Polymerization method for the synthesis of vinyl aromatic polymers with controlled architecture

ARGET-ATRP synthesizes vinyl aromatic polymers with controlled linear, branched, or crosslinked structures by adjusting reaction conditions, addressing the inefficiencies of existing methods and reducing costs.

JP7570923B2Active Publication Date: 2024-10-22VERSALIS SPA
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020562186
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-05-09
Filing Date
2019-05-08
Publication Date
2024-10-22
Estimated Expiration
2039-05-08

AI Technical Summary

Technical Problem

Existing methods for synthesizing vinyl aromatic polymers struggle to control the arrangement of monomers in the chain, leading to the formation of branched or crosslinked structures that require polyfunctional initiators, polyvinyl monomers, or inimers, which are costly and inefficient.

Method used

The use of Atom Transfer Radical Polymerization (ATRP) with an activator that regenerates by electron transfer (ARGET-ATRP) to synthesize vinyl aromatic polymers, controlling the arrangement of monomers through adjustments in reaction temperature and components without polyfunctional initiators or polyvinyl monomers, allowing for the production of linear, branched, or crosslinked structures with reactive functional groups.

Benefits of technology

This method enables the production of vinyl aromatic polymers with controlled structures at reduced costs by minimizing the use of complex catalysts and other components, offering flexibility in structure formation and functionality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570923000001
    Figure 0007570923000001
  • Figure 0007570923000002
    Figure 0007570923000002
  • Figure 0007570923000003
    Figure 0007570923000003
Patent Text Reader

Abstract

The present invention relates to a polymerization method for synthesizing vinyl aromatic polymers with controlled chain sequence and reactive or polar functional groups in linear, branched, soluble, or crosslinked insoluble structures. The method comprises the step of polymerizing vinyl aromatic monomers by electron transfer regenerating activator (ARGET)-mediated atom transfer radical polymerization (ATRP), the reaction being carried out at a temperature between 25°C and 110°C in an inert gas atmosphere in the presence of a complex catalyst comprising a cupric halide and a polydentate amine ligand, and the reaction is provided with an organic initiator having two geminal halogens, an alkali metal (bi)carbonate, a solvent pair consisting of an aliphatic alcohol and an acetate ester of the aliphatic alcohol, and optionally ascorbic acid, with the proviso that no initiators having three or more active halogens, or polyvinyl monomers or inimers, are used. [Selection diagram] None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for the synthesis of vinyl aromatic polymers with control over the sequence of monomers in the chain and linear, branched, soluble or crosslinked insoluble structures with reactive or various polar functional groups.

[0002] The polymers thus produced can be used as is or for the production of block polymers, without the use of multifunctional initiators capable of producing more than two polymer chains, without the use of polyvinyl monomers or inimers used to obtain branched polymer structures, and at reduced cost thanks to the use of low concentrations of complex catalysts and low component costs.

[0003] The method uses an Activator ReGenerated by Electron Transfer (ARGET) Atom Transfer Radical Polymerization (ATRP) reaction of vinyl aromatic monomers, herein denoted as ARGET-ATRP.

[0004] The method can be applied to the synthesis of linear, branched, block functionalized vinyl aromatic polymers to be used as is.The method can also be applied to the preparation of vinyl aromatic compositions with reactive, adhesive, flame retardant, antistatic, or bactericidal functions to make compatible polymer compositions containing vinyl aromatic polymers and other incompatible polymers.

[0005] A polymer with a crosslinked structure means an insoluble polymer that at most swells with a monomer or a suitable solvent, even if no covalent chemical bonds are found between the chains. Similarly, a polymer with a branched structure is a soluble polymer that exhibits a polydispersity, determined by the ratio between the weight average molecular weight (Mw) and the number average molecular weight (Mn), of Mw / Mn greater than 2, and the Mw measured by viscometric detection or multi-angle laser light scattering (MALLS) is greater than 20% of the Mw measured by refractive index detection, even if no covalent chemical bonds are found at the branch points between the chains. A polymer with linear chains is a polymer whose Mw measured by viscometric detection or multi-angle laser light scattering (MALLS) is approximately equal to a maximum value that is 20% greater than the Mw measured by refractive index detection.

[0006] In this patent application, the term (meth)acrylic means an acrylic or methacrylic compound and the term (bi)carbonate means a carbonate or bicarbonate compound.

[0007] In this patent application, all operating conditions contained herein must be considered as preferred conditions, even if not otherwise specified.

[0008] For purposes of this document, the terms "comprise" or "include" also include the terms "consist in" or "essentially consisting of."

[0009] For the purposes of this document, interval definitions always include the extremes unless otherwise specified. [Background technology]

[0010] US Pat. No. 5,399,433 describes atom transfer radical polymerization (ATRP) with activators that regenerate by electron transfer (ARGET).

[0011] In particular, this patent describes a polymerization process in which copolymerizable monomers can be polymerized in the presence of a reducing agent and a polymerization means initially comprising a catalyst having at least one transition metal and a radical initiator, the molar ratio between the transition metal and the radical initiator being less than 0.05 and at most 0.01.

[0012] The catalyst further comprises a polydentate amine ligand in addition to the transition metal. The reducing agent must be suitable to reduce the metal of the catalyst to activate it in reversibly extracting halogen from the initiator or from the dormant radical chain to form a radical that allows propagation by the addition of monomer. The reducing agent can be either inorganic or organic, for example ascorbic acid, stannous compounds, reducing sugars, mercaptans, alcohols. The ARGET-ATRP reaction can be carried out in the presence of a solvent and a base. An excess of the polydentate amine ligand relative to the metal of the catalyst increases the reaction rate. In the absence of a reducing agent, mono- and di-halogenated initiators can be used to obtain linear polymers, and tri- and poly-halogenated initiators, multi-vinyl comonomers and inimers can be used to obtain branched polymers. In an example with vinyl aromatic monomers such as styrene, the reaction is carried out at a temperature of 110°C.

[0013] US Patent No. 5,399,633 describes an ARGET-ATRP process applied to monomers derived from (meth)acrylic acid using a copper-based complex catalyst comprising 5 ppm to 30 ppm by weight of copper atoms and a molar amount of up to 7 mmol % of a polydentate amine as a ligand, where the amine is present in a molar amount of up to 150 mol % relative to the total content of copper atoms.

[0014] The reactant system further comprises at least one reducing agent and at least one base. The reducing agents include alcohols, aldehydes, phenols, and organic acids such as ascorbic acid, as well as salts and esters of ascorbic acid. The base is a monoamine or polyamine organic compound, or an inorganic compound of lithium, sodium, and calcium, including sodium methoxide, potassium ethoxide, hydroxides, carbonates, bicarbonates, phosphates, acetates, oxalates, and ascorbates. When ascorbic acid is used as the reducing agent, the ARGET-ATRP method for the controlled polymerization of (meth)acrylic monomers can be carried out in a solvent suitable for dissolving ascorbic acid, such as an organic or aqueous mixture including methanol, ethanol, propanol, dimethylsulfoxide, dimethylformamide, dimethylacetamide, and N-methylpyrrolidone.

[0015] The resulting (meth)acrylic polymer has a molecular weight distribution in the range of 1.1 to 1.8.

[0016] The ATRP synthesis method is suitable for the preparation of polymers with controlled linear and branched structures with reactive functional groups. The control of the polymerization reaction is regulated by the balance between the inactive (dormant) and active (living) forms of the polymer chains, which in turn depends on the redox balance of the catalyst system used with the polydentate amine ligand. The ligand is selected based on the monomers and halogens present in the reaction system, as described in Non-Patent Document 1. The initiator is selected so that it is more reactive than the inactive polymer chains, thereby promoting the initiation of the polymer chains relative to their growth. In the synthesis carried out by the ATRP method, the vinyl aromatic monomers are less reactive than the (meth)acrylic monomers and require higher temperatures or more effective ligands to shift the reaction balance from the dormant form to the active form. For vinyl aromatic monomers, where more than 80% of the termination of the radical chains occurs by coupling, the use of bifunctional initiators, i.e. initiators with two halogens per molecule, allows the control of the reaction to be maintained even in the case of termination by coupling of two active radical chains. The resulting chains maintain two halogenated ends, although their length is determined by the sum of the two reacting chains. The linear or branched structure cannot be modified by changing the temperature or concentration of the reactants, but only by inserting or not inserting polyfunctional initiators with at least three functional groups, or polyvinyl monomers with at least two vinyl groups per molecule, or vinyl monomers with halogen groups (also known as inimers) that can act both as monomers in the growing polymer chain and as initiators of new chains.

[0017] The previously known ARGET-ATRP makes the ATRP process cheaper by reducing by more than 20-fold the amount of catalyst, including transition metals or polydentate amine ligands, required to carry out the reaction, without modifying the types of polymer structures that can be obtained with the ATRP process. [Prior art documents] [Patent documents]

[0018] [Patent Document 1] U.S. Patent No. 7,893,174 [Patent Document 2] U.S. Patent No. 8,933,183 [Non-patent literature]

[0019] [Non-Patent Document 1] Journal of The American Chemical Society (2008 130(32) 10702-10713) Summary of the Invention

[0020] Applicants have discovered a method for the synthesis of vinyl aromatic polymers that allows control over the sequence of monomers in the chain and linear, branched, soluble or crosslinked insoluble structures with reactive functional groups or varying polarity, using an atom transfer radical polymerization (ATRP) reaction with an activator regenerating by electron transfer of vinyl aromatic monomers (ARGET), herein referred to as ARGET-ATRP.

[0021] The resulting polymer structures (linear, branched or crosslinked) can be obtained without the addition of branching or crosslinking agents, i.e., polyfunctional initiators having at least three functional groups, polyvinyl monomers or inimers that can result in branched polymer structures, simply by adjusting the reaction temperature and / or the relative amounts of the components of the reaction mixture, in particular the reactant and solvent pairs.

[0022] Thus, it is possible to obtain a linear polymer at 100°C and a crosslinked polymer at 70°C, all using the same reactant system components.

[0023] The subject of the present invention is therefore a polymerization process for the synthesis of vinyl aromatic polymers with controlled sequence of monomers in the chain and linear, branched, soluble or crosslinked insoluble structures with reactive or different polar functionalities, comprising a step of polymerizing vinyl aromatic monomers by an atom transfer radical polymerization (ATRP) reaction with an activator regenerating by electron transfer (ARGET), said reaction being carried out in the presence of a complex catalyst comprising a cupric halide and a polydentate amine ligand, in an inert gas atmosphere at a temperature comprised between 25°C and 110°C, said reaction being fed with an organic initiator with two geminal halogens, an alkali metal (bi)carbonate, a solvent pair of an aliphatic alcohol and an acetate of said aliphatic alcohol, and optionally ascorbic acid, with the proviso that no initiator with more than two active halogens, or no polyvinyl monomers or inimers are used.

[0024] The advantage of the process according to the present patent application consists in the possibility to prepare vinyl aromatic polymers with controlled sequence of monomers in the chain and with linear, branched, soluble or crosslinked insoluble structures with reactive functional groups or different polarities, which can be used for the preparation of block polymers without the use of multifunctional initiators with more than two functional groups, polyvinyl monomers and inimers used to obtain branched polymer structures, at reduced cost due to the low complex catalyst concentration and the low cost of the other necessary components.

[0025] The above method allows for a wide range of control over the structure of the vinyl aromatic polymer by varying the temperature and composition of the reaction mixture without the introduction of expensive reactants.

[0026] Detailed Description The method according to the present patent application will now be described in detail.

[0027] Vinyl aromatic monomers are subjected to an atom transfer radical polymerization (ATRP) reaction with an activator that regenerates by electron transfer (ARGET). The reaction is carried out in an inert gas atmosphere at a temperature comprised between 25° C. and 110° C. An organic initiator having two geminal halogens, an alkali metal (bi)carbonate, a solvent pair of an aliphatic alcohol and an acetate of the same, and optionally ascorbic acid, are fed to the reaction, with the exception that no initiators having more than two active halogens, or polyvinyl monomers or inimers are used.

[0028] Through this process, vinyl aromatic polymers can be obtained that have linear, branched, soluble or crosslinked insoluble structures with varying degrees of monomer sequence in the chain and reactive functional groups or varying polarities, by controlling the temperature and concentration of the compounds forming the reaction mixture.

[0029] A vinyl aromatic polymer having a linear structure is synthesized by ARGET-ATRP according to the method of the present invention when the reaction mixture comprises at least one vinyl aromatic monomer, at least one organic initiator having two geminal halogens, at least one catalyst comprising a cupric halide and a polydentate amine ligand, an alkali metal (bi)carbonate, and a solvent pair of an aliphatic alcohol and an acetate of the aliphatic alcohol. The reaction can be carried out in an inert gas atmosphere at a temperature preferably comprised between 70°C and 110°C, more preferably between 80°C and 110°C, even more preferably between 90°C and 110°C, and even more preferably between 90°C and 100°C.

[0030] In the presence of ascorbic acid in the reaction mixture, in addition to the components listed for the synthesis of vinyl aromatic polymers with linear structure, (soluble) branched polymer structures can be obtained at temperatures below 100° C., and in the presence of the solvent pair consisting of ethyl acetate and ethanol at temperatures comprised between 60° C. and 70° C., (insoluble) crosslinked polymer structures can be obtained. In the presence of all other components of the reaction mixture listed for the formation of branched or crosslinked polymers, but using an organic initiator with only one halogen instead of two geminal halogens, only polymers with linear structure can be obtained at temperatures comprised between 25° C. and 110° C. In the absence of alkali metal (bi)carbonates, no polymerization takes place at temperatures comprised between 25° C. and 110° C., even in the presence of all other components of the reaction mixture listed for the formation of linear, branched or crosslinked polymers.

[0031] The vinyl aromatic monomers that can be used in the process according to the present patent application have the general formula (I): [ka] (wherein R is hydrogen or a methyl group, n is 0 or an integer from 1 to 3, and Y is a halogen selected from chlorine or bromine, or Y is an alkyl group or an alkoxy group having 1 to 3 carbon atoms).

[0032] The preferred vinyl aromatic monomer having formula (I) is selected from styrene, α-methyl-styrene, vinyltoluene isomers, ethylstyrene isomers, propylstyrene isomers, chlorostyrene isomers, bromostyrene isomers, methoxystyrene isomers, acetoxystyrene isomers, and mixtures thereof.More preferably, the vinyl aromatic monomer can be selected from styrene and mixtures of styrene and α-methyl-styrene.

[0033] Initiators having two geminal halogens that can be used in the methods described and claimed in this patent application have the formula X2-C-(R1)R2, where X is a halogen selected from F, Cl, Br or I, R1 is H when R2 is an aromatic group, preferably selected from phenyl or substituted phenyl, or R1 is an aliphatic alkyl group having a linear or branched structure having 1 to 20 carbon atoms, preferably 2 to 15 carbon atoms, more preferably 2 to 10 carbon atoms, when R2 is an alkyl ester containing a carboxyl group having a linear or branched alkyl containing 1 to 30 carbon atoms, preferably 1 to 20 carbon atoms, more preferably 1 to 10 carbon atoms.

[0034] X is preferably selected from chlorine and bromine, even more preferably X is chlorine, which is H + It is more suitable when a protic solvent having a labile hydrogen atom that can be generated as an ion is used, and the protic solvent that can be used can be selected from alcohols, diols, polyols, fluoroalcohols or carboxylic acids, with methanol and ethanol being more preferred.

[0035] Protic solvents are described in Journal of Polymer Science, Part A: Polymer Chemistry, 2014, 52(15), 2175-2184.

[0036] Initiators with two geminal halogens (on the same carbon atom) (dihalogenated) ensure greater living character, since they can maintain the halogen functionality as a chain end, even when the radical chain terminates in its activation stage, typically by coupling, as in the case of vinyl aromatic polymers. To be effective, a dihalogenated initiator must have both halogens with a reactivity equal to or greater than the same terminal halogen of a vinyl aromatic chain growing in an inactive form. If one of the two halogens of the initiator is more stable in its initial form relative to the vinyl aromatic chain with the terminal halogen, the polymer chain will continue to grow and no new chains will be initiated. Non-geminal, symmetrical bifunctional initiators have the same reactivity, so if one halogen is active, the other is also active. In the geminal bifunctional initiators used in the described and claimed methods, the second halogen remains more reactive than the first halogen that ends the vinyl aromatic chain due to the reaction, so that in the ideal case of a perfectly controlled reaction, the dual function and growth of two vinyl aromatic chains by the initiator molecule is guaranteed without termination by disproportionation and transfer with removal of the chain-terminating halogen. Preferred initiators with two geminal halogens are selected from benzal halides, ethyl 2-bromo-isobutyrate, (dichloromethyl)benzene, CuCl2, methyl 2,2-dichlorobutanoate, ethyl 2-chloroisobutanoate, ethyl 2,2-dichloropropanoate, methyl 2,2-dichlorobutyrate. Preferred initiators are ethyl 2,2-dichloropropanoate and benzal chloride.

[0037] Solvents that can be used in the process described and claimed in this patent application are mixtures that include acetates of aliphatic alcohols and the aliphatic alcohols themselves.

[0038] Dispersion polymerization is obtained when the alcohol is present in an amount greater than the amount of initial monomer, but in an amount that renders the vinyl aromatic polymer insoluble.

[0039] The aliphatic alcohols that can be used in the described and claimed process can be selected from methanol, ethanol, propanol, isopropanol, tert-butanol, which are also reducing agents for the oxidized form of the catalyst.

[0040] The acetate esters of aliphatic alcohols that can be used in the process described and claimed can be selected from methyl acetate, ethyl acetate, and propyl acetate, isopropyl acetate, tert-butyl acetate.

[0041] Preferred mixtures of solvents between acetates of aliphatic alcohols and the aliphatic alcohols themselves are selected from ethyl acetate and ethyl alcohol, methyl acetate and methanol, isopropyl acetate and isopropanol, tert-butyl acetate and tert-butanol.

[0042] The most preferred solvent mixture, also due to its high environmental compatibility, may be a mixture containing ethyl acetate and ethyl alcohol.

[0043] At temperatures ranging from 60°C to 70°C, with the same volumes of monomer and solvent system, no crosslinking is observed when the ratio between ethyl acetate and ethanol is 7 / 1 or more, but when the ratio is 3 / 1 or less, increasing amounts of crosslinking are present as the amount of ethanol increases.

[0044] Thus, in the temperature range between 60°C and 70°C, the formation of crosslinked insoluble polymers is observed when ethyl acetate / ethanol is used as the solvent pair in ratios comprised between 1 / 1 and 7 / 1, preferably between 1 / 1 and 3 / 1.

[0045] Using a different solvent pair, ethyl acetate / ethanol, over the same temperature range results in the formation of branched but not insoluble polymers.

[0046] Furthermore, it is observed that the reaction rate increases as the polarity of the solvent and reaction mixture increases.

[0047] The complex catalyst used in the described and claimed method comprises a cupric halide and a polydentate amine ligand. The halogen of the cupric halide is preferably the same halogen as present in the initiator. The polydentate amine ligand can be present in an equimolar amount relative to the moles of cupric halide corresponding to the gram atoms of copper or in an excess of up to 200 mol% of the ligand.

[0048] The ARGET-ATRP process has the advantage that the required molar concentration of the catalyst formed from the copper salt and the ligand is significantly lower relative to the initiator initially present in the reaction mixture.

[0049] In the process according to the present patent application, it is preferable to use a molar concentration of copper dihalide to a molar concentration of initiator molecules comprised between 1 / 5 and 1 / 20, preferably comprised between 1 / 10 and 1 / 20, more preferably comprised between 1 / 15 and 1 / 20. If the concentration of copper atoms expressed in gram atoms per liter of reaction mixture to the molar concentration of initiator molecules is less than 1 / 20, especially if the amount of initiator relative to the vinyl aromatic monomer in the initial reaction mixture is less than 1 mol %, optimal reaction control is not guaranteed. Variations in the concentration of catalyst relative to the organic initiator with two geminal halogens, the solvent system of the vinyl aromatic monomer, the carbonate and the concentration of the reducing compound do not modify the structure of the polymer obtained under the same reaction conditions. If an insoluble polymer is obtained with a catalyst to initiator ratio of 1 / 5, then an insoluble polymer is obtained with a ratio of 1 / 20, all under the same reaction conditions with respect to the concentrations of the various components, temperature and reaction time.

[0050] The halogen used in the copper halide is preferably the same as the halogen of the initiator and is preferably selected from chlorine or bromine, with chlorine being most preferred.

[0051] As described in Non-Patent Document 1, multidentate amine ligands, based on their structure, make it possible to adjust the effectiveness of the catalyst with a balance between inactive and active radical forms of vinyl aromatic polymer chains terminated with halogen atoms. A more active ligand can increase the concentration of free radicals and obtain a faster reaction rate, but reduces the control of the structure, since a high concentration of reactive radicals promotes both chain growth and their termination and transfer to monomers. The activity of the ligands in abstracting halogens from the initiator or from the dormant chain increases when going from the multidentate amine 2,2'-bipyridine (bpy) to pentamethyldiethylenetriamine (PMDETA), tris[(2-pyridyl)methyl]-amine (TPMA), 5,5,7,12,12,14-hexaMethyl-1,4,8,11-tetra-azaCyclo-tetradecane (Me6Cyclam), and for the same initiator and monomer, bromine can be abstracted more easily from chlorine.

[0052] An excess of molecules or moles of polydentate amine ligand relative to molecules or moles of copper increases the reaction rate but is a more expensive component, so in the process according to the invention a molar ratio of molecules of polydentate amine ligand to atoms of copper or moles of copper halide between 1 / 1 and 2 / 1, preferably 1.5 / 1, more preferably 1 / 1 is used.

[0053] Preferred are polydentate amines selected from 2,2'-bipyridine (bpy), pentamethyldiethylenetriamine (PMDETA), tris[(2-pyridyl)methyl]-amine (TPMA) and 5,5,7,12,12,14-hexamethyl-1,4,8,11-tetra-azacyclo-tetradecane (Me6Cyclam).

[0054] In the described and claimed process, an alkali metal (bi)carbonate must be used, without which the polymerization reaction of the vinyl aromatic monomers will not occur. This compound is usually used anhydrous and dispersed in the reaction mixture in the form of a powder with a size of less than 500 microns. Alkali metal (bi)carbonates selected from Li, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Ba and Ra are preferred, sodium and potassium (bi)carbonates are more preferred, and sodium (bi)carbonate is the most preferred due to its widespread availability and availability.

[0055] Ascorbic acid or alkali metal salts of ascorbic acid, organotin compounds such as tin 2-ethylhexanoate, organic acids selected from citric acid, oxalic acid, salts and esters of ascorbic acid, organic substances selected from aldehydes or phenols, such as tert-butylcatechol (used as an antioxidant in storage of vinyl aromatic monomers), tin(II) 2-ethylhexanoate and tocopherol, can be added to the reaction mixture at the beginning of the polymerization reaction or during the polymerization reaction. Additional reducing agents used in the described and claimed methods can be acetates of aliphatic alcohols and alcohols present in large excess relative to the copper(II) atom in a solvent pair of aliphatic alcohols, as well as polydentate amine ligands.

[0056] The reducing compound may be present in a lower molar amount than the (bi)carbonate, preferably 1 mol or less of reducing agent per 2 mol of (bi)carbonate. Surprisingly, by using ascorbic acid in controlled amounts and reaction conditions in the ARGET-ATRP process according to the invention, vinyl aromatic polymers can be obtained in branched, soluble, linear structures, and crosslinked, insoluble structures when the solvent pair comprises ethanol, without the use of tri- or multi-functional initiators or divinyl monomers.

[0057] In the absence of anhydrous alkali metal (bi)carbonate, no reaction takes place, even in the presence of a reducing agent such as ascorbic acid dissolved in the reaction mixture by alcohol.

[0058] Although controlled polymerization reactions can be carried out using other reducing agents, the formation of branched soluble polymers is observed only in the presence of ascorbic acid, and insoluble polymers are formed in the temperature range between 60° C. and 70° C. when the solvent pair consists of ethyl acetate and ethanol.

[0059] In the ARGET-ATRP method of the present invention, an inorganic base, including an alkali metal (bi)carbonate, is essential for the reaction to occur. Without an alkali metal (bi)carbonate, the polymerization of vinyl aromatic monomers will not occur, even in the presence of other reducing agents in addition to the alcohol of the solvent system. The function of the inorganic (bi)carbonate base is to neutralize any acid present in the reaction mixture, very effectively shifting the balance in favor of the formation of active radical chains. Therefore, the (bi)carbonate is added in the minimum amount necessary to obtain a sufficiently high reaction rate, but in an amount that does not cause the reaction to get out of control. Since the (bi)carbonate is not soluble in the reaction mixture and is active on its surface, it is preferred to use sodium (bi)carbonate or potassium (bi)carbonate with an average diameter of 500 μm or less, preferably 200 μm or less. Due to its low cost and wide availability, the preferred basic salt is sodium carbonate.

[0060] In the initial reaction mixture of the ARGET-ATRP process, copper is provided in the oxidized form (II), and therefore the presence of at least one reducing agent is required to reduce copper to the reduced form (I) to form the initiating radical or for the propagation of the radical chain.

[0061] When the reducing agent is present in the reaction mixture in a lower molar amount relative to the copper(II) atom, the method is called AGET-ATRP, and when the reducing agent is present in a molar amount equal to or greater than the copper(II) atom, the method is called ARGET-ATRP. In the ARGET-ATRP method according to the present patent application, the reducing agent can be an acetate of an aliphatic alcohol and an alcohol present in large excess relative to the copper(II) atom in a solvent pair of an aliphatic alcohol. Multidentate amine ligands can also be reducing agents, but due to their high cost, it is beneficial to use the multidentate amine ligands in a minimum concentration and in a 1:1 molar ratio with the copper atom.

[0062] The polymerization reaction can be carried out at a temperature comprised between 25° C. and 110° C. The polymerization reaction can be carried out at atmospheric pressure or at superatmospheric pressure up to 20 bar, depending on the reaction and boiling point of the reaction mixture, where the solvent mixture is the most volatile component.

[0063] Some applications of the present invention will now be described, which are for non-limiting illustrative purposes only and which represent preferred embodiments according to the present invention. EXAMPLES

[0064] In all examples, the polymerization reactions described and claimed are carried out at atmospheric pressure.

[0065] Components used in the reaction mixture The following materials were used in the synthesis of the vinyl aromatic polymers: Vinyl aromatic monomer: styrene (St) stabilized with 10 parts per million (ppm) by weight of tert-butylcatechol (TBC) in an air atmosphere (Versalis SpA); Solvents and reducing systems: ethyl acetate (AcOEt), methyl acetate (AcOMet), isopropyl acetate (AcOiPr), tert-butyl acetate (AcOtBu), methanol (Met-OH), ethanol (Et-OH), isopropanol (i-Pr-OH), tert-butanol (tBu-OH), dichloromethane (Merck Sigma-Aldrich), Inorganic base: anhydrous sodium (bi)carbonate (Carlo Erba), Reducing agents: ascorbic acid (AA), tert-butylcatechol (TBC), tin(II) 2-ethylhexanoate (Sn(oct)2) (Merck Sigma-Aldrich), Ligand: tris(2-pyridylmethyl)amine (TPMA), N,N,N',N'',N''-pentamethyldiethylenetriamine (PMDETA) (Merck Sigma-Aldrich); Initiators and cupric halides: ethyl 2-bromoisobutyrate (EBiB), (dichloromethyl)benzene (Cl2TOL), CuCl2 (Merck Sigma-Aldrich).

[0066] Ethyl 2,2-dichloropropanoate (DCPE), methyl 2,2-dichlorobutanoate (DCBM) and ethyl 2-chloroisobutanoate (ECiB) were synthesized as reported below.

[0067] Synthesis of DCPE Sodium 2,2-dichloropropionate (Merck, 90%, 100 g, 1.2 mol) and methanol (Merck Sigma-Aldrich, 99.8%, 250 ml) are inserted into a 500 ml two-neck flask equipped with a magnetic anchor stirrer. H2SO4 (Merck Sigma-Aldrich, 96%, 40 ml) is added using a dropping funnel over about 30 min while stirring in an ice-water bath (T=4°C). Once the reaction is over, the white suspension is stirred for another hour. The solution is separated from the solid by vacuum distillation. The solvent is removed in a rotary evaporator, the liquid is redissolved in ethanol (Merck Sigma-Aldrich, 98%, 200 ml), 2 ml of H2SO4 (Merck Sigma-Aldrich, 96%) is added and the mixture is heated to reflux in an oil bath at 78°C for 8 h with magnetic stirring. After the solution was cooled, it was cooled using a micro-distillation apparatus (SAPLT ROHR System HMS 500C (100 plates), T 浴 = 130°C, T マントル = 78℃, t 還流 =9 seconds, t 取り出し =0.1 sec. The resulting yellow oil was analyzed by spectroscopy ( 1 It has a titer of 93% as determined by H-NMR.

[0068] Synthesis of DCBM The synthesis of methyl 2,2-dichlorobutanoate was carried out by esterification of the chloride of 2,2-dichlorobutanoic acid, synthesized as described in Synthesis 2012 44 605-609, with methanol using a cylindrical tubular reactor equipped with a Liebig condenser, a magnetic anchor stirrer, and a threaded cap with a pierceable baffle through which a Teflon pipette used for the transport of the reaction gases was passed. The reaction chamber, charged with tert-butylammonium chloride (TBAC, 2.7 g, 9.6 mmol) and butanoyl chloride (100 ml, 0.955 mol), was heated to 100 °C while bubbling O2 (40 ml / min to 50 ml / min) through the solution. Once 100°C is reached, the Cl2 flow is opened and added to the solution (35ml / min-45ml / min) over 30 minutes while maintaining the temperature at 100°C, then the reaction mixture is heated to 115°C by 5°C every 30 minutes, and held for a reaction time of more than 7 hours up to a total of 9 hours. Continuing the flow of oxygen and chlorine, the reaction mixture is heated to 120°C, then held at this temperature for a total of 11 hours 30 minutes, and finally heated to 125°C and held at such temperature for a total of 13 hours. Once the reaction is over, the crude product is transferred to a single-neck flask where 1-hexadecene is added to remove any remaining Cl2. This reaction is repeated twice and the crude product is distilled to isolate 2,2-dichlorobutanoyl chloride (yield about 94%). The reaction intermediate is dissolved in 100ml of methanol and then heated under reflux for 4 hours. The product is vacuum distilled and analyzed by NMR (purity >99%).

[0069] Synthesis of ECiB In a 500 mL two-neck flask equipped with a magnetic anchor stirrer, a condenser and an acid vapor scrubber, the following were placed in this order: ethyl 1-hydroxyisobutyrate (Merck, Sigma-Adrich, 800 mL, 600 mmol), CHCl (160 mL), SOCl (Merck, Sigma-Adrich, 60 mL, 827 mmol) and DMF (Merck, Sigma-Adrich, 0.8 mL). The solution was stirred and refluxed for 8 h. After cooling to room temperature, HO (100 mL) was added and neutralized by slow addition of bicarbonate (a large amount of CO formation is observed). The organic phase was separated in a separatory funnel and anhydrified on a column containing anhydrous NaCO. The eluates of the two reactions are collected in a 500 mL flask, AIBN (Merck, Sigma-Adrich, 1 g) is added and refluxed for 18 h to polymerize the ethyl methacrylate formed in parallel with ECiB. A first distillation is then carried out to recover the ester from the bulk of the polymethacrylate (oil bath T = 125 ° C, boiler T = 85 ° C - 100 ° C and p = 230 mbar - 80 mbar). The distillate obtained is then fractionated again (oil bath T = 120 ° C, boiler T = 90 ° C - 100 ° C and p = 190 mbar) to recover ECiB (e.g. 90 ° C - 93 ° C at 190 mmHg). 119.2 g of a colorless liquid are collected (66% yield, GC purity > 99.5%).

[0070] ARGET-ATRP synthesizer To carry out the ARGET-ATRP synthesis of vinyl aromatic polymers, a Schlenk reactor, a glass component suitable for carrying out reactions in a controlled atmosphere (argon or nitrogen), was used as the reaction vessel (useful reaction volume of 25 mL, with an internal diameter of 2.5 cm and equipped with an egg-shaped magnetic anchor stirrer with a length of 2 cm and a diameter of 1 cm). The equipment used is equipped with a screw cap for transporting the reactants and a needle valve for connecting to a gas distributor. This configuration of the Schlenk reactor is suitable for carrying out reactions under slight pressure with solvents having a boiling point lower than the reaction temperature. The screw cap is perforated and equipped with a gasket with Teflon-coated sides that can also act as a rupture disk in case of too high internal pressure. For all reactions carried out under argon or nitrogen, after the initial insertion of the solid reactants, the atmosphere is changed with at least three vacuum / inert gas cycles (as an indication, for a vacuum of 3 minutes, for inert gas, the period is defined by the reappearance of bubbling from the mercury bulb). At this point, in the relevant sequence, liquid reactants (or solutions of solid reactants and solvent) can be inserted by opening the Schlenk reactor with a syringe pipette to allow the inert gas to flow freely, or by using a syringe with a metal needle that penetrates the baffle. Once this operation is completed, check the tightening of the screw cap, close the needle tightly, and finally shut off the gas distributor. Finally, the Schlenk flask is immersed in a thermostatic liquid (if necessary). As mentioned above, this particular reactor is connected to a gas distributor, a device complete with vacuum conduits and inert gas, while it can be connected to a single outlet by the operation of a stopcock. The vacuum pump is directly connected to the distributor, but a direct connection between the distributor and the inert gas cylinder is not possible. The inert gas is distributed from the cylinder through a two-stage pressure reducing valve, the second stage of which is sufficiently precise to be easily adjustable, from where it enters a device adapted to fix the pressure of the gas in the conduit. This is achieved with a mercury bubbler, where the height of the Hg column determines the operating pressure above which bubbling of gas to the outside begins.This way any problems of pressurization of the glass parts are prevented. In the crucial step of directing the inert gas towards the Schlenk vacuum during acclimatization, there must be a reserve volume of 1-2 liters at the top of the bubbler to reduce pressure changes (which may bring back ambient air). All the fittings of the various equipment are made of PVC rubber, which guarantees low gas permeability.

[0071] General Experimental Procedure: Preparation of Reactant Solutions Preparation of titrated 1 mL solutions (=0.2 mol%) of the catalytic complex CuCl2-TPMA (in methanol, ethanol, isopropanol or tert-butanol) (1) Weigh out 351 mg of CuCl2 into a 10 mL measuring flask and dissolve it with alcohol to make up the volume (replace this solution with fresh water every month).

[0072] (2) Weigh 151.6 mg of TPMA into a 10 mL volumetric flask. Dissolve the ligand in 4 mL of alcohol and add 2 mL of the previously prepared CuCl2 solution. Then make up to volume with fresh alcohol. If solubility is insufficient, stir until completely dissolved.

[0073] Preparation of a titrated 1 mL solution (=0.2 mol%) of the catalyst complex CuCl2-PMDETA (in ethanol) (1) Weigh out 351 mg of CuCl2 into a 10 mL measuring flask and dissolve it with ethanol to make up the volume (replace this solution with fresh water every month).

[0074] (2) Volumetrically add 90.5 mg (109 mL) of PMDETA into a 10 mL volumetric flask.

[0075] Dissolve PMDETA in 4 ml of ethanol and add 2 ml of the previously prepared CuCl2 solution. Then make up to volume with fresh ethanol. If solubility is insufficient, stir until completely dissolved.

[0076] Preparation of titrated solutions of DCPE (in methyl acetate, ethyl acetate, isopropyl acetate, and tert-butyl acetate) Volumetrically insert 400 μL of DCPE (2.76 mM) into a 10 mL volumetric flask charged with acetic alcohol (5 mL). Make up the solution to volume with fresh solvent.

[0077] Preparation of titrated solutions of CAM (in ethyl acetate) Into a 10 mL volumetric flask charged with AcOEt (5 mL), 140 μL of CAM (1.381 mM) was volumetrically inserted. The solution was then made up to volume with fresh solvent.

[0078] Preparation of a titrated solution of Sn(II) 2-ethylhexanoate (in ethyl acetate) Weigh out 0.6220 g of 85% Sn(II) 2-ethylhexanoate (1.305 mM) in ethyl acetate into a 10 mL volumetric flask. The solution is then made up to volume with fresh ethyl acetate. This solution should be used within 72 hours, after which it should be reconstituted.

[0079] Preparation of a titrated solution of tert-butylcatechol (TBC) in ethyl acetate Weigh out 0.2126 g of TBC (1.305 mM) into a 10 mL volumetric flask and bring to volume with fresh ethyl acetate.

[0080] General method for adding the components of the reaction mixture into a Schlenk reactor in four steps (example of a reaction mixture with 3 mL of styrene, 3 mL of ethyl acetate and 1 mL of ethanol): a) Weigh out ascorbic acid (if provided) and sodium carbonate in a weighing vessel, introduce the solids into a Schlenk reactor and create an argon atmosphere. b) Styrene (3 mL) is added with a 5 mL graduated pipette. c) Dilute with 2 mL of AcOEt (added with a 5 mL graduated pipette) and 1 mL of the DCPE solution in AcOEt (added with a 2 mL graduated pipette). d) An ethanolic solution of CuCl2-TPMA complex (1 mL) is introduced with a 2 mL graduated pipette while shaking.

[0081] Carrying out the reaction and isolating the polystyrene produced The reaction mixture contained in the Schlenk reactor is thermostated in an oil (or water) bath at a fixed temperature and time while stirring at 400 rpm using a magnetic anchor stirrer. The Schlenk reactor is then cooled in air for 15 minutes before diluting its contents with CHCl (typically 20 mL or more). The dichloromethane solution is then dripped into a large amount of methanol (250 mL) to precipitate the polystyrene. If necessary, a small amount (about 2 mL) of HCl (10% aqueous) can be added at this point (weight / volume) to facilitate the precipitation and filtration of the polystyrene. This is allowed to decant for 2-3 hours and then filtered through a pre-weighed filter funnel P4 (75 mL).

[0082] Molecular weight distribution measurement method The molecular weight distribution of the obtained THF-soluble polymers was performed by liquid gel permeation chromatography (GPC) equipped with a refractive index (RI) detector, a viscometer (VISCO) and a multi-angle laser light scattering (MALLS) detector. Polymers showing a weight average molecular weight (Mw) 20% higher by the MALLS detector compared to the same Mw obtained using the RI detector are considered branched.

[0083] GPC equipment is Waters Alliance E2695 pump-injector module with degasser, A Waters oven equipped with a precolumn and four Phenogel columns (Phenomenex) with dimensions 300×7.8 mm, particle size 5μ, and pore sizes 106 Å, 105 Å, 104 Å, and 103 Å; Waters 410 Refractive Index RI Detector, A Viscotek T50A viscometer detector calibrated with Viscotek polydispersity standards with specific rated viscosities; Equipped with.

[0084] The experimental tests were carried out under the experimental conditions reported here: THF solvent, Column temperature 30°C, Flow rate 1ml / min, Toluene internal standard, Injection volume 200 microliters.

[0085] Samples (polydisperse) are injected at a concentration of 1 mg / ml. A universal calibration curve is constructed by injecting 20 monodisperse polystyrene standards with molecular weights Mp comprised between 2170 Da and 4340000 Da and recording the intrinsic viscosity and elution volume for all molecular weights.

[0086] Data acquisition and processing is performed via Empower2 (Waters) and Omnisec v.4.6.1 software (Viscotek).

[0087] The examples and tables show the formulation, temperature (T) and reaction time (hr), the percentage of polymerized styrene (X) relative to the initial mass inserted, the number average molecular weight (Mn) measured by RI detector, Mw / Mn measured by RI detector, the linear or branched or crosslinked structure obtained, and the notation nd indicates a measurement that cannot be determined.

[0088] In all examples, the ARGET-ATRP reactions were carried out in a Schlenk apparatus according to the general method described above.

[0089] Examples 1 to 9 Formation of linear, branched, and crosslinked polymers with the same formulation and different reaction temperatures The following were introduced into a Schlenk reactor: 3 mL of styrene, 3 mL of AcOEt, 1 mL of Et-OH and reactants in molar proportions [St]:[DCPE]:[CuCl2-TPMA]:[AA]:[Na2CO3]=100:1.06:0.2:0.5:1.5.

[0090] [Table 1]

[0091] As expected, the conversion (X) increases with temperature (T) and reaction time (t). Between 90 and 110°C, linear polymers are obtained, whereas at 80 and 43°C, branched polymer structures are obtained, and at 60°C, crosslinked polymers (gel-like, insoluble) are obtained.

[0092] Comparative Example 10 to Comparative Example 12 In the absence of Na2CO3 or insufficient Na2CO3 relative to the concentration of the reducing agent, ascorbic acid, no polymer is formed.

[0093] 3 mL of styrene, 3 mL of AcOEt, and 1 mL of Et-OH were charged into a Schlenk reactor, and the reaction was carried out at T=100° C. for t=18 hours with the composition in Table 2.

[0094] [Table 2]

[0095] In Comparative Example 10, all the components are present to carry out the ARGET-ATRP polymerization, such as Cu(II), the polydentate amine ligand TPMA in a molar concentration equivalent to the copper atom, ethanol as a reducing agent, and ascorbic acid, but without Na2CO3, no polymerization reaction occurs. In Example 11, even if only ethanol is used as a reducing agent, no polymerization reaction occurs without Na2CO3. In Example 12, even if ascorbic acid is used as a reducing agent in a molar concentration equivalent to Na2CO3, no polymerization reaction occurs.

[0096] Examples 13 to 21 In the presence of Na2CO3 or NaHCO3 and the absence of ascorbic acid, linear polymers are formed.

[0097] 3 mL of styrene (6 mL in Example 21), 3 mL of AcOEt, and 1 mL of Et-OH were introduced into a Schlenk reactor according to the composition and conditions in Table 3.

[0098] [Table 3]

[0099] In Example 13, the polymerization reaction occurs in the presence of Na2CO3 without ascorbic acid, and even at high styrene conversion (98%), no branched polymer is obtained, even with Mw / Mn greater than 2. Similarly, in Examples 17-20, linear polymers are obtained under reaction conditions similar to those of Examples 5-8, but without ascorbic acid. In Example 21, 0.25 mol of Na2CO3 per 100 mol of styrene produces a linear polymer with Mn equal to the theoretical value, which would be obtained in an ideal "controlled living" polymerization where an initiator molecule initiates two polymer chains.

[0100] Example 22 to Example 24 Using reducing agents other than ascorbic acid, no branched or crosslinked polymers are obtained in the presence of Na2CO3.

[0101] 3 mL of styrene, 3 mL of AcOEt, and 1 mL of Et-OH were charged into a Schlenk reactor, and the reaction was carried out at T=70° C. for t=18 hours under the composition and conditions in Table 4.

[0102] [Table 4]

[0103] In Example 22, the use of an ascorbic acid reducing agent at a molar concentration of the catalyst CuCl2-TPMA equal to 0.05% relative to styrene results in a crosslinked polymer, whereas in Examples 23 and 24, the use of tin(II) 2-ethylhexanoate and tert-butylcatechol instead of ascorbic acid results in a linear polymer.

[0104] Examples 25 to 29 and Comparative Examples 30 to 32 Formation of branched polymers using geminal bifunctional initiators DCPE, Cl2TOL, and DCBM, and linear polymers using monofunctional initiators CEB, EBiB, and ECiB 3 mL of styrene, 3 mL of AcOEt, and 1 mL of Et-OH were placed in a Schlenk reactor, and the reaction was carried out at a reaction temperature of T° C. for a time of t hours under the composition and conditions of Table 5.

[0105] [Table 5]

[0106] In Examples 25 to 29, which use geminal dichlorinated initiators, branched polymers are obtained, whereas in Examples 30 to 32, which use monohalogenated initiators but under otherwise identical conditions, linear polymers are obtained.

[0107] Example 33 and Example 34 Use of PMDETA ligand instead of TPMA under the conditions of Example 2 and Example 15 3 mL of styrene, 3 mL of AcOEt, 1 mL of Et-OH and other reactants were charged into a Schlenk reactor in the proportions and conditions listed in Table 6.

[0108] [Table 6]

[0109] The ligand PMDETA is less effective than TPMA in forming active polymer species, leading to lower conversions, other reaction conditions being the same.

[0110] Examples 35 to 40 Using 3 mL of styrene and different solvent mixtures of AcOEt / Et-OH at the same volumetric quantities (3 mL / 1 mL), very different results are obtained under the conditions of Example 2 and Example 15 (Example 2: [St]:[DCPE]:[CuCl2-TPMA]:[AA]:[Na2CO3]=100:1.06:0.2:0.5:1.5, T=100°C, t=4.5 h, Example 15: [St]:[DCPE]:[CuCl2-TPMA]:[AA]:[Na2CO3]=100:1.06:0.2:0:1.5, T=100°C, t=4.5 h).

[0111] Solvents and reactants were introduced into a Schlenk reactor in the amounts and reaction conditions reported in Table 7.

[0112] [Table 7]

[0113] With AA and the solvent pair AcOMet / Met-OH, in Example 35, polymers are obtained in similar yields and with lower Mw / Mn than in Example 2 with AcOEt / Et-OH, whereas with the solvent pairs AcOi-Pr / i-Pr-OH and AcOt-Bu / t-Bu-OH, in Examples 36 and 37, no polystyrene is obtained (X=0%). It is observed in these cases that the solvent pairs do not dissolve the catalysts Cu(II)-TPMA and AA, which tend to agglomerate with the sodium carbonate to form colored residues that are deposited on the walls of the reactor.

[0114] Without AA, the solvent pair AcOMet / Met-OH gives polymer in Example 38 with slightly higher yield and Mw / Mn than Example 15 with AcOEt / Et-OH. The solvent pair AcOi-Pr / i-Pr-OH gives polymer in Example 39 with a significantly higher yield and slightly higher Mw / Mn than Example 15, whereas the solvent pair AcOt-Bu / t-Bu-OH gives polymer in Example 40 with a similar yield to Example 15 with AcOEt / Et-OH but with a higher Mw / Mn.

[0115] Example 41 Under similar reaction and formulation conditions as in Example 7, the use of the solvent pair AcOMet / Met-OH instead of AcOEt / Et-OH does not result in insoluble polymers, but rather in highly branched polymers with high Mw / Mn.

[0116] The following was inserted into the Schlenk reactor: 3 mL of styrene and AcOMet / Met-OH (3 mL / 1 mL), with the concentration ratio between the reactants reported below: [St]:[DCPE]:[CuCl2-TPMA]:[AA]:[Na2CO3]=100:1.06:0.2:0.5:1.5. The results obtained are listed in Table 8.

[0117] [Table 8]

[0118] Examples 42 to 46 At various volume ratios of AcOEt / Et-OH, crosslinked insoluble polymers or branched soluble polymers can be obtained at 60°C.

[0119] 3 mL of styrene and other reactants were charged into the Schlenk reactor in the ratios and conditions listed below: [St]:[DCPE]:[CuCl2-TPMA]:[AA]:[Na2CO3]=100:1.06:0.05:0.5:1.5, T=60° C. The solvent mixture was made up as specified in Table 9.

[0120] [Table 9]

[0121] In Examples 42 to 44, the reaction rate increases with increasing Et-OH content and crosslinking is observed at lower magnifications. In Example 45, using 0.5 mL of Et-OH and a volume ratio of AcOEt / Et-OH of 7 / 1, the reaction rate is slower and in Example 46, with the same AcOEt / Et-OH ratio as in Example 42 but doubling the amount of solvent, no crosslinking is achieved (no insoluble polymer is formed).

[0122] Examples 47 to 50 Using 3 mL of styrene with various amounts of DCPE, AcOEt / Et-OH and AA / Na2CO3 for 18 h at 70° C., crosslinked insoluble polymers and linear soluble polymers are obtained.

[0123] 3 mL of styrene was charged to the Schlenk reactor and the reaction was carried out at 70° C. for 18 hours, and other reactants were charged in the proportions listed in Table 10.

[0124] [Table 10]

[0125] By increasing the ratio [DCPE]:[AA] between initiator and ascorbic acid from 1.06:0.5 to 2.12:0.5 in Example 48 with respect to Example 47, the amounts of other components, the volume of the solvent mixture, the temperature (70°C) and the reaction time (18 hours) are the same, no insoluble polymer is formed, but a linear polymer is formed with a slightly lower conversion. The linear polymer of Example 48 is also obtained with the other concentrations, temperature and reaction time being the same, and by increasing the amount of Et-OH to 2 mL to AcOEt / Et-OH (2 mL / 2 mL) as in Example 49, where an increase in the conversion of styrene is observed at X=83%. In Example 50, the [DCPE]:[AA] ratio is returned to 2.12:1, as in Example 47 (where [DCPE]:[AA] is 1.06:0.5), and an insoluble polymer is obtained with complete styrene conversion.

[0126] Examples 51 to 53 The reaction was carried out at 60 °C for 18 h with 3 mL of styrene, 3 mL of AcOEt, 1 mL of Et-OH, 1.06 mol% DCPE calculated on styrene basis, 0.5 mol% / 1.5 mol% AA / Na2CO3, and varying the molar concentration of CuCl2-TPMA on a molar basis relative to the initial initiator (DCPE) from 1 / 5 (= 0.2% molar concentration) to 1 / 20 (= 0.05% molar concentration) results in no change in the type of polymer as reported in Table 11.

[0127] [Table 11]

[0128] The concentration of the catalyst is irrelevant to the formation of the insoluble polymer.

[0129] Example 54 and Example 55 When the reaction is carried out at 60° C. for 18 h with 3 mL of AcOEt and 1 mL of Et-OH and the content of geminal difunctional initiator DCPE is reduced by half, no insoluble polymer is obtained anymore, as reported in Table 12.

[0130] [Table 12]

[0131] In Example 54, half the amount of DCPE initiator is used relative to Example 53, resulting in a highly branched but not insoluble polymer. In Example 55, double the amount of styrene is used relative to Example 53, again resulting in a branched soluble polymer, but the solution is less viscous than in Example 54.

[0132] Examples 56 to 59 Using 3 mL of styrene, 3 mL of AcOEt and 1 mL of diEt-OH, 1.06 mol % of DCPE initiator relative to [St] and 0.05 mol % of CuCl2-TPMA catalyst, the reaction was carried out at 60° C. for 18 h, and when the AA content or the Na2CO3 content or both were reduced relative to AA / Na2CO3 (0.5 mol % / 1.5 mol %) calculated based on [St] of Example 53, no insoluble polymer was obtained anymore, as reported in Table 13.

[0133] [Table 13]

[0134] Under the same conditions, in Example 53, 0.5 mol% AA and 1.5 mol% Na2CO3 relative to [St] were used to obtain an insoluble polymer. In Example 58, AA was increased to 0.75 mol% relative to [St] to obtain an insoluble polymer. In Example 59, branched polymers were obtained by decreasing Na2CO3 to 1.0 mol% relative to [St], and linear polymers were obtained by decreasing AA / Na2CO3 to 0.25 / 0.75 and 0.25 / 1.5, respectively.

[0135] Comparative Example 60 In Example 42, with 3 mL of styrene (26.1 mmol), 3 mL of AcOEt and 1 mL of Et-OH, 1.06 mol% DCPE initiator relative to [St], 0.05 mol% CuCl2-TPMA catalyst, and 0.5 mol% / 1.5 mol% AA / Na2CO3 content, the reaction was carried out at 60°C for 13 hours to obtain an insoluble (crosslinked) polymer with an X (styrene conversion) of about 74%. Under the same reaction and formulation conditions (reaction time 15 hours instead of 13 hours), 3.25 mL of ethyl acrylate (EA, 26.1 mmol) was replaced with 3 mL of styrene to obtain a linear polymer as reported in Table 14.

[0136] [Table 14]

Claims

1. A polymerization method for synthesizing vinyl aromatic polymers with controlled monomer sequence in the chain and linear, branched, soluble or crosslinked insoluble structures with reactive or various polar functional groups, comprising a step of polymerizing vinyl aromatic monomers by atom transfer radical polymerization (ATRP) reaction with an activator (ARGET) that regenerates by electron transfer, said reaction being carried out in the presence of a complex catalyst comprising a cupric halide and a polydentate amine ligand in an inert gas atmosphere at a temperature comprised between 25° C. and 110° C., said reaction being carried out by the addition of a cyclic amine having two geminal halogens. a solvent pair of an aliphatic alcohol and acetate ester of the aliphatic alcohol selected from the group consisting of ethyl acetate / ethanol, methyl acetate / methanol, isopropyl acetate / isopropanol, and tert-butyl acetate / tert-butanol, and optionally a reducing agent are provided in an amount of 1 mol or less per 2 mol of the alkali metal (bi)carbonate, with the proviso that no initiator having 3 or more active halogens, or polyvinyl monomers or inimers are used.

2. 10. The method of claim 1, wherein a soluble branched polymer structure is obtained when the reducing agent is present at a temperature of 100°C or less.

3. The vinyl aromatic monomer has the general formula (I): 【Chemistry 1】 3. The method of claim 1 or 2, having the formula: wherein R is hydrogen or a methyl group, n is 0 or an integer from 1 to 3, and Y is a halogen selected from chlorine or bromine, or Y is an alkyl or alkoxy group having 1 to 3 carbon atoms.

4. 4. The method of claim 3, wherein the vinyl aromatic monomer is selected from styrene, α-methyl-styrene, vinyltoluene isomers, ethylstyrene isomers, propylstyrene isomers, chlorostyrene isomers, bromostyrene isomers, methoxystyrene isomers, and mixtures thereof.

5. The method of claim 4, wherein the vinyl aromatic monomer is selected from styrene and a mixture of styrene and alpha-methyl-styrene.

6. The organic initiator having two geminal halogens is represented by the formula X 2 6. The method of any one of claims 1 to 5, having the formula -C-(R1)R2, where X is a halogen selected from F, Cl, Br or I, and R1 is H when R2 is an aromatic group, or R1 is an aliphatic alkyl group having a linear or branched structure having 1 to 20 carbon atoms when R2 is an alkyl ester consisting of a carboxylic acid group having a linear or branched alkyl containing 1 to 30 carbon atoms.

7. 7. The method of claim 6, wherein X is selected from chlorine and bromine.

8. The method of claim 6, wherein the organic initiator having two geminal halogens is selected from (dichloromethyl)benzene, methyl 2,2-dichlorobutanoate, ethyl 2,2-dichloropropanoate, and methyl 2,2-dichlorobutyrate.

9. 9. The method according to any one of claims 1 to 8, wherein the polymerization reaction is carried out at a temperature in the range of 60°C to 70°C and an insoluble crosslinked polymer structure is obtained when the solvent pair is a mixture comprising ethyl acetate and ethyl alcohol.

10. 10. The process according to any one of claims 1 to 9, wherein the polydentate amine ligand is present in an equimolar amount relative to the moles of cupric halide or in an excess of ligand of up to 200 mol %.

11. 11. The method according to any one of claims 1 to 10, wherein the concentration of the cupric halide is comprised between 1 / 5 and 1 / 20 relative to the molar concentration of the initiator molecules.

12. A process according to any one of claims 1 to 11, wherein the molar ratio in terms of molecules of multidentate amine ligand to moles of copper atom or cupric halide varies between 1 / 1 and 2 / 1.

13. 13. The method according to any one of claims 1 to 12, wherein the halogen in the cupric halide is selected from chlorine or bromine.

14. 14. The method according to any one of claims 1 to 13, wherein the alkali metal of the (bi)carbonate is selected from Li, Na, K, Rb, Cs.

15. 15. The process according to any one of claims 1 to 14, wherein a reducing agent selected from ascorbic acid, organotin compounds, organic acids, salts and esters of ascorbic acid, aldehydes or phenols, tin(II) 2-ethylhexanoate, and tocopherol is added at the beginning or during the polymerization reaction.

16. 16. The method of claim 15, wherein the reducing agent is selected from stannous 2-ethylhexanoate, citric acid, oxalic acid, tert-butylcatechol.

17. 17. The method of claim 15 or 16, wherein the reducing agent is present in a lower molar amount than the (bi)carbonate.

Citation Information

Patent Citations

  • Improvement of atom or group transfer radical polymerization

    JP2001514697A

  • Atom transfer radical polymerization method

    JP2007527463A

  • Atom Transfer Radical Polymerization Process

    US20070276101A1

  • Atom transfer radical polymerization process

    US7893174B2

  • Manufacturing method of (meth) acrylic polymer

    US8933183B2