Method for cleaning a polyamic acid production system

By adjusting the reaction ratio of polyadditionable compounds in polyamic acid production, the method addresses cleaning inefficiencies, facilitating the removal of high-viscosity solutions and enhancing equipment cleanliness.

JP7570916B2Active Publication Date: 2024-10-22KANEKA CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020217020
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-25
Publication Date
2024-10-22
Estimated Expiration
2040-12-25

AI Technical Summary

Technical Problem

High viscosity polyamic acid solutions are difficult to clean from equipment due to large viscosity differences with solvents, leading to inefficiencies and potential product quality issues, especially in static mixers without driving parts.

Method used

A method involving the use of first and second polyadditionable polymerizable compounds dissolved in solvents to create a mixed solution, adjusting the reaction ratio to lower viscosity, allowing for efficient cleaning by replacing high-viscosity solutions with low-viscosity ones.

Benefits of technology

Improves cleaning efficiency of piping and static mixers by reducing viscosity through controlled reaction ratios, enabling effective removal of high-viscosity polyamic acid solutions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570916000001
    Figure 0007570916000001
Patent Text Reader

Abstract

To provide a cleaning method for improving working efficiency for cleaning a pipe having no driving part and a static mixer in a continuous polyamic acid production system.SOLUTION: A method for cleaning a polyamic acid production system includes lowering viscosity of a polymerization solution by changing a reaction ratio of a first polymerizable compound to a second polymerizable compound so that the reaction ratio of the first polymerizable compound to the second polymerizable compound is farther from 1:1 than the reaction ratio of the first polymerizable compound to the second polymerizable compound when a high viscosity polymerization solution is obtained, in the case where a desired polyamic acid produced in a continuous polyamic acid production system is converted into the high viscosity polymerization solution, and obtaining a low viscosity polymerization solution; and substituting the high viscosity polymerization solution with the low viscosity polymerization solution.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a polyamic acid. [Background technology]

[0002] When a resin composition such as a liquid resin or a resin solution has high viscosity and low miscibility with a solvent, the resin composition adhering to the wall surface cannot be removed unless a large amount of solvent is flowed at a high flow rate, which causes problems such as the generation of a large amount of waste. Once the solvent is flowed, the resin composition and the solvent are mixed by leaving it to stand, and the viscosity is reduced, making it easier to remove, but in this case there is a problem that the work efficiency is low.

[0003] In order to solve the above problem, a separate circulation line for cleaning may be installed, but this may result in a complicated device configuration or a large amount of cleaning solution being required. In addition, if the kneading device has a drive unit such as a screw, it is possible to prepare resin compositions with different viscosities separately and wash them one by one, but this may result in the subsequent resin composition that will become the product being mixed with the washing resin composition remaining in the device, causing a deterioration in the quality of the product resin composition (Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent Publication No. 2018-43219 Summary of the Invention [Problem to be solved by the invention]

[0005] In the production process of high-viscosity polyamic acid, there is a large difference in viscosity between the high-viscosity polyamic acid solution and the solvent, and therefore, there is a problem similar to that in the above-mentioned technical background in that the resin composition adhering to the wall surface cannot be removed unless a large amount of solvent is flowed at a high flow rate. In particular, when a static mixer is installed in the process, there is a problem in that cleaning is particularly difficult because the elements inside the static mixer do not move.

[0006] An object of the present invention is to provide a cleaning method that improves the efficiency of cleaning pipes and static mixers that have no moving parts inside their flow paths in a continuous polyamic acid production system. [Means for solving the problem]

[0007] The present inventors have conducted extensive research to solve the above problems and have completed the present invention.

[0008] [1] A method for cleaning a polyamic acid production system for producing polyamic acid using a first solution in which a first polymerizable compound having a polyaddition property is dissolved and a second solution in which a second polymerizable compound having a polyaddition property that undergoes polyaddition with the first polymerizable compound is dissolved as raw materials, comprising: The system A first supply unit that supplies the first solution; A second supply unit that supplies the second solution; a first mixing section that mixes the first solution and the second solution to generate a first mixed solution; a reaction section that stirs the first mixed solution without contacting it with a gas, and causes a polymerization reaction between the first polymerizable compound and the second polymerizable compound to proceed, thereby producing a polymerization solution in which polyamic acid is dissolved, A method for cleaning a polyamic acid production system, characterized in that, when a desired polyamic acid produced in a polyamic acid production system is a high-viscosity polymerization solution, a reaction ratio of the first polymerizable compound to the second polymerizable compound is changed so that the reaction ratio of the first polymerizable compound to the second polymerizable compound is made farther from 1:1 than the reaction ratio of the first polymerizable compound to the second polymerizable compound when the high-viscosity polymerization solution is obtained, thereby reducing the viscosity of the polymerization solution to obtain a low-viscosity polymerization solution, and the high-viscosity polymerization solution is replaced with the low-viscosity polymerization solution.

[0009] [2] The method for cleaning a polyamic acid production system according to [1], further comprising finally replacing the inside of the piping with only the solvent. Effect of the Invention

[0010] INDUSTRIAL APPLICABILITY The present invention makes it possible to improve the efficiency of cleaning of piping having no moving parts and static mixers in a continuous polyamic acid production system. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 illustrates a continuous polyamic acid production system. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention relates to a method for cleaning a polyamic acid production system for producing a polyamic acid using a first solution in which a first polymerizable compound having a polyaddition property is dissolved and a second solution in which a second polymerizable compound having a polyaddition property that undergoes polyaddition with the first polymerizable compound is dissolved as raw materials, the system comprising: A first supply unit that supplies the first solution; A second supply unit that supplies the second solution; a first mixing section that mixes the first solution and the second solution to generate a first mixed solution; a reaction section that stirs the first mixed solution without contacting it with a gas, and causes a polymerization reaction between the first polymerizable compound and the second polymerizable compound to proceed, thereby producing a polymerization solution in which polyamic acid is dissolved, The method for cleaning a polyamic acid production system is characterized in that, when a desired polyamic acid produced in a polyamic acid production system is a high-viscosity polymerization solution, the viscosity of the polymerization solution is reduced to obtain a low-viscosity polymerization solution by changing the reaction ratio of the first polymerizable compound to the second polymerizable compound so that the reaction ratio of the first polymerizable compound to the second polymerizable compound is made farther from 1:1 than the reaction ratio of the first polymerizable compound to the second polymerizable compound when the high-viscosity polymerization solution is obtained, and the high-viscosity polymerization solution is replaced with the low-viscosity polymerization solution.

[0013] An outline of a continuous polyamic acid production system will be described with reference to Figure 1. The polyamic acid production system is a system for producing polyamic acid using as raw materials a first solution A1 in which a first polymerizable compound having polyaddition properties is dissolved, and a second solution A2 in which a second polymerizable compound having polyaddition properties that undergoes polyaddition with the first polymerizable compound is dissolved.

[0014] In the following, as an example, a case where one of the first polymerizable compound and the second polymerizable compound is a tetracarboxylic dianhydride and the other is a diamine will be described. More specifically, a case where the first polymerizable compound contained in the first solution A1 is a tetracarboxylic dianhydride and the second polymerizable compound contained in the second solution A2 is a diamine will be described.

[0015] The tetracarboxylic dianhydride is not particularly limited, and the same one as that used in conventional polyimide synthesis can be used. Specific examples of the tetracarboxylic dianhydride include 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenyl tetracarboxylic dianhydride, 2,3,3',4'-biphenyl tetracarboxylic dianhydride, pyromellitic dianhydride, 1,3-bis(2,3-dicarboxyphenoxy)benzene dianhydride, 1,4-bis(2,3-dicarboxyphenoxy)benzene dianhydride, 2,3,3',4'-benzophenone tetracarboxylic dianhydride, 2,2',3,3'-benzophenone tetracarboxylic dianhydride, 2,2',3,3'-biphenyl tetracarboxylic dianhydride, 2,2',6,6'-biphenyl tetracarboxylic dianhydride, naphthalene-1,2,4, Examples of the tetracarboxylic acid dianhydride include aromatic tetracarboxylic acid dianhydrides such as 5-tetracarboxylic acid dianhydride, anthracene-2,3,6,7-tetracarboxylic acid dianhydride, phenanthrene-1,8,9,10-tetracarboxylic acid dianhydride, and 2,2-bis(4-hydroxyphenyl)propane dibenzoate-3,3',4,4'-tetracarboxylic acid dianhydride; aliphatic tetracarboxylic acid dianhydride such as butane-1,2,3,4-tetracarboxylic acid dianhydride; alicyclic tetracarboxylic acid dianhydride such as cyclobutane-1,2,3,4-tetracarboxylic acid dianhydride; heterocyclic tetracarboxylic acid dianhydride such as thiophene-2,3,4,5-tetracarboxylic acid dianhydride and pyridine-2,3,5,6-tetracarboxylic acid dianhydride; and the like. The tetracarboxylic acid dianhydride may be used alone or in combination of two or more kinds.

[0016] As the solvent of the first solution A1, one in which tetracarboxylic dianhydride and polyamic acid are dissolved is used. Specific examples of the solvent include amide-based solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, and acetanilide; cyclic ester-based solvents such as γ-butyrolactone; chain ester-based solvents such as ethyl acetate; ketone-based solvents such as 2-propanone, 3-pentanone, acetone, and methyl ethyl ketone; ether-based solvents such as tetrahydrofuran and dioxolane; alcohol-based solvents such as methanol, ethanol, and isopropanol; and aromatic hydrocarbon-based solvents such as toluene and xylene. Among these, amide-based solvents, cyclic ester-based solvents, and ether-based solvents in which polyamic acid is highly soluble are preferred. The solvent may be used alone or in a mixture of two or more. For example, it is possible to improve the solubility of polyamic acid by mixing a highly polar alcoholic solvent with a solvent in which polyamic acid has a relatively low solubility, such as acetone, ethyl acetate, methyl ethyl ketone, toluene, or xylene.

[0017] The first solution A1 may contain a small amount of a tertiary amine such as trimethylamine or triethylamine in order to increase the solubility of the tetracarboxylic dianhydride or to increase the reactivity with the diamine. The diamine is not particularly limited, and the same one as that used in conventional polyimide synthesis can be used. Specific examples of the diamine include 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylether, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-bis(4-aminophenoxy)biphenyl, 1,4'-bis(4-aminophenoxy)benzene, 1,3'-bis(4-aminophenoxy)benzene, o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 3,4'-diaminodiphenylether, 4,4'-diaminodiphenylsulfone, 3,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, 4,4'-methylene-bis(2-chloroaniline), 3,3'-dimethyl-4,4'-diaminobiphenyl, 4,4'- Examples of the diamine include aromatic diamines such as diaminodiphenyl sulfide, 2,6-diaminotoluene, 2,4-diaminochlorobenzene, 1,2-diaminoanthraquinone, 1,4-diaminoanthraquinone, 3,3'-diaminobenzophenone, 3,4'-diaminobenzophenone, 4,4'-diaminobenzophenone, and 4,4'-diaminobibenzyl; aliphatic diamines such as 1,2-diaminoethane, 1,4-diaminobutane, tetramethylenediamine, and 1,10-diaminododecane; alicyclic diamines such as 1,4-diaminocyclohexane, 1,2-diaminocyclohexane, bis(4-aminocyclohexyl)methane, and 4,4'-diaminodicyclohexylmethane; and heterocyclic diamines such as 3,4-diaminopyridine. The diamines may be used alone or in combination of two or more.

[0018] As the solvent of the second solution A2, a solvent capable of dissolving diamine and polyamic acid is used. Specific examples of the solvent include amide-based solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, and acetanilide; cyclic ester-based solvents such as γ-butyrolactone; chain ester-based solvents such as ethyl acetate; ketone-based solvents such as 2-propanone, 3-pentanone, acetone, and methyl ethyl ketone; ether-based solvents such as tetrahydrofuran and dioxolane; alcohol-based solvents such as methanol, ethanol, and isopropanol; and aromatic hydrocarbon-based solvents such as toluene and xylene. Among these, amide-based solvents, cyclic ester-based solvents, and ether-based solvents, which have high solubility of polyamic acid, are preferred. The solvent may be used alone or in a mixture of two or more. For example, it is possible to improve the solubility of polyamic acid by mixing a highly polar alcoholic solvent with a solvent in which polyamic acid has a relatively low solubility, such as acetone, ethyl acetate, methyl ethyl ketone, toluene, or xylene.

[0019] As shown in FIG. 1, the polyamic acid production system is configured to produce polyamic acid by mixing raw materials, a first solution A1 and a second solution A2, in a first mixing section 20 to produce a first mixed solution B, and then causing a polymerization reaction in a reaction section 30 to produce a polymerization solution C.

[0020] Next, a specific configuration of the polyamic acid production system will be described. 1, the polyamic acid production system includes a first tank 11, a second tank 12, a first supply pump 15 (first supply section), a second supply pump 16 (second supply section), a mixing section 20, a reaction section 30, and a liquid delivery line L. The above-mentioned liquid delivery line L has a first liquid delivery section L1, a second liquid delivery section L2, and a third liquid delivery section L3.

[0021] The first tank 11 contains a first solution A1 in which a first polymerizable compound having polyaddition properties is dissolved. In this embodiment, the first tank 11 contains a first solution A1 in which a tetracarboxylic dianhydride is dissolved. The first solution A1 contained in the first tank 11 is supplied to the first mixing section 20 via a first liquid supply section L1.

[0022] The second tank 12 contains a second solution A2 in which a second polymerizable compound capable of polyaddition with the first polymerizable compound is dissolved. In this embodiment, the second tank 12 contains a second solution A2 in which a diamine is dissolved. The second solution A2 contained in the second tank 12 is supplied to the first mixing section 20 via the second liquid supply section L2.

[0023] The first supply pump 15 (first supply section) supplies the first solution A1 contained in the first tank 11 to the first mixing section 20. The first supply pump 15 supplies the first solution A1 at a predetermined delivery rate. For example, the first supply pump 15 is adjusted so as to supply the first solution A1 under conditions that allow polyamic acid with desired properties to be obtained.

[0024] The second supply pump 16 (second supply section) supplies the second solution A2 contained in the second tank 12 to the first mixing section 20. The second supply pump 16 supplies the second solution A2 at a predetermined delivery rate. For example, the second supply pump 16 is adjusted so as to supply the second solution A2 under conditions that allow polyamic acid with desired properties to be obtained.

[0025] The first mixing section 20 is disposed downstream of the first supply pump 15 and the second supply pump 16. The first mixing section 20 mixes the first solution A1 and the second solution A2 to generate a first mixed solution B. The first mixing section 20 is configured with a confluence valve that merges the first solution A1 supplied by the first supply pump 15 and the second solution A2 supplied by the second supply pump 16.

[0026] The first reaction section 30 is a section for promoting a polymerization reaction between the first polymerizable compound and the second polymerizable compound contained in the first mixed solution B. In the reaction section 30, the polymerization reaction between the first polymerizable compound and the second polymerizable compound contained in the mixed solution B gradually progresses, and a polymerization solution C is obtained.

[0027] The reaction section 30 is composed of a double pipe extending in a predetermined direction, and has a reaction stirring section 31 arranged on the inside in the radial direction and a reaction temperature control section 32 arranged on the outside in the radial direction. The reaction section 30 is formed so that the mixed solution B flows therethrough for a desired residence time.

[0028] The reaction stirring unit 31 stirs the mixed solution B obtained by mixing the first solution A1 and the second solution A2 without contacting the gas. In this embodiment, the reaction stirring unit 31 stirs the mixed solution B, the temperature of which has been adjusted to a temperature suitable for the polymerization reaction by the reaction temperature adjustment unit 32, without contacting the gas.

[0029] The reaction stirring section 31 is configured to include, for example, a static mixer such as a static mixer, a nozzle, or an orifice, or a driven mixer such as a centrifugal pump, a volute pump, or an in-line mixer having a stirring blade, preferably includes a static mixer, and more preferably includes a static mixer.

[0030] The static mixer is not particularly limited, and examples thereof include static mixers such as Kenics mixer type, Sulzer SMV type, Sulzer SMX type, Tray Hi-mixer type, Komax mixer type, Lightnin mixer type, Ross ISG type, Bran & Lube mixer type, etc. Among these, the Kenics mixer type static mixer is more preferable because it has a simple structure and therefore has no dead space.

[0031] As described above, the case where one of the first polymerizable compound and the second polymerizable compound is a tetracarboxylic dianhydride and the other is a diamine has been described, but the present invention is not limited thereto. For example, one of the first polymerizable compound and the second polymerizable compound may be a polyamic acid (prepolymer) having an acid anhydride group terminal or an amino group terminal, and the other may be a diamine or a tetracarboxylic dianhydride. In this case, when one of the first polymerizable compound and the second polymerizable compound is a polyamic acid having an acid anhydride group terminal, the other is a diamine. Also, when one of the first polymerizable compound and the second polymerizable compound is a polyamic acid having an amino group terminal, the other is a tetracarboxylic dianhydride.

[0032] 1, after the polymerization reaction of the polyamic acid solution is carried out, a high-viscosity polyamic acid solution exists in the reaction section 30 and the liquid feed line L3. When removing the high-viscosity polyamic acid solution from the reaction section and the liquid feed line L3, a polyamic acid solution having a lower viscosity is polymerized in the reaction section and fed to replace the high-viscosity polyamic acid in the reaction section and the liquid feed line L3, thereby enabling efficient cleaning.

[0033] As described above, the polyamic acid is obtained by the reaction of the first polymerizable compound with the second polymerizable compound, and the closer the reaction ratio (equivalent ratio) of the first polymerizable compound to the second polymerizable compound is to 1:1, the higher the molecular weight of the resulting product. When the desired polyamic acid produced in the polyamic acid production system is a high-viscosity polymerization solution, the reaction ratio of the first polymerizable compound to the second polymerizable compound is changed so that the reaction ratio of the first polymerizable compound to the second polymerizable compound is farther from 1:1 than the reaction ratio of the first polymerizable compound to the second polymerizable compound when the high-viscosity polymerization solution is obtained, thereby lowering the viscosity of the polymerization solution to obtain a low-viscosity polymerization solution, and the high-viscosity polymerization solution can be replaced with the low-viscosity polymerization solution, allowing for easy and efficient cleaning. Hereinafter, the low-viscosity polyamic acid solution for replacing the high-viscosity polymerization solution is referred to as the low-viscosity polymerization solution. In addition, the "viscosity" in this specification is measured by an E-type viscometer at a temperature of 23°C and a shear rate of 0.38 s -1The values ​​were measured under the following conditions.

[0034] A low-viscosity polymerization solution has a lower viscosity than a high-viscosity polymerization solution, and the viscosity of the polymerization solution can be easily reduced by changing the reaction ratio of the first polymerizable compound to the second polymerizable compound so that the reaction ratio of the first polymerizable compound to the second polymerizable compound is away from 1:1. For example, when the reaction ratio of the high-viscosity polymerization solution is the first polymerizable compound:the second polymerizable compound=1:1, the viscosity of the low-viscosity polymerization solution may be reduced stepwise by changing the reaction ratio stepwise to 1:0.95, 1:0.9, 1:0.8, 1:0.5, 1:0 (away from 1:1), or the viscosity may be continuously changed from 1:1 to 1:0. Although the method of reducing the amount of the second polymerizable compound has been exemplified, the same applies if the first polymerizable compound is reduced. Usually, the reaction ratio of the first polymerizable compound to the second polymerizable compound may not be 1:1, and it is preferable to reduce the compound with a lower reaction ratio, since this tends to synthesize a low-viscosity polymerization solution stably.

[0035] When the viscosity is reduced stepwise, it is preferable to feed the low-viscosity polymerization solution while reducing the viscosity by 200 to 1000 poise.

[0036] The viscosity of the low-viscosity polymerization solution is adjusted by reducing the supply amount of the first or second polymerizable compound to polymerize a polyamic acid solution having a lower viscosity than the high-viscosity polymerization solution or low-viscosity polymerization solution that had been polymerized up until that point.

[0037] After replacing the high-viscosity polyamic acid in the reaction section and the liquid feed line L3 with the low-viscosity polymerization solution, the supply of the second polymerizable compound is stopped, and only the first polymerizable compound is fed, so that the cleaning polyamic acid in the first reaction section and the liquid feed line L is replaced and removed with the first polymerizable compound. After the replacement with the first polymerizable compound, the solvent used for the first solution A1 and the second solution A2 is poured into the first tank 11 and the second tank 12, and the solvent is fed to the reaction section and the liquid feed lines L1 to L3, so that the first polymerizable compound and the second polymerizable compound can be replaced and removed with the solvent. In addition, if the solvent is poured from the mixing section toward the reaction section, the reaction section and subsequent sections can be washed. EXAMPLES

[0038] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these.

[0039] Example 1 In a continuous polyamic acid production system, pyromellitic acid and diaminodiphenyl ether were reacted in a molar ratio of 3:4 in an N,N-dimethylformamide (hereinafter abbreviated as DMF) solution to prepare an acid-terminated polyamic acid solution (first solution A1). The viscosity of this acid-terminated polyamic acid solution was 15 poise. A DMF solution of p-phenylenediamine was also prepared and used as second solution A2. First solution A1 and second solution A2 were sent to the reaction section and reacted in a Kenics mixer type static mixer (inner diameter 8 mm, length 335 mm) to obtain a polyamic acid solution of 1870 poise. (Note that the viscosity is the viscosity at 23°C measured with an E-type viscometer, and the viscosity of the polyamic acid solution is the viscosity at the point where it comes out of the static mixer.) The piping corresponding to L1 to L3 in FIG. 1 was a cylindrical pipe having a diameter of 8 mm.

[0040] From a state in which the static mixer and piping were filled with 1870 poise polyamic acid solution, the supply amount of the second solution was gradually reduced, and approximately 25 ml of 1030 poise cleaning polyamic acid solution was fed, approximately 25 ml of 705 poise cleaning polyamic acid solution was fed, approximately 25 ml of 280 poise cleaning polyamic acid solution was fed, the supply amount of the second solution was stopped, approximately 25 ml of only the 15 poise first solution A1 (acid-terminated polyamic acid solution) was fed, and finally approximately 125 ml of DMF was fed. Observation of the inside of the static mixer revealed that the mixture had been completely replaced with DMF, with no polyamic acid solution remaining.

[0041] Comparative Example 1 Using the same method as in the example, the static mixer and the piping were filled with a 1870 poise polyamic acid solution. 250 ml of DMF was sent from the mixing section toward the static mixer to wash it. When the inside of the static mixer was observed, it was found that the polyamic acid solution remained inside the static mixer. Under conditions where the viscosity difference between the high-viscosity polyamic acid and DMF was large, the high-viscosity polyamic acid in the static mixer could not be completely removed. [Explanation of symbols]

[0042] 1. Polyamic acid production system 11 First Tank 12 Second Tank 15 First supply pump (first supply section) 16 Second supply pump (second supply section) 20 Mixing section 30 Reaction section A1 First solution A2 2nd solution B mixed solution C Polymerization solution L Liquid delivery line

Claims

1. 1. A method for cleaning a polyamic acid production system for producing a polyamic acid using as raw materials a first solution in which a first polymerizable compound having a polyaddition property is dissolved and a second solution in which a second polymerizable compound having a polyaddition property that undergoes polyaddition with the first polymerizable compound is dissolved, the method comprising the steps of: The system comprises: A first supply unit that supplies the first solution; A second supply unit that supplies the second solution; a first mixing section that mixes the first solution and the second solution to generate a first mixed solution; a first reaction section for stirring the first mixed solution without contacting it with a gas, to cause a polymerization reaction between the first polymerizable compound and the second polymerizable compound to proceed, and to generate a first polymerization solution in which a polyamic acid is dissolved, The polyamic acid production system includes a static mixer in the first reaction section, A method for cleaning a polyamic acid production system, characterized in that, when a desired polyamic acid produced in a polyamic acid production system is a high-viscosity polymerization solution, a reaction ratio of the first polymerizable compound to the second polymerizable compound is changed so that the reaction ratio of the first polymerizable compound to the second polymerizable compound is made farther from 1:1 than the reaction ratio of the first polymerizable compound to the second polymerizable compound when the high-viscosity polymerization solution is obtained, thereby reducing the viscosity of the polymerization solution to obtain a low-viscosity polymerization solution, and the high-viscosity polymerization solution is replaced with the low-viscosity polymerization solution.

2. Further, the supply of the second polymerizable compound is stopped, and the inside of the pipe is replaced with only the first polymerizable compound, 2. The method for cleaning a polyamic acid production system according to claim 1, wherein the inside of the piping is finally replaced with only the solvent.

Citation Information

Patent Citations

  • Production of polyimide block copolymer and its solution composition

    JP1995157560A

  • Method for cleaning paint pipeline and cleaning liquid

    JP2006167514A

  • Process for producing polycarbonate resin

    JP2008150509A

  • Nozzle cleaning method, and coating device

    JP2018043219A

  • System and method for manufacturing polyamic acid, and system and method for manufacturing polyimide

    WO2019167655A1