Manufacturing method of rigid polyurethane foam
The production method for rigid polyurethane foam using specific polyisocyanate and hydrofluoroolefin blends addresses the high GWP and thermal conductivity issues, achieving superior heat insulation and reduced thermal conductivity.
Patent Information
- Application Number
- JP2020008694
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-01-22
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-01-22
AI Technical Summary
Existing rigid polyurethane foams manufactured using hydrofluoroolefins as blowing agents have high global warming potential (GWP) and require further reduction in thermal conductivity for improved heat insulation properties.
A method for producing rigid polyurethane foam using a polyisocyanate mixture of 4,4'-diphenylmethane diisocyanate and polymethylene polyphenyl polyisocyanate with a high ratio of trinuclear or more components, combined with a hydrofluoroolefin blowing agent, including 1-chloro-3,3,3-trifluoropropene or 1,1,1,4,4,4-hexafluoro-2-butene, and optionally a foam stabilizer and catalyst, to achieve a thermal conductivity of 99.00% or less compared to conventional foams.
The method results in rigid polyurethane foam with excellent heat insulation properties and reduced thermal conductivity, utilizing hydrofluoroolefins with low GWP, enhancing thermal performance and insulation efficiency.
Smart Images

Figure 0007571370000001 
Figure 0007571370000002 
Figure 0007571370000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing rigid polyurethane foam. [Background technology]
[0002] 2. Description of the Related Art It is common to produce rigid polyurethane foams by mixing a polyol, a polyisocyanate, and a blowing agent.
[0003] Conventionally, chlorinated fluorocarbon compounds (chlorofluorocarbons, commonly known as CFCs) such as CCl3F and chlorinated fluorohydrocarbon compounds (hydrochlorofluorocarbons, commonly known as HCFCs) such as CCl2FCH3 have been used as blowing agents. However, the use of CFCs and HCFCs has come to be restricted from the perspective of environmental protection, such as protecting the ozone layer.
[0004] Hydrofluorocarbons (HFCs) are used as blowing agents to replace CFCs and HCFCs. Examples of HFCs used as blowing agents include CHF2CH2CF3 (HFC-245fa) and CF3CH2CF2CH3 (HFC-365mfc). However, although these HFCs have zero ozone depletion potential (ODP), they have a high global warming potential (GWP), so there is a demand for blowing agents with lower GWP.
[0005] Hydrofluoroolefins (HFOs) and hydrochlorofluoroolefins (HCFOs) have been proposed as candidates for blowing agents with low GWP. Patent Documents 1 and 2 disclose a mixture of E-isomer of CF3CF=CHCl (HCFO-1224yd(E)) and CF3CH=CHCF3 (HFO-1336mzz) as an azeotropic mixture, and state that it can be used as a blowing agent for thermosetting or thermoplastic resins. Patent Document 3 describes that E-isomer of 1-chloro-3,3,3-trifluoropropene (HFO-1233zd(E)) can be used as a blowing agent. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2012 / 106565 [Patent Document 2] International Publication No. 2013 / 059550 [Patent Document 3] Patent No. 5562827 Summary of the Invention [Problem to be solved by the invention]
[0007] In the rigid polyurethane foams produced using the HFOs or HCFOs described in Patent Documents 1 to 3 as a blowing agent, there is room for further reduction in thermal conductivity.
[0008] The present invention provides a method for producing a rigid polyurethane foam, which can produce a rigid polyurethane foam with excellent heat insulating properties by using a hydrofluoroolefin having a low global warming potential (GWP) as a blowing agent. [Means for solving the problem]
[0009] [1] A method for producing a rigid polyurethane foam, comprising mixing a polyol, a polyisocyanate, and a blowing agent, the polyisocyanate contains 4,4'-diphenylmethane diisocyanate and a tri- or higher polymethylene polyphenyl polyisocyanate, and the ratio of the tri- or higher polymethylene polyphenyl polyisocyanate to the polyisocyanate is 72.1 mass% or more; the blowing agent comprises a hydrofluoroolefin and water; A method for producing a rigid polyurethane foam, wherein the ratio of the hydrofluoroolefin to the blowing agent is 50 to 99 mass % (however, excluding a method for producing a rigid polyurethane foam using glycerol having a hydroxyl value of 1825 mgKOH / g). [2] The method for producing a rigid polyurethane foam according to [1], further comprising mixing a foam stabilizer and a catalyst. [3] The method for producing a rigid polyurethane foam according to [1] or [2], wherein the hydrofluoroolefin is at least one selected from the group consisting of E-isomer of 1-chloro-3,3,3-trifluoropropene, Z-isomer of 1-chloro-2,3,3,3-tetrafluoropropene, and Z-isomer of 1,1,1,4,4,4-hexafluoro-2-butene. [4] The method for producing a rigid polyurethane foam according to any one of [1] to [3], wherein the amount of the blowing agent per 100 parts by mass of the polyol is 10 to 100 parts by mass. [5] The polyol is Polyether polyol and The method for producing a rigid polyurethane foam according to any one of [1] to [4], which contains a polyester polyol. [6] The method for producing a rigid polyurethane foam according to [5], wherein the proportion of the polyether polyol based on the total amount of the polyols is 30 to 80 mass %. [7] The method for producing a rigid polyurethane foam according to any one of [1] to [6], wherein the thermal conductivity of the rigid polyurethane foam is 99.00% or less relative to the thermal conductivity of rigid polyurethane foam 2 below. Rigid polyurethane foam 2: A rigid polyurethane foam obtained by mixing a polyol, a polyisocyanate, and a blowing agent, wherein the polyisocyanate contains 4,4'-diphenylmethane diisocyanate and a tri- or higher polymethylene polyphenyl polyisocyanate, and the ratio of the tri- or higher polymethylene polyphenyl polyisocyanate to the polyisocyanate is less than 55 mass%. Effect of the Invention
[0010] According to the present invention, there is provided a method for producing a rigid polyurethane foam, which is capable of producing a rigid polyurethane foam with excellent heat insulating properties by using a hydrofluoroolefin having a low GWP as a blowing agent. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The following definitions of terms and descriptions apply throughout the specification and claims. The "hydrofluoroolefin" in the present invention includes so-called hydrofluoroolefins (HFOs) and hydrochlorofluoroolefins (HCFOs). For hydrofluoroolefins, the abbreviation for the compound is written in parentheses after the compound name, but if necessary, the abbreviation can be used instead of the compound name. In addition, the abbreviation may use only the numbers and lowercase letters following the hyphen (-) (for example, "1224yd" for "HCFO-1224yd"). In addition, 1224yd has geometric isomers, Z and E, depending on the position of the substituent bonded to the carbon having a double bond. In this specification, when a compound name or abbreviation of a compound that has Z and E isomers such as 1224yd is used without special mention, it indicates the Z or E isomer, or a mixture of Z and E isomers in any ratio. When a compound name or abbreviation of a compound is followed by (Z) or (E), it indicates that the compound is the Z or E isomer.
[0012] The "weight average molecular weight" (hereinafter referred to as "Mw") is a polystyrene-equivalent molecular weight obtained by measurement by gel permeation chromatography (GPC) using a calibration curve prepared using standard polystyrene samples of known molecular weight.
[0013] The Mw of polyol was analyzed using a GPC system (HLC-8220GPC, Tosoh Corporation) with a differential refractive index detector (RI detector). Two TSK-GEL Super HZ2000 and two Super HZ1000 columns were connected in series in this order. The eluent was 1 L of tetrahydrofuran to which 100 mmol of triethylamine was added. The eluent was passed at a flow rate of 0.35 mL / min, and the column temperature was set to 40°C in the attached column oven. The measurement sample was a solution in which 0.05 mL of polyol was diluted in 10 mL of tetrahydrofuran. A calibration curve was created using monodisperse polystyrene (Agilent Technologies product name, EasiVial) as the standard sample, and the Mw in terms of polystyrene was calculated.
[0014] The "hydroxyl value" is a value measured and calculated by a method based on JIS K 1557-1: 2007. The average hydroxyl value of a polyol is the average value of the hydroxyl values of all the polyols contained, and is a value calculated by measuring a mixture of all the polyols contained in the mixture by the above method.
[0015] The "foaming agent" refers to a compound that foams by utilizing the gas generated by vaporization of the foaming agent, and a compound that foams by utilizing the gas generated by the reaction of the foaming agent with polyisocyanate. The "system liquid" refers to a composition that is to be reacted with a polyisocyanate to obtain a rigid polyurethane foam, and that contains raw materials other than the polyisocyanate. The term "active hydrogen" refers to hydrogen based on at least one group selected from the group consisting of a hydroxyl group, a carboxyl group, an amino group, a hydrazide group, and a mercapto group. A numerical range indicated by "~" indicates a numerical range with the numbers before and after "~" as the lower and upper limits.
[0016] [Manufacturing method of rigid polyurethane foam] The method for producing a rigid polyurethane foam of the present invention is a method for producing a rigid polyurethane foam by mixing a polyol, a polyisocyanate, and a blowing agent. Each of the configurations of the present invention will be described below.
[0017] <Polyol> The "polyol" in the present invention refers to all polyols used in the reaction with the polyisocyanate, and may contain one type of polyol or two or more types of polyols. Examples of the polyol include polyether polyol, polyester polyol, polyester ether polyol, polycarbonate polyol, polymers having a main chain made of a hydrocarbon polymer and having hydroxyl groups introduced at the terminal portions, and polyhydric alcohols.
[0018] As the polyol, it is preferable to use one or both of polyether polyol and polyester polyol, and it is more preferable to use polyether polyol and polyester polyol in combination, since the physical properties of the obtained rigid polyurethane foam are excellent. Two or more kinds of polyether polyol and polyester polyol may be used respectively.
[0019] When a polyether polyol and a polyester polyol are used in combination as the polyol, the ratio of the polyether polyol to the total of the polyols is preferably 30 to 80 mass%, more preferably 35 to 70 mass%. When the ratio is within the above range, good mixability of the polyol and the polyisocyanate is easily obtained.
[0020] Polyether polyols can be produced by conventional methods, and are preferably those obtained by ring-opening addition of a cyclic ether using a compound containing active hydrogen with which the cyclic ether can react as an initiator, optionally in the presence of a ring-opening addition catalyst.
[0021] The initiator may be any of the compounds exemplified below or compounds obtained by adding a small amount of a cyclic ether to these compounds. The compounds exemplified below may be used alone or in combination of two or more. The initiator may be, for example, a polyhydric alcohol, a polyhydric phenol, an alkanolamine, or an amine.
[0022] Specific examples of the polyhydric alcohol include ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, tripropylene glycol, 1,2-butanediol, 1,4-butanediol, 2,2-dimethyl-1,3-propanediol, 1,6-hexanediol, 2-methyl-2,4-pentanediol, 3-methyl-1,5-pentanediol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, glycerin, trimethylolpropane, 1,2,6-hexanetriol, pentaerythritol, diglycerin, tetramethylolcyclohexane, methyl glucoside, sorbitol, mannitol, galactose, galactitol, and sucrose.
[0023] Specific examples of the polyhydric phenol include bisphenol A, a phenol-formaldehyde initial condensation product, and a Mannich condensation product described below.
[0024] Specific examples of the alkanolamine include monoethanolamine, diethanolamine, triethanolamine, isopropanolamine, and N-(2-aminoethyl)ethanolamine.
[0025] Specific examples of the amine include ethylenediamine, propylenediamine, hexamethylenediamine, piperazine, aniline, ammonia, N-aminomethylpiperazine, N-(2-aminoethyl)piperazine, 4-methyl-1,3-phenylenediamine, 2-methyl-1,3-phenylenediamine, 4,4'-diphenylmethanediamine, xylylenediamine, diethylenetriamine, and triethylenetetramine.
[0026] The cyclic ether is preferably a 3- to 6-membered cyclic ether compound having one oxygen atom in the ring. The cyclic ether may be used alone or in combination of two or more kinds. The 3- to 6-membered cyclic ether compound having one oxygen atom in the ring is preferably at least one selected from the group consisting of ethylene oxide (hereinafter sometimes referred to as "EO"), propylene oxide (hereinafter sometimes referred to as "PO") and butylene oxide, and more preferably EO alone, PO alone, or a combination of EO and PO. When two or more of the above cyclic ethers are used in combination, they may be mixed and reacted to give a random polymer, or they may be reacted sequentially to give a block polymer. As the ring-opening addition catalyst which is optionally present when the cyclic ether is subjected to ring-opening addition to the initiator, a known ring-opening addition catalyst can be used. Examples of such ring-opening addition catalysts include alkali metal compound catalysts such as sodium-based catalysts, potassium-based catalysts, and cesium-based catalysts.
[0027] The polyether polyol is preferably a Mannich polyol obtained by ring-opening addition of the above-mentioned cyclic ether to a Mannich condensate obtained by reacting a phenol, an aldehyde and an alkanolamine (Mannich condensation reaction) as an initiator. The Mannich polyol contains an amino group, which tends to increase the activity of the polyol. In addition, the Mannich polyol contains a hydrophilic group and a hydrophobic group, and has surface activity, which tends to improve the mixability of the polyol with the polyisocyanate. Furthermore, the Mannich polyol contains phenols, which tends to form a carbonized film during combustion, which tends to increase the flame retardancy of the rigid polyurethane foam.
[0028] The phenol is preferably at least one selected from the group consisting of phenol and phenol derivatives having a hydrogen atom at at least one ortho position relative to the phenolic hydroxyl group. The phenol derivative is preferably an alkylphenol having a hydrogen atom at at least one ortho position relative to the phenolic hydroxyl group and having one or more other hydrogen atoms bonded to the aromatic ring substituted with an alkyl group having 1 to 15 carbon atoms. The substitution position of the alkyl group in the alkylphenol may be either the ortho-position or the para-position. The number of hydrogen atoms substituted with alkyl groups in one molecule of the alkylphenol is preferably 1 to 4, more preferably 1 or 2, and further preferably 1. The alkyl group in the alkylphenol more preferably has 1 to 10 carbon atoms. The alkylphenol is preferably nonylphenol or cresol, and more preferably nonylphenol from the viewpoint of improving the compatibility between the polyol and the polyisocyanate.
[0029] As the aldehyde, either one or both of formaldehyde and acetaldehyde are preferred, of which formaldehyde is preferred in terms of reactivity in the Mannich condensation reaction. The formaldehyde may be used in any form, specifically, in the form of an aqueous formalin solution, a methanol solution, or paraformaldehyde. When used as paraformaldehyde, formaldehyde generated by heating paraformaldehyde may be used.
[0030] The alkanolamine is preferably at least one selected from the group consisting of monoethanolamine, diethanolamine, and 1-amino-2-propanol. Among these, diethanolamine is preferred in that a Mannich polyol having a low viscosity can be easily obtained.
[0031] The above Mannich condensation product can be obtained by a Mannich condensation reaction according to a known method such as that described in JP-A-2-132115. In the Mannich condensation reaction, the number of moles of aldehyde per mole of phenol is preferably 0.5 to 3 moles, more preferably 1 to 2.5 moles. When the number of moles of aldehyde is within the above range, good dimensional stability of the rigid polyurethane foam is easily obtained. In the Mannich condensation reaction, the number of moles of alkanolamine per mole of phenol is preferably 1 to 3 moles, more preferably 1.5 to 3 moles. When the number of moles of alkanolamine is within the above range, a rigid polyurethane foam having high strength and high flame retardancy is easily obtained. In the Mannich condensation reaction, it is preferable that the number of moles of the aldehyde per mole of the phenol is 0.5 to 3 moles, and the number of moles of the alkanolamine per mole of the phenol is 1 to 3 moles.
[0032] A cyclic ether is added to the active hydrogen of the Mannich condensation product by ring-opening addition to obtain a Mannich polyol. As the cyclic ether, it is preferable to use EO alone, PO alone, or a combination of EO and PO. The proportion of EO in the total amount of cyclic ethers used in the production of the Mannich polyol may be more than 0% by mass and may be 100% by mass, preferably 20 to 100% by mass, more preferably 30 to 100% by mass, and further preferably 40 to 90% by mass. When the proportion of EO is within the above range, the compressive strength of the rigid polyurethane foam tends to be high.
[0033] The number of moles of the cyclic ether added to the Mannich condensation product by ring-opening addition is preferably 1 to 30 moles, more preferably 2 to 20 moles, per mole of the phenols used in the production of the Mannich condensation product. When the number of moles of the cyclic ether added is within the above range, the viscosity of the polyether polyol produced tends to be low, and shrinkage of the resulting rigid polyurethane foam tends to be suppressed.
[0034] The average number of hydroxyl groups in the Mannich polyol is preferably from 2 to 8, and more preferably from 3 to 7. When the average number of hydroxyl groups in the Mannich polyol is within this range, it is easy to adjust the average number of hydroxyl groups in the polyol to be within the above range. The average number of hydroxyl groups in the Mannich polyol is the same as the average number of active hydrogens in the Mannich condensation product. By setting the raw materials and reaction ratios used in the Mannich condensation reaction within the above ranges, the number of active hydrogens in the Mannich condensation product can be adjusted, and the average number of hydroxyl groups in the Mannich polyol can be adjusted to within the above range.
[0035] The hydroxyl value of the Mannich polyol is preferably 100 to 800 mgKOH / g, more preferably 200 to 700 mgKOH / g, and even more preferably 300 to 600 mgKOH / g. When the hydroxyl value of the Mannich polyol is within the above range, the strength of the hydrogen bond due to the hydroxyl group is appropriately adjusted, so that the viscosity of the Mannich polyol is likely to be reduced, the strength of the obtained rigid polyurethane foam is likely to be increased, and good dimensional stability is likely to be obtained.
[0036] The Mw of the Mannich polyol is preferably 100 to 3,000, more preferably 150 to 2,000. When the Mw of the Mannich polyol is within the above range, the strength of hydrogen bonds due to hydroxyl groups is appropriately adjusted, so that the viscosity of the Mannich polyol is likely to decrease, the resulting rigid polyurethane foam is unlikely to become brittle, adhesiveness to a substrate is likely to be exhibited when molded, and the compressive strength is likely to be improved.
[0037] The Mannich polyols may be used alone or in combination of two or more kinds. In the method for producing a rigid polyurethane foam of the present invention, the proportion of the Mannich polyol relative to the total amount of polyol is preferably 10 to 100% by mass, more preferably 20 to 100% by mass, and even more preferably 30 to 100% by mass. 1233zd, 1224yd orWhen it contains 1336mzz, the insulation properties, flame retardancy, and compressive strength tend to be good.
[0038] Commercially available polyether polyols include, for example, EXCENOL NB-615, EXCENOL NB-622, EXCENOL FB-655, EXCENOL FB-800 (all AGC product names), DK Polyol 3776, DK Polyol 3820, DK Polyol 3801, DK Polyol 3810, DK Polyol 3773, DK Polyol 3774 (all Daiichi Kogyo Seiyaku product names), CARPOL MX-425, CARPOL MX-470 (all CARPENTER product names), VORANOL 425XL Polyol (DOW Chemical), JEFFOL R-350X Polyol, JEFFOL R-425X Polyol, and JEFFOL R-470X Polyol (all HUNTSMAN product names).
[0039] Examples of polyester polyols include polyester polyols obtained by polycondensation of polyhydric alcohols and polycarboxylic acids, as well as polyester polyols obtained by polycondensation of hydroxycarboxylic acids, polymerization of cyclic esters (lactones), polyaddition of cyclic ethers to polycarboxylic anhydrides, and transesterification of polyethylene terephthalate.
[0040] Examples of the polyhydric alcohol used in the polycondensation include ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, tripropylene glycol, 1,2-butanediol, 1,4-butanediol, 2,2-dimethyl-1,3-propanediol, 1,6-hexanediol, 2-methyl-2,4-pentanediol, 3-methyl-1,5-pentanediol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, glycerin, trimethylolpropane, 1,2,6-hexanetriol, pentaerythritol, diglycerin, tetramethylolcyclohexane, methyl glucoside, sorbitol, mannitol, galactitol, and sucrose.
[0041] As the polyester polyol, commercially available products can be used. Examples of the commercially available polyester polyols include Maximol RDK-133, Maximol RLK-087, Maximol RFK-505 (all aromatic polyester polyols, Kawasaki Chemical Industries, Ltd. product names), Fantoll 6301, Fantoll 6305, Fantoll PL-272, Fantoll SV-208, Fantoll PH-6102 (all aromatic polyester polyols, Hitachi Chemical Industries, Ltd. product names), STEPANPOL 3152, STEPANPOL 2412, STEPANPOL 2352, STEPANPOL PS2502-A (all aromatic polyester polyols, STEPAN product names), Terate 203, Terate 4020 (all aromatic polyester polyols, INVISTA product names) and Lupraphen 8007 (aromatic polyester polyols, BASF product name).
[0042] Examples of polymers having a main chain made of a hydrocarbon polymer and having hydroxyl groups introduced at the terminals include hydrogenated polybutadiene polyol and polybutadiene polyol. The above-exemplified polyhydric alcohols themselves can be used as the polyol in the present invention. As the polyol, a polyol composition in which fine particles of a vinyl polymer are dispersed in a polyether polyol, which is called a polymer polyol or a graft polyol, can also be used.
[0043] The polyol in the present invention preferably contains at least one selected from the group consisting of Mannich polyols, polyether polyols other than Mannich polyols, and polyester polyols, and preferably contains Mannich polyols, polyether polyols other than Mannich polyols, and polyester polyols, or contains Mannich polyols and polyether polyols other than Mannich polyols. The ratio of the Mannich polyol / polyether polyol other than the Mannich polyol / polyester polyol to the polyol in the present invention is preferably 5-95% by mass / 5-95% by mass / 0-90% by mass, more preferably 10-90% by mass / 10-90% by mass / 0-80% by mass, and further preferably 15-85% by mass / 15-85% by mass / 0-70% by mass. Within the above ranges, the rigid polyurethane foam has better heat insulation and flame retardancy.
[0044] When the polyol in the present invention contains an oxyethylene group, the ratio of the oxyethylene group to the total amount of the oxyalkylene group may be more than 0% by mass and 100% by mass, preferably 20 to 100% by mass, more preferably 30 to 90% by mass, and even more preferably 40 to 90% by mass. When the ratio of the oxyethylene group is within the above range, the solubility of the polyol and the blowing agent described below is appropriately adjusted, and the compressive strength of the rigid polyurethane foam tends to be high. The above ratio is calculated as the ratio of the oxyethylene group to the total amount of the oxyalkylene group in the total amount of the polyol contained.
[0045] The average number of hydroxyl groups in the polyol is preferably 2 to 8, and more preferably 2.5 to 7.5. When the average number of hydroxyl groups is within the above preferred range, the shrinkage of the resulting rigid polyurethane foam is suppressed, and the dimensional stability is improved. In addition, the rapid thickening behavior during foaming and molding is suppressed, and the fluidity and moldability are improved. Here, the average number of hydroxyl groups of the polyol is the molar average value of the numbers of hydroxyl groups of all the polyols contained.
[0046] The Mw of the polyol is preferably 100-3,000, more preferably 150-2,000, and further preferably 200-1,500. When the Mw of the polyol is within the above-mentioned preferred range, the shrinkage of the obtained rigid polyurethane foam is suppressed and the dimensional stability is improved. In addition, the obtained rigid polyurethane foam is less likely to become brittle. Here, the Mw of the polyol is the average value of the Mw of all the polyols contained therein.
[0047] The average hydroxyl value of the polyol is preferably from 100 to 800 mgKOH / g, more preferably from 200 to 700 mgKOH / g, and further preferably from 300 to 600 mgKOH / g. When the average hydroxyl value of the polyol is within the above-mentioned preferred range, the shrinkage of the obtained rigid polyurethane foam is suppressed and the dimensional stability is improved. In addition, the obtained rigid polyurethane foam is less likely to become brittle. Here, the average hydroxyl value of the polyol may be calculated by taking a weighted average of the hydroxyl values of all the polyols contained, or may be a value measured by mixing all the polyols contained.
[0048] <Polyisocyanate> The polyisocyanate used is a mixture of polyisocyanates containing 4,4'-diphenylmethane diisocyanate (MDI) (hereinafter sometimes referred to as "4,4'-MDI") and trinuclear or higher polymethylene polyphenyl polyisocyanate (hereinafter sometimes referred to as "trinuclear or higher component"). "Trinuclear or higher" means that one molecule contains three or more benzene rings. The trinuclear or higher component may contain a dimer.
[0049] When the ratio of the trinuclear or higher component to the total mass of the polyisocyanate is 55% by mass or more, the thermal conductivity of the obtained rigid polyurethane foam tends to be low. The ratio of the trinuclear or higher component to the total mass of the polyisocyanate is preferably 55 to 85% by mass, more preferably 60 to 80% by mass, and even more preferably 65 to 75% by mass. When the ratio of the trinuclear or higher component to the total mass of the polyisocyanate is equal to or less than the upper limit, the thermal conductivity of the obtained rigid polyurethane foam tends to be low and the heat insulation tends to be improved. In addition, when the ratio of the trinuclear or higher component to the total mass of the polyisocyanate is equal to or more than the lower limit, the compressive strength of the polyurethane foam is easily improved.
[0050] The polyisocyanate may contain unavoidably mixed isomers of 4,4'-MDI (2,2'-MDI, 2,4'-MDI) in addition to the 4,4'-MDI and the trinuclear or higher component. The proportion of the 4,4'-MDI isomer is preferably 10% by mass or less of the total mass of the polyisocyanate. The lower limit of the proportion of the isomer is not particularly specified, but may be 0.01% by mass or more.
[0051] The amount of polyisocyanate used is preferably 50 to 300, more preferably 50 to 170, and even more preferably 70 to 150, calculated by multiplying the number of isocyanate groups relative to the total number of active hydrogens in the polyol by 100 (hereinafter, this value is referred to as "isocyanate index"). If the isocyanate index is above the upper limit, unreacted isocyanate is likely to remain, which leads to a deterioration in surface curing property and brittleness, leading to a deterioration in adhesion. If the isocyanate index is below the lower limit, the number of urethane reaction sites is reduced, leading to a decrease in compressive strength.
[0052] <Foaming agent> In the method for producing a rigid polyurethane foam of the present invention, a blowing agent containing a hydrofluoroolefin and water is used.
[0053] As the above hydrofluoroolefin, chlorofluoroolefins and hydrochlorofluoroolefins are preferred, chlorofluoroolefins and hydrochlorofluoroolefins having a GWP of 100 or less are more preferred, and chlorofluoroolefins and hydrochlorofluoroolefins having a GWP of 10 or less are even more preferred. Examples of the hydrofluoroolefin include 1-chloro-3,3,3-trifluoropropene (HFO-1233zd, hereinafter sometimes referred to as "1233zd". GWP is 1 or less), 1-chloro-2,3,3,3-tetrafluoropropene (HCFO-1224yd, hereinafter sometimes referred to as "1224yd". GWP is 1 or less), and 1,1,1,4,4,4-hexafluoro-2-butene (HFO-1336mzz, hereinafter sometimes referred to as "1336mzz". GWP is 2 or less). Either E-form or Z-form can be used. The above HFOs may be used alone or in combination of two or more. The hydrofluoroolefin is preferably one or more selected from the E form of 1233zd (hereinafter may be referred to as "1233zd(E)"), the Z form of 1224yd (hereinafter may be referred to as "1224yd(Z)"), and the Z form of 1336mzz (hereinafter may be referred to as "1336mzz(Z)"). A preferred combination of blowing agents is a combination of water and 1336mzz, more preferably a combination of water and 1224yd, and most preferably a combination of water and 1233zd.
[0054] The boiling point of the hydrofluoroolefin under atmospheric pressure (1013 hPa) is preferably 17 to 33° C., more preferably 18 to 32° C., and even more preferably 19 to 31° C. When the boiling point of the HFO under atmospheric pressure is within the above preferred range, bumping during transportation of the blowing agent is easily prevented. Note that the above boiling point is the boiling point when multiple types of compounds used as the blowing agent are mixed.
[0055] The proportion of the hydrofluoroolefin relative to the total mass of the foaming agent is preferably from 50 to 99 mass %, more preferably from 70 to 97 mass %, and even more preferably from 75 to 95 mass %. The proportion of the water relative to the total mass of the foaming agent is preferably from 1 to 50% by mass, more preferably from 2 to 30% by mass, and even more preferably from 3 to 20% by mass.
[0056] As the blowing agent, other blowing agents may be used in combination with the hydrofluoroolefin and water. The other foaming agent can be appropriately selected from known foaming agents. Examples of the other foaming agent include CF2H2, CF3CF2H, CF3CH3, CHF2CF2H, CF3CH2F, CHF2CH3, CF3CHFCF3, CF3CF2CHFCHFCF3, CHF2CH2CF3, and CH3CF2CH2CF 3、 Cyclopentane, CCl2FCH3, CF3CF2CF2OCH 3、 Examples include CHF2CF2OCH3 and CHCl=CClH. The total proportion of the other blowing agents relative to the total mass of the blowing agents is preferably 50 mass% or less, more preferably 10 mass% or less. When the total proportion of the other blowing agents is not more than the above-mentioned preferable value, the physical properties of the obtained rigid polyurethane foam are not easily impaired.
[0057] In the method for producing a rigid polyurethane foam of the present invention, the amount of the blowing agent used is preferably 10 to 100 parts by mass, more preferably 12 to 60 parts by mass, and even more preferably 15 to 50 parts by mass, based on 100 parts by mass of the total of the polyols. When the amount of the blowing agent used is within the above preferred range, the density of the obtained rigid polyurethane foam becomes appropriate, and the heat insulation property tends to be good. The foaming agent is preferably mixed with the polyol and then mixed with the polyisocyanate.
[0058] In the method for producing a rigid polyurethane foam of the present invention, a composition containing raw materials other than the polyisocyanate, i.e., a polyol and a blowing agent, and optionally a foam stabilizer and a catalyst described below, and further optional components, can be used. This composition is sometimes referred to as a "polyol system liquid."
[0059] <Foam stabilizers and catalysts> In the process for producing a rigid polyurethane foam of the present invention, when the polyol, the polyisocyanate, and the blowing agent are mixed, a foam stabilizer and a catalyst may be further mixed therein.
[0060] The foam stabilizer is used to form better foam. Examples of the foam stabilizer include silicone-based foam stabilizers and fluorine-containing compound-based foam stabilizers. Commercially available products can be used. The content of the foam stabilizer can be appropriately set, and is preferably 0.1 to 10 parts by mass per 100 parts by mass of the polyol. The foam stabilizer is preferably mixed with the polyisocyanate in a state where it is mixed with the polyol.
[0061] The catalyst used is an organic acid salt of an amine in order to suppress deterioration of the reactivity of the urethane reaction. As the catalyst, a trimerization reaction-accelerating catalyst that accelerates the trimerization reaction of an isocyanate group can also be used together with the organic acid salt of an amine.
[0062] The organic acid salt of the amine is preferably a salt of a tertiary amine and an organic acid. Examples of the tertiary amine include N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethylpropylenediamine, N,N,N',N",N"-pentamethyldiethylenetriamine, N,N,N',N",N"-pentamethyl-(3-aminopropyl)ethylenediamine, N,N,N',N",N"-pentamethyldipropylenetriamine, N,N,N',N'-tetramethylguanidine, and 1,3,5-tris(N,N-dimethylaminopropyl)hexahydro-S-triazine. , 1,8-diazabicyclo[5.4.0]undecene-7, triethylenediamine, N,N,N',N'-tetramethylhexamethylenediamine, N,N'-dimethylpiperazine, dimethylcyclohexylamine, N-methylmorpholine, N-ethylmorpholine, bis(2-dimethylaminoethyl)ether, 1-methylimidazole, 1,2-dimethylimidazole, 1-isobutyl-2-methylimidazole, 1-dimethylaminopropylimidazole, N-methyl-N-(N,N-dimethylaminoethyl)ether Ethanolamine, N,N-dimethylaminoethanol, N,N-dimethylaminoethoxyethanol, 2-[2-(2-dimethylaminoethoxy)ethoxy]ethanol, 1-(dimethylamino)-2-propanol, N,N-dimethylaminoethoxyisopropanol, N,N-dimethylaminoethoxyethoxyisopropanol, N,N,N'-trimethylaminoethylethanolamine, N,N-dimethylaminoethyl-N'-methylaminoisopropanol, N,N,N'-trimethyl-N'-(2- N,N,N'-trimethyl-N'-hydroxyisopropyl bis(2-aminoethyl) ether, N,N,N'-trimethyl-N'-(3-aminopropyl) bis(2-aminoethyl) ether, hexamethyltriethylenetetramine, N,N-dimethylaminoethyl-N'-methylaminoethyl-N"-methylaminoisopropanol, and N,N-dimethylaminoethyl-N'-methylaminoethyl-N"-methylaminoethanol. The organic acids include formic acid, acetic acid, propionic acid, butyric acid, caproic acid, citric acid, isocaproic acid, 2-ethylhexanoic acid, caprylic acid, cyanoacetic acid, pyruvic acid, benzoic acid, oxalic acid, malonic acid, succinic acid, adipic acid, azelaic acid, trifluoroacetic acid, methanesulfonic acid, benzenesulfonic acid, polymeric acids such as polyacrylic acid, polymethacrylic acid, and mixtures thereof. A preferred group includes formic acid, acetic acid, caproic acid, citric acid, isocaproic acid, 2-ethylhexanoic acid, phenolic acid, polymeric acids, and combinations thereof. The organic acid salt of an amine can be obtained by reacting the above amine with the above organic acid. The organic acid salt of an amine exhibits lower reactivity with hydrofluoroolefins than a catalyst consisting of an amine alone, and therefore the urethanization reaction proceeds more rapidly. The above-mentioned tertiary amine can be used in a mixture with an acid, as described in paragraphs
[0066] to
[0073] of JP2017-155101A, and preferred embodiments thereof can also be used in the same manner.
[0063] As the trimerization reaction-promoting catalyst, for example, either one or both of organic acid metal salts (excluding tin salts, lead salts and mercury salts) and quaternary ammonium salts can be used.
[0064] Examples of the organic acid metal salt include carboxylate metal salts of potassium acetate, potassium 2-ethylhexanoate, and bismuth 2-ethylhexanoate.
[0065] Examples of the quaternary ammonium salt include tetraalkylammonium halides such as tetramethylammonium chloride; tetraalkylammonium hydroxides such as tetramethylammonium hydroxide; tetraalkylammonium organic acid salts such as tetramethylammonium 2-ethylhexanoate, 2-hydroxypropyltrimethylammonium formate, and 2-hydroxypropyltrimethylammonium 2-ethylhexanoate; and quaternary ammonium compounds obtained by reacting a quaternary ammonium carbonate, obtained by reacting a tertiary amine such as N,N,N',N'-tetramethylethylenediamine with a carbonate diester, with 2-ethylhexanoic acid through anion exchange reaction. These quaternary ammonium salts are sometimes called quaternary ammonium salt-type trimerization reaction-promoting catalysts.
[0066] In the method for producing a rigid polyurethane foam of the present invention, the amount of the catalyst used is preferably 0.01 to 100 parts by mass, more preferably 0.05 to 50 parts by mass, and even more preferably 0.1 to 20 parts by mass, per 100 parts by mass of the total of the polyols. By adjusting the amount of the catalyst used, it is possible to adjust the time from the start of mixing of the components used for foaming to the start of reaction (cream time) or the time until foaming is completed (rise time). The catalyst is preferably mixed with the polyol and then mixed with the polyisocyanate.
[0067] <Optional ingredients> In the process for producing a rigid polyurethane foam of the present invention, components other than the above-mentioned components may be further used, if necessary. As the other components, known compounding agents can be used. Examples of the compounding agents include fillers, antioxidants, flame retardants, plasticizers, colorants, antifungal agents, defoamers, dispersants, and discoloration inhibitors. Examples of the fillers include calcium carbonate and barium sulfate. Examples of the antioxidants include antioxidants and ultraviolet absorbing agents. The content of the other components can be appropriately set depending on the purpose, but is preferably 0.1 to 30 parts by mass per 100 parts by mass of the polyol. It is preferable that the other components are mixed with the polyol and then mixed with the polyisocyanate.
[0068] <Production method of rigid polyurethane foam> The method for producing a rigid polyurethane foam of the present invention comprises mixing the above-mentioned polyol, the above-mentioned polyisocyanate, and the above-mentioned blowing agent, and reacting and foaming the above-mentioned polyol and the above-mentioned polyisocyanate to produce a rigid polyurethane foam.
[0069] The method for reacting the polyol with the polyisocyanate can be a known method, such as an injection method, a continuous board molding method, or a spray method. The injection method is a method in which a raw material containing a system liquid and a polyisocyanate is injected into the frame of a mold or the like to cause foaming. The continuous board molding method is a method for producing a laminate in which a rigid polyurethane foam is sandwiched between two facing materials by supplying a raw material containing a system liquid and a polyisocyanate between the facing materials and foaming the raw material. The spray method is a method in which a raw material containing a system liquid and a polyisocyanate is sprayed onto the surface.
[0070] The injection method can be carried out, for example, by using a high pressure foaming device or a low pressure foaming device. When using a high pressure or low pressure foaming device, the system liquid is injected into various molds and then foamed and cured to produce rigid polyurethane foam. The foaming agent may be mixed into the system liquid in advance, or may be mixed during foaming in the foaming device. Examples of products that can be produced using the injection method include refrigeration equipment such as electric refrigerators, and panels for refrigerated and frozen vehicles. Continuous board forming processes are used, for example, in the production of insulation for building applications.
[0071] The spray method is roughly divided into an air spray method and an airless spray method. Of these, the airless spray method, in which a system liquid and a raw material containing polyisocyanate are mixed in a mixing head and foamed, is particularly preferred. The spray method includes a manufacturing method in which a raw material containing a system liquid and a polyisocyanate is stirred, foamed, and injected into a mold frame.Furthermore, the spray method also includes a method in which a raw material containing a system liquid and a polyisocyanate is supplied by spraying it onto the inside of one of two paired facing materials, and during the foaming process, the other facing material is laminated, thereby continuously manufacturing a laminate in which a rigid polyurethane foam is sandwiched between the facing materials. When applying to vertical surfaces such as walls by spraying, poor reactivity between the system liquid and polyisocyanate can easily cause dripping. Dripping can cause the insulation layer to become ununiform, resulting in the thickness of the insulation layer concentrating at the bottom of the wall, which can lead to problems such as more cutting to make the interior wall even, and increased waste. Poor reactivity can also slow down the thickening during the foaming process, which can promote cell growth and lead to poor insulation of the resulting foam. Examples of articles that can be produced using the spray method include heat insulating materials for preventing condensation in apartments and for building detached houses, heat insulating materials for vehicles and aircraft, and soundproofing materials for buildings, vehicles and aircraft.
[0072] According to the manufacturing method of the present invention, the density is 5 to 300 kg / m 3 It is possible to produce a rigid polyurethane foam having a thermal conductivity of 0.1 to 1.0%, which is the same as that of the rigid polyurethane foam obtained by the above method. As shown in the examples described later, the rigid polyurethane foam obtained by the above method tends to have a low thermal conductivity and a good compressive strength. The density of the rigid polyurethane foam can be controlled by the amount of the blowing agent used. The thermal conductivity can be controlled by adjusting the composition of the polyol and the blowing agent.
[0073] [Hard polyurethane foam] The rigid polyurethane foam produced by the method for producing a rigid polyurethane foam of the present invention (hereinafter sometimes referred to as "rigid polyurethane foam of the present invention") has a thermal conductivity of 0.0210 W / m K or less and is excellent in heat insulation. Here, the thermal conductivity is the thermal conductivity obtained by measurement according to the method described in the examples described later.
[0074] The thermal conductivity of the rigid polyurethane foam of the present invention is preferably 99.00% or less, more preferably 98.00% or less, compared with the case where the ratio of the tri- or higher polymethylene polyphenyl polyisocyanate to the polyisocyanate is less than 55% by mass. Since the thermal conductivity is lowered, the heat insulating property of the rigid polyurethane foam is improved.
[0075] The rigid polyurethane foam of the present invention has a density of 5 to 300 kg / m 3 The density can be controlled by the amount of the foaming agent used. The density is measured in accordance with JIS A 9511:2009.
[0076] (Mechanism of action) Polymeric MDI is a mixture of 4,4'-MDI, its isomers, and trinuclear or higher components. Rigid polyurethane foam obtained using polyisocyanate with a high ratio of trinuclear or higher components in polymeric MDI has finer cell diameters and reduced thermal conductivity, improving insulation. By using a polyisocyanate in which the proportion of trinuclear or higher components relative to the total amount of polyisocyanate is 55 mass % or more, it is possible to produce a rigid polyurethane foam having lower thermal conductivity and better heat insulation than conventional ones. EXAMPLES
[0077] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the examples described below, and various modifications are possible without departing from the gist of the present invention. Among Examples 1 to 12, Examples 3, 7, and 11 are working examples, Examples 4, 8, and 12 are comparative examples, and Examples 1, 2、 5. 6、 9 , and 10 is a reference example.
[0078] [Quantitative method for polymeric MDI] 3g of polyisocyanate and 6g of toluene were added to a 100mL eggplant flask and dissolved by stirring. Then, 18g of methanol was added to the eggplant flask and reacted by mixing and stirring for 1 hour. After that, toluene and excess methanol were removed by an evaporator to obtain a sample in which the terminal of the isocyanate group was converted to methyl urethane. The amount of isocyanate in the sample was determined using a GPC device (LC-20AD, Shimadzu Corporation). A differential refractive index detector (RI-504, Showa Denko Corporation; sensitivity 16) was used as the detector. Two TSKgel Super HZM-N, one HZ4000, one HZ2500, and one HZ1000 (all manufactured by Tosoh Corporation) were connected as columns. Tetrahydrofuran was used as the eluent at a flow rate of 0.45 mL / min, and the temperature was set to 40°C in a column oven (CTO-20A, Shimadzu Corporation). 5 mg of the sample was dissolved in 5 ml of tetrahydrofuran, and the solution was then filtered using a 0.5 μm filter to obtain the measurement sample. 0.02 mL of the measurement sample was injected into the GPC device and measured. Monodisperse polystyrene (manufactured by Tosoh Corporation) was used as the standard sample, and a molecular weight calibration curve was created to identify the molecular weight of the sample. The weight fraction of each component was calculated from the ratio of the peak area in each molecular weight range. The quantitative determination of polymeric MDI was carried out by adding up the mass fractions of monomeric MDI in the molecular weight range of 215 g / mol to 415 g / mol and the mass fractions of monomeric MDI including isomers of 2,2'-MDI, 2,4'-MDI and 4,4'-MDI shown in the molecular weight curve obtained by measurement, and dividing the sum by 100%.
[0079] [Raw materials] The raw materials used in each example are as follows: <Polyol> Polyol A1: Aromatic polyether polyol (EXCENOL NB-615, manufactured by AGC; Mw is 318, and the average hydroxyl value is 590 mgKOH / g). Polyol A2: Aromatic polyester polyol (Maximol RDK-133, manufactured by Kawasaki Chemical Industries, Ltd.; Mw is 471, and the average hydroxyl value is 315 mgKOH / g).
[0080] <Polyisocyanate> Polyisocyanate B1: A polyisocyanate composition containing 59.4% of polymeric MDI components having a molecular weight of 3 or more nuclei, 40.6% of 4,4'-MDI components, 2,2'-MDI and 2,4'-MDI components. Polyisocyanate B2: A polyisocyanate composition containing 67.0% of a polymeric MDI component having a molecular weight of 3 or more nuclei, 33.0% of a 4,4'-MDI component, a 2,2'-MDI component and a 2,4'-MDI component. Polyisocyanate B3: A polyisocyanate composition containing 72.1% of a component having a molecular weight of 3 or more nuclei of polymeric MDI, and 27.9% of a 4,4'-MDI component, a 2,2'-MDI component and a 2,4'-MDI component. Polyisocyanate B4: Polymeric MDI with 3 or more nuclei Has molecular weight A polyisocyanate composition containing 48.4% of a 4,4'-MDI component, 51.6% of a 2,2'-MDI and 2,4'-MDI component.
[0081] <Foaming agent> Foaming agent C0: Distilled water Foaming agent C1: 123 3 zd(E) Foaming agent C2: 1224yd(Z) Foaming agent C3: 1336mzz(Z)
[0082] <Foam stabilizer> Foam stabilizer D1: Silicone foam stabilizer (SH193, Dow Toray)
[0083] <Catalyst> Catalyst E1: Organic acid salt of amine (Polycat 201, Evonik) Catalyst E2: Quaternary ammonium salt-type trimerization reaction promotion catalyst (Dabco TMR-7, Evonik)
[0084] <Flame retardants> Flame retardant F1: Halogenated phosphate ester flame retardant (Phylor PCF, product name of ICL-IP JAPAN; tris(β-chloropropyl)phosphate)
[0085] [Example 1] <Preparation of polyol system liquid and polyisocyanate> Rigid polyurethane foams were produced according to the blending ratios shown in Table 1. The units of values shown in the "blending" column in Table 1 are parts by mass. Specifically, first, a polyol, a foam stabilizer, a catalyst, and a flame retardant were mixed to prepare a polyol system liquid at a liquid temperature of 15° C. The liquid temperature of the polyisocyanate was adjusted to 15° C.
[0086] <Preparation of Foaming Liquid Composition> The prepared polyisocyanate was added to the polyol system liquid, and the mixture was stirred and mixed for 5 seconds at a rotation speed of 3000 revolutions per minute using a mixer equipped with a stirring blade attached to a Hitachi drill press, to prepare a foaming liquid composition.
[0087] <Evaluation using box free form (Form 1)> (Reactivity) The prepared foaming liquid concentrate composition was quickly poured into a container measuring 200 mm in length × 200 mm in width × 200 mm in height to produce a box-free foam (hereinafter also referred to as "foam 1"). The time when mixing of the polyol system liquid and polyisocyanate in the foaming liquid composition began was defined as 0 seconds, and the time until the mixed liquid began to foam was defined as the cream time (ct) (seconds), the time until the foam began to foam and when a 3φ stainless steel rod was pierced, the foam pulled threads and began to harden was defined as the gel time (gt) (seconds), and the time until the surface began to harden and the stickiness of the foam surface disappeared was defined as the tack-free time (tft) (seconds).
[0088] (Core Density) The core part of the foam 1 manufactured in the same manner as above was cut into a cube of length 150 mm × width 150 mm × height 150 mm, and the core density (unit: kg / m 3 ) was calculated.
[0089] <Evaluation using Panel Form (Form 2)> The prepared foaming liquid composition was placed in an aluminum mold having a volume of 50 mm length × 400 mm width × 400 mm height, which was adjusted to a temperature of 40°C and placed vertically, with a polyethylene release bag of the same shape as the mold attached. Immediately after mixing the polyol system liquid and the polyisocyanate, the mixed liquid was poured into the mold with the polyethylene release bag of the same shape as the mold attached. The amount of the mixture was 42 to 44 kg / m 3 The blending ratio and the amount of the foaming liquid concentrate composition added were adjusted so that the .... After the blending, the blending was closed with a lid and sealed, and a panel foam (hereinafter, also referred to as "foam 2") was produced. The mass, density, thermal conductivity and core density of the obtained Foam 2 were measured by the following methods.
[0090] (mass) The mass (unit: kg) of the entire panel foam obtained was measured. (Density) The density (unit: kg / m) of the entire panel foam obtained was measured using a method in accordance with JIS A 9526:2017. 3 ) was measured.
[0091] (Thermal Conductivity) The foam 2 obtained by the above method was cut into a rectangular parallelepiped of 25 mm length × 200 mm width × 200 mm height, and the thermal conductivity (unit: W / m K) was measured in accordance with JIS A 1412: 2016. For the measurement, a thermal conductivity measuring device (Autolambda HC-074 type, product name of Eiko Seiki Co., Ltd.) was used, and the measurement conditions were a high temperature plate of 38°C, a low temperature plate of 10°C, and an average temperature of 23°C.
[0092] (Core Density) The density (unit: kg / m) was calculated from the mass and volume of the foam cut out for the thermal conductivity measurement described above. 3 ) was calculated.
[0093] [Examples 2-12] In the same manner as in Example 1, panel foams were produced according to the formulations shown in Tables 1 to 3. The foam mass, foam density, thermal conductivity and core density of the obtained panel foams were measured in the same manner as in Example 1. The units of the values shown in the "Composition" columns of Tables 2 and 3 are parts by mass, as in Table 1.
[0094] [Table 1]
[0095] [Table 2]
[0096] [Table 3]
[0097] [Results explanation] <Examples 1 to 4> The thermal conductivity of Foam 2 in Examples 1 to 3, which correspond to the examples using Foaming Agent C1, was 0.0194 W / m K or less, and the heat insulating properties were excellent. In particular, Example 3, which used a polyisocyanate containing a larger amount of a trinuclear or higher polymethylene polyphenyl polyisocyanate component, had a thermal conductivity of 0.0189 W / m K, which was the most excellent heat insulating properties. In Example 4, in which the content of trinuclear or higher components in the polyisocyanate was less than 55 mass%, the thermal conductivity of the panel foam exceeded 0.0199 W / m·K, and the heat insulation was inferior to the panel foams of Examples 1 to 3.
[0098] <Examples 5-8> The thermal conductivity of Foam 2 in Examples 5 to 7, which correspond to the examples using Foaming Agent C2, was 0.0197 W / m K or less, and the heat insulating properties were excellent. In particular, Example 7, which used a polyisocyanate containing a larger amount of a trinuclear or higher polymethylene polyphenyl polyisocyanate component, had a thermal conductivity of 0.0188 W / m K, which was the most excellent heat insulating properties. In Example 8, in which the content of trinuclear or higher components in the polyisocyanate was less than 55 mass%, the thermal conductivity of the panel foam exceeded 0.0199 W / m·K, and the heat insulation was inferior to that of the panel foams of Examples 5 to 7.
[0099] <Examples 9-12> The thermal conductivity of Foam 2 in Examples 9 to 11, which correspond to the examples using Foaming Agent C3, was 0.0197 W / m K or less, and the heat insulating properties were excellent. In particular, Example 11, which used a polyisocyanate containing a larger amount of a trinuclear or higher polymethylene polyphenyl polyisocyanate component, had a thermal conductivity of 0.0192 W / m K, which was the most excellent heat insulating properties. In Example 12, in which the content of trinuclear or higher components in the polyisocyanate was less than 55 mass%, the thermal conductivity of the panel foam exceeded 0.0200 W / m·K, and the heat insulation was inferior to the panel foams of Examples 9 to 11.
Claims
1. A method for producing a rigid polyurethane foam, comprising mixing a polyol, a polyisocyanate, and a blowing agent, the polyisocyanate contains 4,4'-diphenylmethane diisocyanate and a tri- or higher polymethylene polyphenyl polyisocyanate, and the ratio of the tri- or higher polymethylene polyphenyl polyisocyanate to the polyisocyanate is 72.1 mass% or more; the blowing agent comprises a hydrofluoroolefin and water; A method for producing a rigid polyurethane foam, wherein the ratio of the hydrofluoroolefin to the blowing agent is 50 to 99 mass % (excluding a method for producing a rigid polyurethane foam using glycerol having a hydroxyl value of 1825 mg KOH / g).
2. The method for producing a rigid polyurethane foam according to claim 1, further comprising mixing a foam stabilizer and a catalyst.
3. The method for producing a rigid polyurethane foam according to claim 1 or 2, wherein the hydrofluoroolefin is at least one selected from the group consisting of an E-isomer of 1-chloro-3,3,3-trifluoropropene, a Z-isomer of 1-chloro-2,3,3,3-tetrafluoropropene, and a Z-isomer of 1,1,1,4,4,4-hexafluoro-2-butene.
4. The method for producing a rigid polyurethane foam according to any one of claims 1 to 3, wherein the amount of the blowing agent per 100 parts by mass of the polyol is 10 to 100 parts by mass.
5. The method for producing a rigid polyurethane foam according to any one of claims 1 to 4, wherein the polyol comprises a polyether polyol and a polyester polyol.
6. The method for producing a rigid polyurethane foam according to claim 5, wherein the proportion of the polyether polyol to the total of the polyols is 30 to 80 mass%.
7. The method for producing a rigid polyurethane foam according to any one of claims 1 to 6, wherein the thermal conductivity of the rigid polyurethane foam is 99.00% or less relative to the thermal conductivity of rigid polyurethane foam 2 below. Rigid polyurethane foam 2: A rigid polyurethane foam obtained by mixing a polyol, a polyisocyanate, and a blowing agent, wherein the polyisocyanate contains 4,4'-diphenylmethane diisocyanate and a tri- or higher polymethylene polyphenyl polyisocyanate, and the ratio of the tri- or higher polymethylene polyphenyl polyisocyanate to the polyisocyanate is less than 55 mass%.
Citation Information
Patent Citations
Oxidation treating method
JP1980062827A
Rigid polyurethane foam
JP1994041271A
Production of rigid polyurethane foam
JP1998279653A
Rigid polyurethane foam, and three-solution-type premix composition and catalyst composition for producing rigid polyurethane foam
JP2018070708A
Catalyst composition for production of haloalkene polyurethane foam
JP2019085496A