convenience of illustration, the actual configuration may be changed without significantly impairing the effects of the present disclosure.

[0011] First, the relationship between the resin composition, the cured resin, and the fiber-reinforced resin of the present disclosure will be described. Hereinafter, unless otherwise specified, when simply referring to a "resin composition," a "cured resin," and a "fiber-reinforced resin," they all refer to the "resin composition of the present disclosure," the "cured resin of the present disclosure," and the "fiber-reinforced resin of the present disclosure."

[0012] The resin composition changes into a cured resin by curing. As described in detail later, a cured resin having an ester group and a hydroxyl group is obtained by reacting an epoxy compound contained in the resin composition with an acid anhydride. In this case, the amount of the epoxy group is, for example, amount The epoxy compound and the acid anhydride are used in amounts less than the theoretical ratio. The acid anhydride usually functions as a curing agent, so this reaction is a curing reaction and usually proceeds by heating. Fiber-reinforced resin is a resin cured product reinforced with fibers, and the explanation for the resin cured product can be applied in the same way, except that it contains fibers.

[0013] Although details will be described later, both the cured resin and the fiber-reinforced resin have ester groups and hydroxyl groups, and when strain occurs due to the application of stress, for example, a transesterification reaction occurs as shown in the following formula (1). Note that the structural formula shown in formula (1) is an example of a structure obtained by a transesterification reaction, and R, R', and R'' represent any chemical structure. On the left and right sides, the structure of item 1 and the structure of item 2 may exist in the same molecule or in different molecules.

[0014] [ka]

[0015] The reaction of formula (1) usually proceeds in the presence of the complex of the present disclosure, which functions as a catalyst, due to an external stimulus such as heating, and the ester bond is rearranged. A covalent bond that causes such rearrangement is called a dynamic covalent bond. By using the following materials as the ester bond, hydroxyl group, and complex of the present disclosure, and appropriately adjusting the amounts used, the transesterification reaction can proceed at a high speed even in the cured resin product after curing, and the stress relaxation time can be shortened.

[0016] The stress relaxation time in this disclosure is defined as the time required for the stress remaining in the test piece to decrease to 30% of the stress (initial stress) applied to the test piece composed of the resin cured product containing the resin and the complex. The recombination of ester bonds (reaction of formula (1)) progresses so as to relax the stress by applying stress, and the stress decreases (i.e., becomes familiar). Therefore, the stress relaxation time is used as an index to evaluate the stress relaxation effect. A specific method for measuring the stress relaxation time will be described later in the Examples.

[0017] The resin composition of the present disclosure includes an epoxy compound having two or more epoxy groups in the molecule, an acid anhydride, and a complex in which an organic ligand is coordinated to manganese (III). Among these, the epoxy group in the epoxy compound and the acid anhydride react with each other, for example, by heating, to generate an ester group and a hydroxyl group in the cured resin. The resin composition has, for example, fluidity, specifically, is, for example, a liquid, and it is preferable that the epoxy compound, the acid anhydride, and the complex are compatible and uniform. The resin composition may contain a solvent as necessary.

[0018] Examples of epoxy compounds include bisphenol A type resins, novolac resins, alicyclic resins, and glycidylamine resins. Specific examples include bisphenol A diglycidyl ether phenol, bisphenol F diglycidyl ether, bisphenol S diglycidyl ether, and rezo R Examples of the glycidyl ether include, but are not limited to, at least one of bisphenol A diglycidyl ether, hexahydrobisphenol A diglycidyl ether, polypropylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, phthalic acid diglycidyl ester, dimer acid diglycidyl ester, triglycidyl isocyanurate, tetraglycidyl diaminodiphenylmethane, tetraglycidyl metaxylenediamine, cresol novolac polyglycidyl ether, tetrabromobisphenol A diglycidyl ether, and bisphenol hexafluoroacetone diglycidyl ether. Among these, the epoxy compound is preferably bisphenol A diglycidyl ether or a novolac resin.

[0019] Examples of acid anhydrides include at least one of phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, 3-dodecenylsuccinic anhydride, octenylsuccinic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, dodecylsuccinic anhydride, chlorendic anhydride, pyromellitic anhydride, benzophenone tetracarboxylic anhydride, ethylene glycol bis(anhydrotrimate), methylcyclohexene tetracarboxylic anhydride, trimellitic anhydride, polyazelaic anhydride, and derivatives thereof, but are not limited thereto. Among these, the acid anhydride preferably includes at least one of phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, or a derivative thereof.

[0020] When the resin composition is cured, as described above, based on the amount of substance of the epoxy group, for example, the acid anhydride is chemically amount It is preferable to use the epoxy compound and the acid anhydride in amounts less than the theoretical ratio, so that during the reaction between the epoxy group and the acid anhydride, the epoxy group can react with, for example, moisture in the air to generate a hydroxyl group due to the lack of the amount of acid anhydride.

[0021] The content of the acid anhydride in the resin composition is, for example, 30 mol % or more, preferably 40 mol % or more, and the upper limit thereof is, for example, 70 mol % or more, based on the epoxy group. %、 Preferably 60 mol %in By adjusting the amount of acid anhydride to the amount described above, hydroxyl groups can be generated after polymerization, so that the reorganization of the polymer structure by dynamic covalent bonds can be efficiently performed. In particular, by adjusting the amount to 30 mol % or more, the curing can be sufficiently advanced. Also, by adjusting the amount to 70 mol % or less, the amount of hydroxyl groups generated can be increased, and the transesterification reaction can be easily advanced.

[0022] The complex of the present disclosure usually catalyzes the transesterification reaction represented by the above formula (1), and is, for example, an organometallic complex in which an organic ligand is coordinated to manganese (III) as described above. The organic ligand is a ligand containing carbon, and is bonded to manganese (III) so as to surround manganese (III). The complex of the present disclosure has high solubility in epoxy compounds and acid anhydrides, and further has high catalytic activity, compared to other catalysts that promote transesterification reactions.

[0023] For example, the inventors have studied that the same complex except for using manganese (II) instead of manganese (III) had lower solubility and catalytic activity than the complex of the present disclosure containing manganese (III). This is thought to be because the inclusion of manganese (III), a trivalent metal, increases the number of organic ligands that contribute to solubility, thereby improving solubility. In addition, manganese (III) shows catalytic activity by coordinating to the oxygen atom of an ester group, but the catalytic activity can be improved by manganese (III) having a strong coordinating power. Therefore, it is thought that these effects are not achieved in complexes containing divalent metals and complexes containing trivalent metals other than manganese (III), and the effect of shortening the stress relaxation time is not obtained. Therefore, according to the complex of the present disclosure, it is possible to add a larger amount than other catalysts at the same addition amount as other catalysts, and further, since the reaction rate of ester exchange can be improved, the stress relaxation time can be shortened by accelerating the stress relaxation.

[0024] The complex of the present disclosure is preferably one that is uniformly dispersed in at least one of the epoxy compound and the acid anhydride contained in the resin composition, and preferably in both.Specific examples include at least one of manganese(III) acetylacetonate, manganese(III) naphthenate, manganese(III) isopropoxide, manganese(III) acetate, manganese(III) di(2-ethylhexanoate), manganese(III) naphthanate, etc., but are not limited thereto. Among these, the complex preferably contains at least one of manganese(III) acetylacetonate, manganese(III) acetate, and manganese(III) naphthanate, because these are highly versatile and readily available.

[0025] The content of the complex of the present disclosure is not particularly limited, but is, for example, 5 mol % or more, preferably 10 mol % or more, more preferably 15 mol % or more, and the upper limit is, for example, 30 mol % or more, based on the epoxy groups. %、 More preferably, 25 moles %in It is preferable that the content is 5 mol % or more. At 5 mol % or more, the catalytic effect exerted by the complex can be increased. In particular, at 10 mol % or more, the amount of the complex used can be increased, and the stress relaxation time can be shortened. Furthermore, at 15 mol % or more, the amount of the complex used can be particularly increased, and the stress relaxation time can be particularly shortened. Furthermore, at 30 mol % or less, the complex can be sufficiently dissolved in at least one of the epoxy compound and the acid anhydride contained in the resin composition, and a homogeneous resin composition can be easily obtained.

[0026] In addition to the above-mentioned epoxy compound, acid anhydride and complex, the resin composition may contain additives such as curing accelerators, flame retardants, antioxidants, light stabilizers, dispersants, lubricants, plasticizers, antistatic agents, pigments and dyes, if necessary. of The resin composition may contain an inorganic filler. Examples of the inorganic filler include powders such as fused silica, crystalline silica, alumina, zircon, calcium silicate, calcium carbonate, potassium titanate, silicon carbide, aluminum nitride, boron nitride, beryllia, zircon, fosterite, stearite, spinel, mullite, and titania, as well as beads and glass fibers obtained by spheroidizing these. The shape of the inorganic filler is not limited, and any shape such as a sphere or a flake may be used.

[0027] The cured resin of the present disclosure is obtained, for example, by curing a resin composition, and includes a resin having an ester group and a hydroxyl group generated, for example, by the reaction of an epoxy group with an acid anhydride. The ester group and the hydroxyl group may be those that already existed before the reaction of the epoxy group with the acid anhydride. Furthermore, the cured resin also includes a complex in which an organic ligand is coordinated to manganese (III), for example, because a complex contained in the resin composition remains. The complex is usually dispersed in the cured resin.

[0028] When applied to a test piece formed from the cured resin (i.e., a test piece containing a resin and a complex), the stress relaxation time is, for example, 11 minutes or less. Of these, a stress relaxation time of 9 minutes or less is preferable. A stress relaxation time of 9 minutes or less can be particularly shorter than that of conventional cured resins.

[0029] The cured resin can be used in various paints, mold resins for transformers, mold sealants, and motor coils. When used as paint for moving objects such as cars and trains, scratches can be repaired by moderate heating. Heating causes an ester exchange reaction in the damaged area, allowing bonds that were once broken to recombine, repairing the damage. It can also be used in paints for building materials.

[0030] Cracks occur in molded resin materials for transformers due to distortion caused by differences in the coefficient of expansion between the resin and other components during molding. However, if the crosslink density of the resin is reduced to improve crack resistance, heat resistance is reduced. If additives such as rubber particles and fillers are used, the resin viscosity increases, making it easier for voids to occur during molding, which can lead to cracks starting from these voids and reduced electrical insulation. However, the resin cured product of the present disclosure can overcome these problems. Furthermore, if the cracks are small, they can be repaired by heating even if they occur after use.

[0031] In mold encapsulants, there is a problem with crack resistance due to the difference in expansion coefficient with other components such as metals. Methods for improving the crack resistance of resins for mold encapsulants include reducing the crosslink density of the resin and reducing the toughness value by additives such as rubber particles and fillers. However, these methods cannot suppress cracks that occur due to strain generated during use of the product after once molding. Therefore, in the resin cured product of the present disclosure, stress relaxation of the bond recombination of the transesterification reaction occurs due to heat generated during use of the product, and the strain generated between the resin and other components after molding is reduced, thereby suppressing the occurrence of cracks.

[0032] Furthermore, motor coils have the problem of cracking due to electromagnetic vibration, etc. However, in the cured resin of the present disclosure, bonds are rearranged due to heat generated during use of the motor, so that the distortion, i.e., stress, that causes cracks can be alleviated.

[0033] By applying the cured resin material of the present disclosure to these products, stress can be relaxed more quickly than with conventional cured resin materials that use the same reaction, thereby improving crack resistance and repairability.

[0034] 1 is a schematic diagram of a fiber-reinforced resin 101 of the present disclosure. The fiber-reinforced resin 101 includes a resin 1 having an ester group and a hydroxyl group, a fiber 2 impregnated with at least the resin 1, and a complex 3 in which an organic ligand is coordinated to manganese (III). The resin 1 is the same as the resin described in the cured resin product of the present disclosure, and the complex 3 is dispersed in the resin 1. Thus, the fiber 2 is impregnated with the resin 1 in which the complex 3 is dispersed.

[0035] Examples of the fiber 2 include inorganic fibers and organic fibers. , GaExamples of the fibers include lath fiber, asbestos fiber, carbon fiber, silica fiber, silica-alumina fiber, alumina fiber, zirconia fiber, potassium titanate fiber, Tyranno fiber, silicon carbide fiber, metal fiber, etc. Examples of the organic fibers include high-strength polyethylene fiber, polyacetal fiber, aliphatic or aromatic polyamide fiber, polyacrylate fiber, fluorine fiber, boron fiber, polyacrylonitrile fiber, aramid fiber, PBO (poly-p-phenylene benzobisoxazole) fiber, etc. These fibers can be used alone or in combination of two or more.

[0036] Among these, the fibers 2 preferably contain at least one of aramid fibers, glass fibers, or organic fibers (e.g., carbon fibers). By containing at least one of these, the mechanical strength of the fiber-reinforced resin 10 can be improved. Depending on the raw material, carbon fibers can be classified into synthetic polymer-derived carbon fibers (polyacrylonitrile-based, polyvinyl alcohol-based, rayon-based carbon fibers, etc.) and mineral-derived carbon fibers (pitch-based carbon fibers, etc.). Of these, synthetic polymer-derived carbon fibers are preferred from the viewpoint of mechanical strength.

[0037] The fibers 2 are used in the form of continuous fibers, long fibers, short fibers, chopped fibers, etc., and in the form of unidirectional materials, plain weaves, non-woven fabrics, etc. They may also be directly added to the resin 1, but the present embodiment is not limited to these fiber shapes and fiber states.

[0038] In the fiber reinforced resin 101, a reversible dissociable transesterification reaction occurs in the resin 1. As a result, the stress generated during curing and use is alleviated, and cracks and peeling are suppressed. In addition, in the fiber reinforced resin 101, the transesterification reaction proceeds by applying an external stimulus such as increasing the temperature, and secondary processing, reprocessing, repair, etc. can be performed. For example, the fiber reinforced resin 101 can be molded into the shape of a mold by pressing it while applying heat using a heat press machine. Furthermore, since the fiber reinforced resin 101 has a higher stress relaxation speed than conventional resins, it can be molded into shapes that were not possible to mold in the past or can be molded at high speed.

[0039] The fiber reinforced resin 101 can be used for vehicle parts as well as parts and bodies used in various fields, such as railroad cars, ships, airplanes, unit baths, septic tanks, printed circuit boards, playground equipment, skis, etc. EXAMPLES

[0040] The present disclosure will be described more specifically below with reference to examples, but the present disclosure is not limited to the following examples.

[0041] <Example 1> The following materials were prepared: Epoxy compounds having two or more epoxy groups in the molecule: Bisphenol A diglycidyl ether (Mitsubishi Chemical Corporation jER828 epoxy resin) Acid anhydride: Methyl-3,6-endo-methylene-1,2,3,6-tetrahydrophthalic anhydride (a derivative of tetrahydrophthalic anhydride, MHAC-P hardener manufactured by Showa Denko Materials (formerly Hitachi Chemical Co., Ltd.)) Manganese(III) complexes with organic ligands: Manganese(III) acetylacetonate (Tokyo Chemical Industry Co., Ltd.) Curing Accelerator: Imidazole-based epoxy resin hardener (2E4MZ-CN, manufactured by Shikoku Kasei Co., Ltd.)

[0042] To 100 parts by mass of the epoxy compound, 47 parts by mass of the acid anhydride (50 mol% relative to the epoxy group), 19 parts by mass of the complex (10 mol% relative to the epoxy group), and 0.3 parts by mass of the curing accelerator were added, and the mixture was stirred and mixed in the air to obtain a resin composition. In the resin composition, the epoxy compound, the acid anhydride, and the complex were compatible with each other, and the resin composition was a viscous liquid. The obtained resin composition was cured by heating at 100°C for 1 hour and at 200°C for 1 hour to obtain a cured resin.

[0043] The stress relaxation time of the prepared cured resin was evaluated by a tensile stress relaxation test using a thermomechanical analyzer. A test piece measuring 10 mm in length, 5 mm in width, and 0.5 mm in thickness was prepared using the obtained cured resin. Using a thermomechanical analyzer at a temperature of 220°C, the test piece was pulled so that it was elongated by 5%. The stress (initial stress) at 5% elongation was set to 100%, and the time it took for the stress to decrease to 30% was used as an index of the stress relaxation time. The measured stress relaxation time was 9 minutes.

[0044] <Example 2> The stress relaxation time was measured in the same manner as in Example 1 except that the amount of the complex used was changed to 27 parts by mass (15 mol % relative to the epoxy groups). The stress relaxation time was 7 minutes.

[0045] <Example 3> The stress relaxation time was measured in the same manner as in Example 1 except that the amount of the complex used was changed to 38 parts by mass (20 mol % relative to the epoxy groups). The stress relaxation time was 5 minutes.

[0046] <Example 4> The stress relaxation time was measured in the same manner as in Example 1 except that the amount of the complex used was changed to 46 parts by mass (25 mol % relative to the epoxy groups). The stress relaxation time was 6 minutes.

[0047] <Example 5> The stress relaxation time was measured in the same manner as in Example 1 except that the amount of the complex used was changed to 57 parts by mass (30 mol % relative to the epoxy groups). The stress relaxation time was 6 minutes.

[0048] <Example 6> The stress relaxation time was measured in the same manner as in Example 1 except that the amount of the complex used was changed to 14 parts by mass (7.5 mol % relative to the epoxy groups). The stress relaxation time was 11 minutes.

[0049] <Comparative Example 1> The stress relaxation time was measured in the same manner as in Example 1, except that the amount and type of the complex used was changed to 14 parts by mass of zinc(II) acetylacetonate (manufactured by Tokyo Chemical Industry Co., Ltd.) (however, the amount used relative to the epoxy group was the same as in Example 1). The stress relaxation time was 13 minutes.

[0050] <Comparative Example 2> The stress relaxation time was measured in the same manner as in Example 3, except that the amount and type of the complex used was changed to 28 parts by mass of zinc(II) acetylacetonate (manufactured by Tokyo Chemical Industry Co., Ltd.) (however, the amount used relative to the epoxy group was the same as in Example 3). The stress relaxation time was 10 minutes.

[0051] <Comparative Example 3> A resin composition was prepared in the same manner as in Example 4, except that the amount and type of the complex used was changed to 35 parts by mass of zinc (II) acetylacetonate (manufactured by Tokyo Chemical Industry Co., Ltd.) (however, the amount used relative to the epoxy group was the same as in Example 4). During preparation, the complex was not dissolved or dispersed in the resin composition. Furthermore, the prepared resin composition did not harden even when heated as in Example 4, and a resin cured product was not obtained, so the stress relaxation time could not be measured.

[0052] <Consideration> Table 1 is a table showing the stress relaxation times of Examples 1 to 6 and Comparative Examples 1 and 2. Fig. 2 is a graph showing the stress relaxation times of Examples 1 to 6 and Comparative Examples 1 and 2. For reference, Comparative Example 3, in which the stress relaxation time could not be measured, is also shown. In Fig. 2, the solid lines show the stress relaxation times of Examples 1 to 6, and the dashed lines show the stress relaxation times of Comparative Examples 1 and 2.

[0053] [Table 1]

[0054] As shown in FIG. 2, in Examples 1 to 6 in which the complex (transesterification catalyst) of the present disclosure was used, the stress relaxation time was shortened overall compared to Comparative Examples 1 and 2 in which a conventional catalyst was used. For example, by setting the content of the complex to 5 mol % or more and 30 mol % or less with respect to the epoxy group, the complex could be dissolved in the resin composition and the stress relaxation time could be shortened. In addition, compared to Example 1 and Comparative Example 1 in which the type of complex was different but the amount used was the same at 10 mol %, the use of the complex of the present disclosure allowed the stress relaxation time to be shortened by approximately 30%, from 13 minutes to 9 minutes. In addition, compared to Example 3 and Comparative Example 2 in which the type of complex was different but the amount used was the same at 20 mol %, the use of the complex of the present disclosure allowed the stress relaxation time to be halved, from 10 minutes to 5 minutes.

[0055] In Comparative Example 3, zinc (II) acetylacetonate did not dissolve, so the upper limit of the amount used is thought to be about 20 mol % when zinc (II) acetylacetonate is used. Since the stress relaxation time increases as the amount used decreases, the stress relaxation time when zinc (II) acetylacetonate is used is estimated to be at least about 10 minutes.

[0056] On the other hand, by setting the content of the complex of the present disclosure to 10 mol % or more and 30 mol % or less relative to the epoxy group, the stress relaxation time can be reduced to 9 minutes (Example 1) or less, which is shorter than the shortest stress relaxation time of about 10 minutes when a conventional catalyst is used. In particular, by setting the content of the complex to 15 mol % or more and 30 mol % or less relative to the epoxy group, the stress relaxation time can be reduced to 5 to 7 minutes, which is particularly short.

[0057] As described above, it has been found that the use of a complex in which an organic ligand is coordinated to manganese(III) can shorten the stress relaxation time, and in particular, by adjusting the amount used, the stress relaxation time can be reduced by up to half compared to the conventional case. Therefore, according to the present disclosure, it is possible to provide a resin composition, a cured resin, and a fiber-reinforced resin that can shorten the stress relaxation time. [Explanation of symbols]

[0058] 1 Resin 2. Fiber 3 Complex 101 Fiber reinforced resin

Claims

1. an epoxy compound having two or more epoxy groups in the molecule; An acid anhydride, A complex in which an organic ligand is coordinated to manganese (III), The content of the complex is 5 mol % or more and 30 mol % or less based on the epoxy group. A resin composition comprising:

2. The complexes include at least one of manganese(III) acetylacetonate, manganese(III) acetate, or manganese(III) naphthanate. The resin composition according to claim 1 .

3. The content of the complex is 10 mol % or more and 30 mol % or less based on the epoxy group. The resin composition according to claim 1 .

4. The content of the complex is 15 mol % or more and 30 mol % or less based on the epoxy group. The resin composition according to claim 2 .

5. The epoxy compound is bisphenol A diglycidyl ether or a novolac resin. The resin composition according to claim 1 or 2.

6. The acid anhydride includes at least one of phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, or derivatives thereof. The resin composition according to claim 1 .

7. An epoxy compound having two or more epoxy groups in the molecule; An acid anhydride, A complex in which an organic ligand is coordinated to manganese (III), The content of the acid anhydride is 30 mol % or more and 70 mol % or less based on the epoxy group. A resin composition comprising:

8. A cured product of the resin composition according to claim 1 or 7. A cured resin product characterized by the above.

9. When a test piece formed from the cured product and having a length of 10 mm, a width of 5 mm, and a thickness of 0.5 mm is applied with a tensile stress so as to cause an elongation of 5% at a temperature of 220°C, the time required for the residual stress in the test piece to decrease to 30% of the applied stress is defined as the stress relaxation time, The stress relaxation time is 11 minutes or less. The cured resin according to claim 8 .

10. The stress relaxation time is 9 minutes or less. The cured resin according to claim 9 .

11. A cured product of the resin composition according to claim 1 or 7, and a fiber impregnated with the resin in the cured product. A fiber reinforced resin characterized by:

12. The fibers include at least one of aramid fibers, glass fibers, or carbon fibers. The fiber reinforced resin according to claim 11.

Citation Information

Patent Citations

  • Solventless type resin compound of high fluidity

    JP1978115800A

  • Curable epoxy resin composition

    JP1979046299A

  • Epoxy resin composition for fiber reinforced composite material, prepreg and fiber reinforced composite material

    JP1997025393A

  • Preparation of agent composition for curing epoxy

    JP1999021334A

  • Epoxy resin composition

    JP2006321899A