Sheet molding compound and its manufacturing method, carbon fiber reinforced plastic molded product and its manufacturing method, and manufacturing method of electrocoated product

The prepreg, composed of a specific epoxy resin composition, addresses the rigidity loss in CFRP at high temperatures by maintaining mechanical integrity through controlled curing, enabling its use in electrodeposition coated products.

JP7571793B2Active Publication Date: 2024-10-23MITSUBISHI CHEM CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022557572
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-06-08
Filing Date
2021-10-20
Publication Date
2024-10-23
Estimated Expiration
2041-10-20

AI Technical Summary

Technical Problem

Carbon fiber reinforced plastic (CFRP) materials experience a significant decrease in rigidity when exposed to high temperatures during the electrodeposition coating process, which limits their suitability for applications requiring high thermal stability.

Method used

A prepreg is developed using an epoxy resin composition containing a bisphenol-type epoxy resin, [4-(glycidyloxy)phenyl]diglycidylamine, and a curing agent, which is cured at controlled temperatures to achieve a glass transition temperature (G'-Tg) between 100°C and 200°C and a dynamic storage modulus at 200°C that is at least 8% of the value at 100°C, enhancing the material's rigidity under heat.

Benefits of technology

The prepreg maintains improved rigidity at elevated temperatures, making it suitable for electrodeposition coated products by suppressing the decrease in mechanical properties typically observed in CFRP during the drying process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571793000005
    Figure 0007571793000005
  • Figure 0007571793000006
    Figure 0007571793000006
  • Figure 0007571793000007
    Figure 0007571793000007
Patent Text Reader

Abstract

The present invention provides a method for producing an electrodeposition-coated article, the method being suitable for producing an electrodeposition-coated article comprising a carbon-fiber-reinforced plastic. The method for producing an electrodeposition-coated article according to the present invention comprises: a molding step in which a prepreg comprising a thickened composition and a carbon fiber reinforcement is hardened to obtain a molded carbon-fiber-reinforced plastic, the thickened composition being one obtained by thickening an epoxy resin composition obtained by mixing a bisphenol A epoxy resin, [4-(glycidyloxy)phenyl]diglycidylamine, and a hardener ingredient; and an electrodeposition coating step in which the molded carbon-fiber-reinforced plastic is coated by electrodeposition. When hardened at 140°C, the epoxy resin composition gives a hardened resin having a glass transition temperature G'-Tg higher than 100°C but lower than 200°C and having a dynamic storage modulus G' at 200°C which is 8% or greater of the G' thereof at 100°C.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an electrodeposition coated article, a prepreg, and an epoxy resin composition. [Background technology]

[0002] Carbon fiber reinforced plastics (CFRP) is a lightweight material with excellent mechanical properties that makes it suitable for parts in automobiles, motorcycles, bicycles, ships, railway vehicles, manned aircraft, unmanned aerial vehicles, and other transportation equipment, and its importance has been increasing in recent years. One method for manufacturing a structure made of carbon fiber reinforced plastic is to use a prepreg such as SMC (sheet molding compound) (Patent Document 1). A prepreg is an intermediate molding material made by previously impregnating carbon fiber reinforcement with resin. Electrodeposition-coated articles formed by electrodeposition-coating carbon fiber reinforced plastic obtained by curing SMC are known (Patent Document 2 and Patent Document 3). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2018 / 190329 [Patent Document 2] JP 2009-13306 A [Patent Document 3] International Publication No. 2016 / 104416 Summary of the Invention [Problem to be solved by the invention]

[0004] In electrocoating, the workpiece reaches its highest temperature during the drying process, where the temperature reaches a maximum of approximately 200°C. Therefore, if a carbon fiber reinforced plastic could be developed that suppresses the loss of rigidity when heated to 200°C, it would be suitable for use as a material for electrocoating products. The present invention has been made through investigations conducted by the present inventors based on this idea, and its main objects are to provide a method for producing an electrodeposition-coated article suitable for producing an electrodeposition-coated article made of carbon fiber reinforced plastic, to provide a prepreg that gives a carbon fiber reinforced plastic that can be preferably used in the production of an electrodeposition-coated article, and to provide an epoxy resin composition that is preferably used in the production of such a prepreg. [Means for solving the problem]

[0005] According to one aspect of the present invention, there is provided a method for producing an electrodeposition-coated article, comprising: a molding step of obtaining a carbon fiber reinforced plastic molded article by curing a prepreg composed of a carbon fiber reinforcing material and an epoxy resin composition containing a bisphenol-type epoxy resin, [4-(glycidyloxy)phenyl]diglycidylamine, and a curing agent component; and an electrodeposition coating step of applying electrodeposition coating to the carbon fiber reinforced plastic molded article. According to another aspect of the present invention, there is provided a prepreg comprising an epoxy resin composition containing a bisphenol-type epoxy resin, [4-(glycidyloxy)phenyl]diglycidylamine, and a curing agent component, and a carbon fiber reinforcing material, the epoxy resin composition giving, when cured at 140°C, a cured resin having a glass transition temperature G'-Tg higher than 100°C and lower than 200°C, and a dynamic storage modulus G' at 200°C that is preferably 8% or more, more preferably 10% or more, and even more preferably 12% or more of the value at 100°C. According to yet another aspect of the present invention, there is provided a prepreg comprising an epoxy resin composition containing a bisphenol-type epoxy resin, [4-(glycidyloxy)phenyl]diglycidylamine, 4,4'-methylenebis(N,N-diglycidylaniline), and a curing agent component, and a carbon fiber reinforcing material. According to yet another aspect of the present invention, there is provided an epoxy resin composition which comprises a bisphenol-type epoxy resin, [4-(glycidyloxy)phenyl]diglycidylamine and a curing agent component and which, when cured at 140°C, gives a cured resin having a glass transition temperature G'-Tg higher than 100°C and lower than 200°C, and a dynamic storage modulus G' at 200°C which is preferably 8% or more, more preferably 10% or more, and even more preferably 12% or more of the value at 100°C. According to yet another aspect of the present invention, there is provided an epoxy resin composition comprising a bisphenol-type epoxy resin, [4-(glycidyloxy)phenyl]diglycidylamine, 4,4'-methylenebis(N,N-diglycidylaniline), and a curing agent component. Effect of the Invention

[0006] According to one embodiment, there is provided a method for producing an electrodeposition-coated article suitable for producing an electrodeposition-coated article made of carbon fiber reinforced plastic. According to another embodiment, there is provided a prepreg which provides a carbon fiber reinforced plastic which can be preferably used for producing an electrocoated article. According to yet another embodiment, there is provided an epoxy resin composition that can be preferably used for producing such a prepreg. [Brief description of the drawings]

[0007] [Figure 1] FIG. 1 is a flow diagram of a method for producing an electrodeposition coated product according to an embodiment. [Diagram 2] FIG. 2 is a graph showing the temperature dependence of the dynamic storage modulus G' of cured resins prepared from three types of epoxy resin compositions. [Diagram 3] FIG. 3 is a schematic diagram showing a sheet molding compound manufacturing apparatus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] 1. Manufacturing method for electrocoating products One embodiment of the present invention relates to a method for producing an electrodeposition coated product, the method comprising a curing step of curing a prepreg to obtain a carbon fiber reinforced plastic molded product, and an electrodeposition coating step of applying electrodeposition coating to the carbon fiber reinforced plastic molded product, the flow of which is shown in FIG.

[0009] For example, when producing electrodeposition-coated products for automobile parts, production efficiency is particularly important, so in the curing step, the prepreg is cured at a curing temperature of preferably 180° C. or less, more preferably 160° C. or less, and even more preferably 150° C. or less. In the case of compression molding, the cure temperature is the temperature of the mold.

[0010] In the electrodeposition coating process, a normal electrodeposition coating technique is used to apply electrodeposition coating to the carbon fiber reinforced plastic molded product obtained in the curing process. The technique disclosed in the above-mentioned Patent Document 3 is also included in the electrodeposition coating techniques that can be used in the electrodeposition coating process. The electrodeposition coating process includes sub-processes of an electrodeposition process, a water washing process, and a drying process, and the object to be coated is exposed to high temperatures of up to about 200°C in the drying process. Therefore, in the electrodeposition coated product manufacturing method according to the embodiment, the rigidity of the carbon fiber reinforced plastic molded product, which is the object to be coated, at 200°C is improved. More specifically, the prepreg, which is the material for the carbon fiber reinforced plastic molded product, is improved so that the rigidity of the carbon fiber reinforced plastic molded product at 200°C is improved.

[0011] 2. Prepreg The prepreg used in the method for producing an electrodeposition coated article according to the embodiment is produced by sequentially carrying out the following first and second steps, or the first to third steps. (First step) An epoxy resin composition is prepared by mixing a plurality of components including an epoxy resin component and a curing agent component. (Second step) A composite is formed by impregnating a fiber reinforcement material with the epoxy resin composition prepared in the first step. (Third step) The epoxy resin composition in the composite formed in the second step is thickened.

[0012] The epoxy resin composition prepared in the first step has a viscosity at 25°C measured after being placed in a sealed container and allowed to stand at 25°C for 30 minutes after preparation (hereinafter also referred to as "initial viscosity") of preferably 30 Pa s or less, more preferably 15 Pa s or less, even more preferably 10 Pa s or less, and may be 5 Pa s or less. The lower the initial viscosity of the epoxy resin composition prepared in the first step, the more efficiently the second step can be carried out without heating the epoxy resin composition in a room with an air temperature suitable for work of 17°C to 28°C.

[0013] The initial viscosity of the epoxy resin composition is measured using a rheometer such as HAAKE (registered trademark) MARS (registered trademark) 40 manufactured by Thermo Fisher Scientific under the conditions of an oscillatory mode, an angular velocity of 10 rad / s, a plate diameter of 25 mm, and a gap (distance between plates) of 0.5 mm.

[0014] The epoxy resin composition prepared in the first step contains at least a bisphenol-type epoxy resin and [4-(glycidyloxy)phenyl]diglycidylamine as epoxy resin components. The epoxy resin component is a component consisting of a compound having an epoxy group, and may be a prepolymer or a monomer. The preferred bisphenol type epoxy resins are bisphenol A type epoxy resins and bisphenol F type epoxy resins, particularly bisphenol A type epoxy resins. The bisphenol A type epoxy resins and bisphenol F type epoxy resins may be used alone or together with other bisphenol type epoxy resins. The bisphenol A type epoxy resins and bisphenol F type epoxy resins may also be used in combination. Bisphenol A epoxy resin is a prepolymer that essentially contains a compound represented by the following formula (a) where n=0, i.e., bisphenol A diglycidyl ether (BADGE), and usually further contains a compound represented by the following formula (a) where n is 1 or more.

[0015] [ka] In commercially available bisphenol A type epoxy resins that are liquid at room temperature, the average value of n in formula (a) is about 0.1 to 0.2.

[0016] [4-(glycidyloxy)phenyl]diglycidylamine is an epoxy compound represented by the following formula (b).

[0017] [ka] For example, by using jER630 (jER is a registered trademark) manufactured by Mitsubishi Chemical Corporation, which is a [4-(glycidyloxy)phenyl]diglycidylamine product having a viscosity of 0.5 to 1 Pa s at 25°C, together with a commercially available bisphenol-type epoxy resin whose components have been adjusted so as to be liquid at 25°C, it is possible to easily prepare an epoxy resin composition having an initial viscosity within the above-mentioned preferred range. As is well known to those skilled in the art, there are several commercially available bisphenol-type epoxy resins with a viscosity of 5 Pa·s or less at 25°C.

[0018] The amounts of the bisphenol epoxy resin and [4-(glycidyloxy)phenyl]diglycidylamine in the epoxy resin composition prepared in the first step are adjusted so that, when the epoxy resin composition is cured, a cured resin is formed which has a glass transition temperature G'-Tg of more than 100°C and less than 200°C, and a dynamic storage modulus G' at 200°C that is preferably 8% or more, more preferably 10% or more, and even more preferably 12% or more of the value at 100°C. The dynamic storage modulus G' is the storage shear modulus measured using a dynamic viscoelasticity measuring device such as ARES-G2 manufactured by TA Instruments under the conditions of a torsion mode, a heating rate of 5° C. / min, a frequency of 1 Hz, a strain of 0.1%, and a temperature of 25 to 250° C. The glass transition temperature G'-Tg is the temperature at the intersection of an approximation line of the flat region of a graph plotting logG' against temperature and an approximation line of the region of the graph where logG' drops sharply.

[0019] For the measurement of the dynamic storage modulus G', a test piece with a length of 50 mm and a width of 12.5 mm cut out from a resin plate with a thickness of 2 mm can be used. To prepare a resin plate, first, the epoxy resin composition immediately after preparation is vacuum degassed and then injected into a gap with a thickness of 2 mm formed between two 4 mm thick glass plates by using a spacer. Next, the epoxy resin composition sandwiched between the two glass plates is placed in a hot air circulation type thermostatic chamber preheated to 70°C, and the temperature inside the chamber is raised from 70°C to 140°C at a rate of 10°C / min so that the surface temperature of the glass plate is increased from 70°C to 140°C. Next, the inside of the chamber is heated for another 30 minutes so that the surface temperature is maintained at 140°C, thereby curing the epoxy resin composition. Finally, the glass plates are removed to obtain a resin plate with a thickness of 2 mm.

[0020] One of the purposes of blending a bisphenol type epoxy resin, particularly a bisphenol A type epoxy resin, in the epoxy resin composition prepared in the first step is to suppress cure shrinkage. The greater the cure shrinkage of the matrix resin, the more likely defects such as cracks and warping are to occur when the prepreg is cured. Therefore, the total amount of the bisphenol-type epoxy resins blended in the epoxy resin composition prepared in the first step is preferably 50% by weight or more of the total epoxy resin components blended in the epoxy resin composition. In a preferred embodiment, 50% by weight or more of the total epoxy resin components blended in the epoxy resin composition may be bisphenol A type epoxy resin. Since bisphenol-type epoxy resins are less expensive than other epoxy resins, increasing the amount of bisphenol-type epoxy resin added also contributes to reducing the cost of the prepreg.

[0021] The purpose of adding [4-(glycidyloxy)phenyl]diglycidylamine to the epoxy resin composition prepared in the first step is to improve the rigidity of the cured resin obtained from the epoxy resin composition when it is heated to nearly 200°C. The present inventors have found that in a cured product of an epoxy resin composition containing a bisphenol-type epoxy resin and [4-(glycidyloxy)phenyl]diglycidylamine, the ratio of the dynamic storage modulus G' at 200°C to the value at 100°C tends to increase according to the amount of [4-(glycidyloxy)phenyl]diglycidylamine added. This tendency was not observed in at least the other three types of glycidylamine, specifically, 4,4'-methylenebis(N,N-diglycidylaniline), [3-(glycidyloxy)phenyl]diglycidylamine and N,N,N',N'-tetraglycidyl-m-xylylenediamine.

[0022] From the viewpoint of increasing the degree of improvement in the rigidity of the cured resin obtained from the epoxy resin composition at 200° C., the total amount of the bisphenol-type epoxy resin is preferably 80% by weight or less, and more preferably 75% by weight or less, of the total epoxy resin components contained in the epoxy resin composition. From the same viewpoint, the amount of [4-(glycidyloxy)phenyl]diglycidylamine is preferably 20% by weight or more, more preferably 25% by weight or more, and even more preferably 30% by weight or more, and may be 35% by weight or more, or 40% by weight or more, of the total epoxy resin components contained in the epoxy resin composition.

[0023] The epoxy resin composition may contain epoxy resin components other than the bisphenol type epoxy resin and the [4-(glycidyloxy)phenyl]diglycidylamine within the scope of the effects of the invention. One suitable example of such an epoxy resin component is 4,4'-methylenebis(N,N-diglycidylaniline). By replacing a part of the bisphenol-type epoxy resin with 4,4'-methylenebis(N,N-diglycidylaniline), the degree of improvement in the rigidity at 200°C of the cured resin obtained from the epoxy resin composition can be increased.

[0024] Other examples of epoxy resin components other than the bisphenol-type epoxy resin and the [4-(glycidyloxy)phenyl]diglycidylamine that can be blended in the epoxy resin composition include, but are not limited to, naphthalene-type epoxy resins, biphenyl-type epoxy resins, novolac-type epoxy resins, epoxy resins having an oxazolidone ring structure, alicyclic epoxy resins, and aliphatic epoxy resins.

[0025] A preferred curing agent component that can be blended in the epoxy resin composition prepared in the first step is a latent curing agent. A latent curing agent is a curing agent that initiates curing of an epoxy resin using heat as a trigger, and is a solid that has low solubility in epoxy resins at room temperature, and only exhibits sufficient function as a curing agent when it is melted or dissolved in an epoxy resin by heating. The use of a latent curing agent is advantageous in suppressing an increase in the initial viscosity of the epoxy resin composition and in improving the storage stability of the completed prepreg.

[0026] Various imidazoles, dicyandiamide and boron trifluoride-amine complexes are typical examples of latent hardeners. Imidazoles are compounds having an imidazole ring, and include substituted imidazoles in which the hydrogen atom of imidazole is replaced with a substituent, as well as imidazolium salts and imidazole complexes. Suitable examples of the substituted imidazole that acts as a latent curing agent include, but are not limited to, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2-phenyl-4-methylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2-phenyl-4-benzyl-5-hydroxymethylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-paratoluyl-4-methyl-5-hydroxymethylimidazole, 2-paratoluyl-4,5-dihydroxymethylimidazole, 2-metatoluyl-4-methyl-5-hydroxymethylimidazole, 2-metatoluyl-4,5-dihydroxymethylimidazole and 1-cyanoethyl-2-phenylimidazole, which have an aromatic ring in the molecule, which may be a heteroaromatic ring.

[0027] Imidazolium salts such as 1-cyanoethyl-2-ethyl-4-methylimidazolium trimellitate, 1-cyanoethyl-2-undecylimidazolium trimellitate and 1-cyanoethyl-2-phenylimidazolium trimellitate are also suitable examples of the imidazole-based latent hardener. Particularly preferred examples of the imidazole-based latent hardener include isocyanuric acid adducts of various substituted imidazoles such as 2-phenylimidazole, 2-methylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole, and in particular, isocyanuric acid adducts of substituted imidazoles having a triazine ring such as 2,4-diamino-6-(2'-methylimidazolyl-(1'))-ethyl-s-triazine, 1-(4,6-diamino-s-triazin-2-yl)ethyl-2-undecylimidazole, and 2,4-diamino-6-[2-(2-ethyl-4-methyl-1-imidazolyl)ethyl]-s-triazine.

[0028] Amine adducts are also a suitable example of latent hardeners. Amine adducts are polymerized compounds made by reacting substituted imidazoles or tertiary amines with epoxy resins or isocyanates, and have relatively low solubility in epoxy resins. The latent curing agents including the imidazoles may be used alone or in combination of two or more kinds. When dicyandiamide is used as the latent curing agent, a urea derivative such as 4,4'-methylenebis(phenyldimethylurea) or 2,4-bis(3,3-dimethylureido)toluene can be preferably used in combination as a curing accelerator.

[0029] The curing agent component that can be blended in the epoxy resin composition prepared in the first step is not limited to a latent curing agent. The epoxy resin composition prepared in the first step may contain a curing agent other than the latent curing agent, such as a carboxylic acid anhydride, an aromatic amine, or a phenol resin, in addition to or instead of the latent curing agent.

[0030] Among the carboxylic acid anhydrides, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride and methyl-5-norbornene-2,3-dicarboxylic anhydride (methyl-3,6-endomethylene-1,2,3,6-tetrahydrophthalic anhydride) all have a viscosity of less than 0.5 Pa s at 25°C, and therefore can be blended with the epoxy resin composition prepared in the first step for the purpose of lowering the initial viscosity. Carboxylic acid anhydrides are known to react with epoxy compounds at low temperatures to form bonds through the catalytic action of a tertiary amine, which may be glycidylamine. Carboxylic acid anhydrides act as thickeners when incorporated in a relatively small amount into an epoxy resin composition, for example, less than 20 parts by weight per 100 parts by weight of the epoxy resin component. The thickening caused by the carboxylic acid anhydride occurs by forming a bond between the carboxylic acid anhydride and the epoxy compound, and therefore the carboxylic acid anhydride in the epoxy resin composition is consumed as the thickening proceeds.

[0031] Amine compounds also act as thickeners when blended in an amount of about 0.1 to 0.5 equivalents of active hydrogen per epoxy group in the epoxy resin composition. Examples of amine compounds that can be preferably used as thickeners include, but are not limited to, isophoronediamine, bis(4-aminocyclohexyl)methane, and 1,3-bis(aminomethyl)cyclohexane. The thickening by the amine compound occurs by forming a bond between the amine compound and the epoxy compound, and therefore, the amine compound added as a thickener to the epoxy resin composition is consumed as the thickening proceeds.

[0032] Polyisocyanates, which may be diisocyanates such as bis(4-isocyanatophenyl)methane and toluene diisocyanate, are suitable examples of thickeners. When polyols, which may be diols such as ethylene glycol, polyethylene glycol, isosorbide, neopentyl glycol, cyclohexanediol, cyclohexanedimethanol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, and 1,6-hexanediol, are used together with polyisocyanates, the thickening of the epoxy resin composition tends to be promoted. The thickening by polyisocyanate occurs by forming a bond between the polyisocyanate and the epoxy compound or the polyol mixed together, and therefore the polyisocyanate in the epoxy resin composition is consumed as the thickening proceeds.

[0033] In addition to the epoxy resin component and the curing agent component, the epoxy resin composition prepared in the first step may contain optional components, including, but not limited to, thickeners, internal mold release agents, low shrinkage agents, colorants, flame retardants, antioxidants, modifiers made of rubber, elastomers, or thermoplastic resins, conductive fillers, and inorganic fillers.

[0034] A suitable example of the flame retardant is a non-halogen flame retardant. Non-halogen flame retardants include, but are not limited to, inorganic phosphorus flame retardants such as red phosphorus, organic phosphorus flame retardants such as phosphate esters, organic phosphates, phosphonates, and phosphinates, nitrogen flame retardants such as triazine compounds, cyanuric acid compounds, and isocyanuric acid compounds, silicone flame retardants, inorganic flame retardants such as metal hydroxides and metal oxides, and organic metal salt flame retardants such as ferrocene and acetylacetone metal complexes. Two or more flame retardants selected from these may be used in combination, and for example, an organic phosphorus flame retardant and a nitrogen flame retardant may be used in combination. From the viewpoint of productivity, it is preferable that the epoxy resin composition is not a varnish. If the epoxy resin composition is a varnish, it is necessary to further provide a step of removing the solvent from the epoxy resin composition after impregnating the fiber reinforcing material in the second step.

[0035] In the second step, a composite material consisting of the fiber reinforcing material and the epoxy resin composition is formed by impregnating a fiber reinforcing material prepared in advance with the epoxy resin composition prepared in the first step. The fiber reinforcement preferably contains carbon fiber, and may be, for example, a carbon fiber mat, a carbon fiber woven fabric, a carbon fiber nonwoven fabric, a carbon fiber non-crimp fabric, or the like. When the prepreg to be produced is a sheet molding compound, the fiber reinforcement is a carbon fiber mat deposited by scattering chopped carbon fiber tows having a predetermined length, for example, in the range of 5 mm to 10 cm, preferably 1 to 6 cm, on a carrier film. In a typical example, the predetermined length can be 0.5 inches (about 1.3 cm), 1 inch (about 2.5 cm), 1.5 inches (about 3.8 cm), or 2 inches (about 5.1 cm).

[0036] In one example, in order to ensure the impregnation of the fiber reinforcing material in a short time in the second step, the epoxy resin composition prepared in the first step may be heated to reduce the viscosity before use. Such heating is performed so that the temperature of the epoxy resin composition does not exceed 80°C, preferably does not exceed 70°C, more preferably does not exceed 50°C, and even more preferably does not exceed 40°C.

[0037] In the optional third step, the epoxy resin composition in the composite formed in the second step is thickened, preferably by holding the composite at a predetermined thickening temperature. The thickening temperature is usually selected between room temperature and about 80°C. The retention time can be set by examining the change in viscosity when only the epoxy resin composition is placed in a sealed container and allowed to stand at the thickening temperature. The viscosity of the epoxy resin composition at 25°C after thickening is at least 500 Pa·s, preferably 1000 Pa·s or more, and is usually 100,000 Pa·s or less, preferably 50,000 Pa·s or less, more preferably 20,000 Pa·s or less, and may be 10,000 Pa·s or less, 8,000 Pa·s or less, 6,000 Pa·s or less, etc.

[0038] The following is a specific explanation of the case where the prepreg to be produced is a sheet molding compound. For producing the sheet molding compound, for example, a sheet molding compound production apparatus shown in FIG. 3 can be used. Referring to FIG. 3, a continuous fiber bundle 10 which is the raw material of the fiber reinforcement material is drawn from a fiber package P and fed to a rotary cutter 1 . The continuous fiber bundle 10 is a carbon fiber bundle consisting of, for example, 1,000 to 100,000, preferably 3,000 to 50,000 carbon fiber filaments per bundle, and may be partially split. The continuous fiber bundle 10 is cut by a rotary cutter 1 into chopped fiber bundles 20 . The fiber length of the chopped fiber bundle 20 is, for example, within a range of 5 mm to 100 mm, and can be 1 cm or more and less than 2 cm, 2 cm or more and less than 3 cm, 3 cm or more and less than 4 cm, or 4 cm or more and less than 6 cm.

[0039] The chopped fiber bundles 20 fall onto the surface of the first carrier film 51 traveling below the rotary cutter 1 to form a fiber mat 30 . Before depositing the fiber mat 30, a first resin paste layer 41L made of a first resin paste 41 is applied to the surface of the first carrier film 51 by a first coater 2a equipped with a doctor blade. The first resin paste 41 is an epoxy resin composition prepared in the first step. The first carrier film 51 is a synthetic resin film that is resistant to the components of the first resin paste 41 . The material of the first carrier film 51 can be appropriately selected from polyolefins such as polyethylene and polypropylene, polyvinylidene chloride, vinyl chloride resins, polyamides, and the like. The first carrier film 51 may be a multi-layer film.

[0040] When the viscosity of first resin paste 41 is 0.1 Pa·s or more, or even 0.5 Pa·s or more, and 30 Pa·s or less, or even 15 Pa·s or less at 25°C, first resin paste layer 41L can be easily formed with a uniform thickness on first carrier film 51 in a room with an air temperature of 17°C or more and 28°C or less, without heating first resin paste 41. The basis weight of the fiber mat 30, the thickness of the first resin paste layer 41L, and the thickness of the second resin paste layer 42L described below are set in consideration of the fiber content and basis weight of the sheet molding compound to be produced. The fiber content of sheet molding compounds in which the fiber reinforcement is carbon fiber can be, for example, from 40 wt% to less than 45 wt%, from 45 wt% to less than 55 wt%, from 55 wt% to less than 65 wt%, from 65 wt% to less than 80 wt%, etc. The basis weight of the sheet molding compound is, for example, 500 g / m2 More than 1000g / m 2 Below 1000g / m 2 More than 1500g / m 2 Below 1500g / m 2 More than 2500g / m 2 Below 2500g / m 2 More than 3500g / m 2 Below 3500g / m 2 More than 5000g / m 2 It could be the following etc. Compared to UD prepregs, sheet molding compounds have a larger basis weight and are typically thicker, for example 1 to 4 mm.

[0041] Following the formation of the fiber mat 30, a first carrier film 51 and a second carrier film 52 are bonded together with the fiber mat 30 sandwiched therebetween, thereby forming a laminate 60. Before lamination, a second resin paste layer 42L made of a second resin paste 42 is applied to one surface of the second carrier film 52 by a second coater 2b equipped with a doctor blade. The second resin paste 42 is the epoxy resin composition prepared in the first step. Laminate 60 is formed so that the surface of first carrier film 51 on which first resin paste layer 41L is applied and the surface of second carrier film 52 on which second resin paste layer 42L is applied face each other. The second carrier film 52 is a synthetic resin film that is resistant to the components of the second resin paste 42 , and the material and structure thereof may be the same as those of the first carrier film 51 .

[0042] The laminate 60 is pressed in an impregnation machine 3 to impregnate the fiber mat 30 with the first resin paste 41 and the second resin paste 42 . The laminate 60 that has passed through the impregnation machine 3 is wound up on a bobbin. The steps up to this point are carried out using the sheet molding compound manufacturing apparatus shown in FIG. The laminate 60 on the bobbin is maintained at a predetermined temperature for a certain period of time to thicken the epoxy resin composition that has permeated the fiber mat 30, thereby completing the sheet molding compound. The viscosity of the epoxy resin composition after thickening at 25°C may be 1000 Pa·s or more and less than 2000 Pa·s, 2000 Pa·s or more and less than 3000 Pa·s, 3000 Pa·s or more and less than 4000 Pa·s, 4000 Pa·s or more and less than 5000 Pa·s, 5000 Pa·s or more and less than 6000 Pa·s, 6000 Pa·s or more and less than 8000 Pa·s, 8000 Pa·s or more and less than 10000 Pa·s, 10000 Pa·s or more and less than 15000 Pa·s, 15000 Pa·s or more and less than 20000 Pa·s, 20000 Pa·s or more and less than 50000 Pa·s, 50000 Pa·s or more and less than 100000 Pa·s, etc.

[0043] The prepreg produced by the above-described production method can be preferably used not only in the above-described method for producing an electrodeposition coated product according to the embodiment, but also in various carbon fiber reinforced plastic products, including those not electrodeposition coated, by producing the prepreg as a material, the rigidity when exposed to a temperature higher than the glass transition temperature G'-Tg can be improved.

[0044] 3. Epoxy resin composition One embodiment of the present invention relates to an epoxy resin composition. In the method for producing a prepreg described in the above item 2, the epoxy resin composition prepared in the first step is included in an embodiment of the present invention.

[0045] 4. Experimental Results Nine types of epoxy resin compositions were prepared using the materials shown in Table 1 below, and the dynamic viscoelasticity of the cured resin obtained by curing each epoxy resin composition was measured.

[0046] [Table 1]

[0047] The formulations of the nine types of epoxy resin compositions (compositions 1 to 9) prepared are shown in Table 2 below.

[0048] [Table 2]

[0049] When preparing compositions 1 to 9 shown in Table 2, the latent curing agents 2MZA-PW and PN-23J were dispersed in jER827 or jER828, respectively, to form master batches, and then mixed with other components. In compositions 1 to 8, the weight ratio of the latent curing agent to jER827 in the master batch was 2:1 (latent curing agent:epoxy resin). In composition 9, the weight ratio of the latent curing agent to jER828 in the master batch was 1:1. When preparing Compositions 1 to 9, a mixture of the components other than HN-2200 was prepared, and then HN-2200 was added to the mixture.

[0050] Table 2 shows the initial viscosity and viscosity after thickening measured for each of Compositions 1 to 9, as well as the glass transition temperature G'-Tg and dynamic storage modulus G' at 100°C and 200°C obtained by dynamic viscoelasticity measurement of the cured resin obtained by curing each of Compositions 1 to 9. The initial viscosity is the viscosity at 25°C measured after placing the epoxy resin composition in a sealed container immediately after preparation and allowing to stand at 25°C for 30 minutes. The viscosity after thickening is the viscosity at 25°C measured after placing the epoxy resin composition in a sealed container immediately after preparation and leaving it to stand at 25°C for 7 days.

[0051] In the dynamic viscoelasticity measurement, a test piece with a length of 50 mm and a width of 12.5 mm cut from a resin plate with a thickness of 2 mm was used. In preparing the resin plate, the epoxy resin composition immediately after preparation was first vacuum degassed and then injected into a gap with a thickness of 2 mm formed between two 4 mm thick glass plates by using a spacer. Next, the epoxy resin composition sandwiched between the two glass plates was placed in a hot air circulation type thermostatic chamber preheated to 70°C, and the temperature in the chamber was raised from 70°C to 140°C at a rate of 10°C / min. Next, the epoxy resin composition was cured by heating the inside of the chamber so that the surface temperature of the glass plate was kept at 140°C for another 30 minutes, and a resin plate with a thickness of 2 mm was obtained. Dynamic viscoelasticity measurements were performed using a TA Instruments ARES-G2 in torsion mode under the conditions of a heating rate of 5°C / min, a frequency of 1 Hz, a strain of 0.1%, and a temperature of 25 to 250°C. In Table 2, B / A is the ratio of the dynamic storage modulus G' at 200°C (B) to the dynamic storage modulus G' at 100°C (A). It can be said that the larger this ratio is, the smaller the decrease in rigidity modulus of a resin when heated to near 200°C.

[0052] Each of compositions 1 to 9 contains a bisphenol A type epoxy resin (jER827 or jER828) and a glycidylamine (jER630, jER604, MY0600, TETRAD-X) as the epoxy resin component. The cured resins obtained from compositions 2 and 3, which contained jER630 ([4-(glycidyloxy)phenyl]diglycidylamine) as the glycidylamine, had a significantly larger B / A than the cured resins obtained from compositions 4 and 5, which had the same blending weight ratio of glycidylamine to bisphenol A type epoxy resin but did not contain jER630. Among the cured resins obtained from Compositions 1 to 3, there was a tendency that the B / A ratio increased as the blending amount of jER630 increased. Among the cured resins obtained from compositions 4 to 7, B / A was comparable regardless of the type and amount of glycidyl amine used. FIG. 2 is a graph showing the temperature dependence of the dynamic storage modulus G′ of the cured resins prepared from Composition 2, Composition 4, and Composition 5, respectively.

[0053] 5. Summary of the embodiment Embodiments of the present invention include, but are not limited to, the following. [Embodiment 1] A method for producing an electrodeposition-coated product, comprising: a molding step of obtaining a carbon fiber reinforced plastic molded product by curing a prepreg composed of a carbon fiber reinforcing material and an epoxy resin composition containing a bisphenol-type epoxy resin, [4-(glycidyloxy)phenyl]diglycidylamine, and a curing agent component; and an electrodeposition coating step of applying electrodeposition coating to the carbon fiber reinforced plastic molded product. [Embodiment 2] A manufacturing method according to embodiment 1, wherein in the molding step, the prepreg is cured at a temperature of preferably 180°C or less, more preferably 160°C or less, and even more preferably 150°C or less. [Embodiment 3] The method of embodiment 1 or 2, in which the epoxy resin composition gives a cured resin when cured at 140°C, which has a glass transition temperature G'-Tg greater than 100°C and less than 200°C, and a dynamic storage modulus G' at 200°C that is preferably 8% or more, more preferably 10% or more, and even more preferably 12% or more of the value at 100°C. [Embodiment 4] The production method according to any one of embodiments 1 to 3, wherein the total amount of bisphenol-type epoxy resins blended in the epoxy resin composition is preferably 50% by weight or more of the total epoxy resin components blended in the epoxy resin composition. [Embodiment 5] The method according to any one of embodiments 1 to 4, wherein the bisphenol-type epoxy resin comprises a bisphenol A-type epoxy resin. [Embodiment 6] The production method according to embodiment 5, wherein the total amount of bisphenol A type epoxy resins blended in the epoxy resin composition is preferably 50% by weight or more of the total epoxy resin components blended in the epoxy resin composition. [Embodiment 7] The production method according to any one of embodiments 1 to 6, wherein the total amount of bisphenol-type epoxy resins blended in the epoxy resin composition is preferably 80% by weight or less, and more preferably 75% by weight or less, of the total epoxy resin components blended in the epoxy resin composition. [Embodiment 8] The production method according to any one of embodiments 1 to 7, wherein the amount of [4-(glycidyloxy)phenyl]diglycidylamine blended in the epoxy resin composition is preferably 20% by weight or more, more preferably 25% by weight or more, and even more preferably 30% by weight or more, and may be 35% by weight or more, or 40% by weight or more, of the total epoxy resin components blended in the epoxy resin composition. [Embodiment 9] The production method according to any one of embodiments 1 to 8, wherein the epoxy resin composition further contains 4,4'-methylenebis(N,N-diglycidylaniline). [Embodiment 10] The manufacturing method according to any one of embodiments 1 to 9, wherein the curing agent component includes a latent curing agent. [Embodiment 11] The manufacturing method according to embodiment 10, wherein the latent curing agent includes one or more curing agents selected from dicyandiamide, imidazoles, and amine adducts. [Embodiment 12] The method according to any one of embodiments 1 to 11, wherein a thickener component is blended into the epoxy resin composition. [Embodiment 13] The method according to any one of embodiments 1 to 12, wherein a carboxylic acid anhydride having a viscosity of less than 0.5 Pa s at 25°C is blended into the epoxy resin composition. [Embodiment 14] The manufacturing method according to any one of embodiments 1 to 13, wherein the prepreg is a sheet molding compound. [Embodiment 15] An electrodeposition coated article produced using the production method according to any one of embodiments 1 to 14. [Embodiment 16] A prepreg comprising an epoxy resin composition containing a bisphenol-type epoxy resin, [4-(glycidyloxy)phenyl]diglycidylamine, and a curing agent component, and a carbon fiber reinforcing material, wherein the epoxy resin composition, when cured at 140°C, gives a cured resin having a glass transition temperature G'-Tg greater than 100°C and less than 200°C, and a dynamic storage modulus G' at 200°C that is preferably 8% or more, more preferably 10% or more, and even more preferably 12% or more of the value at 100°C. [Embodiment 17] A prepreg according to embodiment 16, in which the epoxy resin composition further contains 4,4'-methylenebis(N,N-diglycidylaniline). [Embodiment 18] A prepreg comprising an epoxy resin composition containing a bisphenol-type epoxy resin, [4-(glycidyloxy)phenyl]diglycidylamine, 4,4'-methylenebis(N,N-diglycidylaniline), and a curing agent component, and a carbon fiber reinforcing material. [Embodiment 19] A prepreg according to any one of embodiments 16 to 18, wherein the total amount of bisphenol-type epoxy resins blended in the epoxy resin composition is preferably 50% by weight or more of the total epoxy resin components blended in the epoxy resin composition. [Embodiment 20] The prepreg according to any one of embodiments 16 to 19, wherein the bisphenol type epoxy resin comprises a bisphenol A type epoxy resin. [Embodiment 21] A prepreg according to embodiment 20, wherein the total amount of bisphenol A type epoxy resins blended in the epoxy resin composition is preferably 50% by weight or more of the total epoxy resin components blended in the epoxy resin composition. [Embodiment 22] A prepreg according to any one of embodiments 16 to 21, wherein the total amount of bisphenol-type epoxy resins blended in the epoxy resin composition is preferably 80% by weight or less, and more preferably 75% by weight or less, of the total epoxy resin components blended in the epoxy resin composition. [Embodiment 23] A prepreg relating to any of embodiments 16 to 22, wherein the amount of [4-(glycidyloxy)phenyl]diglycidylamine blended into the epoxy resin composition is preferably 20% by weight or more, more preferably 25% by weight or more, and even more preferably 30% by weight or more, and may be 35% by weight or more, or 40% by weight or more, of the total epoxy resin components blended into the epoxy resin composition. [Embodiment 24] The prepreg according to any one of embodiments 16 to 23, wherein the curing agent component includes a latent curing agent. [Embodiment 25] The prepreg according to [Embodiment 24], wherein the latent curing agent includes one or more curing agents selected from dicyandiamide, imidazoles, and amine adducts. [Embodiment 26] The prepreg according to any one of embodiments 16 to 25, wherein a thickener component is blended into the epoxy resin composition. [Embodiment 27] The prepreg according to any one of embodiments 16 to 26, wherein a carboxylic acid anhydride having a viscosity of less than 0.5 Pa·s at 25°C is blended into the epoxy resin composition. [Embodiment 28] A prepreg according to any one of embodiments 16 to 27, which is a sheet molding compound. [Embodiment 29] A method for producing a carbon fiber reinforced plastic molded product, comprising curing the prepreg according to any one of embodiments 16 to 28. [Embodiment 30] A carbon fiber reinforced plastic molded product made of a cured product of the prepreg according to any one of embodiments 16 to 29. [Embodiment 31] A method for producing an electrodeposition coated product, comprising applying electrodeposition coating to a carbon fiber reinforced plastic molded product of embodiment 30. [Embodiment 32] An epoxy resin composition which, when cured at 140°C, comprises a bisphenol-type epoxy resin, [4-(glycidyloxy)phenyl]diglycidylamine, and a curing agent component, gives a cured resin having a glass transition temperature G'-Tg greater than 100°C and less than 200°C, and a dynamic storage modulus G' at 200°C which is preferably 8% or more, more preferably 10% or more, and even more preferably 12% or more of the value at 100°C. [Embodiment 33] The epoxy resin composition according to embodiment 32, further comprising 4,4'-methylenebis(N,N-diglycidylaniline). [Embodiment 34] An epoxy resin composition comprising a bisphenol type epoxy resin, [4-(glycidyloxy)phenyl]diglycidylamine, 4,4'-methylenebis(N,N-diglycidylaniline), and a curing agent component. [Embodiment 35] The epoxy resin composition according to any one of embodiments 32 to 34, having a viscosity at 25°C of preferably 30 Pa s or less, more preferably 15 Pa s or less, even more preferably 10 Pa s or less, and may be 5 Pa s or less. [Embodiment 36] An epoxy resin composition according to embodiment 35 which is not a varnish. [Embodiment 37] The epoxy resin composition according to any one of embodiments 32 to 36, wherein the total amount of the bisphenol type epoxy resins blended is preferably 50% by weight or more of the total epoxy resin components blended. [Embodiment 38] The epoxy resin composition according to any one of embodiments 32 to 37, wherein the bisphenol-type epoxy resin comprises a bisphenol A-type epoxy resin. [Embodiment 39] An epoxy resin composition according to embodiment 38, in which the total amount of the bisphenol A type epoxy resins blended is preferably 50% by weight or more of the total epoxy resin components blended. [Embodiment 40] An epoxy resin composition according to any one of embodiments 32 to 39, wherein the total amount of the bisphenol-type epoxy resins blended is preferably 80% by weight or less, and more preferably 75% by weight or less, of the total epoxy resin components blended. [Embodiment 41] An epoxy resin composition according to any one of embodiments 32 to 40, wherein the amount of [4-(glycidyloxy)phenyl]diglycidylamine blended is preferably 20% by weight or more, more preferably 25% by weight or more, and even more preferably 30% by weight or more, and may be 35% by weight or more, or 40% by weight or more, of the total epoxy resin components blended. [Embodiment 42] The epoxy resin composition according to any one of embodiments 32 to 41, wherein the curing agent component includes a latent curing agent. [Embodiment 43] The epoxy resin composition according to embodiment 42, wherein the latent curing agent includes one or more curing agents selected from dicyandiamide, imidazoles, and amine adducts. [Embodiment 44] An epoxy resin composition according to any one of embodiments 32 to 43, containing a thickener component. [Embodiment 45] The epoxy resin composition according to any one of embodiments 32 to 44, containing a carboxylic acid anhydride having a viscosity of less than 0.5 Pa·s at 25°C. [Embodiment 46] A method for producing a prepreg, comprising impregnating a carbon fiber reinforcing material with the epoxy resin composition according to any one of embodiments 32 to 45. [Embodiment 47] The method of embodiment 46, further comprising thickening the epoxy resin composition after the impregnation. [Embodiment 48] A manufacturing method according to embodiment 47, wherein the prepreg is a sheet molding compound.

[0054] Although the present invention has been described above with reference to specific embodiments, each embodiment is presented as an example and does not limit the scope of the present invention. Each embodiment described in this specification can be modified in various ways within the scope of the effects of the invention, and can be combined with features described in other embodiments within the scope of feasibility. [Industrial Applicability]

[0055] The electrocoated product manufacturing method according to the embodiment can be used to manufacture a variety of electrocoated products, including automobiles, motorcycles, bicycles, ships, railroad vehicles, manned aircraft, unmanned aircraft and other transportation equipment, sporting goods, leisure goods, home appliances, agricultural machinery, building materials, and the like. The prepreg according to the embodiment can be used to manufacture various carbon fiber reinforced plastic parts contained in automobiles, motorcycles, bicycles, ships, railroad cars, manned aircraft, unmanned aircraft and other transportation equipment, sporting goods, leisure goods, home appliances, agricultural equipment, building materials, and the like. [Explanation of symbols]

[0056] 1 Rotary Cutter 2a First coating machine 2b Second Coating Machine 3 Impregnation machine 10 Continuous fiber bundle 20 Chopped fiber bundles 30 Fiber Mat 41 Daiichi Resin Paste 41L First resin paste layer 42 Second resin paste 42L Second resin paste layer 51 Daiichi Carrier Film 52 Second Carrier Film 60 Laminate

Claims

1. A sheet molding compound comprising an epoxy resin composition containing a bisphenol-type epoxy resin, [4-(glycidyloxy)phenyl]diglycidylamine, and a curing agent component, and a carbon fiber reinforcing material, said epoxy resin composition giving a cured resin when cured at 140°C, which has a glass transition temperature G'-Tg higher than 100°C and lower than 200°C, and a dynamic storage modulus G' at 200°C that is 8% or more of the value at 100°C.

2. 2. The sheet molding compound according to claim 1, wherein the epoxy resin composition further contains 4,4'-methylenebis(N,N-diglycidylaniline).

3. A sheet molding compound comprising an epoxy resin composition containing a bisphenol-type epoxy resin, [4-(glycidyloxy)phenyl]diglycidylamine, 4,4'-methylenebis(N,N-diglycidylaniline) and a curing agent component, and a carbon fiber reinforcing material.

4. The sheet molding compound according to any one of claims 1 to 3, wherein a total amount of bisphenol-type epoxy resins blended in the epoxy resin composition is 50% by weight or more of the total epoxy resin components blended in the epoxy resin composition.

5. The sheet molding compound according to any one of claims 1 to 4, wherein the bisphenol type epoxy resin comprises a bisphenol A type epoxy resin.

6. 6. The sheet molding compound according to claim 5, wherein the total amount of bisphenol A type epoxy resins blended in the epoxy resin composition is 50% by weight or more of the total epoxy resin components blended in the epoxy resin composition.

7. The sheet molding compound according to any one of claims 1 to 6, wherein a total amount of bisphenol-type epoxy resins blended in the epoxy resin composition is 80% by weight or less of the total epoxy resin components blended in the epoxy resin composition.

8. The sheet molding compound according to any one of claims 1 to 7, wherein the amount of [4-(glycidyloxy)phenyl]diglycidylamine blended in the epoxy resin composition is 20% by weight or more of the total epoxy resin components blended in the epoxy resin composition.

9. The sheet molding compound of any one of claims 1 to 8, wherein the hardener component comprises a latent hardener.

10. 10. The sheet molding compound of claim 9, wherein the latent curing agent comprises one or more curing agents selected from dicyandiamide, imidazoles, and amine adducts.

11. The sheet molding compound according to any one of claims 1 to 10, wherein a thickener component is blended into the epoxy resin composition.

12. The sheet molding compound according to any one of claims 1 to 11, wherein the epoxy resin composition is blended with a carboxylic acid anhydride having a viscosity of less than 0.5 Pa·s at 25°C.

13. A method for producing a carbon fiber reinforced plastic molded product, comprising curing the sheet molding compound according to any one of claims 1 to 12.

14. A carbon fiber reinforced plastic molded product comprising a cured product of the sheet molding compound according to any one of claims 1 to 12.

15. A method for producing an electrodeposition-coated article, comprising subjecting the carbon fiber reinforced plastic molded article according to claim 14 to electrodeposition coating.

16. A method for producing a sheet molding compound includes impregnating a carbon fiber reinforcing material with an epoxy resin composition which is a blend of a bisphenol-type epoxy resin, [4-(glycidyloxy)phenyl]diglycidylamine, and a curing agent component, and which, when cured at 140°C, gives a cured resin having a glass transition temperature G'-Tg higher than 100°C and lower than 200°C, and a dynamic storage modulus G' at 200°C that is 8% or more of the value at 100°C.

17. The method according to claim 16, wherein the epoxy resin composition further contains 4,4'-methylenebis(N,N-diglycidylaniline).

18. A method for producing a sheet molding compound includes impregnating a carbon fiber reinforcing material with an epoxy resin composition containing a bisphenol-type epoxy resin, [4-(glycidyloxy)phenyl]diglycidylamine, 4,4'-methylenebis(N,N-diglycidylaniline), and a curing agent component.

19. The method according to any one of claims 16 to 18, wherein the epoxy resin composition has a viscosity of 30 Pa·s or less at 25°C.

20. The method according to claim 19, wherein the epoxy resin composition is not a varnish.

21. The method according to any one of claims 16 to 20, wherein in the epoxy resin composition, a total amount of the bisphenol type epoxy resins blended is 50% by weight or more of the total epoxy resin components blended.

22. The method according to any one of claims 16 to 21, wherein in the epoxy resin composition, the bisphenol type epoxy resin comprises a bisphenol A type epoxy resin.

23. The method according to claim 22, wherein the total amount of the bisphenol A type epoxy resins blended in the epoxy resin composition is 50% by weight or more of the total epoxy resin components blended.

24. The method according to any one of claims 16 to 23, wherein in the epoxy resin composition, a total amount of the bisphenol type epoxy resins blended is 80% by weight or less of the total epoxy resin components blended.

25. The method according to any one of claims 16 to 24, wherein the amount of [4-(glycidyloxy)phenyl]diglycidylamine blended in the epoxy resin composition is 20% by weight or more of the total epoxy resin components blended.

26. The method of any one of claims 16 to 25, wherein the hardener component comprises a latent hardener.

27. The method of claim 26, wherein the latent curing agent comprises one or more curing agents selected from dicyandiamide, imidazoles, and amine adducts.

28. The method according to any one of claims 16 to 27, wherein a thickener component is blended into the epoxy resin composition.

29. The method according to any one of claims 16 to 28, wherein a carboxylic acid anhydride having a viscosity of less than 0.5 Pa·s at 25°C is blended into the epoxy resin composition.

30. The method of any one of claims 16 to 29, comprising thickening the epoxy resin composition after the impregnation.

Citation Information

Patent Citations

  • Carbon fiber reinforced sheeted molding material and its manufacturing method

    JP2009013306A

  • Curable resin composition, and prepreg, film and fiber-reinforced plastic including the same

    JP2019157057A

  • Roller reduction gear and variable valve device of internal combustion engine

    JP2020070771A

  • Method for manufacturing carbon-fiber-reinforced plastic molded article

    WO2016104416A1

  • Sheet molding compound and fiber-reinforced composite material

    WO2018190329A1