Automotive interior materials

A thermoplastic elastomer composition for automobile interiors, combining propylene polymer, block copolymers, and light stabilizers, addresses the shortcomings of existing materials by enhancing scratch resistance, tactile feel, and heat resistance, suitable for luxury and sustainable automotive design.

JP7571645B2Active Publication Date: 2024-10-23MAZDA MOTOR CORP +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021053301
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-26
Publication Date
2024-10-23
Estimated Expiration
2041-03-26

AI Technical Summary

Technical Problem

Existing thermoplastic elastomer compositions used in automobile interiors lack sufficient scratch resistance, tactile sensation, and heat resistance, failing to meet the demands for luxury and environmental sustainability in automotive design.

Method used

A thermoplastic elastomer composition comprising propylene polymer, a block copolymer with aromatic vinyl and conjugated diene compound units, a hydrocarbon rubber softener, high-viscosity polyorganosiloxane, and specific light stabilizers, formulated in precise mass ratios to enhance scratch resistance, tactile feel, and heat resistance.

Benefits of technology

The composition provides automobile interior members with excellent scratch resistance, tactile sensation, and heat resistance, improving the quality and comfort of interior spaces while reducing environmental impact through paintless interiors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571645000001
    Figure 0007571645000001
  • Figure 0007571645000002
    Figure 0007571645000002
  • Figure 0007571645000003
    Figure 0007571645000003
Patent Text Reader

Abstract

To provide an automobile interior member that is excellent in tactile sensation, scratch resistance, light resistance and heat resistance.SOLUTION: Provided is an automobile interior member that is made of a thermoplastic elastomer composition containing the following components (A) to (G) in specific proportions. Component (A) propylene-based polymer. Component (B) a (hydrogenated) block copolymer having two or more aromatic vinyl compound polymer blocks P and one or more conjugated diene compound polymer blocks Q. Component (C) a softener for hydrocarbon-based rubber. Component (D) high viscosity polyorganosiloxane. Component (E) specific aralkyl group-containing polyorganosiloxane. Component (F) N,N',4,7-tetrakis{4,6-bis[N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidyl)amino]-1,3,5-triazin-2-yl}-4,7-diazadecane-1,10-diamine. Component (G) 2,4-bis(1,1-dimethylethyl)phenyl-3,5-bis(1,1-dimethylethyl)-4-hydroxy-benzoate.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an automobile interior component made of a specific thermoplastic elastomer composition. [Background technology]

[0002] Thermoplastic elastomers are being used as environmentally friendly materials to replace conventionally used vulcanized rubber, polyvinyl chloride resin, etc., for automobile interior components. Thermoplastic elastomers soften and become fluid when heated, and have rubber elasticity when cooled. They have the advantages of having moldability similar to that of thermoplastic resins, unique rubber elasticity, and recyclability, but have problems with being inferior to conventional materials in terms of scratch resistance, flexibility, touch, and abrasion resistance.

[0003] In response to such problems, Patent Document 1 describes that by using a thermoplastic elastomer composition in which a silicone oil having a viscosity (JIS Z8803, 25°C) of 100,000 centistokes (cSt) or more is added to a styrene-based or olefin-based rubber and polypropylene, it is possible to improve low-temperature impact resistance and surface scratch resistance while maintaining mechanical strength.

[0004] Patent Document 2 describes that by using a hydrogenated styrene-based block copolymer, a polypropylene-based resin, and a mineral oil-based rubber softener, as a thermoplastic elastomer composition, and a silicone oil having a viscosity (25°C) of 1,000,000 centistokes or more, the composition has excellent moldability and the resulting molded products have excellent flexibility, touch, and abrasion resistance. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 08-176353 [Patent Document 2] JP 2002-348433 A Summary of the Invention [Problem to be solved by the invention]

[0006] In recent years, there has been a demand for a luxurious feel and comfort in the interior space of an automobile, while at the same time, there has been a trend towards paintless construction in order to reduce the environmental impact and the number of processes involved. In response to such demands, there is also a demand for automobile interior materials to have further improvements in scratch resistance and tactile feel while maintaining the light resistance and heat resistance required for the automobile's usage environment.

[0007] According to the investigations of the present inventors, it is believed that the molded article of the thermoplastic elastomer composition described in Patent Document 1 is still insufficient in terms of scratch resistance, tactile feel, and heat resistance required for automobile interior components, and it is difficult to achieve all of these properties at the same time. The molded article of the thermoplastic elastomer composition described in Patent Document 2 is considered to be insufficient in terms of the touch and heat resistance required for automobile interior parts, and it has been difficult to achieve both of these properties.

[0008] An object of the present invention is to solve the above problems and to provide an automobile interior member having excellent tactile feel, scratch resistance, light resistance and heat resistance. [Means for solving the problem]

[0009] As a result of intensive research aimed at solving the above-mentioned problems, the present inventors have found that it is possible to provide an automobile interior component that is excellent in all of tactile feel, scratch resistance, light resistance, and heat resistance by combining a thermoplastic elastomer component containing a propylene-based polymer, a block copolymer having a polymer block P mainly composed of aromatic vinyl compound units and at least one polymer block Q mainly composed of conjugated diene compound units and / or a hydrogenated product thereof, and a hydrocarbon-based rubber softener in a specific mass ratio, with two specific types of polyorganosiloxanes and a specific light stabilizer in a specific mass ratio, thereby completing the present invention. That is, the present invention has the following features.

[0010] [1] An automobile interior member formed from a thermoplastic elastomer composition, the thermoplastic elastomer composition containing the following components (A) to (G), in which the thermoplastic elastomer composition contains 30 to 40 mass% of component (A), 20 to 30 mass% of component (B), and 35 to 45 mass% of component (C) relative to 100 mass% of the total of components (A) to (C), and contains 1.1 to 2.5 parts by mass of component (D), 0.5 to 1.5 parts by mass of component (E), 0.01 to 0.5 parts by mass of component (F), and 0.001 to 0.05 parts by mass of component (G) relative to 100 parts by mass of the total of components (A) to (C). Component (A) Propylene-based polymer Component (B) A block copolymer having at least two polymer blocks P mainly composed of aromatic vinyl compound units and at least one polymer block Q mainly composed of conjugated diene compound units, and / or a hydrogenated product thereof. Component (C) Hydrocarbon-based rubber softener Component (D) Polyorganosiloxane with a viscosity (JIS Z8803, 25°C) of 100,000 cSt or more Component (E) An aralkyl group-containing polyorganosiloxane having a repeating unit represented by the following general formula (1) in the molecule: [ka] (R in general formula (1) 1 represents a hydrocarbon group having 1 to 18 carbon atoms, R 2 represents an aralkyl group having 7 to 12 carbon atoms. Component (F) N,N',4,7-tetrakis{4,6-bis[N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidyl)amino]-1,3,5-triazin-2-yl}-4,7-diazadecane-1,10-diamine Component (G) 2,4-bis(1,1-dimethylethyl)phenyl-3,5-bis(1,1-dimethylethyl)-4-hydroxy-benzoate [2] The automotive interior component according to [1], wherein component (D) is a polyorganosiloxane having a viscosity (JIS Z8803, 25°C) of 1,000,000 cSt or more. [3] The automobile interior member according to [1] or [2], wherein the aromatic vinyl compound unit of component (B) is a styrene unit, and the conjugated diene compound unit is a butadiene unit. Effect of the Invention

[0011] According to the present invention, it is possible to provide an automobile interior member having excellent scratch resistance, tactile feel, light resistance and heat resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The following describes in detail the embodiments of the present invention, but the present invention is not limited to the following description, and can be modified as desired without departing from the gist of the present invention. In this specification, when a numerical value or physical property value is enclosed before and after "~", the value before and after the "~" is included.

[0013] [Thermoplastic elastomer composition] The thermoplastic elastomer composition constituting the automobile interior component of the present invention (hereinafter, may be referred to as the "thermoplastic elastomer composition of the present invention") is characterized by containing the following components (A) to (G) in specified proportions. Component (A) Propylene-based polymer Component (B) A block copolymer having at least two polymer blocks P mainly composed of aromatic vinyl compound units and at least one polymer block Q mainly composed of conjugated diene compound units, and / or a hydrogenated product thereof. Component (C) Hydrocarbon-based rubber softener Component (D) Polyorganosiloxane with a viscosity (JIS Z8803, 25°C) of 100,000 cSt or more Component (E) An aralkyl group-containing polyorganosiloxane having a repeating unit represented by the following general formula (1) in the molecule: [ka] (R in general formula (1) 1 represents a hydrocarbon group having 1 to 18 carbon atoms, R 2represents an aralkyl group having 7 to 12 carbon atoms. Component (F) N,N',4,7-tetrakis{4,6-bis[N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidyl)amino]-1,3,5-triazin-2-yl}-4,7-diazadecane-1,10-diamine Component (G) 2,4-bis(1,1-dimethylethyl)phenyl-3,5-bis(1,1-dimethylethyl)-4-hydroxy-benzoate

[0014] <Component (A)> The propylene polymer of component (A) used in the present invention (hereinafter may be referred to as "propylene polymer (A)") may contain 50% by mass or more of propylene units in the monomer units constituting the propylene polymer (A), but from the viewpoints of heat resistance, rigidity, crystallinity, chemical resistance, etc., the content of propylene units in the propylene polymer (A) is preferably 60% by mass or more, more preferably 75% by mass or more, and even more preferably 90% by mass or more. On the other hand, the upper limit of the content of propylene units is not particularly limited and may be 100% by mass. The content of the propylene unit in component (A) and each of the structural units of the other copolymerization components described below can be determined by infrared spectroscopy.

[0015] The type of the propylene polymer (A) is not particularly limited, and specific examples thereof include a propylene homopolymer and a propylene-ethylene copolymer (e.g., a propylene-ethylene random copolymer, a propylene-ethylene block copolymer), and any of these can be used.

[0016] The melt flow rate (JIS K7210, 230°C, 21.2N load) of the propylene polymer (A) is not particularly limited, but is usually 0.05 to 2000g / 10min, preferably 0.05 to 500g / 10min, and more preferably 0.1 to 200g / 10min. By controlling the melt flow rate within the above range, excellent moldability and good appearance of the obtained automobile interior member are obtained, and mechanical properties, particularly tensile breaking strength, can be controlled within a desired range.

[0017] The catalyst used in producing the propylene polymer (A) is not particularly limited, but for example, a polymerization method using a stereoregular catalyst is preferred. Examples of the stereoregular catalyst include, but are not limited to, Ziegler catalysts and metallocene catalysts. Among these catalysts, metallocene catalysts are preferred.

[0018] Examples of Ziegler catalysts include, but are not limited to, two-component catalysts consisting of a transition metal component, such as a titanium halide compound such as titanium trichloride, titanium tetrachloride, or trichloroethoxytitanium, or an organometallic component, such as an alkylaluminum compound or its halide, hydride, or alkoxide, and a three-component catalyst obtained by adding an electron-donor compound containing nitrogen, carbon, phosphorus, sulfur, oxygen, silicon, or the like to any of the above components.

[0019] The metallocene catalyst is not limited to the following, but may be, for example, a catalyst consisting of a transition metal compound of Group 4 of the periodic table containing a ligand having a cyclopentadienyl skeleton (so-called metallocene compound), a cocatalyst capable of activating the metallocene compound to a stable ionic state by reacting with the metallocene compound, and, if necessary, an organoaluminum compound, and any known catalyst can be used. The metallocene compound is preferably a bridged metallocene compound capable of stereoregular polymerization of propylene, and more preferably a bridged metallocene compound capable of isoregular polymerization of propylene.

[0020] Examples of the method for producing the propylene-based polymer (A) include a slurry method using an inert solvent in the presence of the catalyst, a solution method, a gas phase method substantially without a solvent, and a bulk polymerization method using a polymerization monomer as a solvent. For example, in the case of a slurry method, the polymerization can be carried out in an inert hydrocarbon or liquid monomer such as n-butane, isobutane, n-pentane, isopentane, hexane, heptane, octane, cyclohexane, benzene, toluene, or xylene. The polymerization temperature is usually -80 to 150°C, preferably 40 to 120°C. The polymerization pressure is preferably 1 to 60 atm. The molecular weight of the resulting propylene-based polymer (A) can be adjusted with hydrogen or other known molecular weight regulators. The polymerization is carried out by a continuous or batch reaction, and the conditions may be those usually used. Furthermore, the polymerization reaction may be carried out in one stage or multiple stages.

[0021] The propylene polymer (A) may be a commercially available product, and examples thereof include polypropylene block copolymer manufactured by Sunallomer Corporation, Novatec (registered trademark) PP, and WAYMAX (registered trademark) manufactured by Japan Polypropylene Corporation.

[0022] The propylene-based polymer (A) may be used alone or in combination of two or more kinds having different copolymerization compositions, physical properties, and the like.

[0023] <Ingredient (B)> Component (B) used in the present invention is a block copolymer and / or a hydrogenated product thereof (hereinafter sometimes referred to as a "(hydrogenated) block copolymer") having a polymer block P (hereinafter sometimes referred to as a "block P") mainly composed of at least two aromatic vinyl compound units and a polymer block Q (hereinafter sometimes referred to as a "block Q") mainly composed of at least one conjugated diene compound unit.

[0024] Here, the term "mainly composed of" means that the target monomer unit is contained in the target polymer block in an amount of 50 mol % or more.

[0025] The aromatic vinyl compound constituting the block P is not particularly limited, and examples thereof include styrene, α-methylstyrene, p-methylstyrene, divinylbenzene, 1,1-diphenylethylene, N,N-dimethyl-p-aminoethylstyrene, and N,N-diethyl-p-aminoethylstyrene. Among these, from the viewpoints of availability and productivity, styrene, α-methylstyrene, and p-methylstyrene are preferably used. Styrene is more preferred. The block P may be composed of one type of aromatic vinyl compound unit or two or more types of aromatic vinyl compound units, and may contain monomer units other than vinyl aromatic compound units.

[0026] The conjugated diene compound constituting the block Q is a diolefin having a pair of conjugated double bonds, and includes, but is not limited to, 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, and 1,3-hexadiene. Among these, 1,3-butadiene and isoprene are preferably used from the viewpoint of productivity. More preferably, 1,3-butadiene is used. Block Q may be composed of one type of conjugated diene compound unit or may be composed of two or more types of conjugated diene compound units, and may contain monomer units other than conjugated diene compound units.

[0027] The block polymer having at least two blocks P and at least one block Q may be linear, branched, radial, or the like, but is preferably a block copolymer represented by the following formula (I) or (II): P-(QP)m (I) (PQ)n (II) (In the formula, P represents a block P, Q represents a block Q, m represents an integer of 1 to 5, and n represents an integer of 2 to 5. When a plurality of blocks P and a plurality of blocks Q are present, the compound units may be the same or different.

[0028] From the viewpoint of rubber elasticity of the composition, component (B) used in the present invention is preferably a block copolymer represented by formula (I), more preferably a block copolymer represented by formula (I) in which m is 3 or less, even more preferably a block copolymer represented by formula (I) in which m is 2 or less, and particularly preferably a block copolymer represented by formula (I) in which m is 1.

[0029] Component (B) used in the present invention may be a hydrogenated product of a block copolymer having a block P and a block Q. In this case, it is preferably a hydrogenated product of a block copolymer represented by formula (I), more preferably a hydrogenated product of a block copolymer represented by formula (I) in which m is 3 or less, even more preferably a hydrogenated product of a block copolymer represented by formula (I) in which m is 2 or less, and particularly preferably a hydrogenated product of a block copolymer represented by formula (I) in which m is 1.

[0030] The content of block P in the block copolymer of component (B) is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, and particularly preferably 20% by mass or more. The content of block P in the block copolymer of component (B) is preferably 70% by mass or less, more preferably 60% by mass or less, even more preferably 50% by mass or less, and particularly preferably 40% by mass or less. The higher the content of block P in the above range, the better the mechanical strength, and the lower the content, the better the flexibility and the less prone to bleeding out. By setting the content in the above range, it becomes easier to achieve both mechanical strength and flexibility while suppressing bleeding out.

[0031] The proportion of block Q in the block copolymer of component (B) is preferably high from the viewpoint of flexibility and resistance to bleeding out of the thermoplastic elastomer composition, and is preferably low from the viewpoint of mechanical strength. Specifically, the content of block Q in the block copolymer of component (B) is preferably 30% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, and particularly preferably 60% by mass or more. The proportion of block Q in the block copolymer of component (B) is preferably 95% by mass or less, more preferably 90% by mass or less, even more preferably 85% by mass or less, and particularly preferably 80% by mass or less. The higher the proportion of block Q in the above range, the more excellent the flexibility and the more difficult it is to bleed out, and the lower the proportion, the more excellent the mechanical strength. By setting the proportion in the above range, it becomes easier to achieve both mechanical strength and flexibility while suppressing bleeding out. When the aromatic vinyl compound constituting block Q in the block copolymer of component (B) is a styrene unit, the above-mentioned content of block Q can be expressed as a styrene unit content.

[0032] The weight average molecular weight (Mw) of the (hydrogenated) block copolymer of component (B) is preferably 10,000 or more, more preferably 30,000 or more, and on the other hand, is preferably 800,000 or less, more preferably 650,000 or less, and even more preferably 500,000 or less. In terms of heat resistance and mechanical strength, the Mw of the (hydrogenated) block copolymer of component (B) is preferably larger in the above range, and is preferably smaller in terms of molded appearance, fluidity, and moldability. By setting the Mw of the (hydrogenated) block copolymer of component (B) within the above range, a thermoplastic elastomer composition excellent in heat resistance, mechanical strength, molded appearance, fluidity, and moldability can be obtained.

[0033] Here, Mw is a weight average molecular weight in terms of polystyrene measured by gel permeation chromatography (hereinafter sometimes abbreviated as "GPC") under the following conditions. (Measurement conditions) Equipment: "150C ALC / GPC" manufactured by Nihon Millipore Column: Showa Denko "AD80M / S" x 3 Detector: FOXBORO infrared spectrophotometer "MIRANIA" Wavelength: 3.42μm Solvent: o-dichlorobenzene Temperature: 140℃ Flow rate: 1cm 3 / min Injection volume: 200 microliters Concentration: 2mg / cm 3 0.2% by mass of 2,6-di-t-butyl-p-phenol was added as an antioxidant.

[0034] Preferable examples of the component (B) used in the present invention include styrene-butadiene-styrene block copolymers and hydrogenated products thereof, and styrene-isoprene / butadiene-styrene block copolymers and hydrogenated products thereof.

[0035] Commercially available products may also be used as component (B). Specific examples include Kraton (registered trademark) G manufactured by Kraton Polymers, Septon (registered trademark) manufactured by Kuraray Co., Ltd., Tuftec (registered trademark) and SOE (registered trademark) manufactured by Asahi Kasei Corporation, and TAIPOL (registered trademark) manufactured by TSRC.

[0036] The (hydrogenated) block copolymer of component (B) may be used alone or in combination of two or more kinds.

[0037] <Ingredient (C)> The hydrocarbon-based rubber softener, component (C), used in the present invention is effective in improving the flexibility and flowability of the thermoplastic elastomer composition of the present invention.

[0038] As the hydrocarbon-based rubber softener, mineral oil-based softeners and synthetic resin-based softeners are preferred because of their high affinity for component (B), and mineral oil-based softeners are more preferred.

[0039] Mineral oil-based softeners are generally mixtures of aromatic hydrocarbons, naphthenic hydrocarbons and paraffinic hydrocarbons, and those in which 50% or more of the total carbon atoms are derived from paraffinic hydrocarbons are called paraffinic oils, those in which about 30-45% of the total carbon atoms are derived from naphthenic hydrocarbons are called naphthenic oils, and those in which 35% or more of the total carbon atoms are derived from aromatic hydrocarbons are called aromatic oils. The hydrocarbon-based rubber softener used as component (C) may be any one of the above-mentioned softeners or a mixture of multiple types, but among these, paraffinic oils are preferred because of their good hue. In addition, examples of synthetic resin-based softeners include polybutene and low molecular weight polybutadiene.

[0040] The kinematic viscosity at 40°C (based on JIS K2283) of the hydrocarbon-based rubber softener is preferably low in terms of improving the fluidity of the thermoplastic elastomer composition of the present invention, but is preferably high in terms of preventing fogging and the like. Specifically, it is preferably 20 centistokes (cSt) or more, more preferably 50 centistokes or more. On the other hand, it is preferably 800 centistokes or less, and more preferably 600 centistokes or less.

[0041] The hydrocarbon rubber softener of component (C) can be obtained as a commercially available product. Examples of the commercially available product include the "Nippon Oil Polybutene (registered trademark) HV" series manufactured by JX Nippon Oil & Energy Corporation and the "Diana (registered trademark) Process Oil PW" series manufactured by Idemitsu Kosan Co., Ltd., and the relevant product can be appropriately selected and used from these.

[0042] The hydrocarbon-based rubber softeners of component (C) may be used alone or as a mixture of two or more kinds in any combination and ratio.

[0043] <Ingredient (D)> Component (D) is a polyorganosiloxane having a viscosity (JIS Z8803, 25°C) of 100,000 cSt or more (hereinafter, may be simply referred to as "high viscosity polyorganosiloxane"), and there is no particular upper limit on the viscosity of component (D). The higher the viscosity of component (D), the higher the effect of improving scratch resistance and abrasion resistance, which is preferable. From this viewpoint, it is particularly preferable that the viscosity (JIS Z8803, 25°C) of component (D) is 1,000,000 cSt or more.

[0044] The type of substituent bonded to the siloxane main chain in the molecular structure of the high-viscosity polyorganosiloxane is not particularly limited, but dimethyl silicone (dimethylpolysiloxane), methylphenyl silicone, or alkyl-modified silicone is preferably used. In order to thoroughly mix the high viscosity polyorganosiloxane with other materials of the present invention, it is preferable to use it as a master batch of a propylene polymer or an ethylene polymer. As the propylene polymer that can be used as a master batch, for example, the propylene polymer described in the propylene polymer of component (A) above can be used.

[0045] The high viscosity polyorganosiloxane of component (D) is available as a commercially available product. Examples of the commercially available products include the "DOW CORNING TORAY (registered trademark)" series and "DOW CORNING (registered trademark)" series manufactured by DuPont Toray Specialty Materials Co., Ltd., "X-22-2101" manufactured by Shin-Etsu Chemical Co., Ltd., and "MB50-001G2" manufactured by Dow Corning Toray Co., Ltd., and the relevant product can be appropriately selected and used from these.

[0046] The high viscosity polyorganosiloxane of component (D) may be used alone or as a mixture of two or more kinds in any combination and ratio.

[0047] <Ingredient (E)> Component (E) is an aralkyl group-containing polyorganosiloxane having a repeating unit represented by the following general formula (1) in the molecule (hereinafter sometimes simply referred to as "aralkyl group-containing polyorganosiloxane").

[0048] [ka]

[0049] (R in general formula (1) 1 represents a hydrocarbon group having 1 to 18 carbon atoms, R 2 represents an aralkyl group having 7 to 12 carbon atoms.

[0050] By using the high-viscosity polyorganosiloxane of component (D) in combination with the aralkyl group-containing polyorganosiloxane of component (E), it is possible to improve the tactile feel and scratch resistance while maintaining the heat resistance of the automotive interior component of the present invention.

[0051] In the general formula (1), R 1 R is a hydrocarbon group having 1 to 18 carbon atoms, and examples of such alkyl groups include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, and an octyl group. 1 is preferably an alkyl group having 1 to 3 carbon atoms, and more preferably a methyl group.

[0052] R 2 is an aralkyl group having 7 to 12 carbon atoms, and examples of such phenylalkyl groups include benzyl, phenylethyl, phenylpropyl, and 2-phenylpropyl groups. By having an aralkyl group in the organopolysiloxane, it is possible to obtain a thermoplastic elastomer composition that maintains transparency and has an excellent touch. From the viewpoints of maintaining transparency and improving the touch, R 2 is preferably a 2-phenylpropyl group.

[0053] Component (E) is preferably an aralkyl group-containing polyorganosiloxane having in the molecule a repeating unit represented by the general formula (1) above as well as a repeating unit represented by the following general formula (2):

[0054] [ka]

[0055] (R in general formula (2) 3 and R 4 each independently represents an organic group having 1 to 18 carbon atoms.

[0056] In the general formula (2), R 3 ,R 4 Examples of the organic group having 1 to 18 carbon atoms include an alkyl group, an aryl group, an alkenyl group, an alkoxy group, and an epoxy group, and specific examples thereof include a methyl group, an ethyl group, a propyl group, a butyl group, a hexyl group, a cyclohexyl group, an octyl group, a nonyl group, a decyl group, a dodecyl group, a tetradecyl group, a phenyl group, a methoxy group, and an ethoxy group. 3 ,R 4 is preferably an alkyl group, more preferably an alkyl group having 1 to 3 carbon atoms, and particularly preferably a methyl group.

[0057] The content of aralkyl groups in the aralkyl group-containing polyorganosiloxane of component (E) used in the present invention is preferably 1 to 60 mol %, more preferably 5 to 55 mol %, and even more preferably 5 to 50 mol %, of all organic groups bonded to silicon atoms. When the content of aralkyl groups is within the above range, it becomes easier to obtain a thermoplastic elastomer composition having excellent touch and scratch resistance.

[0058] The kinetic viscosity (25°C) of the aralkyl group-containing polyorganosiloxane of component (E) used in the present invention is preferably 1 cSt or more, more preferably 5 cSt or more, and even more preferably 10 cSt or more. There is no particular upper limit, but it usually does not exceed 100,000 cSt. The higher the kinetic viscosity in the above range, the greater the effect of improving abrasion resistance, and the lower the kinetic viscosity, the greater the effect of improving stickiness and the better the touch. By setting the kinetic viscosity (25°C) of component (E) in the above range, it is possible to obtain the desired abrasion resistance and stickiness improvement effect. Here, the kinetic viscosity of component (E) is the kinetic viscosity at 25° C. measured using an Ubbelohde viscometer in accordance with ASTM D445-46T (or JIS Z8803).

[0059] Commercially available products can also be used as component (E). An example of a commercially available product of component (E) is "KF-410" manufactured by Shin-Etsu Chemical Co., Ltd.

[0060] The aralkyl group-containing polyorganosiloxane of component (E) may be used alone or in combination of two or more kinds.

[0061] <Component (F)> The component (F) used in the present invention, N,N',4,7-tetrakis{4,6-bis[N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidyl)amino]-1,3,5-triazin-2-yl}-4,7-diazadecane-1,10-diamine, is a hindered amine light stabilizer and is effective in suppressing light-resistant bleeding of the thermoplastic elastomer composition of the present invention. Commercially available products can also be used as component (F). An example of a commercially available product of component (F) is "SABOSTAB UV119" manufactured by SONGWON.

[0062] <Ingredients (G)> The component (G) used in the present invention, 2,4-bis(1,1-dimethylethyl)phenyl-3,5-bis(1,1-dimethylethyl)-4-hydroxybenzoate, is a benzoate-based light stabilizer and is effective in suppressing light-resistant bleeding of the thermoplastic elastomer composition of the present invention. As the component (G), a commercially available product can also be used. An example of a commercially available product of the component (G) is "Tinuvin 120" manufactured by BASF.

[0063] <Mixing ratio> In the thermoplastic elastomer composition of the present invention, the content ratios of components (A), (B), and (C) relative to the total of 100 mass% are 30 to 40 mass% for component (A), 20 to 30 mass% for component (B), and 35 to 45 mass% for component (C), preferably 32 to 38 mass% for component (A), 22 to 28 mass% for component (B), and 37 to 43 mass% for component (C), and more preferably 32 to 36 mass% for component (A), 24 to 28 mass% for component (B), and 38 to 42 mass% for component (C).

[0064] The contents of component (D), component (E), component (F) and component (G) are, relative to 100 parts by mass of the total of components (A) to (C), 1.1 to 2.5 parts by mass of component (D), 0.5 to 1.5 parts by mass of component (E), 0.01 to 0.1 parts by mass of component (F), and 0.001 to 0.05 parts by mass of component (G), preferably 1.2 to 2.4 parts by mass of component (D), 0.7 to 1.3 parts by mass of component (E), 0.01 to 0.08 parts by mass of component (F), and 0.001 to 0.04 parts by mass of component (G), and more preferably 1.3 to 2.3 parts by mass of component (D), 0.8 to 1.2 parts by mass of component (E), 0.01 to 0.07 parts by mass of component (F), and 0.001 to 0.01 parts by mass of component (G).

[0065] When the thermoplastic elastomer composition of the present invention contains the propylene-based polymer of component (A) in the above range, the effect of improving the heat resistance and mechanical properties of component (A) can be sufficiently obtained while the blending effects of the other components can be sufficiently obtained. In addition, by including the (hydrogenated) block copolymer of component (B) in the above range, the effects of improving flexibility, good touch, and scratch resistance due to component (B) can be fully obtained while the blending effects of the other components can be fully obtained. Furthermore, by including the hydrocarbon rubber softener of component (C) in the above range, the effect of improving flexibility and flowability of component (C) can be fully obtained while fully obtaining the compounding effects of the other components. Furthermore, by including components (D) and (E) in the above-mentioned ratios relative to 100 parts by mass of the total of components (A) to (C), it is possible to obtain a sufficient effect of improving scratch resistance while maintaining a good touch and heat resistance. Furthermore, by containing components (F) and (G) in the above-mentioned ratios relative to 100 parts by mass of the total of components (A) to (C), it is possible to obtain a product that has excellent light resistance while maintaining a good feel and heat resistance and sufficiently improving scratch resistance.

[0066] <Other ingredients> The thermoplastic elastomer composition of the present invention may contain other components (hereinafter simply referred to as "other components") other than the components (A) to (G) as necessary, within the scope of the object of the present invention. Examples of other components include resins and elastomers other than the components (A) and (B) (hereinafter collectively referred to as "other resins"), and various additives.

[0067] Examples of other resins that may be contained in the thermoplastic elastomer composition of the present invention include polyolefin resins (excluding those corresponding to the above-mentioned component (A)), polyester resins, polyamide resins, styrene resins (excluding those corresponding to the above-mentioned component (B)), acrylic resins, polycarbonate resins, polyphenylene ethers, polyvinyl chloride resins, and other resins; olefin-based elastomers such as ethylene-propylene copolymer rubber (EPM), ethylene-propylene-non-conjugated diene copolymer rubber (EPDM), ethylene-butene copolymer rubber (EBM), and ethylene-propylene-butene copolymer rubber; polyamide-based elastomers such as polyamide-polyol copolymers; polyvinyl chloride-based elastomers and polybutadiene-based elastomers, their hydrogenated products, those modified with acid anhydrides, etc. to introduce polar functional groups, and those grafted, randomly, and / or block copolymerized with other monomers. The above-mentioned other resins may be used alone or in combination of two or more types.

[0068] Furthermore, examples of additives that may be contained in the thermoplastic elastomer composition of the present invention include molding processing aids such as antioxidants, crystal nucleating agents, lubricants, ultraviolet absorbers, light stabilizers other than components (F) and (G), hydrolysis resistance improvers, colorants such as pigments and dyes, antistatic agents, conductive agents, reinforcing agents, fillers, plasticizers (excluding those corresponding to component (C) above), release agents, and foaming agents.

[0069] In addition, the thermoplastic elastomer composition of the present invention may contain an antioxidant (heat stabilizer), such as a hydroxylamine-based antioxidant, a dithiocarbamate-based antioxidant, a hindered phenol-based antioxidant, a sulfur-based antioxidant, or a phosphorus-based antioxidant.

[0070] As the hydroxylamine-based antioxidant, N,N-dialkylhydroxylamines are preferred, and are represented by the general formula R a R b NOH (in the formula, R a and R b Each independently represents an alkyl group.a or R b is a dodecyl group, a tetradecyl group, a hexadecyl group, an octadecyl group, or a heptadecyl group. Particularly preferred dialkylhydroxylamines are N,N-dioctadecylhydroxylamine and N,N-dihexadecylhydroxylamine or mixtures thereof, and examples of commercially available products include "Irganox (registered trademark) 1010" manufactured by BASF.

[0071] As the dithiocarbamate-based antioxidant, metal salts of dialkyldithiocarbamic acid are preferred, among which nickel dialkyldithiocarbamate is preferred, and nickel dibutyldithiocarbamate is particularly preferred because of its large effect of improving heat aging resistance.

[0072] Known hindered phenol-based antioxidants can be used, and it is preferable to use those having a molecular weight of 500 or more, such as tetrakis[methylene-3(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane.

[0073] The sulfur-based antioxidants are compounds containing sulfur, such as thioethers, dithioacid salts, mercaptobenzimidazoles, thiocarbanilides, and thiodipropionate compounds. However, they do not include compounds equivalent to the dithiocarbamate antioxidants. Among these, thiodipropionate compounds are particularly preferred.

[0074] Examples of phosphorus-based antioxidants include phosphorus-containing compounds such as phosphoric acid, phosphorous acid, hypophosphorous acid derivatives, phenylphosphonic acid, polyphosphonates, dialkyl pentaerythritol diphosphites, and dialkyl bisphenol A diphosphites.

[0075] These antioxidants may be used alone or in combination of two or more.

[0076] When the thermoplastic elastomer composition of the present invention contains an antioxidant, the content of the antioxidant is preferably 0.01 to 5 parts by mass per 100 parts by mass of the total of components (A), (B) and (C). A content of 0.01 parts by mass or more is preferable from the viewpoint of improving the heat deterioration resistance, while a content of 5 parts by mass or less is preferable from the viewpoint of preventing problems such as bleeding and the mechanical strength of the composition.

[0077] The total content of the additives such as the antioxidants in the thermoplastic elastomer composition of the present invention is preferably 2 parts by mass or less, and more preferably 1 part by mass or less, per 100 parts by mass of the total of component (A), component (B), and component (C).

[0078] <Method of producing thermoplastic elastomer composition> The method for producing the thermoplastic elastomer composition of the present invention is not particularly limited, and the composition can be produced, for example, by dry blending components (A) to (G) and other components used as necessary, followed by melt kneading in a conventional manner. The mixing device used in this case is not particularly limited, but examples thereof include kneading devices such as a Banbury mixer, a Labo Plastomill, a single screw extruder, and a twin screw extruder. Among these, the melt mixing method using an extruder is preferable from the viewpoints of productivity and good kneading properties. The melt temperature during kneading can be appropriately set, but is usually in the range of 130 to 300°C, and preferably in the range of 150 to 250°C.

[0079] [Automotive interior components] The automobile interior member of the present invention is produced by molding the thermoplastic elastomer composition of the present invention. The thermoplastic elastomer composition of the present invention can be molded by various molding methods such as ordinary injection molding and extrusion molding.

[0080] The molding conditions for injection molding the thermoplastic elastomer composition of the present invention are as follows. The molding temperature is usually 160 to 250°C, preferably 170 to 220°C. The injection pressure is usually 5 to 100 MPa, preferably 10 to 80 MPa. The mold temperature is usually 10 to 80°C, preferably 20 to 60°C.

[0081] The injection molded article obtained by injection molding the thermoplastic elastomer composition of the present invention can also be heat fused to an olefinic hard resin such as a propylene resin to form a composite molded article for use in automobile interior parts. EXAMPLES

[0082] Hereinafter, specific aspects of the present invention will be described in more detail using examples, but the present invention is not limited to the following examples as long as it does not deviate from the gist of the present invention. Note that the values ​​of various manufacturing conditions and evaluation results in the following examples are meant as preferred upper or lower limit values ​​in the embodiments of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit values ​​and the values ​​of the following examples or values ​​of the examples.

[0083] In the following Examples and Comparative Examples, the raw materials used in the preparation of the thermoplastic elastomer compositions and the methods for evaluating the obtained thermoplastic elastomer compositions are as follows.

[0084] [Raw materials used] <Component (A)> A-1: "Novatec (registered trademark) PP BC06C" manufactured by Japan Polypropylene Corporation Propylene-Ethylene Block Copolymer Propylene unit content: 91% by mass MFR (JIS K7210, 230℃, 21.2N load): 60g / 10 minutes

[0085] <Ingredient (B)> B-1: “TAIPOL (registered trademark) 6159” manufactured by TSRC Hydrogenated styrene-butadiene-styrene block copolymer Weight average molecular weight: 400,000 Styrene unit content: 30% by mass

[0086] <Ingredient (C)> C-1: Idemitsu Kosan's "Diana Process Oil PW90" Paraffin oil Kinematic viscosity (40℃): 90cSt

[0087] <Ingredient (D)> D-1: Toray Dow Corning "MB50-001G2" Dimethylpolysiloxane Masterbatch Dimethylpolysiloxane content: 50% by mass Viscosity (JIS Z8803, 25℃): 1,000,000cSt or more <Ingredient (E)> E-1: Shin-Etsu Chemical Co., Ltd. "KF-410" An aralkyl group-containing organopolysiloxane having a repeating unit represented by the general formula (1) and a repeating unit represented by the general formula (2). R in general formula (1) 1 : Methyl group R in general formula (1) 2 : 2-phenylpropyl group R in general formula (2) 3 ,R 4 : Methyl group Aralkyl group content: 39 mol% Kinematic viscosity (25℃): 900cSt

[0088] <Component (F)> F-1: SONGWON "SABOSTAB UV119"

[0089] <Ingredients (G)> G-1: BASF "Tinuvin 120"

[0090] <Component (X)> X-1: Shin-Etsu Chemical Co., Ltd. "KF96-1000cs" Dimethylpolysiloxane Viscosity (JIS Z8803, 25℃): 1000cSt

[0091] [Evaluation of Thermoplastic Elastomer Composition] <Tactile evaluation> The injection molded articles (350 mm × 100 mm × 2 mm, leather texture for automobile interiors) made from the pellets of the thermoplastic elastomer compositions obtained in the Examples and Comparative Examples were examined for tactile sensation when touched with the index finger, and evaluated according to the following criteria. The feel of the injection molded article is preferably such that no bleeding occurs on the surface and the article does not stick to the hands, and more preferably has a smooth feel. ○: Smooth and does not feel sticky on the hands ×: Sticky or dry but feels sticky on hands

[0092] <Scratch resistance evaluation> For injection-molded articles (350 mm x 100 mm x 2 mm) made from pellets of the thermoplastic elastomer compositions obtained in the Examples and Comparative Examples, the degree of scratching on the surface of the test piece was visually inspected using a scratching needle with a tip curvature radius of 0.7 mm at a scratching speed of 100 mm / sec and a load of 300 g, and evaluated according to the following criteria. ○: No change or slight change was observed △: Changes are observed ×: Significant change

[0093] <Light resistance evaluation> In accordance with JIS B7753, the Sunshine Weatherometer S80 manufactured by Suga Test Instruments was used. Discharge with Sunshine Carbon Arc (Ultra Long Life Carbon 4 pairs) light source The voltage was set to 50 V, the discharge current was set to 60 A, and irradiation was performed for 200 hours under the conditions of a black panel temperature of 63°C and a relative humidity of 50% on a square plate surface (width 100 mm x length 100 mm x thickness 2 mm) cut out from an injection molded body made from pellets of the thermoplastic elastomer composition obtained in the Examples and Comparative Examples. A type glass filter was used. After the irradiation treatment, the bleeding and stickiness of the surface were visually confirmed and evaluated according to the following criteria. ○: No change observed △: Slight changes observed ×: Changes are observed

[0094] <Heat resistance evaluation> For injection molded articles (350 mm x 100 mm x 2 mm) made from pellets of the thermoplastic elastomer compositions obtained in the Examples and Comparative Examples, test pieces were collected after standing in a thermostatic chamber at 85°C for 10 hours. Thereafter, the initial gloss and gloss after the heat resistance test were measured, the amount of change was calculated, and the evaluation was performed according to the following criteria. The gloss was measured at an angle of 60° from the plate surface of the test piece using a gloss meter (BYK, micro-TRI-gloss, Cat. No. 4563). ○: Glossiness change is less than ±0.2 ×: Gloss change is ±0.2 or more

[0095] [Example 1] Component (A-1): 34 parts by mass, component (B-1): 26 parts by mass, component (C-1): 40 parts by mass, 100 parts by mass in total, component (D-1): 1.5 parts by mass (the amount of dimethylpolysiloxane in component (D-1) (50% of the actual amount)), component (E-1): 1.0 part by mass, component (F-1): 0.05 parts by mass, component (G-1): 0.01 part by mass, and antioxidant (BASF product name Irganox (registered trademark) 1010) 0.1 part by mass were mixed, and the resulting mixture was melt-kneaded (cylinder temperature 180 ° C to 220 ° C) with a twin-screw kneader to produce pellets of a thermoplastic elastomer composition. The obtained thermoplastic elastomer composition was injected and filled into a sheet-shaped mold of 350 mm length x 100 mm width x 2 mm thickness at an injection speed of 40 mm / sec using an electric injection molding machine (manufactured by Sumitomo Heavy Industries, Ltd.) with a mold clamping force of 180 t, a cylinder temperature of 220°C, and a mold temperature of 40°C. After filling was completed, the molded article was cooled for 30 seconds and then removed. The obtained injection molded article was evaluated for touch, scratch resistance, light resistance, and heat resistance. The results are shown in Table 1.

[0096] [Example 2, Comparative Examples 1 to 4] Pellets of a thermoplastic elastomer composition were obtained in the same manner as in Example 1, except that the raw material blending amounts were as shown in Table 1. The obtained thermoplastic elastomer composition was evaluated in the same manner as in Example 1. The evaluation results are shown in Table 1.

[0097] [Table 1]

[0098] [Evaluation Results] It can be seen from Table 1 that Examples 1 and 2, which correspond to the thermoplastic elastomer compositions of the present invention, are excellent in terms of touch, scratch resistance, and heat resistance. In contrast, Comparative Example 1 is an example in which the content of component (D) does not satisfy the lower limit of 1.1 parts by mass, and the touch and scratch resistance are poor. Comparative Example 2 is an example in which component (X) is contained in place of components (D) and (E), and is inferior in all respects of touch, scratch resistance, and heat resistance. Comparative Example 3 is an example that does not contain component (D) and contains component (E) in an amount exceeding the upper limit of 1.5 parts by mass, and is inferior in touch and heat resistance. Comparative Example 4 is an example in which component (D) is contained within the specified range but component (E) is not contained, and the touch and heat resistance are poor. Comparative Example 5 does not contain the component (G) and has poor light resistance. Comparative Example 6 does not contain the component (F) and has poor light resistance. [Industrial Applicability]

[0099] Automobile interior parts obtained from the thermoplastic elastomer composition of the present invention have excellent touch, scratch resistance, light resistance and heat resistance, and are used to make automobile interior spaces more luxurious and comfortable. Furthermore, from the viewpoints of reducing environmental load and process steps, they are preferably used to achieve paint-free applications.

Claims

1. An automobile interior member formed from a thermoplastic elastomer composition, the thermoplastic elastomer composition containing the following components (A) to (G), in which the thermoplastic elastomer composition contains 30 to 40 mass% of component (A), 20 to 30 mass% of component (B), and 35 to 45 mass% of component (C) relative to 100 mass% of the total of components (A) to (C), and the automobile interior member contains 1.1 to 2.5 mass parts of component (D), 0.5 to 1.5 mass parts of component (E), 0.01 to 0.5 mass parts of component (F), and 0.001 to 0.05 mass parts of component (G) relative to 100 parts by mass of the total of components (A) to (C). Component (A) Propylene-based polymer Component (B) A block copolymer having at least two polymer blocks P mainly composed of aromatic vinyl compound units and at least one polymer block Q mainly composed of conjugated diene compound units, and / or a hydrogenated product thereof. Component (C) Hydrocarbon-based rubber softener Component (D) Polyorganosiloxane having a viscosity (JIS Z8803, 25°C) of 100,000 cSt or more Component (E) An aralkyl group-containing polyorganosiloxane having a repeating unit represented by the following general formula (1) in the molecule: 【Chemistry 1】 (R in general formula (1) 1 represents a hydrocarbon group having 1 to 18 carbon atoms; R 2 represents an aralkyl group having 7 to 12 carbon atoms. Component (F): N,N',4,7-tetrakis{4,6-bis[N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidyl)amino]-1,3,5-triazin-2-yl}-4,7-diazadecane-1,10-diamine Component (G) 2,4-bis(1,1-dimethylethyl)phenyl-3,5-bis(1,1-dimethylethyl)-4-hydroxybenzoate

2. 2. The automobile interior member according to claim 1, wherein component (D) is a polyorganosiloxane having a viscosity (JIS Z8803, 25°C) of 1,000,000 cSt or more.

3. 3. The automobile interior member according to claim 1 or 2, wherein the aromatic vinyl compound unit of component (B) is a styrene unit, and the conjugated diene compound unit is a butadiene unit.

Citation Information

Patent Citations

  • Thermoplastic elastomer good in scuff resistance

    JP1996176353A

  • Composite molding

    JP2002347178A

  • Thermoplastic elastomer composition

    JP2002348433A

  • Automobile part obtained by injection-molding polypropylene resin composition

    JP2010174254A

  • Molded article

    JP2013237728A