Plate-shaped composite material

A composite material with optimized porous and nonporous inorganic fine particle aggregates in a fluororesin balances dielectric properties, addressing performance challenges in microstrip patch antennas for millimeter wave radars.

JP7571040B2Active Publication Date: 2024-10-22NITTO DENKO CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021551656
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-10-10
Filing Date
2020-10-06
Publication Date
2024-10-22
Estimated Expiration
2040-10-06

AI Technical Summary

Technical Problem

Existing microstrip patch antenna substrates for millimeter wave radars face challenges in achieving a well-balanced combination of dielectric constant and dielectric loss tangent, which are crucial for performance and efficiency.

Method used

A plate-shaped composite material is developed, comprising a fluororesin with specific ratios of porous and nonporous inorganic fine particle aggregates, optimized to balance dielectric properties through a precise formulation of inorganic fine particle aggregates and nonporous inorganic fine particles, with a porosity of 15% or more by volume.

Benefits of technology

The composite material achieves a well-balanced dielectric constant and dielectric loss tangent, enhancing the performance of microstrip patch antennas by improving mechanical, thermal, and electrical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571040000007
    Figure 0007571040000007
  • Figure 0007571040000008
    Figure 0007571040000008
  • Figure 0007571040000009
    Figure 0007571040000009
Patent Text Reader

Abstract

Provided is an excellent plate-shaped composite material that is well balanced with respect to various characteristics such as relative permittivity and dielectric tangent. This excellent plate-shaped composite material is well balanced in a variety of characteristics such as relative permittivity and dielectric tangent, includes a fluorinated resin and a filler, and is characterized in that: the filler comprises non-porous inorganic fine particles having an average primary particle diameter of 2-50 μm and a porous inorganic fine particle aggregate formed as a result of aggregation of inorganic fine particles having an average primary particle diameter of 5-200 nm; the total content of the porous inorganic fine particle aggregate and the non-porous inorganic fine particles is 20-90 mass% of the composite material; and the mass ratio of the content of the non-porous inorganic fine particles to the total content of the porous inorganic fine particle aggregate and the non-porous inorganic fine particles (content of non-porous inorganic fine particles / (content of porous inorganic fine particle aggregate + content of non-porous inorganic fine particles)) is 0.15-0.90.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a plate-shaped composite material suitable for use as a substrate for a microstrip patch antenna used in a millimeter wave radar or the like. [Background technology]

[0002] In recent years, the automotive industry has been actively researching and developing ADAS (Advanced Driver Assistance Systems) and autonomous driving, and millimeter-wave radar is becoming increasingly important as a sensing technology that supports these. From the perspectives of small size, high performance, and low cost, the use of "microstrip patch antennas," which are flat antennas with antenna elements (patches) printed on a resin substrate, is promising for automotive millimeter-wave radar, and studies are underway on antenna pattern designs and substrate materials to improve performance.

[0003] One of the promising substrate materials used for these antennas is polytetrafluoroethylene (PTFE), which has a small dielectric tangent, and in order to further improve the mechanical, thermal, and electrical properties, it has been proposed to blend in granular fillers such as boron nitride, silicon dioxide (silica), and titanium oxide (titania), as well as fillers such as glass fiber and carbon fiber (see Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 03-212987 [Patent Document 2] Japanese Patent Application Publication No. 06-119810 Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention provides an excellent composite material plate having well-balanced properties such as dielectric constant and dielectric loss tangent. [Means for solving the problem]

[0006] Means for Solving the Problems The present inventors have conducted extensive research to find a solution to the above problems, and as a result have found that by incorporating specific porous inorganic fine particle aggregates and specific nonporous inorganic fine particles in a fluororesin in specific ranges, an excellent composite material can be obtained that is well-balanced in terms of various properties such as dielectric constant and dielectric loss tangent. That is, the present invention is as follows. <1> A plate-shaped composite material comprising a fluorine-based resin and a filler, the filler comprising porous inorganic fine particle aggregates formed by aggregation of inorganic fine particles having an average primary particle diameter of 5 to 200 nm, and nonporous inorganic fine particles having an average primary particle diameter of 0.2 to 50 μm, the total content of the porous inorganic fine particle aggregates and the nonporous inorganic fine particles being 20 to 90 mass% of the composite material, and the mass ratio of the content of the nonporous inorganic fine particles to the total content of the porous inorganic fine particle aggregates and the nonporous inorganic fine particles (the content of the nonporous inorganic fine particles / (the content of the porous inorganic fine particle aggregates+the content of the nonporous inorganic fine particles)) being 0.15 to 0.90. <2> The porosity is 15% by volume or more. <1> A plate-shaped composite material according to claim 1. Effect of the Invention

[0007] According to the present invention, it is possible to provide an excellent composite plate material that is well-balanced in terms of various properties such as the dielectric constant and the dielectric loss tangent. [Brief description of the drawings]

[0008] [Figure 1] 1 is a SEM image (drawing substitute photograph) of porous inorganic fine particle aggregates formed by aggregation of inorganic fine particles having an average primary particle size of 5 to 200 nm. [Diagram 2] 1 is a graph showing the relationship between the filler content and the dielectric loss tangent of plate-shaped composite materials according to Examples and Comparative Examples. [Diagram 3]1 is a graph showing the relationship between the filler content and the thermal expansion coefficient of the plate-shaped composite materials according to the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] In explaining the present invention, specific examples will be given. However, the present invention is not limited to the following contents as long as it does not deviate from the spirit of the present invention, and can be modified appropriately.

[0010] <Plate-shaped composite material> A plate-shaped composite material (hereinafter may be abbreviated as "composite material") according to one embodiment of the present invention is a plate-shaped composite material containing a fluororesin and a filler, characterized in that the filler contains "porous inorganic fine particle aggregates (hereinafter may be abbreviated as "inorganic fine particle aggregates") formed by aggregation of inorganic fine particles having an average primary particle diameter of 5 to 200 nm" and "nonporous inorganic fine particles having an average primary particle diameter of 0.2 to 50 μm (hereinafter may be abbreviated as "nonporous inorganic fine particles")", the total content of the inorganic fine particle aggregates and nonporous inorganic fine particles is 20 to 90 mass% of the composite material, and the mass ratio of the content of the nonporous inorganic fine particles to the total content of the inorganic fine particle aggregates and nonporous inorganic fine particles (content of nonporous inorganic fine particles / (content of inorganic fine particle aggregates+content of nonporous inorganic fine particles)) is 0.15 to 0.90. As a result of extensive research into a plate-shaped composite material that can be used as a substrate for a microstrip patch antenna or the like, the inventors have found that by containing inorganic microparticle aggregates and nonporous inorganic microparticles in the above-mentioned ranges, the advantages of each filler are adequately expressed, resulting in an excellent composite material that is well-balanced in terms of various properties such as dielectric constant and dielectric tangent. The "fluororesin", as well as "fillers" such as "inorganic fine particle aggregates" and "nonporous inorganic fine particles" will be described in detail below.

[0011] <Fluorine-based resin> The type of fluororesin is not particularly limited, and any fluororesin used for substrates or the like can be appropriately used. Examples of fluorine-based resins include polytetrafluoroethylene (PTFE), perfluoroalkoxyalkane (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), polychlorotrifluoroethylene (PCTEF), tetrafluoroethylene-ethylene copolymer (ETFE), chlorotrifluoroethylene-ethylene copolymer (ECTFE), and polyvinylidene fluoride (PVDF), with PTFE being particularly preferred. These may be used alone or in combination of two or more.

[0012] The fluororesin is preferably "fibrillated (fibrous structured)". The fibers in the fibrillation are more preferably oriented not only in one direction but in multiple directions, and it is particularly preferable that the fibrils and inorganic fine particle aggregates described later are linked to form a "three-dimensional fine mesh structure". When the fluororesin is fibrillated, particularly when a three-dimensional fine mesh structure is formed, it is possible to ensure excellent mechanical strength and dimensional stability as a composite material. The fibrillation of the fluororesin can be confirmed by surface observation using an SEM or the like. The fibrillation of the fluororesin can be promoted by applying a shear force, for example, and more specifically, it can be carried out by multi-stage rolling described later, and the three-dimensional fine mesh structure can be further carried out by different direction multi-stage rolling described later.

[0013] <Filling agent> The composite material contains inorganic fine particle aggregates and nonporous inorganic fine particles as fillers, and the inorganic fine particle aggregate is specifically as shown in the SEM photograph of Figure 1, and means an aggregate formed by fusing a plurality of inorganic fine particles, which has voids between the inorganic fine particles and is porous. Note that the inorganic fine particles in the aggregate need only be fused at the time of formulation, and may be unfused by subsequent mixing with a fluororesin, etc. On the other hand, the "nonporous" of nonporous inorganic fine particles is an expression in contrast to the "porous" characteristic of inorganic fine particles, and nonporous inorganic fine particles are inorganic fine particles that are not "porous." In other words, nonporous inorganic fine particles do not need to be completely devoid of pores, and may have pores to the extent that they are not recognized as "porous." The "inorganic fine particle aggregate" and the "nonporous inorganic fine particles" will be described in detail below.

[0014] (Inorganic fine particle aggregate) The material of the inorganic fine particles in the inorganic fine particle aggregate is usually an oxide of a typical element such as silicon oxide (silicon monoxide, silicon dioxide (silica), etc.) and aluminum oxide (alumina) (including composite oxides); a transition metal oxide such as titanium oxide (titanium dioxide (titania)), iron oxide, and zirconium oxide (zirconium dioxide (zirconia)) (including composite oxides); and a nitride of a typical element such as boron nitride and silicon nitride, among which an oxide of a typical element is preferred, and silicon dioxide (silica) is particularly preferred. When it is an oxide of a typical element, the relative dielectric constant of the composite material can be kept extremely low, and the composite material can be produced at a lower cost. The crystallinity of the inorganic fine particles is not particularly limited, but silicon dioxide is usually amorphous.

[0015] The average primary particle diameter of the inorganic fine particles in the inorganic fine particle aggregate is 5 to 200 nm, but is preferably 10 nm or more, more preferably 15 nm or more, even more preferably 20 nm or more, and is preferably 150 nm or less, more preferably 120 nm or less, even more preferably 100 nm or less, particularly preferably 80 nm or less, and most preferably 70 nm or less. Within the above range, the inorganic fine particle aggregate is not easily broken even when subjected to processing such as mixing, molding, rolling, etc., and good voids can be secured between the inorganic fine particles, and a smooth surface can be easily secured as a plate-shaped composite material. The average primary particle diameter of the inorganic fine particles in the inorganic fine particle aggregate is a numerical value obtained by measuring the particle diameter by observation with a SEM and averaging the measured values. Specifically, the procedure is to randomly select inorganic fine particle aggregates (100 pieces), measure the particle diameter (the major axis of the particle) of each, and average the obtained particle diameters to obtain a numerical value.

[0016] The average particle size of the primary aggregates of inorganic fine particles in the inorganic fine particle aggregate is usually 100 nm or more, preferably 120 nm or more, more preferably 150 nm or more, and usually 400 nm or less, preferably 380 nm or less, more preferably 350 nm or less. The average particle size of the secondary aggregates of inorganic fine particles (aggregates of primary aggregates) in the inorganic fine particle aggregate is usually 0.1 μm or more, preferably 1 μm or more, more preferably 2 μm or more, and usually 100 μm or less, preferably 90 μm or less, more preferably 80 μm or less. The inorganic fine particle aggregate in the composite material is preferably in a state of secondary aggregates. In the state of secondary aggregates, the above-mentioned three-dimensional fine network structure is easily formed. In addition, the average particle size of the primary aggregates and the average particle size of the secondary aggregates can be calculated by the same method as the average primary particle size of the inorganic fine particles in the inorganic fine particle aggregate described above.

[0017] The BET specific surface area of ​​inorganic fine particle aggregates is usually 10 m 2 / g or more, preferably 20m 2 / g or more, more preferably 30m 2 / g or more, more preferably 40m 2 / g or more, usually 250m 2 / g or less, preferably 240m 2 / g or less, more preferably 210m 2 / g or less, more preferably 150m 2 / g or less, particularly preferably 80m 2 / g or less. Within this range, a high porosity can be ensured as a composite material, and an increase in the dielectric tangent can be suppressed. In particular, if the BET specific surface area is too high, the dielectric tangent of the composite material tends to be high. The BET specific surface area of ​​the inorganic fine particle aggregate is a value calculated by substituting the gas adsorption amount measured by a gas adsorption method (particularly nitrogen adsorption isotherm) into the BET formula, and is expressed as a value before being used to manufacture a composite material.

[0018] The apparent specific gravity of the inorganic fine particle aggregate is usually 10 g / L or more, preferably 20 g / L or more, more preferably 30 g / L or more, and even more preferably 40 g / L or more, and usually 100 g / L or less, preferably 90 g / L or less, more preferably 80 g / L or less, even more preferably 70 g / L or less, and particularly preferably 60 g / L or less. Within the above range, a high porosity can be ensured as a composite material, and the inorganic fine particle aggregate is less likely to be broken. The apparent specific gravity of the inorganic fine particle aggregate is determined by filling the inorganic fine particle aggregate in a container capable of measuring the volume, such as a 250 mL graduated cylinder, measuring the filling mass (Xg) and filling volume (YmL) of the inorganic fine particle aggregate, and dividing the filling mass by the filling volume ([apparent specific gravity (g / L)] = X / Y × 1000).

[0019] As inorganic fine particle aggregates, commercially available products such as the Mizukasil series (manufactured by Mizusawa Chemical Industry Co., Ltd.), the Sylysia series (manufactured by Fuji Silysia Chemical Co., Ltd.), the AEROSIL series (manufactured by Nippon Aerosil Co., Ltd.), and the Nipseal series (manufactured by Tosoh Silica Corporation) can be suitably used, and among these, fumed silica from the AEROSIL series (manufactured by Nippon Aerosil Co., Ltd.) is particularly preferred.

[0020] (Non-porous inorganic fine particles) Examples of the material of the nonporous inorganic fine particles include oxides of typical elements such as silicon oxide (silicon monoxide, silicon dioxide (silica), etc.) and aluminum oxide (alumina) (including composite oxides); transition metal oxides such as titanium oxide (titanium dioxide (titania)), iron oxide, and zirconium oxide (zirconium dioxide (zirconia)) (including composite oxides); and nitrides of typical elements such as boron nitride and silicon nitride, among which silicon oxide is preferred. Examples of composite oxides include cordierite, talc, wollastonite, mullite, steatite, and forsterite. The material of the nonporous inorganic fine particles is not limited to one type, and two or more types may be combined.

[0021] The average primary particle diameter of the nonporous inorganic fine particles is 0.2 to 50 μm, preferably 0.3 μm or more, more preferably 0.4 μm or more, even more preferably 0.5 μm or more, and preferably 40 μm or less, more preferably 30 μm or less, even more preferably 20 μm or less, particularly preferably 10 μm or less, and most preferably 5 μm or less. Within the above range, a moderate specific surface area is obtained, and a good dielectric tangent can be secured, and the surface of the composite material is easily made smooth, making it a material more suitable for high frequency substrates. The average primary particle diameter of the nonporous inorganic fine particles is a numerical value obtained by measuring the particle diameter by observation with a SEM and averaging the measured values. Specifically, the procedure is to randomly select inorganic fine particle aggregates (100 pieces), measure the particle diameter (the major axis of the particle) of each, and average the obtained particle diameters to obtain a numerical value.

[0022] The BET specific surface area of ​​non-porous inorganic particles is usually 0.1 m 2 / g or more, preferably 0.5m 2 / g or more, more preferably 1m 2 / g or more, more preferably 2m 2 / g or more, usually 30m 2 / g or less, preferably 25m 2 / g or less, more preferably 20m 2 / g or less, more preferably 15m 2 / g or less, particularly preferably 10m 2 / g or less. Within this range, a good dielectric tangent can be ensured, and the surface of the composite material is easily made smooth, making the material more suitable for use as a substrate for high frequencies. The BET specific surface area of ​​the nonporous inorganic fine particles is a value calculated by substituting the amount of gas adsorption measured by a gas adsorption method (particularly nitrogen adsorption isotherm) into the BET formula, and is expressed as a value before use in the production of a composite material.

[0023] The dielectric constant of the nonporous inorganic fine particles is usually 10 or less, preferably 8 or less, more preferably 7 or less, even more preferably 6 or less, particularly preferably 5 or less, and is usually at least 3. The dielectric constant of the nonporous inorganic fine particles is a value determined by a method in accordance with Japanese Industrial Standard JIS C2565.

[0024] Commercially available nonporous inorganic fine particles include fused silica such as SFP-130MC, SFP-30M, FB-3SDC manufactured by Denka Corporation; cordierite such as cordierite powder FINE type, ELP-150N, ELP-325N manufactured by AGC Ceramics Co., Ltd.; boron nitride such as FS-1, HP-P1, HP40J series manufactured by Mizushima Ferroalloy Co., Ltd.; and talc such as Nano Ace D-600, D-800, D-1000, FG-15 manufactured by Nippon Talc Co., Ltd.

[0025] (Other fillers) The composite material may contain a filler that does not fall under the category of inorganic fine particle aggregates and nonporous inorganic fine particles (hereinafter, sometimes abbreviated as "other fillers"). It is also preferable that the filler is composed only of inorganic fine particle aggregates and nonporous inorganic fine particles. Examples of the other fillers include granular fillers and fibrous fillers. Examples of the granular fillers include solid carbon such as carbon black and graphite; hollow inorganic particles such as silica balloons and glass balloons; and examples of the fibrous fillers include glass fiber and carbon fiber. The other fillers are not limited to one type, and two or more types may be combined.

[0026] The filler (including inorganic fine particle aggregates and nonporous inorganic fine particles) is preferably surface-modified with a surface modifier having a hydrophobic group (hereinafter sometimes abbreviated as "surface modifier"). The modification with the "surface modifier" will be described in detail below.

[0027] The hydrophobic group of the surface modifier is a fluoro group (-F), a hydrocarbon group (-C n H 2n+1 (n=1 to 30)), among which a fluoro group that exhibits liquid repellency not only to water but also to oily agents is particularly preferred. The surface modifier may be one that chemically adsorbs (reacts) to the surface of the filler, or one that physically adsorbs to the surface of the filler, and may be a low molecular weight compound or a high molecular weight compound. The surface modifier that chemically adsorbs (reacts) to the surface of the filler usually has a reactive functional group that reacts with the surface functional group of the filler (hydroxyl group (-OH) etc.), and examples of the reactive functional group include an alkoxysilyl group (-SiOR (R has 1 to 6 carbon atoms)), a chlorosilyl group (-SiCl), a bromosilyl group (-SiBr), a hydrosilyl group (-SiH) and the like. The method of modifying the surface of the filler with the surface modifier can be appropriately adopted from known methods, and examples thereof include contacting the filler with the surface modifier.

[0028] The surface modifiers can be used alone or in combination of two or more kinds. For example, a surface modifier of a low molecular weight compound having a reactive functional group may be reacted with the surface of the filler, and then a surface modifier of a high molecular weight compound having a hydrophobic group may be physically adsorbed thereon. If the filler material is silicon dioxide (silica) or the like, it may dissolve (decompose) when exposed to a basic aqueous solution, but by modifying it in this way, it is possible to increase the resistance to the basic aqueous solution.

[0029] The thermal decomposition temperature of the surface modifier is usually 250° C. or higher, preferably 300° C. or higher, more preferably 350° C. or higher, even more preferably 360° C. or higher, and particularly preferably 370° C. or higher. Within the above range, decomposition can be suppressed even when treatment such as high-temperature heating is performed. The thermal decomposition temperature of the surface modifier is defined as the temperature at which the weight is reduced by 5% when the temperature is increased at a rate of 20° C. / min, as measured by thermogravimetry-dependent thermogravimetry analysis (TG-DTA).

[0030] Examples of surface modifiers that are low molecular weight compounds having a fluoro group and a reactive functional group include those represented by the following formula: The compounds represented by the following formula are commercially available and can be obtained as appropriate and used as surface modifiers. [ka]

[0031] Examples of the surface modifying agent of a polymer compound having a fluoro group include those represented by the following formula: [ka]

[0032] A commercially available solution may be used as the surface modifier, and suitable examples include T1770 manufactured by Tokyo Chemical Industry Co., Ltd. and Novec (registered trademark) 2202 manufactured by 3M. Novec (registered trademark) 2202 contains a polymeric compound having a fluoro group, and it has been announced that it contains a "fluoroalkylsilane polymer." When Novec (registered trademark) 2202 is used as a surface modifier, it has the advantage that the critical liquid repellency tension of the composite material can be easily reduced by a relatively simple operation.

[0033] The content of the surface modifier in the filler (content of organic matter) is usually 0.1 mass% or more, preferably 1 mass% or more, more preferably 2 mass% or more, even more preferably 3 mass% or more, and particularly preferably 4 mass% or more, and is usually 50 mass% or less, preferably 40 mass% or less, more preferably 30 mass% or less, even more preferably 25 mass% or less, and particularly preferably 20 mass% or less.

[0034] (composite material) The composite material has a total content of inorganic fine particle aggregates and nonporous inorganic fine particles of 20 to 90% by mass, and the "total content" means the total content of the inorganic fine particle aggregates and the nonporous inorganic fine particles when the composite material is taken as 100% by mass. When the inorganic fine particle aggregates and / or nonporous inorganic fine particles contain two or more types of inorganic fine particle aggregates and / or nonporous inorganic fine particles, it means the total content of all of them. The total content of the inorganic fine particle aggregates and nonporous inorganic fine particles is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 50% by mass or more, and preferably 80% by mass or less, more preferably 75% by mass or less, and even more preferably 70% by mass or less. In addition, when the total of the fluorine-based resin, the inorganic fine particle aggregates and nonporous inorganic fine particles is taken as 100 parts by mass, the total content of the inorganic fine particle aggregates and nonporous inorganic fine particles is usually 20 to 90 parts by mass, preferably 30 parts by mass or more, more preferably 40 parts by mass or more, and even more preferably 50 parts by mass or more, and preferably 80 parts by mass or less, more preferably 75 parts by mass or less, and even more preferably 70 parts by mass or less. Within the above range, various properties such as the dielectric constant and the dielectric loss tangent can be easily balanced.

[0035] The composite material has a mass ratio of the content of the nonporous inorganic microparticles to the total content of inorganic microparticle aggregates and the nonporous inorganic microparticles (content of the nonporous inorganic microparticles / (content of the inorganic microparticle aggregates+content of the nonporous inorganic microparticles)) of 0.15 to 0.90, preferably 0.2 or more, more preferably 0.3 or more, even more preferably 0.4 or more, and most preferably 0.5 or more, and preferably 0.8 or less, more preferably 0.75 or less, even more preferably 0.7 or less, and most preferably 0.65 or less.

[0036] The total content of the filler in the composite material is usually 20 to 90 mass%, preferably 30 mass% or more, more preferably 40 mass% or more, even more preferably 50 mass% or more, and preferably 80 mass% or less, more preferably 75 mass% or less, and even more preferably 70 mass% or less. When the total of the fluororesin and the filler is 100 mass parts, the total content of the filler is usually 20 to 90 mass parts, preferably 30 mass parts or more, more preferably 40 mass parts or more, even more preferably 50 mass parts or more, and preferably 80 mass parts or less, more preferably 75 mass parts or less, and even more preferably 70 mass parts or less. When it is within the above range, it is easy to achieve a balance in various properties such as the relative dielectric constant and the dielectric loss tangent.

[0037] The composite material may contain materials other than the above-mentioned fluororesin and filler (including inorganic fine particle aggregates and nonporous inorganic fine particles), but the total content of the fluororesin and filler in the composite material is usually 60 mass% or more, preferably 70 mass% or more, more preferably 80 mass% or more, even more preferably 90 mass% or more, and particularly preferably 100 mass%.

[0038] The composite material has a plate-like shape, and its thickness is usually 2.0 to 3000 μm, preferably 10 μm or more, more preferably 50 μm or more, even more preferably 80 μm or more, and most preferably 100 μm or more, and preferably 2000 μm or less, more preferably 1000 μm or less, even more preferably 800 μm or less, particularly preferably 600 μm or less, and most preferably 400 μm or less. If it is within the above range, a good relative dielectric constant, etc. of the composite material can be ensured.

[0039] The dimensions of the composite material (maximum diameter, vertical or horizontal length) are usually 20 to 1500 mm, but are preferably 30 mm or more, more preferably 40 mm or more, even more preferably 50 mm or more, and most preferably 60 mm or more, and are preferably 1400 mm or less, more preferably 1300 mm or less.

[0040] The porosity of the composite material is usually 10 to 90% by volume, but is preferably 15% by volume or more, more preferably 20% by volume or more, even more preferably 30% by volume or more, particularly preferably 40% by volume or more, and is preferably 80% by volume or less, more preferably 70% by volume or less, and even more preferably 60% by volume or less. Within the above range, the composite material can ensure good properties such as dielectric constant and thermal expansion coefficient. The porosity of the composite material is a value calculated by measuring the volume of the composite material, the specific gravity and mass (blended mass) of the fluororesin, and the specific gravity and mass (blended mass) of the filler, and substituting them into the following formula. [Porosity (volume%)] = ([Volume of composite material] - [Mass of fluororesin / specific gravity of fluororesin] - [Mass of filler / specific gravity of filler]) / [Volume of composite material] x 100

[0041] The dielectric constant of the composite material (frequency: 10 GHz) is usually 3.0 or less, preferably 2.60 or less, more preferably 2.40 or less, further preferably 2.00 or less, particularly preferably 1.80 or less, and is usually 1.55 or more. The dielectric constant of the composite material is the numerical value of the real part (εr') calculated by measuring the complex dielectric constant by the cavity resonator perturbation method (measurement frequency: 10 GHz).

[0042] The dielectric loss tangent of the composite material (frequency: 10 GHz) is usually 0.01 or less, preferably 0.008 or less, more preferably 0.006 or less, further preferably 0.004 or less, particularly preferably 0.002 or less, and is usually 0.0005 or more. The relative dielectric constant of the composite material is defined as the ratio (εr" / εr') of the imaginary part (εr") to the real part (εr') calculated by measuring the complex dielectric constant by the cavity resonator perturbation method (measurement frequency: 10 GHz).

[0043] The thermal expansion coefficient (Z-axis direction) of the composite material is usually 100 ppm / K or less, preferably 90 ppm / K or less, more preferably 80 ppm / K or less, even more preferably 70 ppm / K or less, particularly preferably 60 ppm / K or less, and most preferably 50 ppm / K or less, and is usually 5 ppm / K or more. The thermal expansion coefficient (Z-axis direction) of the composite material is a value calculated from a formula in accordance with Japanese Industrial Standard JIS R3251-1990 using laser interference method (laser thermal dilatometer, measurement temperature range: -50 to 200°C, heating rate: 2°C / min, atmosphere: He, load: 17g).

[0044] The tensile strength of the composite material is usually 1 to 50 MPa, preferably 5 MPa or more, more preferably 7 MPa or more, and even more preferably 10 MPa or more, and preferably 45 MPa or less, more preferably 40 MPa or less, and even more preferably 35 MPa or less. The tensile strength is a value measured in accordance with the method defined in Japanese Industrial Standard JIS K7161 (see below for detailed conditions).

[0045] The tensile modulus of the composite material is usually 0.05 to 1 GPa, preferably 0.08 GPa or more, more preferably 0.1 GPa or more, and even more preferably 0.15 GPa or more, and preferably 0.8 GPa or less, more preferably 0.6 GPa or less, and even more preferably 0.4 GPa or less. The tensile modulus is a value measured in accordance with the method specified in Japanese Industrial Standard JIS K7161 (see below for detailed conditions).

[0046] <Applications of composite materials> The use of the composite material is not particularly limited, but is preferably an electronic circuit board, more preferably a circuit board for a mobile phone, a computer, etc., a substrate for a microstrip patch antenna for a millimeter wave radar, etc. That is, a substrate (hereinafter sometimes abbreviated as "substrate") containing the above-mentioned composite material is also an embodiment of the present invention.

[0047] The substrate comprises a composite material, and preferably has a layer comprising a thermoplastic resin (hereinafter sometimes abbreviated as "resin layer") attached to one or both sides of the composite material, and a fluorine-based resin is particularly preferred as the thermoplastic resin. Examples of fluorine-based resins include polytetrafluoroethylene (PTFE, melting point: 327°C), perfluoroalkoxyalkane (PFA, melting point: 310°C), tetrafluoroethylene-hexafluoropropylene copolymer (FEP, melting point: 260°C), polychlorotrifluoroethylene (PCTEF, melting point: 220°C), tetrafluoroethylene-ethylene copolymer (ETFE, melting point: 270°C), chlorotrifluoroethylene-ethylene copolymer (ECTFE, melting point: 270°C), and polyvinylidene fluoride (PVDF, melting point: 151 to 178°C), with PTFE and PFA being particularly preferred. These may be used alone or in combination of two or more.

[0048] The thickness of the resin layer is usually 0.050 to 30 μm, but is preferably 0.100 μm or more, more preferably 0.40 μm or more, even more preferably 1.0 μm or more, and most preferably 1.5 μm or more, and is preferably 20 μm or less, more preferably 10 μm or less, even more preferably 8.0 μm or less, particularly preferably 6.0 μm or less, and most preferably 5.0 μm or less. The substrate is exposed to various chemicals used in the manufacturing process of antennas and the like. For example, when exposed to a highly penetrating treatment liquid, the treatment liquid may penetrate into the substrate, causing poor appearance and changes in characteristics. Since the resin layer also has the function of suppressing the penetration of the treatment liquid, if the thickness is within the above range, peeling of the conductor layer and the like can be effectively suppressed, and poor appearance and changes in characteristics are unlikely to occur even when exposed to a highly penetrating treatment liquid used in the manufacture of electronic circuit boards. The thickness of the resin layer means a numerical value obtained by measuring the distance from the end of the resin layer in the thickness direction to the interface between the composite material and the resin layer at about 5 to 10 points and averaging the measured values.

[0049] The resin layer may be laminated (attached) not only on one side of the composite material, but also on both sides of the composite material.

[0050] The peel strength between the composite material and the resin layer is usually 0.2 to 2.5 N / mm, preferably 0.3 N / mm or more, more preferably 0.4 N / mm or more, and even more preferably 0.5 N / mm or more, and preferably 2.4 N / mm or less, more preferably 2.2 N / mm or less, and even more preferably 2 N / mm or less. The peel strength is a value measured in accordance with the method defined in Japanese Industrial Standard JIS C6481:1996 (see below for detailed conditions).

[0051] The substrate is usually provided with a conductor layer, which is usually a metal layer. If the substrate has a resin layer, the conductor layer is laminated on the resin layer. Examples of the metal species of the metal layer include gold (Au), silver (Ag), platinum (Pt), copper (Cu), aluminum (Al), and alloys containing these metal species. The thickness of the metal layer is usually 5 μm or more, preferably 10 μm or more, more preferably 15 μm or more, and usually 50 μm or less, preferably 45 μm or less, more preferably 40 μm or less.

[0052] The maximum height Rz of the contact surface of the conductor layer with the composite material or resin layer is usually 0.020 μm or more, preferably 0.050 μm or more, more preferably 0.10 μm or more, even more preferably 0.20 μm or more, and particularly preferably 0.30 μm or more, and is usually 10 μm or less, preferably 8.0 μm or less, more preferably 6.0 μm or less, even more preferably 4.0 μm or less, and particularly preferably 2.0 μm or less. The "maximum height Rz" means a value determined by a method conforming to the Japanese Industrial Standard JIS B0601:2013 (a Japanese Industrial Standard created without changing the technical content of the International Organization for Standardization standard ISO4287). In addition, the "maximum height Rz of the contact surface of the conductor layer with the composite material or resin layer" may be directly measured, or may be considered by using the maximum height Rz of the material used for the conductor layer as it is.

[0053] The thickness obtained by subtracting the maximum height Rz of the conductor layer from the thickness of the resin layer ((thickness of resin layer) - (maximum height Rz of conductor layer)) is usually 0.005 μm or more, preferably 0.010 μm or more, more preferably 0.050 μm or more, even more preferably 0.10 μm or more, and particularly preferably 0.50 μm or more, and is usually 29.98 μm or less, preferably 20 μm or less, more preferably 15 μm or less, even more preferably 10 μm or less, and particularly preferably 5.0 μm or less. If it is within the above range, the thickness of the resin layer is sufficiently ensured, so that poor appearance and changes in characteristics are unlikely to occur even when exposed to highly penetrative treatment solutions used in the manufacture of electronic circuit boards.

[0054] <Method of manufacturing composite materials> The composite material is preferably produced by a production method including the following resin preparation step, filler preparation step, mixing step, molding step, and rolling step (hereinafter, sometimes abbreviated as "composite material production method"). A resin preparation process for preparing a fluororesin (hereinafter, may be abbreviated as "resin preparation process"). A filler preparation process for preparing a filler (hereinafter, may be abbreviated as "filler preparation process"). A mixing step of mixing the fluororesin, the filler, and the volatile additive to obtain a precursor composition (hereinafter, sometimes abbreviated as "mixing step"). A molding step of molding the precursor composition to obtain a rollable object (hereinafter, may be abbreviated as "molding step"). A rolling process (hereinafter, sometimes abbreviated as "rolling process") in which the rolled object is rolled to obtain a composite material. The "resin preparation step," "filler preparation step," "mixing step," "molding step," "rolling step," etc. will be described in detail below.

[0055] The resin preparation step is a step of preparing a fluororesin, which may be obtained or produced by the user. The average particle size (median diameter d50) of the fluororesin granules (secondary particles or later particles) to be prepared is usually 0.5 μm or more, preferably 1.0 μm or more, more preferably 10 μm or more, and even more preferably 30 μm or more, and usually 700 μm or less, preferably 300 μm or less, more preferably 150 μm or less, even more preferably 100 μm or less, and particularly preferably 50 μm or less. Within the above range, the fluororesin and the filler are easily dispersed uniformly. The fluororesin granules can be determined by a method conforming to the Japanese Industrial Standard JIS Z8825:2001.

[0056] The filler preparation step is a step of preparing a filler, and the filler (including inorganic fine particle aggregates and nonporous inorganic fine particles) may be obtained or produced by the process itself. The average particle diameter (median diameter d50) of the filler to be prepared, particularly the granulated product (secondary particles or later particles) of inorganic fine particle aggregates, is usually 0.1 μm or more, preferably 0.5 μm or more, more preferably 1 μm or more, and even more preferably 3 μm or more, and is usually 500 μm or less, preferably 200 μm or less, more preferably 100 μm or less, and even more preferably 50 μm or less, and especially preferably 20 μm or less. The average particle diameter (median diameter d50) of the granulated product (secondary particles or later particles) of nonporous inorganic fine particles is usually 1 μm or more, preferably 3 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more, and is usually 2000 μm or less, preferably 1000 μm or less, more preferably 500 μm or less, and even more preferably 100 μm or less, and especially preferably 50 μm or less. Within the above range, the fluororesin and the filler can be easily dispersed uniformly. The granulated filler can be determined by a method conforming to Japanese Industrial Standard JIS Z8825:2001. In addition, the filler is preferably surface-modified with the above-mentioned surface modifier.

[0057] The particle size ratio of the average particle size of the granulated product of the fluororesin and the granulated product of the inorganic fine particle aggregate (average particle size of the fluororesin (median size d50) / average particle size of the inorganic fine particle aggregate (median size d50)) is usually 150 or less, preferably 100 or less, more preferably 60 or less, even more preferably 40 or less, particularly preferably 30 or less, most preferably 10 or less, and usually 1 or more. The particle size ratio of the average particle size of the granulated product of the fluororesin and the granulated product of the nonporous inorganic fine particles (average particle size of the fluororesin (median size d50) / average particle size of the nonporous inorganic fine particles (median size d50)) is usually 500 or less, preferably 300 or less, more preferably 200 or less, even more preferably 100 or less, particularly preferably 50 or less, most preferably 30 or less, and usually 0.01 or more. Within the above range, the fluororesin and the filler can be uniformly dispersed.

[0058] The mixing step is a step of mixing the fluororesin, the filler, and the volatile additive to obtain a precursor composition. The mixing can be carried out by appropriately adopting a known method such as a dry method or a wet method, or by using a mixer or the like. In the case of a dry system, the rotation speed (circumferential speed) of the stirrer or the like is usually 0.5 m / sec or more, preferably 1 m / sec or more, more preferably 5 m / sec or more, even more preferably 10 m / sec or more, particularly preferably 15 m / sec or more, and usually 200 m / sec or less, preferably 180 m / sec or less, more preferably 140 m / sec or less, even more preferably 100 m / sec or less, particularly preferably 50 m / sec or less, and most preferably 20 m / sec or less. If it is within the above range, the fluororesin and filler can be easily dispersed uniformly.

[0059] In the case of a dry mixing method, the mixing time is usually 10 seconds or more, preferably 20 seconds or more, more preferably 30 seconds or more, even more preferably 40 seconds or more, particularly preferably 1 minute or more, and most preferably 5 minutes or more, and usually 60 minutes or less, preferably 50 minutes or less, more preferably 40 minutes or less, even more preferably 30 minutes or less, particularly preferably 20 minutes or less, and most preferably 15 minutes or less. When it is within the above range, the fluororesin and the filler can be easily dispersed uniformly.

[0060] In the case of a wet method, the rotation speed (circumferential speed) of the stirrer or the like is usually 1 m / sec or more, preferably 5 m / sec or more, more preferably 10 m / sec or more, even more preferably 15 m / sec or more, particularly preferably 20 m / sec or more, and most preferably 25 m / sec or more, and is usually 160 m / sec or less, preferably 130 m / sec or less, more preferably 100 m / sec or less, even more preferably 80 m / sec or less, particularly preferably 60 m / sec or less, and most preferably 40 m / sec or less. Within the above range, the fluororesin and filler can be easily dispersed uniformly.

[0061] In the case of a wet mixing method, the mixing time is usually 5 seconds or more, preferably 10 seconds or more, more preferably 20 seconds or more, even more preferably 30 seconds or more, particularly preferably 40 seconds or more, and most preferably 50 seconds or more, and usually 60 minutes or less, preferably 50 minutes or less, more preferably 40 minutes or less, even more preferably 20 minutes or less, particularly preferably 10 minutes or less, and most preferably 5 minutes or less. When it is within the above range, the fluororesin and the filler can be easily dispersed uniformly.

[0062] The volatile additive has the function of forming sufficient pores in the composite material by finally volatilizing and removing it. The volatile additive means a compound that has a boiling point of 30 to 300°C and is liquid at room temperature (25°C), and the boiling point of the volatile additive is preferably 50°C or higher, more preferably 100°C or higher, and even more preferably 200°C or higher, and is preferably 280°C or lower, more preferably 260°C or lower, and even more preferably 240°C or lower.

[0063] The types of volatile additives include low-reactivity hydrocarbons, ethers, esters, alcohols, etc., but aliphatic saturated hydrocarbons are preferred. Specific examples include hexane (boiling point: 69°C), heptane (boiling point: 98°C), octane (boiling point: 126°C), nonane (boiling point: 151°C), decane (boiling point: 174°C), undecane (boiling point: 196°C), dodecane (boiling point: 215°C), tridecane (boiling point: 234°C), tetradecane (boiling point: 254°C), etc. These can be used alone or in combination of two or more.

[0064] The amount of the volatile additive added is usually 1 part by mass or more, preferably 5 parts by mass or more, more preferably 10 parts by mass or more, even more preferably 20 parts by mass or more, and particularly preferably 30 parts by mass or more, and usually 200 parts by mass or less, preferably 150 parts by mass or less, more preferably 130 parts by mass or less, even more preferably 110 parts by mass or less, and particularly preferably 100 parts by mass or less, when the total amount of the fluorine-based resin and the filler is 100 parts by mass. When the amount is within the above range, a good porosity can be ensured as a composite material.

[0065] In the mixing step, it is preferable to add and mix a solvent in addition to the fluorine-based resin, the filler, and the volatile additive. The solvent has the function of making the precursor composition into a paste and enabling it to be uniformly dispersed. Examples of the solvent include water, lower alcohols such as methanol, ethanol, isopropanol, and butanol. These can be used alone or in combination of two or more kinds.

[0066] The molding step is a step of molding the precursor composition to obtain a rollable object, and examples of the molding machine used in the molding step include an FT die (fishtail extrusion die), a press machine, an extrusion molding machine, a calendar roll, etc. In particular, an FT die is preferred.

[0067] The rolling process is a process in which the rolled object is rolled to obtain a composite material, and is preferably "multi-stage rolling" in which the obtained rolled object is stacked and rolled as the rolled object multiple times, and is particularly preferably "multi-stage different direction rolling" in which the rolled object is rolled in a direction different from the previous rolling direction. As an example of the multi-stage different direction rolling, the rolled object is stacked so that they face the same rolling direction to obtain the rolled object, and the rolling direction of the rolled object is rotated 90° from the previous rolling direction to perform rolling repeatedly.

[0068] The number of layers of the rolled product in the multi-stage rolling is usually 2 or more, preferably 3 or more, more preferably 4 or more, even more preferably 10 or more, and particularly preferably 30 or more, and is usually 2000 or less, preferably 1000 or less, more preferably 700 or less, even more preferably 500 or less, and particularly preferably 300 or less.

[0069] The rolling ratio in the rolling step is usually 10 or more, preferably 20 or more, more preferably 40 or more, even more preferably 50 or more, and particularly preferably 100 or more, and is usually 20,000 or less, preferably 15,000 or less, more preferably 10,000 or less, even more preferably 5,000 or less, and particularly preferably 3,000 or less.

[0070] The apparatus used in the rolling step includes a press, an extruder, a rolling roll (for example, a calender roll), and the like.

[0071] The method for producing a composite material or a substrate may include other steps, specifically the following steps: An additive removal step of removing the volatile additive from the rolled product (hereinafter, may be abbreviated as "additive removal step"). A hot compression process for hot compressing the rolled product (hereinafter, sometimes abbreviated as "hot compression process"). A resin layer forming step of forming a resin layer containing a fluorine-based resin on one or both sides of the composite material (hereinafter, sometimes abbreviated as "resin layer forming step"). A step of forming a conductor layer on one or both sides of the composite material (hereinafter, sometimes abbreviated as "conductor layer forming step"). A patterning process for patterning the conductor layer (hereinafter, sometimes abbreviated as "patterning process"). The "additive removing step", "heat compression step", "resin layer forming step", "conductor layer forming step", "patterning step", etc. will be described in detail below.

[0072] The additive removing step is a step of removing the volatile additive from the rolled product, and typically includes a method of heating the rolled product in a heating furnace that can be used for drying. The heating conditions can be appropriately selected depending on the boiling point of the volatile additive, etc.

[0073] The hot compression step is a step of hot compressing the rolled product, and typically includes a method of hot compressing using a press, etc. Hot compression conditions can be appropriately selected, but it is preferable to apply pressure uniformly in the plane of the rolled product.

[0074] The resin layer forming step is a step of forming a resin containing a fluororesin on one or both sides of the composite material, and the resin layer can be formed by a method of attaching a resin film containing a fluororesin to the composite material by heating and pressurizing it using a press machine, etc. By heating and pressurizing the resin film containing a fluororesin, the fluororesin permeates the composite material, effectively preventing peeling of the conductor layer, etc., and ensuring a good relative dielectric constant, etc., for the composite material. The thickness of the resin film containing a fluorine-based resin is usually 0.050 μm or more, preferably 0.10 μm or more, more preferably 0.40 μm or more, even more preferably 1.0 μm or more, and particularly preferably 1.5 μm or more, and is usually 30 μm or less, preferably 20 μm or less, more preferably 10 μm or less, even more preferably 8.0 μm or less, particularly preferably 6.0 μm or less, and most preferably 5.0 μm or less.

[0075] The pressure in the resin layer forming step is usually 0.01 MPa or more, preferably 0.10 MPa or more, more preferably 0.50 MPa or more, even more preferably 0.80 MPa or more, and particularly preferably 1.00 MPa or more, and is usually 50 MPa or less, preferably 40 MPa or less, more preferably 30 MPa or less, even more preferably 20 MPa or less, and particularly preferably 10 MPa or less. Within the above range, peeling of the conductor layer and the like can be effectively suppressed, and a good relative dielectric constant and the like of the composite material can be ensured.

[0076] The temperature in the resin layer formation step is usually 250° C. or higher, preferably 280° C. or higher, more preferably 300° C. or higher, even more preferably 320° C. or higher, and particularly preferably 340° C. or higher, and usually 500° C. or lower, preferably 480° C. or lower, more preferably 460° C. or lower, even more preferably 440° C. or lower, and particularly preferably 420° C. or lower. Within the above range, peeling of the conductor layer and the like can be effectively suppressed, and a good relative dielectric constant and the like of the composite material can be ensured.

[0077] The heating and pressing time in the resin layer forming step is usually 1 second or more, preferably 30 seconds or more, more preferably 1 minute or more, even more preferably 2 minutes or more, and particularly preferably 3 minutes or more, and is usually 180 minutes or less, preferably 120 minutes or less, more preferably 60 minutes or less, even more preferably 30 minutes or less, and particularly preferably 20 minutes or less. Within the above range, peeling of the conductor layer and the like can be effectively suppressed, and a good relative dielectric constant and the like of the composite material can be ensured.

[0078] Examples of the device used in the resin layer forming step include a press machine, a heat roll laminator, and a belt press machine.

[0079] The conductor layer forming step is a step of forming a conductor layer on one or both sides of the composite material. Examples of the method for forming the conductor layer include sputtering, plating, pressure bonding of metal foil, lamination, and the like.

[0080] The patterning step is a step of patterning the metal layer, and examples of the patterning method include an additive method using a photoresist or the like, and a subtractive method using etching. EXAMPLES

[0081] The present invention will be described in more detail below with reference to examples, but the examples can be modified as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be construed as being limited to the specific examples shown below.

[0082] <Example 1> As inorganic fine particle aggregates, hydrophilic fumed silica (manufactured by Nippon Aerosil Co., Ltd., product number "AEROSIL50", BET specific surface area 50±15 m 2 / g, average primary particle size 40 nm, average particle size of secondary aggregates 0.2 μm) was modified with triethoxy-1H,1H,2H,2H-tridecafluoro-n-octylsilane (manufactured by Tokyo Chemical Industry Co., Ltd., product number "T1770") represented by the following formula as a surface modifier. [ka]

[0083] Specifically, 40.8 g of the surface modifier, 22.1 g of acetic acid, 43.2 g of pure water, and 80 g of the inorganic fine particle aggregate were added to 832.9 g of isopropanol, and the mixture was stirred for 24 hours to obtain a dispersion of the inorganic fine particle aggregate. The dispersion was then heated at 100° C. for 1 hour and further heated at 200° C. for 2 hours to obtain a surface-modified inorganic fine particle aggregate.

[0084] Next, fused silica (manufactured by Denka, product number "SFP-130MC", BET specific surface area 6.2 m) was used as a non-porous inorganic fine particle. 2 / g, average primary particle size 0.6 μm) was similarly modified using triethoxy-1H,1H,2H,2H-tridecafluoro-n-octylsilane (Tokyo Chemical Industry Co., Ltd., product number "T1770") as a surface modifier.

[0085] Specifically, 6.8 g of the surface modifier, 2.1 g of acetic acid, 4.3 g of pure water, and 80 g of nonporous inorganic fine particles were added to 83.3 g of isopropanol, and the mixture was stirred for 24 hours to obtain a dispersion of nonporous inorganic fine particles. The dispersion was then heated at 100°C for 1 hour and further heated at 200°C for 2 hours to obtain surface-modified nonporous inorganic fine particles.

[0086] Next, polytetrafluoroethylene (hereinafter sometimes abbreviated as "PTFE"), inorganic fine particle aggregates, nonporous inorganic fine particles, and volatile additives were mixed using a high-speed flow mixer. Specifically, polytetrafluoroethylene (manufactured by Daikin, product number "Polyflon PTFE F-104", average particle size 550 μm) was prepared, and polytetrafluoroethylene, surface-modified inorganic fine particle aggregates, and nonporous inorganic fine particles were added in a mass ratio of 44:46:10 in consideration of the solid content, and the mixture was stirred and mixed for 1 minute at a rotation speed of 14 m / sec and a temperature of 24°C, and then a hydrocarbon oil (manufactured by Exxon Mobil, product number "Isopar M") was added as a volatile additive in an amount of 65 parts by mass when the total amount of polytetrafluoroethylene, inorganic fine particle aggregates, and nonporous inorganic fine particles was 100 parts by mass, and the mixture was mixed for 5 minutes at a rotation speed of 3 m / sec and a temperature of 24°C to obtain a paste.

[0087] The paste was passed through a pair of rolling rolls to form an elliptical mother sheet (sheet-shaped molded body) with a thickness of 3 mm, a width of 10 to 50 mm, and a length of 150 mm, and a plurality of these mother sheets were produced. Next, two of these mother sheets were stacked with the same rolling direction, and this stack was rolled by passing it between the rolling rolls in the same rolling direction to produce a plurality of first rolled laminate sheets. Next, four of the first rolled laminate sheets were stacked with the same rolling direction, and rolled in the same direction to produce a second rolled laminate sheet. In this way, the process of stacking and rolling the sheets was repeated a total of five times, counting from the stacking and rolling of the mother sheet, to produce a third rolled laminate sheet (number of constituent layers: 512). Next, four third rolled laminate sheets were stacked, and the laminate sheets were rotated 90 degrees from the previous rolling direction while keeping the sheet surfaces parallel, and rolled by passing them between the rolls, and the gap between the rolls was narrowed by 0.5 mm each time, and rolled several times to obtain a sheet with a thickness of about 0.18 mm. The obtained rolled laminate sheet was heated at 150°C for 20 minutes to remove the volatile additives, and a sheet-like composite material was produced.

[0088] Next, Fluon (registered trademark) PTFE dispersion AD939E (AGC, solid content 60 mass%) was applied by dip coating to one side of the polyimide carrier so that the wet thickness was 4 μm, and heated at 150 ° C for 5 minutes and at 380 ° C for 5 minutes to prepare a resin film that would become a resin layer. A Cu foil (JX Metals, product number "BHFX-HS-92F") that would become a conductor layer was prepared, and the resin film and the Cu foil were laminated, and pressed with a press machine at a pressure of 6 MPa, a temperature of 360 ° C, and 10 minutes to prepare a resin conductor sheet. This resin conductor sheet and the above-mentioned sheet-like composite material were laminated, and pressure-molded at 360 ° C for 5 minutes at 4 MPa to prepare a laminate sheet with a conductor layer. The obtained laminate sheet was measured for the peel strength of the plate-like composite material and the resin conductor sheet described later. Next, the obtained laminated sheet was immersed in a 38% by mass aqueous solution of ferric chloride (etchant H-200A, manufactured by Sanhayato Corporation) for 30 minutes to remove the conductive layer, and then washed with pure water and dried to obtain a plate-shaped composite material.

[0089] <Example 2> A composite material was obtained in the same manner as in Example 1, except that when mixing in the high-speed flow mixer, polytetrafluoroethylene, surface-modified inorganic fine particle aggregates, and nonporous inorganic fine particles were added in a mass ratio of 44:28:28.

[0090] <Example 3> A composite material was obtained in the same manner as in Example 1, except that when mixing in the V-type mixer, polytetrafluoroethylene, the surface-modified inorganic fine particle aggregates, and the nonporous inorganic fine particles were added in a mass ratio of 44:15:41.

[0091] <Example 4> A composite material was obtained in the same manner as in Example 1, except that cordierite powder (FINE type manufactured by AGC Ceramics Co., Ltd.) with an average particle diameter of 25 μm was used as the nonporous inorganic microparticles, and when mixing in a high-speed flow mixer, polytetrafluoroethylene, surface-modified inorganic microparticle aggregates, and nonporous inorganic microparticles were added in a mass ratio of 44:30:26, and a volatile additive was added in an amount of 50 parts by mass per 100 parts by mass of the total of polytetrafluoroethylene, inorganic microparticle aggregates, and nonporous inorganic microparticles.

[0092] <Example 5> A composite material was obtained in the same manner as in Example 1, except that when mixing in the high-speed flow mixer, polytetrafluoroethylene, surface-modified inorganic fine particle aggregates, and nonporous inorganic fine particles were added in a mass ratio of 38:28:34.

[0093] <Example 6> A composite material was obtained in the same manner as in Example 1, except that when mixing in the high-speed flow mixer, polytetrafluoroethylene, surface-modified inorganic fine particle aggregates, and nonporous inorganic fine particles were added in a mass ratio of 34:28:38.

[0094] <Example 7> A composite material was obtained in the same manner as in Example 1, except that when mixing in the high-speed flow mixer, polytetrafluoroethylene, surface-modified inorganic fine particle aggregates, and nonporous inorganic fine particles were added in a mass ratio of 30:28:42.

[0095] <Example 8> A composite material was obtained in the same manner as in Example 1, except that when mixing in the high-speed flow mixer, polytetrafluoroethylene, surface-modified inorganic fine particle aggregates, and nonporous inorganic fine particles were added in a mass ratio of 26:28:46.

[0096] <Comparative Example 1> A composite material was obtained in the same manner as in Example 1, except that when mixing in the high-speed flow mixer, polytetrafluoroethylene, surface-modified inorganic fine particle aggregates, and nonporous inorganic fine particles were added in a mass ratio of 60:40:0.

[0097] <Comparative Example 2> A composite material was obtained in the same manner as in Example 1, except that when mixing in the high-speed flow mixer, polytetrafluoroethylene, surface-modified inorganic microparticle aggregates, and nonporous inorganic microparticles were added in a mass ratio of 40:60:0, and a volatile additive was added in an amount of 100 parts by mass per 100 parts by mass of the total of polytetrafluoroethylene, inorganic microparticle aggregates, and nonporous inorganic microparticles.

[0098] <Comparative Example 3> A composite material was obtained in the same manner as in Example 1, except that when mixing in the high-speed flow mixer, polytetrafluoroethylene, surface-modified inorganic microparticle aggregates, and nonporous inorganic microparticles were added in a mass ratio of 20:80:0, and a volatile additive was added in an amount of 150 parts by mass per 100 parts by mass of the total of polytetrafluoroethylene, inorganic microparticle aggregates, and nonporous inorganic microparticles.

[0099] <Comparative Example 4> A composite material was obtained in the same manner as in Example 1, except that when mixing in the high-speed flow mixer, polytetrafluoroethylene, surface-modified inorganic microparticle aggregates, and nonporous inorganic microparticles were added in a mass ratio of 60:0:40, and a volatile additive was added in an amount of 45 parts by mass per 100 parts by mass of the total of polytetrafluoroethylene, inorganic microparticle aggregates, and nonporous inorganic microparticles.

[0100] <Comparative Example 5> A composite material was obtained in the same manner as in Comparative Example 4, except that when mixing in the high-speed flow mixer, polytetrafluoroethylene, surface-modified inorganic fine particle aggregates, and nonporous inorganic fine particles were added in a mass ratio of 40:0:60.

[0101] <Comparative Example 6> A composite material was obtained in the same manner as in Comparative Example 4, except that when mixing in the high-speed flow mixer, polytetrafluoroethylene, surface-modified inorganic fine particle aggregates, and nonporous inorganic fine particles were added in a mass ratio of 20:0:80.

[0102] <Comparative Example 7> A composite material was obtained in the same manner as in Example 1, except that when mixing in the high-speed flow mixer, polytetrafluoroethylene, surface-modified inorganic fine particle aggregates, and nonporous inorganic fine particles were added in a mass ratio of 44:50:6.

[0103] <Comparative Example 8> A composite material was obtained in the same manner as in Example 1, except that cordierite powder (FINE type manufactured by AGC Ceramics) with an average particle diameter of 25 μm was used as the nonporous inorganic microparticles, and when mixed in a high-speed flow mixer, polytetrafluoroethylene, surface-modified inorganic microparticle aggregates, and nonporous inorganic microparticles were added in a mass ratio of 44:0:56, and a volatile additive was added in an amount of 30 parts by mass per 100 parts by mass of the total of polytetrafluoroethylene, inorganic microparticle aggregates, and nonporous inorganic microparticles.

[0104] <Comparative Example 9> A composite material was obtained in the same manner as in Example 1, except that when mixing in the high-speed flow mixer, polytetrafluoroethylene, surface-modified inorganic microparticle aggregates, and nonporous inorganic microparticles were added in a mass ratio of 70:30:0, and a volatile additive was added in an amount of 54 parts by mass per 100 parts by mass of the total of polytetrafluoroethylene, inorganic microparticle aggregates, and nonporous inorganic microparticles.

[0105] <Comparative Example 10> A composite material was obtained in the same manner as in Example 1, except that when mixing in the high-speed flow mixer, polytetrafluoroethylene, surface-modified inorganic microparticle aggregates, and nonporous inorganic microparticles were added in a mass ratio of 50:50:0, and a volatile additive was added in an amount of 82 parts by mass per 100 parts by mass of the total of polytetrafluoroethylene, inorganic microparticle aggregates, and nonporous inorganic microparticles.

[0106] <Comparative Example 11> A composite material was obtained in the same manner as in Example 1, except that when mixing in the high-speed flow mixer, polytetrafluoroethylene, surface-modified inorganic microparticle aggregates, and nonporous inorganic microparticles were added in a mass ratio of 30:70:0, and a volatile additive was added in an amount of 122 parts by mass per 100 parts by mass of the total of polytetrafluoroethylene, inorganic microparticle aggregates, and nonporous inorganic microparticles.

[0107] For each of the obtained plate-shaped composite materials, the porosity, peel strength, dielectric constant, dielectric loss tangent, tensile strength, tensile modulus, and thermal expansion coefficient were measured as described below. The results are shown in Tables 1 to 3.

[0108] <Porosity> The volume of the composite material, the specific gravity and mass (blended mass) of polytetrafluoroethylene (PTFE), the specific gravity and mass (blended mass) of the inorganic microparticle agglomerates, the specific gravity and mass (blended mass) of the nonporous inorganic microparticles, and the specific gravity and mass (blended mass) of other fillers were measured and calculated by substituting them into the formula below. [Porosity (%)] = ([Volume of composite material] - [Mass of PTFE / Specific gravity of PTFE] - [Mass of inorganic fine particle aggregate / Specific gravity of inorganic fine particle aggregate] - [Mass of nonporous inorganic fine particles / Specific gravity of nonporous inorganic fine particles] - [Mass of other fillers / Specific gravity of other fillers]) / [Volume of composite material] x 100

[0109] <Peel strength> A copper-clad laminate test for printed wiring boards in accordance with Japanese Industrial Standard JIS C6481: 1996 was carried out for each of the composite materials of Examples 1 to 8 and Comparative Examples 1 to 11. A test piece with a length of approximately 100 mm was prepared in a state where the conductor layer was laminated with a width of 10 mm, and the average load when the conductor layer portion was peeled off in a direction of 90° at a speed of 50 mm / min was measured as the peel strength.

[0110] <Dielectric constant / dielectric tangent> The measurement frequency was set to 10 GHz, and the complex dielectric constant was measured by the cavity resonator perturbation method, and the real part (εr') was taken as the relative dielectric constant. The dielectric loss tangent was calculated from the ratio (εr" / εr') of the real part to the imaginary part (εr"). A rectangular sample (sample size: width 2 mm x length 70 mm) was cut from each sheet and measured using a dielectric constant measuring device (Agilent Technologies' Network Analyzer N5230C and Kanto Electronics Application Development's Cavity Resonator 10 GHz).

[0111] <Tensile strength / tensile modulus> The tensile strength (tensile breaking strength) and tensile modulus of the plate-shaped composite material were measured in accordance with the method specified in the Japanese Industrial Standard JIS K7161. More specifically, a bench-top precision universal testing machine Autograph AGS-X (manufactured by Shimadzu Corporation) was used as a tensile tester, and a tensile test was performed in the longitudinal direction (MD direction) of a test piece with a dumbbell-shaped No. 1 or dumbbell-shaped No. 2 shape (width of parallel part: 10 mm) under the measurement conditions of a measurement temperature of 25°C, a tensile speed of 100 mm / min, and an initial grip distance of 10 mm. The maximum tensile force recorded until the test piece was broken was obtained, and the value obtained by dividing this by the cross-sectional area of ​​the test piece was taken as the tensile strength (unit: MPa), and the slope of the stress / strain curve corresponding to the two points of strain of 0.05% and 0.25% during the tensile test was taken as the tensile modulus (unit: GPa).

[0112] <Thermal expansion coefficient> The average coefficient of linear thermal expansion from -50°C to 200°C was used as the thermal expansion coefficient, and was calculated using the TMA (Thermal Mechanical Analysis) method. A thermomechanical analyzer (BRUKER AXS, "TMA4000SA") was used to fix a composite material with a width of 4 mm and a length of 20 mm in the lengthwise direction, and a load of 2 g was applied. The material was heated from room temperature to 200°C at a heating rate of 10°C / min, and held for 30 minutes to remove residual stress. The material was then cooled to -50°C at 10°C / min, held for 15 minutes, and then heated to 200°C at 2°C / min. The average linear thermal expansion coefficient from -50°C to 200°C during the second heating process was taken as the thermal expansion coefficient.

[0113] [Table 1]

[0114] [Table 2]

[0115] [Table 3]

[0116] FIG. 2 shows a graph representing the relationship between the total filler content and the dielectric loss tangent of the composite materials of Examples 5 to 8, Comparative Examples 2 to 3, and 10 to 11, and FIG. 3 shows a graph representing the relationship between the total filler content and the thermal expansion coefficient of the composite materials of Examples 5 to 8, Comparative Examples 2 to 3, and 9 to 11. From the graph of FIG. 2, it is clear that when the filler is a porous inorganic fine particle aggregate such as fumed silica alone, the dielectric loss tangent increases with an increase in the filler content, and that this can be significantly suppressed by blending nonporous inorganic fine particles such as fused silica. From the graph of FIG. 3, it is also clear that the increase in the thermal expansion coefficient associated with a decrease in the content of the porous inorganic fine particle aggregate can be suppressed by blending nonporous inorganic fine particles appropriately. In other words, it can be said that a plate-shaped composite material in which a porous inorganic fine particle aggregate and nonporous inorganic fine particles are appropriately blended is an excellent material that is well-balanced in terms of various properties.

[0117] In the above embodiment, specific embodiments of the present invention are shown, but the above embodiment is merely illustrative and should not be interpreted as being limiting. Various modifications that are obvious to those skilled in the art are intended to be within the scope of the present invention. [Industrial Applicability]

[0118] The composite material according to one embodiment of the present invention can be used as a circuit board for mobile phones, computers, etc., a substrate for a microstrip patch antenna for a millimeter wave radar, etc.

Claims

1. A plate-shaped composite material containing a fluorine-based resin and a filler, the filler comprises porous inorganic fine particle aggregates formed by agglomeration of inorganic fine particles having an average primary particle size of 5 to 200 nm, and non-porous inorganic fine particles having an average primary particle size of 0.2 to 50 μm; A plate-shaped composite material, characterized in that the total content of the porous inorganic fine particle aggregate and the nonporous inorganic fine particles is 20 to 90 mass % of the composite material, and the mass ratio of the content of the nonporous inorganic fine particles to the total content of the porous inorganic fine particle aggregate and the nonporous inorganic fine particles (the content of the nonporous inorganic fine particles / (the content of the porous inorganic fine particle aggregate+the content of the nonporous inorganic fine particles)) is 0.15 to 0.

90.

2. 2. The composite material plate according to claim 1, having a porosity of 15 volume % or more.

Citation Information

Patent Citations

  • Composite material for electrical use, laminated sheet and printed wiring board

    JP1991212987A

  • Fluororesin laminated sheet

    JP1991231843A

  • Dielectric composite

    JP1994119810A

  • Prepreg, metal-clad laminate, printed wiring board, and semiconductor device

    JP2012056994A

  • Resin composition, prepreg, resin sheet and laminate

    JP2017179311A