Aggregate of resin particles, organic solvent dispersion of resin particles, and method for producing aggregate of resin particles
Resin particles with disulfide bonds, anionic, and cationic surfactants are produced to address the inefficiencies in existing photosoftening compositions, enabling light-induced softening and aggregation for diverse applications.
Patent Information
- Application Number
- JP2020173287
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-14
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-10-14
AI Technical Summary
Existing photosoftening compositions do not effectively utilize resin particles with disulfide bonds to achieve efficient light-induced softening and aggregation in organic solvent dispersions.
The development of resin particles containing a compound with a disulfide bond, an anionic surfactant, and a cationic surfactant, produced through a method involving emulsion formation and solvent removal, followed by aggregation with a surfactant pairing step, to create a photosoftening resin particle aggregate.
The method enables the production of resin particles that soften upon light irradiation, facilitating their use in various applications such as photoresist agents, softeners, and adhesive tapes, with enhanced water dispersibility and moldability.
Smart Images

Figure 0007571454000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an aggregate of resin particles, an organic solvent dispersion of resin particles, and a method for making the aggregate of resin particles. [Background technology]
[0002] Photosoftening compositions that are softened by irradiation with light are used in a variety of applications. For example, Patent Document 1 discloses an image forming apparatus equipped with a recording member having a photosoftening resin layer made of a photosoftening resin. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 11-190883 Summary of the Invention [Problem to be solved by the invention]
[0004] A primary object of the present disclosure is to provide a photosoftenable resin particle aggregate, an organic solvent dispersion of resin particles, and a method for producing the resin particle aggregate. [Means for solving the problem]
[0005] One aspect of the present disclosure relates to resin particles comprising a compound having a disulfide bond, an anionic surfactant, and a cationic surfactant.
[0006] Another aspect of the present disclosure relates to an aqueous dispersion of resin particles, comprising a compound having a disulfide bond, an anionic surfactant, and a cationic surfactant.
[0007] Another aspect of the present disclosure relates to a method for producing an aggregate of resin particles, comprising the steps of: adding an organic solvent solution containing a compound having a disulfide bond to an aqueous solution containing a first surfactant having an ionic group to prepare an emulsion; removing the organic solvent from the emulsion to obtain an aqueous dispersion of resin particles; and adding to the aqueous dispersion a solution containing a second surfactant having an ionic group that pairs with the ionic group to aggregate the resin particles. Effect of the Invention
[0008] According to the present disclosure, there are provided a photosoftenable resin particle aggregate, an organic solvent dispersion of resin particles, and a method for producing the resin particle aggregate. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is an image diagram showing a cross section of a resin particle according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, embodiments of the present disclosure will be described, however, the present disclosure is not limited to the following embodiments.
[0011] In this specification, "photosoftening" refers to a property that viscosity decreases, modulus decreases, loss tangent (tan δ) increases, hardness decreases, etc., due to light irradiation. In this specification, the term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes, as long as the intended effect of the process is achieved. In this specification, a numerical range indicated using "~" indicates a range including the numerical values described before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in stages in this specification, the upper limit or lower limit of a numerical range of a certain stage may be replaced by the upper limit or lower limit of a numerical range of another stage. In the numerical ranges described in this specification, the upper limit or lower limit of the numerical range may be replaced by the value shown in the examples. In addition, the upper limit and lower limit values described individually can be arbitrarily combined.
[0012] In this specification, the content of each component in the composition means the total amount of the multiple substances present in the composition when the composition contains multiple substances corresponding to each component, unless otherwise specified. In addition, the exemplified materials may be used alone or in combination of two or more types, unless otherwise specified. "A or B" may contain either A or B, or may contain both. In this specification, "(meth)acryloyl group" means an acryloyl group or a methacryloyl group, and other similar expressions are the same.
[0013] [Resin particle aggregates] The resin particle aggregate according to this embodiment contains a compound having a disulfide bond (hereinafter, sometimes referred to as “component (A)”) and a surfactant (hereinafter, sometimes referred to as “component (B)”).
[0014] Component (A): Compound having a disulfide bond The component (A) has a disulfide bond capable of generating a thiyl radical upon irradiation with light. The component (A) is not particularly limited as long as it is a compound having a disulfide bond (-SS-), but since the component (A) is reduced in molecular weight upon irradiation with light, it may be a high molecular weight component of a polymer or oligomer. The component (A) may be used alone or in combination of two or more types. It is preferable that the component (A) has multiple (two or more) disulfide bonds.
[0015] The component (A) may be, for example, a copolymer obtained by reacting a monomer having a disulfide bond and a functional group (hereinafter sometimes referred to as "component (A-1)") with a monomer having a substituent capable of reacting with the functional group (hereinafter sometimes referred to as "component (A-2)"), in other words, a reaction product of component (A-1) and component (A-2), i.e., a copolymer containing monomer units of component (A-1) and monomer units of component (A-2).
[0016] Examples of the functional group in the (A-1) component include a thiol group, a carboxy group, a hydroxyl group, an amino group, and an allyl group. The functional group in the (A-1) component may be, for example, at least one selected from the group consisting of a thiol group, a carboxy group, a hydroxyl group, an amino group, and an allyl group. The number of functional groups in the (A-1) component may be 2 or more from the viewpoint of increasing the molecular weight. On the other hand, the lower the degree of crosslinking of the (A) component, the easier it tends to be to soften the photosoftenable resin composition to a liquid state (liquid) when irradiated with light. Therefore, it is preferable to use a monomer having two functional groups as the (A-1) component, and when multiple monomers having different functional groups are used, it is preferable to increase the proportion of the monomer having two functional groups. The proportion of the monomer having two functional groups may be 75 to 100 mass%, 85 to 100 mass%, or 90 to 100 mass% based on the total amount of the (A-1) component. The proportion of monomers having three or more functional groups may be 0 to 10 mass %, 0 to 15 mass %, or 0 to 25 mass % based on the total amount of the component (A-1).
[0017] Examples of commercially available products of the component (A-1) include the Thiokol LP series (polysulfide polymer, manufactured by Toray Fine Chemicals Co., Ltd.), 3,3'-dithiodipropionic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), dithiodiethanol (manufactured by Tokyo Chemical Industry Co., Ltd.), cystamine hydrochloride (manufactured by Tokyo Chemical Industry Co., Ltd.), and diallyl disulfide (manufactured by Tokyo Chemical Industry Co., Ltd.). These components (A-1) may be used alone or in combination of two or more.
[0018] The (A-2) component is a monomer having a substituent capable of reacting with a functional group, and can be used without any particular limitation as long as it has a substituent capable of reacting with a functional group. Examples of the substituent include a group containing a cyclic ether (e.g., a glycidyl group, etc.), an isocyanate group, a (meth)acryloyl group, an aldehyde group, an amino group, a hydroxyl group, a carboxyl group, and an alkoxysilyl group. The substituent in the (A-2) component may be, for example, at least one selected from the group consisting of a group containing a cyclic ether, an isocyanate group, and a (meth)acryloyl group. The number of substituents in the (A-2) component may be two or more from the viewpoint of increasing the molecular weight. On the other hand, the lower the degree of crosslinking of the (A) component, the easier it tends to be to soften the photosoftenable resin composition to a liquid state (liquid) when irradiated with light, so it is preferable to use a monomer having two substituents as the (A-2) component, and when multiple monomers having different numbers of substituents are used, it is preferable to increase the proportion of the monomer having two substituents.
[0019] In one embodiment of the (A-2) component, the proportion of monomers having three or more substituents may be 20% by mass or more, 30% by mass or more, 40% by mass or more, or 50% by mass or more, and 90% by mass or less or 75% by mass or less, based on the total amount of the (A-2) component. The proportion of monomers having two substituents may be 10% by mass or more or 25% by mass or more, and 80% by mass or less, 70% by mass or less, 60% by mass or less, or 50% by mass or less, based on the total amount of the (A-2) component.
[0020] In another embodiment of the component (A-2), the proportion of monomers having two substituents may be 75 to 100 mass%, 85 to 100 mass%, or 90 to 100 mass%, based on the total amount of the component (A-2). The proportion of monomers having three or more substituents may be 0 to 10 mass%, 0 to 15 mass%, or 0 to 25 mass%, based on the total amount of the component (A-2).
[0021] Examples of the component (A-2) include a monomer having two or more cyclic ether-containing groups in one molecule; a monomer having two or more isocyanate groups in one molecule; a monomer having two or more (meth)acryloyl groups in one molecule; a monomer having two or more amino groups in one molecule, a monomer having two or more isocyanate groups and (meth)acryloyl groups in one molecule; a monomer having a cyclic ether-containing group and two or more alkoxysilyl groups in one molecule; a compound having two or more isocyanate groups in one molecule, or a monomer having two or more cyclic ether-containing groups in one molecule. Examples of the monomer include a combination of a compound having a group containing one or more cyclic ethers and a compound having an amino group, an acid anhydride skeleton, or a thiol group, and an alkoxyl group in one molecule; a monomer that is a combination of a compound having two or more isocyanate groups in one molecule and a compound having a hydroxyl group and a (meth)acryloyl group in one molecule; a monomer that is a combination of a compound having a group containing two or more cyclic ethers in one molecule and a compound having a carboxyl group and a (meth)acryloyl group in one molecule. These (A-2) components may be used alone or in combination of two or more.
[0022] Suitable combinations of the (A-1) component and the (A-2) component include, for example, a combination of a monomer having a disulfide bond and a thiol group or a hydroxyl group, and at least one selected from the group consisting of a monomer having two or more cyclic ether-containing groups in one molecule, a monomer having two or more (meth)acryloyl groups in one molecule, and a monomer having two or more isocyanate groups in one molecule; and a combination of a monomer having a disulfide bond and a carboxy group, and at least one selected from the group consisting of a monomer having two or more cyclic ether-containing groups in one molecule, a monomer having two or more amino groups in one molecule, and a monomer having two or more isocyanate groups in one molecule.
[0023] When the copolymer (A) is obtained by reacting the (A-1) component with the (A-2) component, the reaction ratio of these components can be appropriately adjusted based on the functional group equivalent of the (A-1) component and the substituent equivalent of the (A-2) component. The reaction between the (A-1) component and the (A-2) component may be carried out while heating. The reaction temperature may be, for example, 0 to 200°C, and the reaction time may be, for example, 0.1 to 240 hours.
[0024] When reacting the (A-1) component with the (A-2) component, a curing catalyst may be used as necessary. The curing catalyst can be selected arbitrarily according to the type of functional group of the (A-1) component and the type of substituent of the (A-2) component. When reacting a monomer having a thiol group or a hydroxyl group as a functional group as the (A-1) component with a monomer having an isocyanate group as a substituent as the (A-2) component, the curing catalyst may be, for example, a tin-based catalyst or an amine-based catalyst. When reacting a monomer having a carboxyl group as a functional group as the (A-1) component with a monomer having a group containing a cyclic ether as a substituent as the (A-2) component, the curing catalyst component may be, for example, an amine-based catalyst or a phosphorus-based catalyst. When a monomer having a thiol group or a hydroxyl group as a functional group as the component (A-1) is reacted with a monomer having a (meth)acryloyl group as a substituent as the component (A-2), an amine catalyst that promotes the Michael addition reaction between the thiol group or the hydroxyl group and the (meth)acryloyl group may be used.
[0025] Examples of tin-based catalysts include dibutyltin dilaurate, dibutyltin dichloride, dibutyltin oxide, dibutyltin dibromide, dibutyltin dimaleate, dioctyltin dilaurate, dibutyltin diacetate, dibutyltin sulfide, tributyltin sulfide, tributyltin oxide, tributyltin acetate, triethyltin ethoxide, tributyltin ethoxide, dioctyltin oxide, tributyltin chloride, tributyltin trichloroacetate, and tin 2-ethylhexanoate.
[0026] Examples of the amine catalyst include triethylamine, triethylenediamine, 1,8-diazabicyclo[5.4.0]undecene-7 (DBU), and 1,5-diazabicyclo[4.3.0]nonene-5 (DBN).
[0027] Examples of phosphorus-based catalysts include triphenylphosphine and its addition reaction products, (4-hydroxyphenyl)diphenylphosphine, bis(4-hydroxyphenyl)phenylphosphine, and tris(4-hydroxyphenyl)phosphine.
[0028] The content of the curing catalyst may be 0.005 to 10 mass %, 0.01 to 5 mass %, or 0.02 to 3 mass % based on the total of the components (A-1) and (A-2).
[0029] The molecular weight or weight average molecular weight (Mw) of the component (A) may be 200 to 10,000,000, 1,000 to 2,000,000, or 2,500 to 1,000,000. Mw is a polystyrene-equivalent value obtained by gel permeation chromatography (GPC) using a calibration curve with standard polystyrene.
[0030] (B) Component: Surfactant The surfactant contains an anionic surfactant (hereinafter, sometimes referred to as "component (B-1)") and a cationic surfactant (hereinafter, sometimes referred to as "component (B-2)").
[0031] Examples of anionic surfactants include fatty acid oils such as sodium oleate and castor oil potassium, alkyl sulfate ester salts such as sodium lauryl sulfate and ammonium lauryl sulfate, alkyl benzene sulfonates such as sodium dodecylbenzene sulfonate, alkyl naphthalene sulfonates, alkanesulfonates, dialkyl sulfosuccinates such as sodium dioctyl sulfosuccinate, alkenyl succinates (dipotassium salts), alkyl phosphate ester salts, naphthalene sulfonate-formaldehyde condensates, polyoxyethylene alkyl ether sulfates such as polyoxyethylene alkyl phenyl ether sulfate ester salts and sodium polyoxyethylene lauryl ether sulfate, polyoxyethylene alkyl sulfate ester salts, polyoxyethylene lauryl ether acetates such as sodium polyoxyethylene lauryl ether acetate, alkyl benzene sulfonic acids such as dodecylbenzene sulfonic acid, alpha olefin sulfonates such as sodium tetradecene sulfonate, alkyl sulfate ester salts, alkyl ether sulfate ester salts, alaninates such as N-lauroyl-N-methyl-β-alanine sodium salt and their salts, and fatty acid soaps.
[0032] Examples of cationic surfactants include alkylamine salts such as laurylamine acetate and stearylamine acetate; and quaternary ammonium salts such as cetyltrimethylammonium bromide, cetyltrimethylammonium chloride, lauryltrimethylammonium bromide and lauryltrimethylammonium chloride. can be done.
[0033] The amount of the (B-1) component added may be 0.01 to 50 parts by mass, 0.05 to 40 parts by mass, or 0.1 to 30 parts by mass, relative to 100 parts by mass of the (A) component, from the viewpoint of further improving the water dispersibility of the resin particles. The amount of the (B-2) component added may be 0.01 to 50 parts by mass, 0.05 to 40 parts by mass, or 0.1 to 30 parts by mass, relative to 100 parts by mass of the (A) component, from the viewpoint of further improving the water dispersibility of the resin particles.
[0034] Component (C): Polymeric dispersant The resin particles according to the present embodiment may further contain a polymeric dispersant as component (C). Examples of polymeric dispersants include polyvinyl alcohol and ion-modified polyvinyl alcohol. The ion-modified polyvinyl alcohol may have a carboxy group, a sulfo group, or a quaternary ammonium salt. The component (C) preferably contains a carboxy-modified polyvinyl alcohol because it is easy to form an ionic bond with the component (B-2).
[0035] The amount of the component (C) added may be 0.01 to 50 parts by mass, 0.05 to 40 parts by mass, or 0.1 to 30 parts by mass per 100 parts by mass of the component (A), from the viewpoint of further enhancing the water dispersibility of the resin particles.
[0036] (D) Photoradical generator The resin particles according to the present embodiment may contain a photoradical generator as component (D). In this case, component (D) is contained in polymer particle 1 together with component (A). The photoradical generator may be a component that reacts with a thiyl radical generated when the resin particles are irradiated with light, or a component that generates a photoinduced radical. As the photoradical generator, a photoradical polymerization initiator or the like can be used. When the resin particles are prepared by adding component (D), it is preferable to handle the component (D) under light-shielded conditions in order to suppress decomposition caused by light.
[0037] Examples of the photoradical generator include an intramolecular cleavage type photoradical polymerization initiator and a hydrogen abstraction type photoradical polymerization initiator. Examples of the intramolecular cleavage type photoradical polymerization initiator include a benzyl ketal type photoradical polymerization initiator; an α-hydroxyacetophenone type photoradical polymerization initiator; a benzoin type photoradical polymerization initiator; an aminoacetophenone type photoradical polymerization initiator; an oxime ketone type photoradical polymerization initiator; an acylphosphine oxide type photoradical polymerization initiator; a titanocene type photoradical polymerization initiator; a thiobenzoic acid S-phenyl polymerization initiator; and high molecular weight derivatives thereof. Examples of the hydrogen abstraction type photoradical polymerization initiator include a benzophenone type photoradical polymerization initiator, a thioxanthone type photoradical polymerization initiator, and an anthraquinone type photoradical polymerization initiator.
[0038] The content of the (D) component may be 1 part by mass or more, 5 parts by mass or more, or 10 parts by mass or more, and may be 40 parts by mass or less, 30 parts by mass or less, or 25 parts by mass or less, per 100 parts by mass of the (A) component.
[0039] The resin particle aggregate of this embodiment can be produced by a method comprising the steps of: preparing an emulsion by adding an organic solvent solution containing a compound having a disulfide bond to an aqueous solution containing a first surfactant having an ionic group; removing the organic solvent from the emulsion to obtain an aqueous dispersion of resin particles containing the compound having a disulfide bond and the first surfactant; and adding to the aqueous dispersion a solution containing a second surfactant having an ionic group that pairs with the ionic group, thereby agglomerating the resin particles containing the compound having a disulfide bond, the first surfactant, and the second surfactant.
[0040] The aqueous dispersion of resin particles can be prepared by a method including the steps of: preparing an emulsion by adding an organic solvent solution containing a compound having a disulfide bond (A) to an aqueous solution containing a first surfactant; and removing the organic solvent from the emulsion. The first surfactant can be an anionic surfactant or a cationic surfactant.
[0041] Examples of the organic solvent include aromatic hydrocarbons such as benzene, xylene, and toluene; ketones such as cyclohexanone and methyl ethyl ketone; cyclic ethers such as dioxane and tetrahydrofuran; and esters such as ethyl acetate, butyl acetate, and propyl acetate.
[0042] The organic solvent solution containing the component (A) is added to an aqueous solution containing the first surfactant, and then dispersed in water using a dispersing device such as a homogenizer to form polymer particles, thereby obtaining an emulsion of resin particles having the first surfactant attached to the surface of the polymer particles. The temperature for preparing the emulsion may be 0 to 80°C, and is preferably 40°C or lower in order to prevent particle aggregation.
[0043] Since the polymer particles in the emulsion contain an organic solvent, an aqueous dispersion of the resin particles can be obtained by removing the organic solvent from the emulsion. The temperature at which the organic solvent is removed may be appropriately set depending on the boiling point of the organic solvent.
[0044] A solution containing a second surfactant is added to the aqueous dispersion to aggregate the resin particles, thereby obtaining an aggregate of the resin particles. The second surfactant has an ionic group that pairs with the first surfactant. When an anionic surfactant is used as the first surfactant, a cationic surfactant is used as the second surfactant, and when a cationic surfactant is used as the first surfactant, an anionic surfactant is used as the second surfactant.
[0045] [Dispersion of resin particles in organic solvent] The resin particle aggregate according to this embodiment can be dispersed in an organic solvent and used as an organic solvent dispersion of resin particles containing a compound having a disulfide bond, an anionic surfactant, and a cationic surfactant.
[0046] Examples of the organic solvent include aromatic hydrocarbons such as benzene, xylene, and toluene; ketones such as cyclohexanone; cyclic ethers such as dioxane and tetrahydrofuran; and esters such as ethyl acetate, butyl acetate, and propyl acetate.
[0047] The average particle diameter (D50) of the resin particles according to the present embodiment is preferably 50 to 1000 nm, more preferably 50 to 500 nm, further preferably 60 to 400 nm, and particularly preferably 65 to 300 nm. The average particle diameter can be calculated by measuring the particle size distribution of the resin particles by a dynamic light scattering method.
[0048] 1 is an image diagram showing a cross section of a resin particle 10 according to this embodiment. The resin particle 10 is composed of a polymer particle 1 containing component (A), a first surfactant 2 present in the vicinity of the surface of the polymer particle 1, and a second surfactant 4 ionically bonded to the first surfactant. In the resin particle 10, an ionic group possessed by the first surfactant 2 and an ionic group possessed by the second surfactant 4 form an ionic bond.
[0049] The resin particles or aggregates thereof according to the present embodiment can be formed into a film and used as a photosoftenable resin film. In addition, the resin particles or aggregates thereof can be formed into a block and used as a photosoftenable resin block. The method for forming the resin particles or aggregates thereof into a film or block is not particularly limited, and known methods can be applied.
[0050] The resin particles or aggregates thereof according to the embodiment may be mixed with other components to prepare a resin composition. Examples of the other components include thermosetting resins such as epoxy resins, thermoplastic resins, adhesion improvers such as coupling agents, polymerization inhibitors, light stabilizers, antifoaming agents, fillers, chain transfer agents, thixotropy-imparting agents, flame retardants, release agents, surfactants, lubricants, antistatic agents, and other additives.
[0051] The resin particles or aggregates thereof according to the present embodiment have a property that, by irradiation with light, the disulfide bond (-SS-) in the compound is broken, and the compound having the disulfide bond is reduced in molecular weight and softened. The resin particles can also be softened to a liquid (liquid state). In addition, the resin particles have a property of being easily molded into a film or block shape. By utilizing such a property, the resin particles or aggregates thereof according to the present embodiment can be applied to, for example, photoresist agents for photolithography, and can be used as a photosensitive resin composition or a photosensitive resin film. The photosensitive resin composition or the photosensitive resin film can be patterned by irradiation with light (exposure), and further can be developed by washing with water after irradiation with light (exposure). The resin particles according to the present embodiment can be suitably used for forming a pattern film.
[0052] The resin particles or aggregates thereof according to this embodiment can also be used in a variety of applications, such as a softener or easy-removal agent for strong adhesive tapes; an adhesive for weakly adhesive or non-adhesive films; a partial softener for coating materials, adhesives, or adhesives; a partial softener for molding materials; an ultra-low elasticity film that can be punched and obtained by irradiating light after punching; a moisture-proofing agent; a capsule coating that softens and dissolves when irradiated with light; and a thickener that reduces viscosity when irradiated with light.
[0053] By irradiating the resin particles or aggregates thereof according to the embodiment with light, a softened resin particle can be obtained. The light for light irradiation is not particularly limited, and may be, for example, ultraviolet light or visible light. The wavelength of the light for light irradiation may be 150 to 830 nm. The light irradiation is performed, for example, using a light irradiation device with an irradiation dose of 100 mJ / cm. 2 The irradiation can be performed under the above conditions. The amount of irradiation means the product of illuminance and irradiation time (seconds). Examples of light sources for irradiating ultraviolet light or visible light include low pressure mercury lamps, medium pressure mercury lamps, high pressure mercury lamps, metal halide lamps, LED lamps, etc. The light irradiation may be performed directly on the resin particles or through glass or the like. EXAMPLES
[0054] The present disclosure will be described in more detail below with reference to examples, although the present disclosure is not limited to these examples.
[0055] (Production Example 1) In a sample tube, 0.61 g of Miramer M240 (EO-modified diacrylate of bisphenol A, manufactured by Bigen Specialty Chemical Co., Ltd.), 4.39 g of Thiokol LP-55 (dithiol having a disulfide bond, average molecular weight: 4000, manufactured by Toray Fine Chemical Co., Ltd.), and 7.5 g of toluene were added, and a mixture was obtained by stirring at 80 rpm using a mix rotor. Next, 0.02 g of DBU (1,8-diazabicyclo[5.4.0]undecene-7, manufactured by San-Apro Co., Ltd.) was added to the mixture and mixed, after which the inside of the sample tube was replaced with nitrogen and the reaction was carried out while stirring at 80 rpm using a mix rotor for 30 minutes. Then, 7.5 g of toluene was added to the reactant and stirred at 80 rpm using a mix rotor. As a result, a polymer solution containing component (A) (polymer concentration: 25% by mass) was obtained.
[0056] In order to prepare an aggregate of resin particles, the following materials were prepared. Anionic surfactant: Neopex G-15 (sodium dodecylbenzenesulfonate (soft type): 16% by mass, water: 84% by mass, manufactured by Kao Corporation) Cationic surfactant: CTAB (cetyltrimethylammonium bromide, Fujifilm Wako Pure Chemical Industries, Ltd.) Polymer dispersant: AP-17 (carboxyl-modified polyvinyl alcohol, manufactured by Nippon Vacuum & Poval Co., Ltd.) Organic solvent: Toluene (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)
[0057] [Example 1] 82.8g of pure water, 4.5g of 2% AP-17-containing aqueous solution, and 2.7g of G-15 were mixed to prepare 90g of the first surfactant aqueous solution. 10g of the polymer solution was slowly dropped into the surfactant aqueous solution at room temperature, and while cooling the solution in an ice bath, the solution was ultrasonically dispersed for 5 minutes using a homogenizer to obtain 100g of emulsion. Then, while heating the emulsion at an internal temperature of 85°C, toluene was removed to obtain an aqueous dispersion of resin particles a. Resin particles a are resin particles containing component (A), component (B-1), and component (C).
[0058] 2 g of the aqueous dispersion of resin particles a was collected and centrifuged at room temperature for 20 minutes (rotation speed: 1000 rpm), the supernatant was discarded, 1400 μL of water was added, and the resin particles were dispersed in water again using a Voltarex mixer. When 900 μL of a 0.1% by mass CTAB aqueous solution was added to the aqueous dispersion as a second surfactant, the resin particles were aggregated in water. Next, 1400 μL of toluene was added, and the aggregates of resin particles b were extracted into the organic layer (toluene layer), and a toluene dispersion of resin particles b was obtained. Resin particles b are resin particles containing components (A), (B-1), (B-2), and (C).
[0059] It is predicted that by blending a photoradical generator with the above-mentioned resin particle aggregates, photosoftening properties will be exhibited. [Explanation of symbols]
[0060] 1...polymer particle, 2...first surfactant, 4...second surfactant, 10...resin particle.
Claims
1. An aggregate of resin particles, comprising a compound having a disulfide bond, an anionic surfactant, and a cationic surfactant, wherein the compound having a disulfide bond is a high molecular weight component of a polymer or oligomer having a disulfide bond.
2. 10. The agglomerate of claim 1 further comprising a polymeric dispersant.
3. The flocculant according to claim 2 , wherein the polymeric dispersant contains a carboxy-modified polyvinyl alcohol.
4. An organic solvent dispersion of resin particles comprising a compound having a disulfide bond, an anionic surfactant, and a cationic surfactant, wherein the compound having a disulfide bond is a high molecular weight component of a polymer or oligomer having a disulfide bond.
5. The organic solvent dispersion according to claim 4 , wherein the resin particles further comprise a polymeric dispersant.
6. The organic solvent dispersion according to claim 5 , wherein the polymeric dispersant contains a carboxy-modified polyvinyl alcohol.
7. A step of preparing an emulsion by adding an organic solvent solution containing a compound having a disulfide bond to an aqueous solution containing a first surfactant having an ionic group; removing the organic solvent from the emulsion to obtain an aqueous dispersion of resin particles; and adding a solution containing a second surfactant having an ionic group that pairs with the ionic group to the aqueous dispersion to aggregate the resin particles, A method for producing an aggregate of resin particles, wherein the compound having a disulfide bond is a high molecular weight component of a polymer or oligomer having a disulfide bond.
8. The method of claim 7 , wherein the aqueous solution further comprises a polymeric dispersant.
9. The method according to claim 8 , wherein the polymeric dispersant contains a carboxy-modified polyvinyl alcohol.
Citation Information
Patent Citations
Powdered polysulfide rubber and its production
JP1991139563A
Curable composition
JP1993025392A
Preparation of toner composition
JP1994214418A
Preparation of toner composition and preparation of toner
JP1995146585A
Image forming device and recording material
JP1999190883A