Method for producing optical resin composition

Heat-treating fluoropolymers in low water vapor conditions addresses coloring and water absorption issues in optical resin compositions, enhancing their performance for optical applications.

JP7571264B2Active Publication Date: 2024-10-22NITTO DENKO CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023201174
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-11-29
Publication Date
2024-10-22
Estimated Expiration
2039-12-04

AI Technical Summary

Technical Problem

Optical resin compositions containing fluoropolymers experience coloring and increased water absorption during heat molding due to terminal groups derived from the polymerization initiator, leading to light absorption loss.

Method used

A method involving heat treatment of fluoropolymers in an atmosphere with a water vapor concentration of 100 volppm or less to thermally decompose and remove terminal groups, thereby suppressing coloring and water absorption.

Benefits of technology

The method produces an optical resin composition with low water absorption and minimal coloring, resulting in high internal transmittance and reduced light scattering, suitable for optical members.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571264000001
    Figure 0007571264000001
  • Figure 0007571264000002
    Figure 0007571264000002
  • Figure 0007571264000003
    Figure 0007571264000003
Patent Text Reader

Abstract

To provide a manufacturing method of an optical resin composition with sufficiently low water absorption while preventing pigmentation.SOLUTION: A manufacturing method of an optical resin composition includes conducting a heat treatment under an atmosphere with a concentration of moisture vapor 100 vol ppm or less, with regard to a fluorine-containing polymer obtained by polymerizing a monomer group including a fluorine-containing compound having a carbon-carbon double bond by an organic peroxide. For instance, in the manufacturing method of an optical resin composition, a heat treatment is conducted to a terminal group of the fluorine-containing polymer to apply thermal decomposition, while a low molecular weight compound generated at the thermal decomposition is vaporized.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an optical resin composition and an optical resin composition. [Background technology]

[0002] Resin compositions containing fluorinated polymers are used in a wide range of fields as materials for optical components such as plastic optical fibers (hereinafter referred to as "POF") and exposure components. In this specification, resin compositions used as materials for optical components are referred to as "optical resin compositions".

[0003] The fluorine-containing polymer can be prepared, for example, by polymerizing a monomer group containing a fluorine-containing compound having a carbon-carbon double bond with a polymerization initiator. As the polymerization initiator for polymerizing the monomer group containing the fluorine-containing compound, an organic peroxide is generally used. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 4160918 Summary of the Invention [Problem to be solved by the invention]

[0005] When producing an optical component, the optical resin composition is, for example, heated and melted to be molded, and coloring may occur during this heat molding. This coloring is particularly noticeable when a bulk optical resin composition is heated and melted. According to the present inventors' investigations, it was found that the cause of coloring of the optical resin composition is the terminal group of the fluorine-containing polymer derived from the polymerization initiator.

[0006] Based on this finding, the present inventors have further investigated and found that if the terminal groups of the fluorine-containing polymer are decomposed in advance, the coloring of the optical resin composition can be suppressed while the water absorption of the optical resin composition is increased. In the field of optical components, it is known that water increases the absorption loss of light (for example, Patent Document 1).

[0007] Therefore, an object of the present invention is to provide a method for producing an optical resin composition which is suppressed from being discolored and has sufficiently low water absorbency. [Means for solving the problem]

[0008] The present invention relates to The present invention provides a method for producing an optical resin composition, which comprises subjecting a fluorine-containing polymer obtained by polymerizing a monomer group including a fluorine-containing compound having a carbon-carbon double bond with an organic peroxide to a heat treatment in an atmosphere having a water vapor concentration of 100 vol ppm or less. Effect of the Invention

[0009] According to the present invention, a method for producing an optical resin composition which is suppressed from being discolored and has sufficiently low water absorbency can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention will be described, but the following description is not intended to limit the present invention to a specific embodiment.

[0011] The method for producing an optical resin composition of this embodiment includes subjecting a fluoropolymer obtained by polymerizing a monomer group containing a fluorine-containing compound having a carbon-carbon double bond with an organic peroxide to a heat treatment in an atmosphere having a water vapor concentration of 100 volppm or less. In this specification, the fluoropolymer before the heat treatment is sometimes called "fluoropolymer (A)" and the fluoropolymer after the heat treatment is sometimes called "fluoropolymer (B)". The optical resin composition obtained by the production method of this embodiment contains the fluoropolymer (B).

[0012] The fluorine-containing polymer (A) before heat treatment has a terminal group derived from a polymerization initiator (organic peroxide). This terminal group is, for example, an ester group. As described later, the fluorine-containing compound has, for example, a carbon-carbon double bond located at a terminal, and all hydrogen atoms bonded to the carbon atoms constituting the double bond are substituted with fluorine atoms. The terminal group of the fluorine-containing polymer (A) formed from this fluorine-containing compound is, for example, represented by the following formula (4). [ka]

[0013] In formula (4), R i is determined depending on the structure of the organic peroxide, and is, for example, a hydrocarbon group having 1 to 12 carbon atoms. i The hydrogen atoms contained in the hydrocarbon group of R may be substituted with fluorine atoms. i The hydrocarbon group may contain an aromatic ring. For example, when perfluorobenzoyl peroxide is used as the organic peroxide, R i is a perfluorophenyl group. Note that "perfluoro" means that all hydrogen atoms bonded to carbon atoms are replaced with fluorine atoms.

[0014] When the fluoropolymer (A) is subjected to a heat treatment, the terminal groups of the fluoropolymer (A) are thermally decomposed. As an example, the terminal group represented by formula (4) undergoes a decomposition reaction represented by the following formula (5a): [ka]

[0015] Thus, in the production method of this embodiment, the terminal group of the fluoropolymer (A) can be converted to a functional group represented by the following formula (1) by heat treatment. In other words, the fluoropolymer (B) after heat treatment has a terminal group represented by the following formula (1). It is noted that the fluoropolymer (B) has a terminal group represented by the following formula (1) when measured by carbon-13 nuclear magnetic resonance spectroscopy ( 13 This may be confirmed by C-NMR. [ka]

[0016] In the atmosphere during the heat treatment, the water vapor concentration may be 100 volppm or less, and preferably 50 volppm or less. The atmosphere during the heat treatment preferably does not substantially contain water vapor, but the water vapor concentration may be 0.1 volppm or more.

[0017] The components contained in the atmosphere during the heat treatment are not particularly limited, but preferably contain an inert gas as a main component, and more preferably consist essentially of an inert gas. In this specification, "contains an inert gas as a main component" means that the inert gas is contained in the largest amount by weight in the atmosphere. "consists essentially of an inert gas" means that the content of the inert gas in the atmosphere is 95 wt% or more, preferably 99 wt% or more. Examples of the inert gas include nitrogen gas and argon gas, and nitrogen gas is preferred. It is preferred that the atmosphere during the heat treatment consists essentially of nitrogen gas. The heat treatment may be performed in a reduced pressure atmosphere or a vacuum atmosphere.

[0018] The temperature of the heat treatment is not particularly limited as long as the thermal decomposition of the terminal group of the fluoropolymer (A) proceeds, and is, for example, 100°C or more and 400°C or less, and preferably 200°C or more and 350°C or less. The time of the heat treatment is also not particularly limited, and may be, for example, 50 minutes or more, or 250 minutes or more. The time of the heat treatment may be 1500 minutes or less. The fluoropolymer (A) may or may not melt by the heat treatment. Before the heat treatment, the shape of the fluoropolymer (A) is not particularly limited, and may be, for example, powder.

[0019] The production method of this embodiment includes, for example, pyrolysis of a terminal group of the fluoropolymer (A) to produce a low molecular weight compound (e.g., R i -C(=O)-F) from the optical resin composition. The method for removing the low molecular weight compound from the optical resin composition is not particularly limited. For example, the conditions (temperature, time, etc.) of the heat treatment may be appropriately set to remove the low molecular weight compound from the optical resin composition by volatilizing the low molecular weight compound. In other words, in the production method of the present embodiment, the end group of the fluorine-containing polymer (A) may be thermally decomposed by the heat treatment, and the low molecular weight compound generated by the thermal decomposition may be volatilized. When the fluorine-containing polymer (A) is melted by the heat treatment, if the height of the liquid surface of the molten fluorine-containing polymer (A) is 1 mm or less, the low molecular weight compound generated by the thermal decomposition is likely to volatilize. In the optical resin composition, the weight concentration of the low molecular weight compound generated by the thermal decomposition of the end group of the fluorine-containing polymer (A) is, for example, 1% or less.

[0020] As described above, in the production method of this embodiment, the end groups of the fluorine-containing polymer (A) derived from the organic peroxide are thermally decomposed by heat treatment. That is, the fluorine-containing polymer (B) contained in the optical resin composition has almost no end groups derived from the organic peroxide. Therefore, in the stage of heat-molding the optical resin composition into an optical component, low molecular weight compounds are hardly generated by thermal decomposition of the end groups derived from the organic peroxide. According to the study by the present inventors, if low molecular weight compounds are generated in the stage of heat-molding the optical resin composition into an optical component, the optical resin composition tends to be colored. According to the production method of this embodiment, the above-mentioned low molecular weight compounds can be removed in advance, and thus an optical resin composition with suppressed coloring can be obtained.

[0021] Furthermore, in the production method of this embodiment, the heat treatment is carried out in an atmosphere in which the concentration of water vapor is 100 vol ppm or less. Therefore, the end group of the fluoropolymer (B) can be suppressed from being further hydrolyzed during the heat treatment. If the end group represented by formula (1) is hydrolyzed, a carboxyl group is formed by the reaction represented by the following formula (5b). A functional group containing an OH group such as a carboxyl group tends to increase the water absorption of the optical resin composition. According to the production method of this embodiment, the hydrolysis of the end group of the fluoropolymer (B) is suppressed, so that the increase in the water absorption of the optical resin composition can be suppressed and the water absorption can be maintained at a sufficiently low level. [ka]

[0022] When a functional group containing an OH group such as a carboxyl group is formed, the density fluctuation within the molecule of the fluoropolymer increases. The density fluctuation within the molecule can cause light scattering. In the production method of this embodiment, the hydrolysis of the terminal group of the fluoropolymer (B) is suppressed, thereby suppressing an increase in the density fluctuation within the molecule, and thus it is possible to suppress an increase in the scattering of light by the optical resin composition.

[0023] [Fluorine-containing compounds] The fluorine-containing compound contained in the monomer group is not particularly limited as long as it contains a carbon-carbon double bond and a fluorine atom.From the viewpoint of suppressing light absorption due to the stretching energy of C-H bond, it is preferable that the fluorine-containing compound does not substantially contain hydrogen atoms, and it is particularly preferable that all hydrogen atoms bonded to carbon atoms are replaced with fluorine atoms.In this specification, the fluorine-containing compound does not substantially contain hydrogen atoms means that the content of hydrogen atoms in the total amount of the fluorine-containing compound contained in the monomer group is 1 mol% or less.

[0024] The carbon-carbon double bond contained in the fluorine-containing compound is preferably located at a terminal of the fluorine-containing compound, and further, all hydrogen atoms bonded to the carbon atoms constituting the double bond are preferably substituted with fluorine atoms.

[0025] The fluorine-containing compound preferably has a fluorine-containing aliphatic ring structure. The fluorine-containing compound may have a polymerizable double bond between a carbon atom constituting a ring and a carbon atom not constituting a ring, or may have a polymerizable double bond between two carbon atoms constituting a ring. Examples of the fluorine-containing compound having a polymerizable double bond between a carbon atom constituting a ring and a carbon atom not constituting a ring include fluorine-containing compounds having a 1,3-dioxolane structure such as perfluoro-2-methylene-4-methyl-1,3-dioxolane. Examples of the fluorine-containing compound having a polymerizable double bond between two carbon atoms constituting a ring include fluorine-containing compounds having a 1,3-dioxole structure such as perfluoro-4-methyl-1,3-dioxole and perfluoro-4-methyl-1,3-dioxole.

[0026] The fluorine-containing compound can be obtained by a known production method, for example, the production method disclosed in JP-A-2007-504125. An example of the fluorine-containing compound having a fluorine-containing alicyclic structure is a compound represented by the following formula (2). [ka]

[0027] In formula (2), R ff 1 ~R ff 4 R each independently represents a fluorine atom, a perfluoroalkyl group having 1 to 7 carbon atoms, or a perfluoroalkyl ether group having 1 to 7 carbon atoms. ff 1 and R ff 2 may be linked to form a ring. In formula (2), the number of carbon atoms in the perfluoroalkyl group is preferably 1 to 5, more preferably 1 to 3, and further preferably 1. The perfluoroalkyl group may be linear or branched. Examples of the perfluoroalkyl group include a trifluoromethyl group, a pentafluoroethyl group, and a heptafluoropropyl group.

[0028] In the formula (2), the number of carbon atoms in the perfluoroalkyl ether group is preferably 1 to 5, and more preferably 1 to 3. The perfluoroalkyl ether group may be linear or branched. Examples of the perfluoroalkyl ether group include a perfluoromethoxymethyl group.

[0029] R ff 1 and R ff 2 When they are linked to form a ring, the ring may be a 5-membered ring or a 6-membered ring. Examples of the ring include a perfluorotetrahydrofuran ring, a perfluorocyclopentane ring, and a perfluorocyclohexane ring.

[0030] Specific examples of the compound represented by the above formula (2) include compounds represented by the following formulae (M1) to (M8). [ka]

[0031] The compound represented by formula (2) is preferably a compound represented by formula (M2), ie, a compound represented by the following formula (3), among the compounds represented by the above formulas (M1) to (M8).

[0032] [ka]

[0033] The fluorine-containing compound contained in the monomer group may be one kind or two or more kinds. That is, the fluorine-containing polymer (A) may be a fluorine-containing polymer obtained by homopolymerizing one kind of fluorine-containing compound, or a fluorine-containing copolymer obtained by copolymerizing two or more kinds of fluorine-containing compounds.

[0034] The fluorine-containing polymer (A) may be, for example, a fluorine-containing copolymer obtained by copolymerizing the above-mentioned fluorine-containing compound having a fluorine-containing alicyclic structure (hereinafter referred to as fluorine-containing compound (a)) with a fluorine-containing compound other than the fluorine-containing compound (a). Examples of the fluorine-containing compound other than the fluorine-containing compound (a) include the following fluorine-containing compounds (b) to (d).

[0035] The fluorine-containing compound (b) is a fluorine-containing vinyl ether such as perfluorovinyl ether, etc. The fluorine-containing vinyl ether is represented, for example, by the following formula (6). [ka]

[0036] In formula (6), R 1 ~R 3 Each independently represents a fluorine atom or a perfluoroalkyl group having 1 to 7 carbon atoms. 4represents a perfluoroalkyl group having 1 to 7 carbon atoms. The perfluoroalkyl group may have a ring structure. Some of the fluorine atoms may be substituted with halogen atoms other than fluorine atoms. Some of the fluorine atoms in the perfluoroalkyl group may be substituted with halogen atoms other than fluorine atoms.

[0037] The fluorine-containing compound (c) is a fluorine-containing olefin such as tetrafluoroethylene, chlorotrifluoroethylene, etc. The fluorine-containing olefin is represented, for example, by the following formula (7). [ka]

[0038] In formula (7), R 5 ~R 8 each independently represents a fluorine atom or a perfluoroalkyl group having 1 to 7 carbon atoms. The perfluoroalkyl group may have a ring structure. Some of the fluorine atoms may be substituted with halogen atoms other than fluorine atoms. Some of the fluorine atoms in the perfluoroalkyl group may be substituted with halogen atoms other than fluorine atoms.

[0039] The fluorine-containing compound (d) is a fluorine-containing compound which has two or more polymerizable double bonds and can undergo cyclopolymerization. The fluorine-containing compound (d) is represented, for example, by the following formula (8). [ka]

[0040] In formula (8), Z is an oxygen atom, a single bond, or -OC(R 19 R 20 )O-, R 9 ~R 20each independently represents a fluorine atom, a perfluoroalkyl group having 1 to 5 carbon atoms, or a perfluoroalkoxy group having 1 to 5 carbon atoms. Some of the fluorine atoms may be substituted with halogen atoms other than fluorine atoms. Some of the fluorine atoms in the perfluoroalkyl group may be substituted with halogen atoms other than fluorine atoms. Some of the fluorine atoms in the perfluoroalkoxy group may be substituted with halogen atoms other than fluorine atoms. s and t each independently represent an integer of 0 to 5, and s+t is an integer of 1 to 6 (with the proviso that Z is -OC(R 19 R 20 )O-, s+t may be 0.

[0041] As the fluorine-containing compound (d), a fluorine-containing compound represented by the following formula (9) may be used. The fluorine-containing compound represented by the following formula (9) is the compound represented by the above formula (8) in which Z is an oxygen atom, s is 0, and t is 2. [ka]

[0042] In formula (9), R 141 , R 142 , R 151 , and R 152 each independently represents a fluorine atom, a perfluoroalkyl group having 1 to 5 carbon atoms, or a perfluoroalkoxy group having 1 to 5 carbon atoms. Some of the fluorine atoms may be substituted with halogen atoms other than fluorine atoms. Some of the fluorine atoms in the perfluoroalkyl group may be substituted with halogen atoms other than fluorine atoms. Some of the fluorine atoms in the perfluoroalkoxy group may be substituted with halogen atoms other than fluorine atoms.

[0043] Specific examples of the fluorine-containing compound (d) include the following compounds. CF 2 =CFOCF 2 CF=CF 2 CF 2 =CFOCF(CF 3 )CF=CF 2 CF 2 =CFOCF 2 CF 2 CF=CF 2 CF 2 =CFOCF 2 CF(CF 3 )CF=CF 2 CF 2 =CFOFCF(CF 3 )CF 2 CF=CF 2 CF 2 =CFOCFClCF 2 CF=CF 2 CF 2 =CFOCCl 2 CF 2 CF=CF 2 CF 2 =CFOCF 2 OCF=CF 2 CF 2 =CFOC(CF 3 ) 2 OCF=CF 2 CF 2 =CFOCF 2 CF(OCF 3 )CF=CF 2 CF 2 =CFCF 2 CF=CF 2 CF 2 =CFCF 2 CF 2 CF=CF 2 CF 2 =CFCF 2 OCF 2 CF=CF 2 CF 2 =CFOCF 2 CFClCF=CF 2 CF 2 =CFOCF 2 CF 2 CCl=CF 2 CF 2 =CFOCF 2 CF 2 CF = CFCl CF 2 =CFOCF 2 CF(CF 3 )CCl=CF 2 CF 2 =CFOCF 2 OCF=CF 2 CF 2 =CFOCCl 2 OCF=CF 2 CF 2 =CClOCF 2 OCCl=CF 2

[0044] [Monomer group] The monomer group preferably contains the above-mentioned fluorine-containing compound as a main component, and more preferably consists essentially of the fluorine-containing compound. The monomer group may further contain other polymerizable compounds other than the fluorine-containing compound.

[0045] [Organic peroxide] In the manufacturing method of the present embodiment, the organic peroxide functions as a polymerization initiator for the monomer group. The organic peroxide preferably contains diacyl peroxide or a peroxide ester, and more preferably contains diacyl peroxide. The organic peroxide is preferably fluorinated. The organic peroxide is more preferably substantially free of hydrogen atoms and fully fluorinated. Here, the organic peroxide substantially free of hydrogen atoms means that the content of hydrogen atoms is 1 mol% or less relative to the total amount of the organic peroxide used. A preferred example of the organic peroxide is perfluorobenzoyl peroxide.

[0046] [Method for producing fluorine-containing polymer (A)] The fluorine-containing polymer (A) can be produced by polymerizing the above-mentioned monomer group using the above-mentioned organic peroxide. As the polymerization method, a known polymerization method can be used. For example, the above-mentioned monomer group can be radically polymerized by a conventional method to produce the fluorine-containing polymer (A).

[0047] [Fluorine-containing polymer] As described above, the fluorine-containing polymers (A) and (B) have different terminal groups. Except for the terminal groups, the structure of the fluorine-containing polymer (A) may be the same as that of the fluorine-containing polymer (B). Hereinafter, the structural units that the fluorine-containing polymers (A) and (B) have in common will be described.

[0048] The fluorine-containing polymer contains, for example, a structural unit (a) represented by the following formula (10). The structural unit (a) is derived from the above-mentioned fluorine-containing compound (a). In formula (10), R ff 1 ~R ff 4 is the same as equation (2). [ka]

[0049] Specific examples of the structural unit (a) include structural units represented by the following formulas (a1) to (a8). [ka]

[0050] Of the structural units represented by the above formulas (a1) to (a8), the structural unit (a) is preferably the structural unit (a2), that is, the structural unit represented by the following formula (11). [ka]

[0051] The fluorine-containing polymer may contain one or more kinds of structural units (a). In the fluorine-containing polymer, the content of the structural unit (a) is preferably 20 mol% or more, more preferably 40 mol% or more, based on the total of all structural units. When the structural unit (a) is contained in an amount of 20 mol% or more, the fluorine-containing polymer tends to have higher heat resistance. When the structural unit (a) is contained in an amount of 40 mol% or more, the fluorine-containing polymer tends to have higher transparency and high mechanical strength in addition to high heat resistance. In the fluorine-containing polymer, the content of the structural unit (a) is preferably 95 mol% or less, more preferably 70 mol% or less, based on the total of all structural units.

[0052] The fluorine-containing polymer may further contain other structural units in addition to the structural unit (a). Examples of the other structural units include the following structural units (b) to (d).

[0053] The structural unit (b) is represented by the following formula (12). The structural unit (b) is derived from the above-mentioned fluorine-containing compound (b). In formula (12), R 1 ~R 4 is the same as equation (6). [ka]

[0054] The fluorine-containing polymer may contain one or more types of structural unit (b). In the fluorine-containing polymer, the content of the structural unit (b) is preferably 5 to 10 mol% based on the total of all structural units. The content of the structural unit (b) may be 9 mol% or less, or may be 8 mol% or less.

[0055] The structural unit (c) is represented by the following formula (13). The structural unit (c) is derived from the above-mentioned fluorine-containing compound (c). In formula (13), R 5 ~R 8 is the same as equation (7). [ka]

[0056] The fluorine-containing polymer may contain one or more types of structural unit (c). In the fluorine-containing polymer, the content of the structural unit (c) is preferably 5 to 10 mol% based on the total of all structural units. The content of the structural unit (c) may be 9 mol% or less, or may be 8 mol% or less.

[0057] The structural unit (d) is represented by the following formula (14). The structural unit (d) is derived from the above-mentioned fluorine-containing compound (d). In formula (14), Z, R 9 ~R 18 , s and t are the same as in equation (8). [ka]

[0058] The structural unit (d) is preferably represented by the following formula (15). The structural unit (d) represented by the following formula (15) is derived from a fluorine-containing compound represented by formula (9). In formula (15), R 141 , R 142 , R 151 , and R 152 is the same as equation (9). [ka]

[0059] The fluorine-containing polymer may contain one or more types of structural unit (d). In the fluorine-containing polymer, the content of the structural unit (d) is preferably 30 to 67 mol% based on the total of all structural units. The content of the structural unit (d) is, for example, 35 mol% or more, and may be 60 mol% or less, or may be 55 mol% or less.

[0060] The fluorine-containing polymer may further contain other structural units than the structural units (a) to (d), but preferably does not substantially contain other structural units than the structural units (a) to (d). The term "fluorine-containing polymer does not substantially contain other structural units than the structural units (a) to (d)" means that the total of the structural units (a) to (d) is 95 mol % or more, preferably 98 mol % or more, based on the total of all structural units in the fluorine-containing polymer.

[0061] The glass transition temperature (Tg) of the fluoropolymer is not particularly limited and is, for example, 100° C. to 140° C., and may be 105° C. or higher, or 120° C. or higher. In this specification, Tg refers to the midpoint glass transition temperature (T mg )

[0062] [Optical resin composition] The optical resin composition obtained by the production method of this embodiment preferably contains the fluoropolymer (B) and consists essentially of the fluoropolymer (B). The optical resin composition may further contain additives such as a refractive index adjuster.

[0063] As described above, according to the manufacturing method of this embodiment, hydrolysis of the terminal group of the fluorine-containing polymer (B) is suppressed, so that the water absorption of the optical resin composition is sufficiently low. The water absorption of the optical resin composition is, for example, 0.1% or less, and preferably 0.05% or less. The water absorption of the optical resin composition can be specified by the following method. First, the optical resin composition is set as a measurement sample in a commercially available moisture adsorption / desorption measuring device. Next, the measurement sample is held for 600 minutes under conditions of 85°C and 0% RH, and further held for 600 minutes under conditions of 85°C and 85% RH. At this time, when the measurement sample absorbs water vapor in the device (moisture absorption), the weight of the measurement sample increases. The ratio of the increase in the weight of the measurement sample due to the moisture absorption treatment to the weight of the measurement sample after the moisture absorption treatment is specified as the water absorption rate.

[0064] Furthermore, since the water absorption of the optical resin composition is sufficiently low, the water content (moisture content) in the optical resin composition is also maintained at a low level. The moisture content of the optical resin composition is, for example, 0.1 wt% or less, preferably 0.07 wt% or less, and more preferably 0.05 wt% or less. The lower limit of the moisture content of the optical resin composition is not particularly limited, and is, for example, 0.01 wt%.

[0065] According to the optical resin composition obtained by the manufacturing method of this embodiment, coloring is unlikely to occur when the composition is heated and molded into an optical member. Furthermore, since the water content of the optical resin composition is low, the absorption loss of light due to the water contained in the optical resin composition is low. Therefore, when a molded body is produced from the optical resin composition, the internal transmittance of the molded body is sufficiently low. As an example, the internal transmittance of a plate-shaped molded body having a thickness of 10 mm produced from the optical resin composition for light with a wavelength of 850 nm is, for example, 98% or more, preferably 99% or more. In this specification, the internal transmittance means the transmittance that does not include the reflection loss due to the reflection (Fresnel reflection) of light on the surface of the molded body. The internal transmittance of the molded body can be specified in accordance with the provisions of the Japan Optical Glass Industry Association Standard (JOGIS) 17-2012. EXAMPLES

[0066] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto.

[0067] [Fluorine-containing polymer (A)] First, 22.6 g of perfluoro-2-methylene-4-methyl-1,3-dioxolane (a compound represented by formula (M2)) was dissolved in 50 mL of 1,1,1,2,2,3,4,5,5,5-decafluoropentane (Bertrel XF manufactured by Mitsui-Chemours Fluoroproducts) under an argon atmosphere at room temperature (20°C ± 15°C). While maintaining the argon atmosphere, 0.155 g of perfluorobenzoyl peroxide was added to the obtained solution and mixed by stirring. Next, dissolved oxygen was removed from the solution by freeze degassing. The solution was heated to 40°C with stirring and reacted for 72 hours. The obtained reaction mixture was added to 300 mL of chloroform. The precipitate formed by this operation was collected by filtration. The residue obtained was a polymer of perfluoro-2-methylene-4-methyl-1,3-dioxolane (fluorine-containing polymer (A)). The amount of the fluoropolymer (A) obtained was 19.2 g, and the yield was 81.0%.

[0068] (Sample 1) First, aluminum foil was placed on an aluminum tray, and the powdered fluoropolymer (A) was placed on the shiny side of the aluminum foil. The tray was placed inside an oven, and the fluoropolymer (A) was heat-treated at 270°C for 5 hours under a nitrogen atmosphere. The nitrogen atmosphere was adjusted by feeding nitrogen into the oven at a flow rate of 1 L / min. The concentration of water vapor in the nitrogen atmosphere was 40 volppm. The fluoropolymer (A) was melted by the heat treatment. The height of the liquid surface of the molten fluoropolymer (A) was 1 mm or less. Furthermore, the end groups of the fluoropolymer (A) were thermally decomposed by the heat treatment, and the low molecular weight compounds generated by the thermal decomposition were volatilized. Thus, the optical resin composition of Sample 1 was obtained. The optical resin composition of Sample 1, which was cooled to room temperature, was in the form of a plate having a thickness of 1 mm or less.

[0069] (Sample 2) An optical resin composition of Sample 2 was obtained in the same manner as Sample 1, except that the heat treatment time was changed to 24 hours.

[0070] (Sample 3) Except for the fact that the heat treatment was carried out in the air, an optical resin composition of Sample 3 was obtained in the same manner as Sample 1. The water vapor concentration in the air was 1.4 vol%.

[0071] (Sample 4) An optical resin composition of Sample 4 was obtained in the same manner as Sample 3, except that the heat treatment time was changed to 24 hours.

[0072] [Water absorption rate] The water absorption rate was measured for the optical resin composition of Samples 1 to 4. First, a measurement sample of 1 cm square was cut out from the optical resin composition. This measurement sample was set in a moisture adsorption / desorption measuring device (IGA-SORP manufactured by Hiden). Next, the measurement sample was held for 600 minutes under the condition of 85°C and 0% RH, and further held for 600 minutes under the condition of 85°C and 85% RH. The ratio of the increase in the weight of the measurement sample due to the moisture absorption treatment to the weight of the measurement sample after the moisture absorption treatment was determined as the water absorption rate. The results are shown in Table 1. In Table 1, ◯ means that the water absorption rate is 0.05% or less. × means that the water absorption rate is greater than 0.05%.

[0073] [Internal transmittance] For the optical resin compositions of Samples 1 to 4, the internal transmittance of a 10 mm thick plate-shaped molded body made from the optical resin composition for light with a wavelength of 850 nm was specified by the following method in accordance with the provisions of JOGIS 17-2012. First, a cylinder was made from aluminum foil, and the bottom of the cylinder was sealed with polyimide tape. The inside of this cylinder was filled with the optical resin composition. Next, this cylinder was set in a rod-making container made of Hastelloy. The inside of the container was made into a vacuum atmosphere, and the temperature of the container was raised to 270°C over about 2 hours. After the temperature of the container reached 270°C, the container was heated at 270°C for 3 hours. Next, a rod was molded from the optical resin composition by slowly cooling the container to room temperature. The rod was a columnar shape with a bottom diameter of 20 mm and a thickness of 20 mm.

[0074] Next, a 5 mm thick disk D1 and a 12 mm thick disk D2 were cut out from the prepared rod using a diamond wheel saw. Next, the disk D1 was placed inside a sample cup. At this time, carbon tape was attached to the bottom surface of the disk D1, and the disk D1 was fixed to the sample cup by this carbon tape. Next, a resin composition (EPOFIX manufactured by Struers) was filled inside the sample cup, and the resin composition was cured. In this way, a measurement sample S1 was obtained. The measurement sample S1 had a cylindrical shape with a bottom diameter of 25 mm and a thickness of about 5 mm.

[0075] Next, the measurement sample S1 was set in a sample holder of an automatic benchtop polisher, and the following steps 1 to 6 were carried out on the bottom surface of the measurement sample S1 on the side where the carbon tape was attached. Step 1: Polish with "SIC PAPER #1000" and remove the carbon tape. Step 2: Polish for 5 minutes using a STRUERS "MD SAT 9μM". Step 3: Polish for 5 minutes using a STRUERS "MD SAT 6μM." Step 4: Polish with STRUERS' "MD DUR 3 μM" for 10 minutes. Step 5: Polish with STRUERS' "MD NAP 1 μM" for 5 minutes. Step 6: Polish for 5 minutes using STRUERS' MD CHEM OP-S.

[0076] The bottom surface polished in steps 1 to 6 was protected with filter paper. Next, the measurement sample S1 was set on a plane polishing jig, and the surface (top surface) facing the bottom surface of the measurement sample S1 was polished. This polishing was performed using "SiC Paper #220" until the thickness of the measurement sample S1 became approximately 4 mm. At this time, the thickness of the measurement sample S1 was confirmed by a digital micrometer. Furthermore, the top surface of the measurement sample S1 was polished using "SiC Paper #1000" until the thickness of the measurement sample S1 became approximately 3.5 mm. Furthermore, the above steps 2 to 6 were performed on the top surface of the measurement sample S1 to obtain a measurement sample S1 with a thickness of approximately 3.5 mm.

[0077] Next, a measurement sample S2 having a thickness of 10 mm was obtained from the disk D2 using the same method as the measurement sample S1. Note that the measurement sample S2 before polishing had a cylindrical shape with a bottom diameter of 25 mm and a thickness of approximately 12 mm. The upper surface of the measurement sample S2 was polished using "SiC Paper #220" until the thickness of the measurement sample S2 was approximately 11 mm. The upper surface of the measurement sample S2 was polished using "SiC Paper #1000" until the thickness of the measurement sample S2 was approximately 10.5 mm.

[0078] Next, the spectral transmittance including the reflection loss due to Fresnel reflection was measured for each of the measurement samples S1 and S2 in accordance with the provisions of JIS Z8722:2009. The spectral transmittance was measured using a Hitachi High-Tech Science ultraviolet-visible near-infrared spectrophotometer UH4150 under the conditions of a measurement wavelength of 200 nm to 1300 nm, a sampling interval of 1 nm, and a scan speed of 600 nm / min. From the obtained spectral transmittance, the internal transmittance of a 10 mm thick plate-shaped molded body made from an optical resin composition for light with a wavelength of 850 nm was determined based on the following formula (1). The results are shown in Table 1.

number

[0079] In the above formula (1), τ means the internal transmittance of a plate-shaped molded body having a thickness of L mm (10 mm). a is a value calculated by the following formula (2). In formula (2), d 1 means the thickness (mm) of the measurement sample S1, and d 2 means the thickness (mm) of the measurement sample S2. 1 means the transmittance of the measurement sample S1 to light with a wavelength of 850 nm, and T 2 means the transmittance of the measurement sample S2 for light with a wavelength of 850 nm. 1 and T 2 Each of them includes the reflection loss due to Fresnel reflection.

number

[0080] In Table 1, ◯ means that the internal transmittance determined by the above method is 98% or more, and × means that the internal transmittance determined by the above method is less than 98%.

[0081] [Table 1]

[0082] As can be seen from Table 1, the optical resin compositions of Samples 1 and 2 obtained by subjecting the fluoropolymer (A) to heat treatment in an atmosphere with a water vapor concentration of 100 volppm or less had lower water absorption than the optical resin compositions of Samples 3 and 4 obtained by heat treatment in an atmosphere with a water vapor concentration of more than 100 volppm. The optical resin compositions of Samples 1 and 2 had low water absorption and contained almost no water, so that a 10 mm-thick plate-shaped molded product made from the optical resin composition had a high internal transmittance for light with a wavelength of 850 nm. [Industrial Applicability]

[0083] The optical resin composition obtained by the manufacturing method of this embodiment is suitable as a material for optical components such as plastic optical fibers, optical waveguide materials, optical lenses, prisms, and photomasks, and is particularly suitable as a material for plastic optical fibers, optical waveguides, and optical lenses.

Claims

1. A method for producing an optical resin composition, comprising: polymerizing a monomer group containing a fluorine-containing compound having a carbon-carbon double bond with an organic peroxide, to obtain a fluorine-containing polymer; and heat-treating the fluorine-containing polymer in an atmosphere having a water vapor concentration of 100 vol ppm or less.

2. 2. The production method according to claim 1, wherein the heat treatment thermally decomposes the terminal groups of the fluoropolymer and volatilizes low molecular weight compounds produced by the thermal decomposition.

3. The process according to claim 1 or 2, wherein an end group of the fluoropolymer is converted into a functional group represented by the following formula (1) by the heat treatment: 【Chemistry 1】

4. The method according to any one of claims 1 to 3, wherein the organic peroxide comprises a diacyl peroxide or a peroxide ester.

5. The method according to any one of claims 1 to 4, wherein the atmosphere consists essentially of nitrogen gas.

6. The method according to any one of claims 1 to 5, wherein the heat treatment temperature is 100°C or higher and 400°C or lower.

7. The method according to any one of claims 1 to 6, wherein the carbon-carbon double bond is located at an end of the fluorine-containing compound, and all hydrogen atoms bonded to carbon atoms constituting the double bond are substituted with fluorine atoms.

Citation Information

Patent Citations

  • JP1971005642Y1

  • Cyclic ether containing fluorine and its production

    JP1996012668A

  • functionalized fluorinated copolymer

    JP2018532028A

  • Molding material and tube

    JP2019172967A

  • Fluorine resin and method for producing the same

    JP2020139093A