Poly(arylene sulfide) polymers and corresponding polymer compositions and articles

Incorporating dihalocarbazole-containing monomers with halogens in the 2,7-position into PAS polymers addresses the limitations of amine content and molecular weight, resulting in enhanced compatibility and performance for diverse applications.

JP7571135B2Active Publication Date: 2024-10-22SOLVAY SPECIALTY POLYMERS USA LLC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022522368
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-11-04
Filing Date
2020-10-09
Publication Date
2024-10-22
Estimated Expiration
2040-10-09

AI Technical Summary

Technical Problem

Existing poly(arylene sulfide) (PAS) polymers lack sufficient amine content and high molecular weight when incorporating traditional amine components, limiting their compatibility and performance in polymer blends.

Method used

Incorporation of dihalocarbazole-containing monomers, particularly with halogens in the 2,7-position, into PAS polymers to enhance amine content while maintaining high molecular weight.

Benefits of technology

The resulting PAS polymers exhibit improved amine content and high molecular weight, enhancing compatibility and performance in various applications, including automotive, aerospace, and oil and gas components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571135000001
    Figure 0007571135000001
  • Figure 0007571135000002
    Figure 0007571135000002
  • Figure 0007571135000003
    Figure 0007571135000003
Patent Text Reader

Abstract

Disclosed herein are poly(arylene sulfide) ("PAS") polymers (PASPs) comprising repeat units formed from dihalocarbazole-containing monomers. Surprisingly, it has been discovered that such monomers can be incorporated into PAS polymers at desirable concentrations to provide improved amine content. Additionally, it has been surprisingly discovered that the PAS polymers (PASPs) described herein exhibit increased glass transition temperatures ("T") compared to PAS homopolymers and PAS polymers incorporating repeat units containing primary amines. g "). PAS polymers (PASPs) and PAS polymer compositions can be desirably incorporated into a variety of articles, including, but not limited to, automotive articles and oil and gas articles.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application is a national stage entry of International Application No. PCT / EP2020 / 078357, filed October 9, 2020, which claims priority to U.S. Provisional Patent Application No. 62 / 915155, filed October 15, 2019, and European Patent Application No. 19206825.2, filed November 04, 2019, the entire contents of each of which are incorporated herein by reference for all purposes.

[0002] Poly(arylene sulfide) ("PAS") polymers are provided that have excellent thermal and mechanical properties. PAS polymer compositions, methods of making the PAS polymers and PAS compositions, and articles incorporating the PAS polymers and PAS polymer compositions are also provided. [Background technology]

[0003] Poly(arylene sulfide) (PAS) polymers with pendant amines are desirable because the amines can react with many types of functional groups, including, but not limited to, at least carboxylic acids, carboxylates, anhydrides, epoxides, urethanes, amides, ketones, isocyanates, ureas, halogens, activated ethers, esters, and acid chlorides. The ability of the pendant amines to react with a variety of functional groups enhances the compatibility between the PAS polymer and other polymers in a PAS polymer blend, as compared to a similar PAS polymer that does not contain a pendant amine group. Summary of the Invention

[0004] In a first aspect, a poly(arylene sulfide) ("PAS") polymer is provided. The poly(arylene sulfide) ("PAS") polymer comprises repeating units R represented by the following formulas (1) and (2), respectively: PAS1 and R PAS2 Including: [-Ar1-S-], (1) [-Ar2-S-], (2) (In the formula, - -Ar1- is represented by the following formula [ka] selected from the group consisting of; - -Ar2- is represented by the following formula [ka] Represented by; R and R' are, in each case, C1 to C 12 Alkyl groups, C7-C 24 Alkylaryl group, C7-C 24 Aralkyl groups, C6-C 24 Arylene groups and C6-C 18 aryloxy groups; - T is selected from the group consisting of a bond, -CO-, -SO2-, -O-, -C(CH3)2, phenyl, and -CH2-; - i, at each occurrence, is an independently selected integer from 0 to 4; - i and k, at each occurrence, are independently selected integers from 0 to 3.

[0005] In some embodiments, the PAS polymer has a T g Additionally or alternatively, in some embodiments, the PAS polymer has a T m In yet additional or alternative embodiments, the PAS polymer comprises an impact strength of at least 30 J / g as determined according to ASTM D256.

[0006] In a second aspect, a polymer composition (PC) is provided. The polymer composition (PC) comprises a PAS polymer and an additional polymer comprising a functional group selected from the group consisting of carboxylic acid, carboxylate, anhydride, epoxide, urethane, amide, ketone, isocyanate, urea, halogen, activated ether, ester, and acid chloride. In some embodiments, the additional polymer is a thermoplastic polymer. In some embodiments, the additional polymer is a thermosetting polymer or a thermosetting precursor. In some embodiments, additionally or alternatively, the polymer composition (PC) comprises a fibrous reinforcing filler or toughening agent, preferably a fibrous reinforcing filler.

[0007] In a further aspect, there is provided an automotive component, an aerospace component, or an oil and gas component comprising the PAS polymer or polymer composition (PC).

[0008] In yet another aspect, a method for making a PAS polymer (PASP) is provided, the method comprising reacting in a reaction mixture a dihaloaromatic compound having the formula: X1-Ar1-X2, a dihalocarbazole-containing monomer having the formula: X3-Ar2-X4, and a sulfur compound ("SC"), where X1-X4 are independently selected halogens, and Ar1 and Ar2 are as defined above, and the sulfur compound is selected from the group consisting of thiosulfates, thioureas, thioamides, elemental sulfur, thiocarbamates, metal disulfides and oxysulfides, thiocarbonates, organic mercaptans, organic mercaptides, organic sulfides, alkali metal sulfides and disulfides, and hydrogen sulfide, preferably the sulfur compound is an alkali metal sulfide, and most preferably the sulfur compound is Na2S. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Described herein are poly(arylene sulfide) ("PAS") polymers (PASPs) that contain repeat units formed from dihalocarbazole-containing monomers. Surprisingly, it has been found that the incorporation of such monomers into the PAS polymers at desirable concentrations can improve the amine content while maintaining high molecular weight. Additionally, it has been surprising to discover that the PAS polymers described herein exhibit increased glass transition temperatures (T g It has been found that the PAS polymers and PAS polymer compositions can be desirably incorporated into a variety of articles, including, but not limited to, automotive articles, aerospace articles, aviation articles, and oil and gas articles.

[0010] As mentioned above, it has been surprisingly found that the incorporation of a dihalocarbazole-containing monomer into a PAS polymer at a desired concentration can improve the amine content while maintaining a high molecular weight. Conventional methods for introducing an amine component into a PAS polymer include copolymerization with dichloroaniline ("DCA") (e.g., 3,5-DCA). However, as shown in the examples below, it has been surprisingly found that at relatively low comonomer concentrations, 3,5-DCA cannot be used to form a high molecular weight (e.g., >10,000 g / mol) PAS polymer. Furthermore, it has also been surprisingly found that for PAS polymers with a desired dihalocarbazole comonomer concentration, high molecular weight PAS polymers can only be obtained when the dihalocarbazole-containing monomer has a halogen at the 2,7-position.

[0011] As used herein, "free" of a given repeat unit means that the concentration of the given repeat unit in the PAS polymer is less than 1 mol %, preferably less than 0.5 mol %, more preferably less than 0.1 mol %, even more preferably less than 0.01 mol %, even more preferably less than 0.001 mol %, and most preferably 0 mol % (undetectable).

[0012] In this application, any description, even if described in relation to a particular embodiment, is applicable to and interchangeable with other embodiments of the present disclosure. Furthermore, when an element or component is said to be included and / or selected from a list of recited elements or components, in the relevant embodiments expressly contemplated herein, the element or component may be any one of the individual recited elements or components, or may be selected from a group consisting of any two or more of the explicitly recited elements or components; it should be understood that any element or component recited in a list of elements or components may be omitted from such list. In addition, any recitation herein of numerical ranges by endpoints includes all numbers subsumed within the recited ranges, as well as the endpoints and equivalents of the ranges.

[0013] Unless specifically limited otherwise, the terms "alkyl" and derived terms such as "alkoxy", "acyl" and "alkylthio" as used herein include within their scope straight chain, branched chain and cyclic moieties. Examples of alkyl groups are methyl, ethyl, 1-methylethyl, propyl, 1,1-dimethylethyl, and cyclopropyl. Unless specifically stated otherwise, each alkyl and aryl group is unsubstituted or substituted with halogen, hydroxy, sulfo, C1-C6 alkoxy, C1-C6 alkylthio, C1-C6 acyl, formyl, cyano, C6-C6 alkylthio, C1 ... 15 Aryloxy or C6~C 15 It may be substituted with one or more substituents selected from, but not limited to, aryl, provided that the substituents are sterically compatible and chemical bonding and strain energy rules are satisfied. The term "halogen" or "halo" includes fluorine, chlorine, bromine and iodine, with fluorine being preferred.

[0014] The term "aryl" refers to a phenyl, indanyl, or naphthyl group. An aryl group may contain one or more alkyl groups, in which case it may be referred to as an "alkylaryl"; for example, it may be composed of an aromatic group and two C1-C6 groups (e.g., methyl or ethyl). An aryl group may also contain one or more heteroatoms, such as N, O, or S, in which case it may be referred to as a "heteroaryl" group; these heteroaromatic rings may be fused with other aromatic systems. Such heteroaromatic rings include, but are not limited to, furanyl, thienyl, pyrrolyl, pyrazolyl, imidazolyl, triazolyl, isoxazolyl, oxazolyl, thiazolyl, isothiazolyl, pyridyl, pyridazyl, pyrimidyl, pyrazinyl, and triazinyl ring structures. An aryl or heteroaryl substituent may be unsubstituted or may be selected from the group consisting of halogen, hydroxy, C1-C6 alkoxy, sulfo, C1-C6 alkylthio, C1-C6 acyl, formyl, cyano, C6-C6 alkylthio, C1-C6 aryl ... 15 Aryloxy or C6~C 15 It may be substituted with one or more substituents selected from, but not limited to, aryl, provided that the substituents are sterically compatible and chemical bonding and strain energy rules are satisfied.

[0015] PAS Polymer The PAS polymer is composed of repeating units (R PAS1 ) and repeating unit (R PAS2 ): [-Ar1-S-], (1) [-Ar2-S-], (2) Including, -Ar1- is a group of formulae: [ka] and wherein the formula is selected from R is C1 to C in each case. 12 Alkyl groups, C7-C 24 Alkylaryl group, C7-C 24 Aralkyl groups, C6-C 24Arylene groups and C6-C 18 aryloxy groups; T is selected from the group consisting of a bond, -CO-, -SO2-, -O-, -C(CH3)2, phenyl, and -CH2-; i, at each occurrence, is an integer independently selected from 0 to 4; and j, at each occurrence, is an integer independently selected from 0 to 3. For clarity, each benzyl ring in the above formula has 4-i hydrogens (formulas (3) and (4)) or 3-j hydrogens (formula (5)). Thus, when i or j is zero, the corresponding benzyl ring is unsubstituted. Similar notation is used throughout this specification. Additionally, each formula (3)-(5) contains two dashed bonds, one of which is connected to a repeat unit (R PAS1 ) to a distinct sulfur atom, and the other bond is to the repeat unit (R PAS1 ) to an atom outside the repeat unit (e.g., to an adjacent repeat unit). Similar notation is used throughout.

[0016] In a preferred embodiment, i and j are zero in each instance. Preferably, -Ar1- is represented by either formula (3) or (4), more preferably formula (3) (corresponding to the repeating unit of polyphenylene sulfide [-Ar1-S-]), and even more preferably -Ar1- is represented by the following formula: [ka] It is represented by: More preferably, -Ar1- is represented by formula (3') and i is zero.

[0017] Preferably, -Ar2- has the following formula: [ka] is represented by In the formula, R' is, in each case, C1 to C 12 Alkyl groups, C7-C 24 Alkylaryl group, C7-C 24 Aralkyl groups, C6-C 24Arylene groups and C6-C 18 aryloxy groups, and k, at each occurrence, is an independently selected integer from 0 to 3. Preferably, k is zero at each occurrence (e.g., -Ar2- is formed from 2,7-dihalocarbazole).

[0018] In some embodiments, the repeating units (R PAS1 ) and (R PAS2 ) is at least 50 mol%, at least 60 mol%, at least 70 mol%, at least 80 mol%, at least 90 mol%, at least 95 mol%, at least 98 mol%, at least 99 mol%, or at least 99.9 mol%. As used herein, the molar concentration of a repeat unit in a polymer is relative to the total number of repeat units in that polymer, unless expressly specified otherwise. In some embodiments, the molar concentration of the repeat unit (R PAS1 ) is at least 50 mol%, at least 60 mol%, at least 70 mol%, at least 80 mol%, at least 85 mol%, at least 88 mol%, at least 90 mol%, at least 95 mol%, at least 97 mol%, at least 98 mol%, at least 98.5 mol%, or at least 99 mol%.

[0019] In some embodiments, the repeating unit (R PAS2 In some embodiments, the concentration of repeating units (R PAS2 In some embodiments, the concentration of the repeat unit (R PAS2 ) is at least 0.5 mol % to 15 mol %, 0.5 mol % to 12 mol %, 0.5 mol % to 10 mol %, 0.5 mol % to 8 mol %, 1 mol % to 15 mol %, 1 mol % to 12 mol %, 1 mol % to 10 mol %, 1 mol % to 8 mol %, 2 mol % to 8 mol %, or 2.5 mol % to 8 mol %.

[0020] In some embodiments, the PAS polymer has a higher concentration of repeat units (R PAS2 In such an embodiment, the repeat unit (R PAS2 ) is from 0.5 mol % to 99 mol % or less, 80 mol % or less, 70 mol % or less, 60 mol % or less, 50 mol % or less, 40 mol % or less, 30 mol % or less, or 20 mol % or less.

[0021] Of course, in some embodiments, the PAS polymers are different from each other and have repeat units (R PAS1 ) and (R PAS2 In one such embodiment, the PAS polymer comprises one or more additional repeat units according to formula (1), or one or more additional repeat units according to formula (2). In some embodiments that include additional repeat units according to formulas (1) and (2), the total concentration of repeat units according to formulas (1) and (2) is determined by the repeat units (R PAS1 ) and (R PAS2 ) is within the ranges given above for repeat units (R PAS1 ) and (R PAS2 Of course, in another embodiment, the concentration of the additional repeat units according to formulas (1) and (2), and the total number of additional repeat units according to formula (1) relative to the number of repeat units according to formulas (1) and (2), is within the ranges given above for the repeat units (R PAS1 ) and (R PAS2 ) are different from the ranges given above.

[0022] In some embodiments, the PAS polymer has a weight average molecular weight ("M") of at least 10,000 g / mole, at least 20,000 g / mole, at least 25,000 g / mole, at least 30,000 g / mole, or at least 35,000 g / mole. wIn some embodiments, the PAS polymer has an M of 150,000 g / mole or less, 100,000 g / mole or less, 90,000 g / mole or less, 85,000 g / mole or less, or 80,000 g / mole or less. w In some embodiments, the PAS polymer has an M of 10,000 g / mol to 150,000 g / mol, 20,000 g / mol to 100,000 g / mol, 25,000 g / mol to 90,000 g / mol, 30,000 g / mol to 85,000 g / mol, or 35,000 g / mol to 80,000 g / mol. w M w can be measured as described in the Examples below.

[0023] PAS polymers may be amorphous or semi-crystalline. As used herein, amorphous polymers are defined as polymers having an enthalpy of fusion ("ΔH f Those skilled in the art will appreciate that if a PAS is amorphous, it will have a detectable T m It will be appreciated that the PAS polymer does not have a Tm. Thus, one of ordinary skill in the art will appreciate that when a PAS polymer has a Tm, it is referred to as a semi-crystalline polymer. Preferably, the PAS polymer is semi-crystalline. In some embodiments, the PAS polymer has a ΔH of at least 10 J / g, at least 20 J / g, at least, or at least 25 J / g. f In some embodiments, the PAS polymer has a ΔH of 90 J / g or less, 70 J / g or less, or 60 J / g or less. f In some embodiments, the PAS polymer has a ΔH of 10 J / g to 90 J / g or 20 J / g to 70 J / g. f ΔH f can be measured as described in the Examples below.

[0024] In some embodiments, the PAS polymer has a T g In some embodiments, the PAS polymer has a T of 200° C. or less, or 150° C. or less. gIn some embodiments, the PAS polymer has a T of 95° C. to 200° C., 99° C. to 150° C., 95° C. to 200° C., or 99° C. to 150° C. g In some embodiments, the PAS polymer has a melting temperature ("T") of at least 200°C, at least 220°C, at least 240°C, or at least 250°C. m In some embodiments, the PAS polymer has a T of 350° C. or less, 320° C. or less, 300° C. or less, or 285° C. or less. m In some embodiments, the PAS polymer has a T of 200° C. to 350° C., 220° C. to 320° C., 240° C. to 300° C., or 250° C. to 285° C. m In some embodiments, the PAS polymer has a crystallization temperature ("T") of at least 140°C or at least 150°C. c In some embodiments, the PAS polymer has a T of 250° C. or less, or 220° C. or less. c In some embodiments, the PAS polymer has a T of 140° C. to 250° C. or 150° C. to 220° C. c T g , T m and Tc can be measured as described in the Examples below. In some embodiments, the PAS polymer is amorphous and has a Tg of at least 90°C, at least 95°C, or at least 100°C.

[0025] In some embodiments, the PAS polymer has an impact strength of at least 30 Joules per gram ("J / g"), or at least 35 J / g. In some embodiments, the PAS polymer has an impact strength of 150 J / g or less, or 125 J / g or less. In some embodiments, the PAS polymer has an impact strength of 30 J / g to 150 J / g, 35 J / g to 150 J / g, 30 J / g to 125 J / g, or 35 J / g to 125 J / g. Unless otherwise specified, impact strength as used herein refers to notched Izod impact strength measured as described in the Examples below.

[0026] Synthesis of PAS polymer PAS polymer can be synthesized by methods known in the art. In one approach, the synthesis of PAS polymer includes a polymerization process and a subsequent recovery process. The polymerization process includes a polymerization reaction in which a dihaloaromatic monomer, a dihalocarbazole-containing monomer (different from the first dihaloaromatic monomer), and a sulfur compound are polymerized in a solvent to form a PAS polymer, and a termination reaction in which the polymerization reaction is stopped.

[0027] The polymerization reaction involves reacting in a reaction mixture a dihaloaromatic monomer of the formula: X1-Ar1-X2, a dihalocarbazole-containing monomer having the formula: X3-Ar2-X4, and a sulfur compound (SC) (collectively "reactants") in a polymerization solvent according to the following scheme:

number

[0028] The sulfur compound (SC) is selected from the group consisting of thiosulfuric acid, thiourea, thioamides, elemental sulfur, thiocarbamates, metal disulfides and oxysulfides, thiocarbonates, organic mercaptans, organic mercaptides, organic sulfides, alkali metal sulfides and disulfides, and hydrogen sulfide. Preferably, the sulfur compound is an alkali metal sulfide. In some embodiments, the alkali metal sulfide is generated in situ from an alkali metal hydrosulfide and an alkali metal hydroxide. For example, Na2S is a particularly desirable alkali metal sulfide. Na2S can be generated in situ from NaSH and NaOH.

[0029] The polymerization solvent is selected to be a solvent for the reactants at the reaction temperature (described below). In some embodiments, the polymerization solvent is a polar aprotic solvent. Examples of desirable polar aprotic solvents include, but are not limited to, hexamethylphosphoramide, tetramethylurea, n,n-ethylenedipyrrolidone, n-methyl-2-pyrrolidone ("NMP"), pyrrolidone, caprolactam, n-ethylcaprolactam, sulfolane, n,n'-dimethylacetamide, and 1,3-dimethyl-2-imidazolidinone. Preferably, the polymerization solvent is NMP. In embodiments where the polymerization solvent includes NMP, NMP can be reacted with NaOH to form n-methyl-1,4-aminobutanoate.

[0030] As noted above, in some embodiments, the reaction components further include a molecular weight modifier. The molecular weight modifier increases the molecular weight of the PAS polymer compared to a PAS polymer prepared by a synthesis scheme that does not include a molecular weight modifier. Preferably, the molecular weight modifier is an alkali metal carboxylate. Alkali metal carboxylates have the formula: R'CO2M', where R' is a C1-C 20 Hydrocarbyl groups, C1-C 10A hydrocarbyl group, or a C1-C5 hydrocarbyl group, M' is selected from the group consisting of lithium, sodium, potassium, rubidium, or cesium. Preferably, M' is sodium or potassium, and most preferably sodium. Preferably, the alkali metal carboxylic acid is sodium acetate.

[0031] The polymerization reaction is carried out by contacting the reactants at a reaction temperature selected such that X1-Ar1-X2, X3-Ar2-X4, and SC polymerize to form a PAS polymer. In some embodiments, the reaction temperature is from 170° C. to 450° C., or from 200° C. to 285° C. The reaction time (duration of the polymerization reaction) can be from 10 minutes to 3 days, or from 1 hour to 8 hours. The pressure (reaction pressure) is selected to maintain the reactants in the liquid phase during the polymerization reaction. In some embodiments, the reaction pressure can be from 0 pounds per square inch gauge ("psig") to 400 psig, from 30 psig to 300 psig, or from 100 psig to 250 psig.

[0032] The polymerization reaction can be stopped by cooling the reaction mixture to a temperature at which the polymerization reaction ceases. "Reaction mixture" refers to the mixture formed during the polymerization reaction, including any remaining reaction components, the PAS polymer formed, and reaction by-products. Cooling can be accomplished using a variety of techniques known in the art. In some embodiments, cooling can be accomplished by rapidly flashing the reaction mixture. In some embodiments, cooling can include liquid quenching. In liquid quenching, a quenching liquid is added to the reaction mixture to cool the reaction mixture. In some embodiments, the quenching liquid is selected from the group consisting of the polymerization solvent, water, and combinations thereof. In some embodiments, the temperature of the quenching liquid can be from about 15°C to 99°C. In some embodiments, the temperature of the quenching liquid can be from 54°C to 100°C (e.g., in embodiments where the quenching liquid is a solvent) or from 15°C to 32°C (e.g., in embodiments where the quenching liquid is water). Cooling can be further facilitated by cooling the reaction vessel in which the polymerization reaction occurs (the "polymerization reactor") using a reactor jacket or coils. For clarity, stopping the polymerization reaction does not imply complete reaction of the reaction components. Generally, termination is initiated when the polymerization reaction i) is substantially complete; ii) reaches a target yield; or iii) when further reaction of the reactants does not result in a significant increase in the average molecular weight of the PAS polymer.

[0033] After termination, the PAS polymer exists as a PAS polymer mixture. The PAS polymer mixture includes water, polymerization solvent, reaction by-products including salts (e.g., sodium chloride and sodium acetate), PAS oligomers, and unreacted reaction components (collectively "post-reaction compounds"). Typically, after termination, the PAS polymer mixture exists as a slurry (precipitated from the solvent during liquid quenching or flashing) having a liquid phase including the PAS polymer and a solid phase. In some embodiments, the PAS polymer mixture can exist as a wet PAS polymer, for example, by filtration of the slurry after termination.

[0034] Following the cessation, a recovery process is performed. The recovery process includes one or more washes, each of which includes contacting the PAS polymer formed during polymerization with a liquid. Each wash liquid is independently selected from water, an aqueous acid solution, and an aqueous metal cation solution. Based on the disclosure herein, one of ordinary skill in the art will know how to select a recovery process to obtain the PAS polymer described herein.

[0035] Following the recovery process, the PAS polymer mixture can be dried. Drying can be carried out at any temperature that can substantially dry the PAS polymer mixture to obtain a dried PAS polymer. Desirably, the drying process is selected to help prevent oxidative hardening of the PAS polymer. For example, if the drying process is carried out at a temperature of at least 100° C., the drying can be carried out in a substantially non-oxidizing atmosphere (e.g., a substantially oxygen-free atmosphere, or at a pressure less than atmospheric pressure, e.g., under vacuum). If the drying process is carried out at a temperature less than 100° C., the drying process can be accelerated by carrying out the drying at a pressure less than atmospheric pressure, thereby allowing the liquid components to evaporate from the PAS polymer mixture. If the drying is carried out at a temperature less than 100° C., the presence of a gaseous oxidizing atmosphere (e.g., air) generally does not result in detectable hardening of the PAS polymer.

[0036] PAS polymer synthesis, including polymerization, termination, recovery (including water treatment, acid treatment, and metal cation treatment), and drying, is described in U.S. Patent Application Publication No. 2015 / 0175748 to Fodor et al., filed December 19, 2013, which is incorporated herein by reference in its entirety.

[0037] PAS polymer composition The polymer composition (PC) comprises a PAS polymer and at least one other component selected from the group consisting of additional polymers, thermosetting precursors (e.g., epoxy resins), curing agents (e.g., aliphatic, cycloaliphatic, and aromatic monoamines and polyamines), reinforcing agents, toughening agents, plasticizers, colorants, pigments, antistatic agents, dyes, lubricants, heat stabilizers, light stabilizers, flame retardants (such as, but not limited to, halogen-free flame retardants), nucleating agents, and antioxidants.

[0038] In some embodiments, the concentration of the PAS polymer in the polymer composition (PC) is at least 1 wt%, at least 5 wt%, at least 10 wt%, at least 20 wt%, or at least 40 wt%. In some embodiments, the concentration of the PAS polymer in the polymer composition (PC) is 99.95 wt% or less, 99 wt% or less, 95 wt% or less, 90 wt% or less, 85 wt% or less, 80 wt% or less, 70 wt% or less, or 60 wt% or less. In some embodiments, the concentration of the PAS polymer in the polymer composition (PC) is 20 wt% to 99.95 wt%, 20 wt% to 95 wt%, 20 wt% to 85 wt%, 20 wt% to 80 wt%, 20 wt% to 70 wt%, or 20 wt% to 60 wt%. As used herein, the concentration of a component in a polymer composition is based on the total weight in the polymer composition (PC) unless otherwise specified.

[0039] As mentioned above, the PAS polymer can desirably be incorporated into a polymer blend, and the polymer composition (PC) includes the PAS polymer and the additional polymer described below. The pendant amines of the PAS polymer (from the dihalocarbazole-containing monomer) can react with a variety of functional groups, including, but not limited to, carboxylic acids, carboxylates, anhydrides, epoxides, urethanes, amides, ketones, isocyanates, ureas, halogens, activated ethers, esters, and acid chlorides. In some embodiments, the polymer composition (PC) can include the PAS polymer and an additional polymer that includes a functional group selected from the group consisting of carboxylic acids, carboxylates, anhydrides, epoxides, urethanes, amides, ketones, isocyanates, ureas, halogens, activated ethers, esters, and acid chlorides. The functional groups can be present at the chain ends of the additional polymer or on the backbone of the additional polymer (i.e., in repeat units that do not terminate the polymer chain). In some embodiments, the additional polymer is a thermoplastic polymer. In some such embodiments, the additional polymer is selected from the group consisting of poly(arylethersulfone), polyamide, polyamideimide, liquid crystal polymer, polyimide, polyetherimide, poly(aryletherketone), polyurethane, polyester, and polycarbonate. In some such embodiments, the additional polymer is a thermosetting polymer or a thermosetting precursor. In some such embodiments, the additional polymer is selected from the group consisting of epoxy resins, epoxy novolac resins, benzoxazines, bismaleimides, polyamic acid solutions, polyester thermosets, vinyl esters, cyanate esters, and urea-formaldehyde resins. Of course, in some embodiments, the polymer composition (PC) can include more than one of the additional polymers mentioned above, which may be all thermoplastic polymers, all thermosetting polymers, or mixtures thereof.

[0040] In some embodiments, the polymer composition (PC) further comprises reinforcing agents (also called reinforcing fibers or fillers). They can be selected from fibrous and particulate reinforcing agents. Fibrous reinforcing fillers are considered herein to be materials having a length, width and thickness where the average length is significantly greater than both the width and thickness. Generally, such materials have an aspect ratio, defined as the average ratio between the length and the maximum width and thickness, of at least 5, at least 10, at least 20, or at least 50. In some embodiments, the reinforcing fibers (e.g., glass fibers or carbon fibers) have an average length of 3 mm to 50 mm. In some such embodiments, the reinforcing fibers have an average length of 3 mm to 10 mm, 3 mm to 8 mm, 3 mm to 6 mm, or 3 mm to 5 mm. In alternative embodiments, the reinforcing fibers have an average length of 10 mm to 50 mm, 10 mm to 45 mm, 10 mm to 35 mm, 10 mm to 30 mm, 10 mm to 25 mm, or 15 mm to 25 mm. The average length of the reinforcing fibers can be understood as the average length of the reinforcing fibers before they are incorporated into the polymer composition (PC) or as the average length of the reinforcing fibers in the polymer composition (PC). In the case of glass fibers, they can be round (circular cross-section) or flat (non-circular cross-section, such as, but not limited to, oval, elliptical or rectangular).

[0041] The reinforcing fillers may be selected from mineral fillers (talc, mica, kaolin, calcium carbonate, calcium silicate, magnesium carbonate, etc.), glass fibres, carbon fibres, synthetic polymer fibres, aramid fibres, aluminium fibres, titanium fibres, magnesium fibres, boron carbide fibres, rock wool fibres, steel fibres and wollastonite.

[0042] Among the fibrous fillers, glass fibers are preferred; these include chopped strand A-, E-, C-, D-, S- and R-glass fibers as described in Additives for Plastics Handbook, 2nd edition, John Murphy, chapter 5.2.3, p. 43-48. Preferably, the filler is selected from fibrous fillers. More preferably, the filler is a reinforcing fiber that can withstand high temperature applications.

[0043] In some embodiments, the concentration of the reinforcing agent (e.g., glass or carbon fiber) in the polymer composition (PC) is at least 5 wt%, at least 10 wt%, at least 15 wt%, or at least 20 wt%. In some embodiments, the concentration of the reinforcing agent in the polymer composition (PC) is 70 wt% or less, 65 wt% or less, or 60 wt% or less. In some embodiments, the concentration of the reinforcing agent in the polymer composition (PC) is 5 wt%-70 wt%, 10 wt%-70 wt%, 10 wt%-65 wt%, 10 wt%-60 wt%, 15 wt%-60 wt%, or 20 wt%-60 wt%.

[0044] In some embodiments, the polymer composition (PC) further comprises a flame retardant. The flame retardant may be a halogen-free flame retardant or a halogenated flame retardant. Preferably, the flame retardant is a halogen-free flame retardant. The halogen-free flame retardant includes, but is not limited to, organophosphorus compounds selected from the group consisting of phosphinates ("phosphinates"), diphosphinates ("diphosphinates"), and condensation products thereof. Phosphinates are halogen-free flame retardants. Suitable phosphinates include, but are not limited to, those described in U.S. Patent No. 6,365,071, issued April 2, 2002 to Jenewein et al., which is incorporated herein by reference. Particularly preferred phosphinates are aluminum phosphinate, calcium phosphinate, and zinc phosphinate. Among the aluminum phosphinates, aluminum ethyl methyl phosphinate and aluminum diethyl phosphinate, and combinations thereof, are preferred. Halogenated flame retardants include, but are not limited to, 1,2-bis(tribromophenoxy)ethane, brominated epoxy oligomers, brominated polystyrene, chlorendic anhydride, chlorinated paraffins, decabromo biphenyl, decabromodiphenylethane, decabromodiphenyl oxide, dechlorane plus, dibromoneopentyl glycol, ethylene-bis(5,6-dibromonorbornane-2,30 dicarboximide), ethylene-bis(tetrabromophthalimide), halogenated polyether polyols, hexabromocyclododecane, octabromodiphenyl oxide, octabromotrimethylphenylindane, pentabromodiphenyl oxide, poly(dibromostyrene), poly(pentabromobenzyl acrylate), tetrabromo-bisphenol-A, tetrabromo-bisphenol-A, bis(2,3-dibromopropyl ether), tetrabromophthalate diol, and tetrabromophthalic anhydride. Preferably, the halogenated flame retardant is a brominated or chlorinated compound or polymer.

[0045] In some embodiments, the concentration of the flame retardant in the polymer composition (PC) is at least 1 wt%, at least 3 wt%, or at least 5 wt%. In some embodiments, the concentration of the flame retardant in the polymer composition (PC) is 30 wt% or less, 25 wt% or less, or 20 wt% or less. In some embodiments, the concentration of the flame retardant in the polymer composition (PC) is 1 wt% to 30 wt%, 3 wt% to 25 wt%, or 5 wt% to 20 wt%.

[0046] The polymer composition (PC) may also include a toughening agent. The toughening agent generally has a low T g and has a T below room temperature, below 0°C, or even below -25°C. g Its low T g As a result, the toughening agent is typically elastomeric at room temperature. The toughening agent may be a functionalized polymer backbone.

[0047] The polymer backbone of the toughening agent may be selected from elastomeric backbones comprising polyethylene and their copolymers, such as ethylene-butene; ethylene-octene; polypropylene and their copolymers; polybutene; polyisoprene; ethylene-propylene-rubber (EPR); ethylene-propylene-diene monomer rubber (EPDM); ethylene-acrylate rubber; butadiene-acrylonitrile rubber, ethylene-acrylic acid (EAA), ethylene-vinyl acetate (EVA); acrylonitrile-butadiene-styrene rubber (ABS), block copolymer styrene ethylene butadiene styrene (SEBS); block copolymer styrene butadiene styrene (SBS); core-shell elastomers of the methacrylate-butadiene-styrene (MBS) type, or mixtures of one or more of the above.

[0048] When the toughening agent is functionalized, the backbone functionalization can result from copolymerization of monomers containing functional groups or from grafting the polymer backbone with additional functionalizing components.

[0049] Specific examples of functionalized toughening agents include, but are not limited to, terpolymers of ethylene, acrylic esters, and glycidyl methacrylate, copolymers of ethylene and butyl ester acrylate, copolymers of ethylene, butyl ester acrylate, and glycidyl methacrylate, ethylene-maleic anhydride copolymers, EPR grafted with maleic anhydride, styrene copolymers grafted with maleic anhydride, SEBS copolymers grafted with maleic anhydride, styrene-acrylonitrile copolymers grafted with maleic anhydride, and ABS copolymers grafted with maleic anhydride. Further specific examples of functionalized toughening agents include copolymers of ethylene and glycidyl methacrylate, as well as copolymers of ethylene and methacrylic acid.

[0050] The toughening agents may be present in composition (C) in a total amount of more than 1 wt%, more than 2 wt%, or more than 3 wt%, based on the total weight of composition (C). The toughening agents may be present in composition (C) in a total amount of less than 30 wt%, less than 20 wt%, less than 15 wt%, or less than 10 wt%, based on the total weight of polymer composition (PC).

[0051] Composition (C) may also contain other conventional additives commonly used in the art, such as plasticizers, colorants, pigments (e.g., black pigments such as carbon black and nigrosine), antistatic agents, dyes, lubricants (e.g., linear low density polyethylene, calcium or magnesium stearate, or sodium montanate), heat stabilizers, light stabilizers, flame retardants, nucleating agents, and antioxidants.

[0052] In some embodiments, the polymer composition (PC) consists essentially of a PAS polymer and glass fibers. In some embodiments, the polymer composition (PC) consists essentially of a PAS polymer and a reinforcing agent. In some embodiments, the polymer composition (PC) consists essentially of a PAS polymer, glass fibers, and a reinforcing agent. As used herein with respect to the polymer composition (PC), "consists essentially of" indicates that the concentration of components other than those explicitly listed is less than 5 wt%, less than 2 wt%, less than 1 wt%, less than 0.5 wt%, less than 0.1 wt%, less than 0.05 wt%, or less than 0.01 wt%.

[0053] In some embodiments, the polymer composition (PC) comprises a PAS polymer and 10% to 60% by weight of glass fiber (which may of course include other ingredients such as reinforcing agents). In some such embodiments, the concentration of the PAS polymer in the polymer composition (PC) is 20% to 90% by weight. In some embodiments, the polymer composition (PC) comprises a PAS polymer and 5% to 30% by weight of a reinforcing agent. In some such embodiments, the concentration of the PAS polymer in the polymer composition (PC) is 70% to 95% by weight.

[0054] Preparation of polymer composition (PC) The polymer composition (PC) can be prepared using methods well known in the art. In one approach, the polymer composition (PC) can be prepared by melt blending the PAS polymer with certain ingredients (e.g., additional polymers, reinforcing fillers, flame retardants, stabilizers, and other optional ingredients).

[0055] Any melt blending method can be used to mix the polymeric and non-polymeric components. For example, the polymeric and non-polymeric components can be fed into a melt mixer such as a single or twin screw extruder, a stirrer, a single or twin screw kneader or a Banbury mixer, and the adding step can be simultaneous addition of all components or batchwise stepwise addition. When the polymeric and non-polymeric components are added gradually in a batchwise manner, a part of the polymeric and / or non-polymeric components is added first and then melt mixed with the remaining polymeric and non-polymeric components added thereafter until a well-mixed composition is obtained. When the reinforcing agent exhibits a long physical shape (e.g., long glass fibers), stretch extrusion can be used to prepare the reinforced composition.

[0056] As explained in detail above, when the polymer composition (PC) comprises a thermosetting polymer or a thermosetting precursor, the PAS polymer in powder form (characterized by a D50 of 1 micron to 500 microns, preferably 2 microns to 200 microns, most preferably 5 microns to 100 microns) can be blended with the thermosetting polymer or thermosetting precursor along with any other additives using any equipment known in the prior art to disperse the additives in the thermosetting precursor.

[0057] Articles and uses The PAS polymers and polymer compositions (PC) can be desirably incorporated into articles.

[0058] The Articles can be used in portable electronic devices, LED packaging, oil and gas components, food contact components (including, but not limited to, food films and casings), electrical and electronic components (including, but not limited to, computer power supply components, data systems and office equipment, and connectors and contacts compatible with surface mount technology), medical equipment components, construction components (including, but not limited to, pipes, connectors, manifolds, and valves for cooling and heating systems; boiler and meter components; gas system pipes and fittings; and electrical protection devices for mini-circuit breakers, contactors, switches, and sockets), industrial components, plumbing components (including, but not limited to, pipes, valves, fittings, manifolds, shower taps, and shower valves), automotive components, and aerospace components (including, but not limited to, ship cabin components), among others.

[0059] The article may be, for example, a portable electronic device component. As used herein, "portable electronic device" refers to an electronic device that is intended to be conveniently carried and used in various places. Portable electronic devices may include, but are not limited to, mobile phones, personal digital assistants ("PDAs"), laptop computers, tablet computers, wearable computing devices (e.g., smart watches, smart glasses, etc.), cameras, portable audio players, portable radios, global positioning system receivers, and portable game consoles. The portable electronic device component may include, for example, a wireless antenna and the composition (C). In this case, the wireless antenna may be a WiFi antenna or an RFID antenna. The portable electronic device component may also be an antenna housing.

[0060] In some embodiments, the portable electronic device component is an antenna housing. In some such embodiments, at least a portion of the wireless antenna is disposed on the polymer composition (PC). Additionally or alternatively, at least a portion of the wireless antenna can be offset from the polymer composition (PC). In some embodiments, the device component can be an attachment component having a mounting hole or other fastening device (including, but not limited to, a snap-fit ​​connector between itself and another component of the portable electronic device, including, but not limited to, a circuit board, a microphone, a speaker, a display, a battery, a cover, a housing, an electrical or electronic connector, a hinge, a wireless antenna, a switch, or a switch pad). In some embodiments, the portable electronic device can be at least a portion of an input device.

[0061] Examples of electrical and electronic devices include, but are not limited to, connectors, contactors, switches, flexible and non-flexible printed circuit boards.

[0062] Examples of oil and gas related components include, but are not limited to, compressor rings, poppets, back-up seal rings, electrical connectors, labyrinth seals, motor end plates, bearings, bushings, suck rod guides, and downhole tubing.

[0063] Examples of automotive parts include, but are not limited to, thermal management system components (such as, but not limited to, thermostat housings, water inlet / outlet valves, water pumps, water pump impellers, and heater cores and end caps), air management system components (such as, but not limited to, turbocharger actuators, turbocharger bypass valves, turbocharger hoses, EGR valves, CAC housings, exhaust gas recirculation systems, electronically controlled throttle valves, and hot air ducts), transmission and launch gear components (such as, but not limited to, dual clutch transmissions, automated manual transmissions, continuously variable transmissions, automatic transmissions, torque converters, dual mass flywheels, power take-offs, clutch cylinders, seal rings, thrust washers, thrust bearings, needle bearings, and check balls), automotive electronics, automotive lighting components (such as, but not limited to, motor end caps, sensors, ECU housings, bobbins, and solenoids). , connectors, circuit protection / relays, actuator housings, Li-ion battery systems, and fuse boxes), traction motors and power electronics components (such as, but not limited to, battery packs), fuel and selective catalytic reduction ("SCR") systems (such as, but not limited to, SCR module housings and connectors, SCR module housings and connectors, fuel flanges, rollover valves, quick connects, filter housings, fuel rails, fuel delivery modules, fuel hoses, fuel pumps, fuel injector O-rings, and fuel hoses), fluid system components (e.g., fuel system components) (such as, but not limited to, inlet and outlet valves, and fluid pump components), interior components (such as, but not limited to, dashboard components, display components, and seat components), and structural and lightweight components (such as, but not limited to, gears and bearings, sunroofs, brackets and mounts, electric battery housings, thermal management components, braking system elements, and pumps and EGR systems).

[0064] Articles can be molded from the PAS polymer or polymer composition (PC) by any process compatible with thermoplastics, such as extrusion, injection molding, blow molding, rotational molding or compression molding.

[0065] Articles can be printed from PAS polymers or polymer compositions (PC), for example by a process comprising a step of extrusion of the material in the form of a filament, or by a process comprising a step of laser sintering of the material, in which case the material is in powder form.

[0066] In some embodiments, the PAS polymer or polymer composition (PC) may be desirably incorporated into three-dimensional printing applications. One application relates to a method for producing a three-dimensional ("3D") object with an additive manufacturing system, comprising providing a part material comprising the PAS polymer or polymer composition (PC) and printing layers of the three-dimensional object from the part material.

[0067] Thus, the PAS polymer or polymer composition (PC) may be in the form of a thread or filament for use in the process of 3D printing, for example fused filament manufacturing (also known as fused deposition modeling "FDM").

[0068] The PAS polymer or polymer composition (PC) may be in the form of a powder, for example a substantially spherical powder, for use in 3D printing, for example in the process of selective laser sintering (SLS).

[0069] The PAS polymer or polymer composition (PC) can be incorporated into a composite material. The composite material includes continuous reinforcing fibers embedded in a thermoplastic matrix. In some embodiments, the continuous reinforcing fibers are selected from glass fibers, carbon fibers, aluminum fibers, titanium fibers, magnesium fibers, boron carbide fibers, rock wool fibers, steel fibers, aramid fibers, natural fibers (e.g., cotton, linen, and wood), and any combination of one or more of these. Preferably, the continuous reinforcing fibers are glass fibers or carbon fibers. As used herein, continuous reinforcing fibers are reinforcing fibers having an average length in their longest dimension of at least 5 millimeters ("mm"), at least 10 mm, at least 25 mm, or at least 50 mm. The thermoplastic matrix includes the PAS polymer or polymer composition (PC). The composite material can be a unidirectional composite (e.g., a tape) or a multidirectional composite (e.g., a woven fabric, mat, or layered fabric).

[0070] The use of the PAS polymers and polymer compositions (PC) or articles for manufacturing the above-mentioned articles is also envisaged, as is the use of the above-mentioned PAS polymers or polymer compositions (C) for 3D printing objects. EXAMPLES

[0071] This example demonstrates the synthesis and thermal and impact performance of the PAS polymers described herein.

[0072] raw materials 1-Methyl-2-pyrrolidone ("NMP") (>99.0%): obtained from TCI Sodium hydrogen sulfide ("NaSH") (55-60% by weight): available from AkzoNobel 1,4-Dichlorobenzene ("DCB") (≧99): obtained from Alfa Aesar Sodium hydroxide (≥97.0%): obtained from Fisher Chemical Sodium acetate (≥99%): obtained from VWR Chemicals 3,5-Dichloroaniline ("3,5-DCA") (≥98%): Obtained from Alfa Aesar 3,6-Dibromocarbazole ("3,6-DBC") (≥98.0%): obtained from TCI 2,7-Dibromocarbazole ("2,7-DBC") (≥97%): obtained from AccelaChemBio

[0073] Synthesis of PAS polymer Example 1: (2.5 mol% 2,7-DBC co-PAS) A 1 L autoclave reactor was charged with 31.25 g sodium hydroxide (0.781 mol), 20.74 g sodium acetate (0.253 mol), 74.05 g NaSH (58.00 wt%, 0.766 mol), 6.22 g 2,7-DBC (0.019 mol), and 205 mL NMP. The reactor was purged and pressurized to 10 psig with nitrogen and set for continuous stirring at 400 rpm. A separate addition vessel was charged with 109.80 g DCB (0.747 mol) and 50 g NMP. The addition vessel was purged and pressurized to 90 psig with nitrogen and heated to 100°C. The reactor was heated to 240°C at 1.5°C / min. After reaching 150°C, the reactor was passed through a condenser and approximately 40 mL of clear condensate was collected under a small nitrogen flow (60 mL / min) until the reactor reached 200°C. At this point the condenser was removed, the nitrogen flow was stopped, and the DCB / NMP mixture in the addition vessel was quickly added to the reactor. The addition vessel was charged with an additional 30 mL of NMP, purged and pressurized to 90 psig with nitrogen, and the contents were immediately added to the reactor. The sealed reactor was held at 240°C for 2 hours, heated to 265°C at 1.5°C / min, held at 265°C for 2 hours, cooled to 200°C at 1.0°C / min, and finally allowed to cool to room temperature. The resulting slurry was diluted with 200 mL of NMP, removed from the reactor, heated to 80°C, and filtered through a medium porosity sintered glass filter. The filter cake was washed once with 100 mL of warm NMP (60°C). The solid was stirred in 300 mL of heated DI water (70° C.) for 15 minutes and filtered through a medium porosity glass filter. This process was repeated a total of five times. The rinsed solid was dried in a vacuum oven under nitrogen at 100° C. overnight to give 77.15 g of a white granular solid. GPC, DSC, ASTM Type V tensile, and ASTM notched Izod data for this and subsequent examples are shown in the table below.

[0074] Example 2: (5 mol% 2,7-DBC co-PAS) Synthesized according to the procedure of Example 1 using 31.52 g sodium hydroxide (0.788 mol), 20.92 g sodium acetate (0.255 mol), 74.68 g NaSH (58.00 wt%, 0.773 mol), 12.55 g 2,7-DBC (0.039 mol), 107.89 g DCB (0.734 mol), and a total of 287 mL NMP. 83.30 g of a fine white granular solid was obtained.

[0075] Example 3: (10 mol% 2,7-DBC co-PAS) Synthesized according to the procedure of Example 1 using 31.35 g sodium hydroxide (0.784 mol), 20.80 g sodium acetate (0.254 mol), 72.76 g NaSH (59.21 wt%, 0.768 mol), 24.97 g 2,7-DBC (0.077 mol), 101.66 g DCB (0.692 mol), and a total of 286 mL NMP. 82.60 g of a white powder was obtained.

[0076] Counterexample 1: (PAS homopolymer) Synthesized according to the procedure of Example 1 (except that 2,7-DBC was not used) using 45.89 g sodium hydroxide (1.147 mol), 30.45 g sodium acetate (0.371 mol), 106.95 g NaSH (58.96 wt%, 1.125 mol), 165.34 g DCB (1.125 mol), and a total of 418 mL NMP. 112.60 g of a granular white solid was obtained.

[0077] Counterexample 2: (10 mol% 3,5-DCA co-PAS) was synthesized according to the procedure of Example 1 (except that 3,5-DCA was used instead of 2,7-DBC) using 37.30 g sodium hydroxide (0.932 mol), 24.75 g sodium acetate (0.302 mol), 86.56 g NaSH (59.21 wt%, 0.914 mol), 14.81 g 3,5-DCA (0.091 mol), 120.95 g DCB (0.823 mol), and a total of 340 mL NMP. The polymerization resulted in a higher than normal maximum pressure (170 psig vs. typical 150 psig). The reaction mixture was a brown sludge with a strong odor of thiophenol and other decomposition species. Rinsing yielded a light brown powder.

[0078] Counterexample 3: (10 mol% 3,6-DBC co-PAS) was synthesized according to the procedure of Example 1 (except that 3,6-DBC was used instead of 2,7-DBC) using 31.17 g sodium hydroxide (0.779 mol), 20.69 g sodium acetate (0.252 mol), 72.35 g NaSH (59.21 wt%, 0.764 mol), 24.83 g 3,6-DBC (0.076 mol), 101.09 g DCB (0.688 mol), and a total of 204 mL NMP. The polymerization resulted in a higher than normal maximum pressure (170 psig vs. typical 150 psig). The reaction mixture was a brown sludge with a strong odor of thiophenol and other decomposition species. Rinsing yielded a light brown powder.

[0079] Test Method Thermal performance: T g , T m , and ΔH f was determined using differential scanning calorimetry ("DSC") according to ASTM D3418 using heating and cooling rates of 20°C / min. Three scans were used for each DSC test: a first heat to 350°C, followed by a first cool to 30°C, followed by a second heat to 350°C. g , T m , and ΔH f was determined from the second heat.

[0080] Molecular weight: M w was determined by gel permeation chromatography (GPC) at 210° C. using a PL 220 high temperature GPC with a 1-chloronaphthalene mobile phase and polystyrene standards.

[0081] Impact Performance: Notched Izod values ​​were determined according to ASTM D256 using a 0.125 inch bend bar at room temperature.

[0082] Thermal and shock performance The test results are shown in Table 1. In the table, "E" indicates an example and "CE" indicates a counter example. [Table 1]

[0083] With reference to Table 1, a comparison of E3 and CE2 indicates that conventional approaches to incorporating amine moieties into PAS polymers do not provide sufficient molecular weight at desirable monomer concentrations. For example, CE2, with 10 mol % repeat units formed from 3,5-DCA, had a molecular weight of 4,300 g / mol. On the other hand, E3, with 10 mol % repeat units formed from 2,7-DBC, had a molecular weight of 40,900 g / mol, which corresponds to a high molecular weight PAS. Similarly, a comparison of E3 and CE3 demonstrates that high molecular weight PAS polymers can only be obtained when the halogens of the dihalocarbazole-containing monomer are in the 2,7-position. CE3, with 10 mol % repeat units formed from 3,6-DBC, had a molecular weight of only 3,600 g / mol. On the other hand, E3, with 10 mol % repeat units formed from 2,7-DBC, had a molecular weight of 40,900 g / mol. Surprisingly, the sample containing only 2.5 mol % 2,7-DCB (E1) exhibited improved impact strength compared to the PAS homopolymer (CE1). w is too low g No measurements were obtained (recorded above as "not observed").

[0084] The above embodiments are intended to be illustrative and not limiting. Further embodiments are within the concept of the present invention. In addition, although the present invention has been described with reference to specific embodiments, those skilled in the art will recognize that changes in form and detail may be made without departing from the spirit and scope of the present invention. Any incorporation by reference of the above documents is limited so that subject matter contrary to the express disclosure herein is not incorporated.

Claims

1. Repeating units R each represented by the following formula PAS1 and R PAS2 and a poly(arylene sulfide) ("PAS") polymer comprising: [-Ar 1 -S-], (1) [-Ar 2 -S-], (2) (In the formula, --Ar 1 - is the following formula [Formula 1] selected from the group consisting of: --Ar 2 - is the following formula [chemical 2] Represented by: R and R' are in each case C 1 ~C 12 Alkyl group, C 7 ~C 24 Alkylaryl group, C 7 ~C 24 Aralkyl group, C 6 ~C 24 Arylene group, and C 6 ~C 18 aryloxy groups; - T is a bond, -CO-, -SO 2 -, -O-, -C(CH 3 ) 2 , phenyl, and -CH 2 - selected from the group consisting of; - i, at each occurrence, is an independently selected integer from 0 to 4; j and k, at each occurrence, are independently selected integers from 0 to 3.

2. -Ar 1 - is of the following formula: [C3] The PAS polymer according to claim 1 ,

3. The PAS polymer of claim 1 or 2, wherein k at each position is zero.

4. The ratio of the number of repeating units in the PAS polymer to the total number of repeating units in the PAS polymer (R PAS2 4. The PAS polymer according to claim 1, wherein the concentration of said polyether ether is 0.5 mol % to 15 mol %.

5. The ratio of the number of repeating units in the PAS polymer to the total number of repeating units in the PAS polymer (R PAS2 5. The PAS polymer according to claim 1, wherein the concentration of said polyphenylene sulfide is 0.5 mol % to 8 mol %.

6. T of at least 95°C g The PAS polymer according to any one of claims 1 to 5, comprising:

7. T of at least 200° C. m The PAS polymer according to any one of claims 1 to 6, comprising:

8. The PAS polymer of any one of claims 1 to 7 comprising an impact strength of at least 30 J / g determined according to ASTM D256.

9. A polymer composition (PC) comprising a PAS polymer according to any one of claims 1 to 8 and an additional polymer comprising functional groups selected from the group consisting of carboxylic acids, carboxylates, anhydrides, epoxides, urethanes, amides, ketones, isocyanates, ureas, halogens, activated ethers, esters, and acid chlorides.

10. 10. The polymer composition (PC) according to claim 9, wherein said additional polymer is a thermoplastic polymer.

11. 10. The polymer composition (PC) according to claim 9, wherein said additional polymer is a thermosetting polymer or a thermosetting precursor.

12. 12. The polymer composition (PC) of claim 11, wherein said additional polymer is selected from the group consisting of epoxy resins, epoxy novolac resins, benzoxazines, bismaleimides, polyamic acid solutions, polyester thermosets, vinyl esters, cyanate esters, and urea-formaldehyde resins.

13. A polymer composition (PC) according to any one of claims 10 to 12, further comprising a fibrous reinforcing filler or toughening agent.

14. An automotive or aerospace component comprising a PAS polymer according to any one of claims 1 to 8 or a polymer composition (PC) according to any one of claims 9 to 13.

15. In the reaction mixture, The following formula: 1 -Ar 1 -X 2 a dihaloaromatic monomer having the formula The following formula: 3 -Ar 2 -X 4 a dihalocarbazole-containing monomer having the formula: Sulfur compounds, A method for producing the PAS polymer according to any one of claims 1 to 8, comprising reacting -X 1 ~X 4 are independently selected halogens; --Ar 1 - is the following formula [C4] selected from the group consisting of: --Ar 2 - is the following formula [C5] Represented by: R and R' are, in each case, C 1 ~C 12 Alkyl group, C 7 ~C 24 Alkylaryl group, C 7 ~C 24 Aralkyl group, C 6 ~C 24 Arylene group, and C 6 ~C 18 aryloxy groups; T is a bond, -CO-, -SO 2 -, -O-, -C(CH 3 ) 2 , phenyl, and -CH 2 - selected from the group consisting of; i, at each occurrence, is an independently selected integer from 0 to 4; j and k, at each occurrence, are independently selected integers from 0 to 3; the sulfur compound is selected from the group consisting of thiosulfates, thioureas, thioamides, elemental sulfur, thiocarbamates, metal disulfides and oxysulfides, thiocarbonates, organic mercaptans, organic mercaptides, organic sulfides, alkali metal sulfides and disulfides, and hydrogen sulfide.

Citation Information

Patent Citations

  • Polyarylene sulfide having the terminal treated wite sulfonic acid and / or sulfonic acid derivative group

    JP1990294332A

  • Polyarylene sulfide polymer alloy

    JP1992001268A

  • New aromatic compound and polyarylene-based copolymer having nitrogen-containing aromatic ring

    JP2010031231A

  • Arylene sulfide polymers

    US5296579A