Chlorine-containing polyether polyol composition
The chlorine-containing polyether polyol composition with epoxy and aluminum compounds addresses thermal instability issues in chlorinated polyether polyols, enhancing polyurethane's mechanical properties and flame retardancy while maintaining moldability.
Patent Information
- Application Number
- JP2023004082
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-01-28
- Filing Date
- 2023-01-13
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2043-01-13
AI Technical Summary
Chlorinated polyether polyols used as flame retardants for polyurethane foam have insufficient thermal stability, leading to hydrochloric acid generation that deactivates catalysts, affecting moldability and mechanical properties.
A chlorine-containing polyether polyol composition containing 0.5 to 20 parts by weight of an epoxy compound and 100 parts by weight of a chlorine-containing polyether polyol with a molecular weight of 400 to 5,000, along with an aluminum compound, enhances thermal stability and mechanical properties.
The composition results in polyurethane with improved mechanical properties, thermal stability, and flame retardancy, maintaining moldability.
Smart Images

Figure 0007571808000001 
Figure 0007571808000002 
Figure 0007571808000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a chlorine-containing polyether polyol that has excellent thermal stability and moldability and is a raw material for polyurethane that has excellent mechanical properties and flame retardancy. [Background technology]
[0002] Polyurethane is produced by mixing a polyol and an isocyanate compound.
[0003] Conventionally, flame retardants have been added to polyurethane foam to make it flame-retardant, and most of the flame retardants used are liquid at room temperature, such as phosphate ester monomers.
[0004] Generally, when phosphate ester monomers that are liquid at room temperature are used as flame retardants for polyurethane foams, there is a problem that the moldability of the polyurethane tends to decrease as the amount of flame retardant used increases because the monomers have a plasticizing effect.
[0005] In order to solve the above problems, a method has been proposed in which a chlorinated polyether polyol obtained by ring-opening polymerization of 3,4-dichloro-1,2-epoxybutane is used (Patent Document 1). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 202573 / 1999 Summary of the Invention [Problem to be solved by the invention]
[0007] However, such chlorinated polyether polyols have insufficient thermal stability due to the inclusion of thermally unstable chlorine groups. In addition, when used as a raw material for polyurethane, hydrochloric acid generated by thermal decomposition reduces the activity of the polyurethane-forming catalyst, which causes problems in moldability and results in poor mechanical properties of the polyurethanes produced. [Means for solving the problem]
[0008] The various aspects of the present invention are as follows [1] to [6]. [1] A chlorine-containing polyether polyol composition comprising 100 parts by weight of a chlorine-containing polyether polyol having a molecular weight of 400 to 5,000 and 0.5 to 20 parts by weight of an epoxy compound. [2] The chlorine-containing polyether polyol composition according to [1], wherein the chlorine-containing polyether polyol is a compound represented by the following formula (1):
[0009] [ka]
[0010] (In the above formula (1), R 1 represents a hydroxy compound residue having a molecular weight of 100 or more and 2500 or less, n represents an integer of 1 or more and less than 25, and m represents 2 or 3. [3] The chlorine-containing polyether polyol composition according to [1] or [2], wherein the epoxy compound is a liquid epoxy compound having an epoxy equivalent of 100 to 1,000. [4] The chlorine-containing polyether polyol composition according to any one of [1] to [3], further comprising 1 to 100 ppm of an aluminum compound. [5] The chlorine-containing polyether polyol composition according to [4], wherein the aluminum compound is aluminum hydroxide. [6] A polyurethane which is a reaction product of the chlorine-containing polyether polyol composition according to any one of [1] to [5] and an isocyanate compound. Effect of the Invention
[0011] The chlorine-containing polyether polyol composition according to one embodiment of the present invention can be used as a raw material for polyurethane having excellent mechanical properties, thermal stability, moldability and flame retardancy. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Exemplary embodiments for carrying out the present invention are described in detail below.
[0013] <Chlorine-containing polyether polyol composition> The chlorine-containing polyether polyol composition according to one embodiment of the present invention contains 100 parts by weight of a chlorine-containing polyether polyol having a molecular weight of 400 to 5,000 and 0.5 to 20 parts by weight of an epoxy compound.
[0014] <Chlorine-containing polyether polyol> The chlorine-containing polyether polyol contained in the chlorine-containing polyether polyol composition according to one embodiment of the present invention has a molecular weight of 400 to 5,000, preferably 400 to 3000. If the molecular weight is less than 400, the mechanical properties are not sufficiently improved, and if it exceeds 5000, the viscosity increases, making it difficult to handle, and the compatibility with epoxy compounds decreases, causing the chlorine-containing polyether polyol composition to become cloudy.
[0015] The chlorine-containing polyether polyol is not particularly limited, but examples thereof include the structure represented by the above formula (1).
[0016] In the above formula (1), R 1 R represents a hydroxy compound residue having a molecular weight of 100 or more and 2500 or less. 1Examples of the hydroxy compound residue represented by the formula (I) include, but are not limited to, residues of dipropylene glycol, tripropylene glycol, 1,6-hexanediol, 1,9-nonanediol, 2,5-hexanediol, 1,3-cyclohexanediol, 3-methylpentane-1,5-diol, 2,5-dimethyl-2,5-hexanediol, hexanetriol, 2-naphthol, bisphenol, polyether polyol having a hydroxyl group, polyester polyol, polycarbonate polyol, and the like.
[0017] Among these hydroxy compound residues, residues of tripropylene glycol, 3-methylpentane-1,5-diol, polyether polyols having a molecular weight of 200 or more and 1,000 or less, polyester polyols or polycarbonate polyols having a molecular weight of 500 or more and 1,000 or less are preferred, since they enable efficient production of chlorine-containing polyether polyols, and residues of tripropylene glycol, polyether polyols having a molecular weight of 200 or more and 1,000 or less, polyester polyols or polycarbonate polyols having a molecular weight of 500 or more and 1,000 or less are particularly preferred.
[0018] The polyether polyols include, but are not limited to, polypropylene glycol, polyethylene glycol, polytetramethylene glycol, and propylene oxide-ethylene oxide copolymers.
[0019] The polyester polyol is not particularly limited, but examples thereof include those produced by subjecting an aromatic and / or aliphatic polybasic acid, acid anhydride or methyl ester to an esterification reaction with a compound having two or three hydroxyl groups (polyhydric alcohol) by a known method, and those produced by ring-opening polymerization of ε-caprolactone using a compound having two or three hydroxyl groups (polyhydric alcohol) as an initiator.
[0020] The polycarbonate polyol is not particularly limited, but examples thereof include those produced by reacting an alkanediol such as 1,6-hexanediol, 1,5-pentanediol, or 3-methyl-1,5-pentanediol with a carbonate ester such as dimethyl carbonate or diethyl carbonate as raw materials by a known method.
[0021] The degree of unsaturation of the chlorine-containing polyether polyol is preferably 0.02 meq / g or less, and particularly preferably 0.01 meq / g or less, since the physical properties of the resulting polyurethane, such as hysteresis loss and compression set rate, are improved.
[0022] The Mw / Mn of the chlorine-containing polyether polyol is preferably 2.00 or less, and more preferably 1.80 or less, in order to improve moldability when made into a polyurethane resin (wherein Mn is the number average molecular weight and Mw is the weight average molecular weight determined by gel permeation chromatography measurement using polystyrene as the standard substance).
[0023] The primary terminal hydroxyl group ratio in the chlorine-containing polyether is not particularly limited, but is preferably less than 10% because this reduces variation in reactivity, allows for a uniform reaction, and tends to result in a uniform molecular weight distribution and composition of the resulting polyurethane.
[0024] The number of hydroxyl groups (functional groups) contained in one molecule of the chlorine-containing polyether polyol is not particularly limited, but is preferably 2 to 8, and particularly preferably 2 to 3, in order to obtain a polyurethane with good mechanical properties.
[0025] The method for producing chlorine-containing polyether polyol is not particularly limited, and can be produced by a conventionally known method.For example, the method of adding chlorine-containing alkylene oxide to a bifunctional or higher hydroxy compound to a predetermined molecular weight using Lewis acid catalyst or composite metal cyanide complex catalyst, or the method of carrying out ring-opening polymerization of chlorine-containing alkylene oxide in the presence of a bifunctional or higher hydroxy compound, an onium salt catalyst such as phosphazenium salt, ammonium salt, or phosphonium salt, and a Lewis acid catalyst.
[0026] An example of the chlorine-containing alkylene oxide is epichlorohydrin.
[0027] The polymerization temperature when producing the chlorine-containing polyether polyol is not particularly limited, but since the polyalkylene oxide is not likely to decompose and the molecular weight distribution is not likely to broaden, and the catalytic activity is likely to be exhibited, it is preferably 150°C or less, and more preferably in the range of 70 to 110°C.
[0028] In the method for producing a chlorine-containing polyether polyol, the polymerization reaction is preferably carried out without a solvent, but can also be carried out in a solvent. Examples of the solvent that can be used include benzene, toluene, xylene, cyclohexane, 1,2-dichloroethane, chlorobenzene, dichlorobenzene, 1,4-dioxane, and 1,2-dimethoxyethane.
[0029] <Epoxy compounds> The epoxy compound contained in the chlorine-containing polyether polyol composition according to one embodiment of the present invention is not particularly limited, but examples thereof include epoxidized vegetable oils obtained by epoxidizing linseed oil, soybean oil, coconut oil, safflower oil, sunflower oil, cottonseed oil, sunflower oil, etc.; epoxidized fatty acid monoesters such as epoxidized octyl stearate; epoxidized fatty acid diesters obtained by epoxidizing glycol esters of unsaturated fatty acids; alicyclic epoxides such as epoxidized hexahydrophthalic acid esters; epoxidized unsaturated hydrocarbons such as epoxidized polybutadiene; and epoxy resins such as bisphenol A diglycidyl ether. Among these, epoxidized vegetable oils and bisphenol A diglycidyl ether are particularly preferred because of their good versatility and ease of handling.
[0030] The epoxy compound is not particularly limited, but is preferably a liquid epoxy compound, since it efficiently achieves a stabilizing effect by capturing hydrogen chloride generated by thermal decomposition of the chlorine-containing polyether polyol and is easy to handle.
[0031] The epoxy equivalent of the epoxy compound is not particularly limited, but is preferably 100 to 1000 g / eq, and particularly preferably 150 to 800 g / eq, in order to efficiently impart thermal stability.
[0032] The amount of the epoxy compound is 0.5 to 20 parts by weight relative to 100 parts by weight of the chlorine-containing polyether polyol, and is preferably 0.5 to 15 parts by weight, and particularly preferably 0.5 to 10 parts by weight, since better flame retardancy is exhibited by combining with the chlorine-containing polyether polyol. If the amount is too small, sufficient thermal stability and flame retardancy cannot be obtained, and if the amount is too large, problems such as impaired moldability during polyurethane production occur.
[0033] <Aluminum compounds> The chlorine-containing polyether polyol composition according to one embodiment of the present invention may contain an aluminum compound.The aluminum compound is not particularly limited, but can be, for example, aluminum hydroxide, aluminum oxide, aluminum silicate, polyaluminum chloride, aluminum sulfate, aluminum alcoholate, etc., because it improves the mechanical properties of polyurethane produced by reacting with isocyanate compound.Among these, aluminum hydroxide is preferred because it improves the mechanical properties of polyurethane produced.
[0034] The content of the aluminum compound is not particularly limited, but is preferably 1 to 100 ppm, and particularly preferably 1 ppm to 50 ppm. Within this content range, the mechanical properties are improved, the moldability during polyurethane production is not impaired, and the physical properties do not decrease.
[0035] <Polyurethane> A polyurethane according to one embodiment of the present invention is a reaction product of the above chlorine-containing polyether polyol composition and an isocyanate compound.
[0036] The structure of the polyurethane is not particularly limited as long as it contains a residue of the chlorine-containing polyether polyol contained in the chlorine-containing polyether polyol composition according to one embodiment of the present invention in its molecular structure, and may be crosslinked, linear, or branched.
[0037] The method for producing the polyurethane is not particularly limited, but may involve reacting the chlorine-containing polyether polyol composition according to one aspect of the present invention with an isocyanate compound.
[0038] The isocyanate compound is not particularly limited, and examples thereof include aromatic isocyanate compounds, aliphatic isocyanate compounds, alicyclic isocyanate compounds, and polyisocyanate derivatives thereof.
[0039] Among these, examples of aromatic isocyanate compounds include tolylene diisocyanate (2,4- or 2,6-tolylene diisocyanate, or a mixture thereof) (TDI), phenylene diisocyanate (m- or p-phenylene diisocyanate, or a mixture thereof), 4,4'-diphenyl diisocyanate, diphenylmethane diisocyanate (4,4'-, 2,4'-, or 2,2'-diphenylmethane diisocyanate, or a mixture thereof) (MDI), 4,4'-toluidine isocyanate (TODI), 4,4'-diphenyl ether diisocyanate, xylylene diisocyanate (1,3- or 1,4-xylylene diisocyanate, or a mixture thereof) (XDI), tetramethyl xylylene diisocyanate (T ... Examples of the isocyanate include rylene diisocyanate (1,3- or 1,4-tetramethylxylylene diisocyanate, or a mixture thereof) (TMXDI), ω,ω'-diisocyanato-1,4-diethylbenzene, naphthalene diisocyanate (1,5-, 1,4-, or 1,8-naphthalene diisocyanate, or a mixture thereof) (NDI), triphenylmethane triisocyanate, tris(isocyanatophenyl)thiophosphate, polymethylene polyphenylene polyisocyanate, nitrodiphenyl-4,4'-diisocyanate, 3,3'-dimethyldiphenylmethane-4,4'-diisocyanate, 4,4'-diphenylpropane diisocyanate, and 3,3'-dimethoxydiphenyl-4,4'-diisocyanate.
[0040] Examples of the aliphatic isocyanate compound include trimethylene diisocyanate, 1,2-propylene diisocyanate, butylene diisocyanate (tetramethylene diisocyanate, 1,2-butylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate), hexamethylene diisocyanate, pentamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, 2,6-diisocyanate methylcaprate, lysine diisocyanate, lysine ester triisocyanate, 1,6,11-undecane triisocyanate, 1,3,6-hexamethylene triisocyanate, trimethylhexamethylene diisocyanate, and decamethylene diisocyanate.
[0041] Examples of monocyclic alicyclic isocyanate compounds include 1,3-cyclopentane diisocyanate, 1,3-cyclopentene diisocyanate, cyclohexane diisocyanate (1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate), 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate (isophorone diisocyanate, IPDI), methylene bis(cyclohexyl isocyanate) (4,4'-, 2,4'- or 2,2'-methylene bis(cyclohexyl isocyanate), or mixtures thereof. Examples of the isocyanate include methyl cyclohexane diisocyanate (methyl-2,4-cyclohexane diisocyanate, methyl-2,6-cyclohexane diisocyanate, bis(isocyanatomethyl)cyclohexane (1,3- or 1,4-bis(isocyanatomethyl)cyclohexane, or a mixture thereof) (hydrogenated XDI), dimer acid diisocyanate, trans cyclohexane 1,4-diisocyanate, hydrogenated tolylene diisocyanate (hydrogenated TDI), and hydrogenated tetramethylxylylene diisocyanate (hydrogenated TMXDI).
[0042] Examples of the crosslinked cyclic alicyclic isocyanate compound include norbornane diisocyanate, norbornane diisocyanate methyl, bicycloheptane triisocyanate, diisocyanatomethyl bicycloheptane, and di(diisocyanatomethyl)tricyclodecane.
[0043] Examples of the derivatives of these isocyanates include polymers of the isocyanate compounds (dimers, trimers, pentamers, heptamers, uretidinedione, ureitonimine, isocyanurate modified products, polycarbodiimides, etc.), urethane modified products (e.g., urethane modified products in which a portion of the isocyanate groups in the isocyanate compounds or polymers is modified or reacted with a monool or polyol), biuret modified products (e.g., biuret modified products produced by the reaction of the isocyanate compounds with water), allophanate modified products (e.g., allophanate modified products produced by the reaction of the isocyanate compounds with a monool or polyol component), urea modified products (e.g., urea modified products produced by the reaction of the isocyanate compounds with a diamine), and oxadiazinetriones (e.g., oxadiazinetriones produced by the reaction of the isocyanate compounds with carbon dioxide gas, etc.).
[0044] The above-mentioned isocyanate compounds or derivatives thereof may be used alone or in combination of two or more kinds.
[0045] When a polyurethane is obtained by reacting a chlorine-containing polyether polyol with a polyisocyanate compound, the reaction between the chlorine-containing polyether polyol and the isocyanate compound can be accelerated by, for example, heating the composition up to 200°C or adding a catalyst such as dioctyltin dilaurate, dibutyltin dilaurate, triethylamine, triethylenediamine, stannous octoate, dibutyltin di-2-ethylhexanoate, sodium o-phenylphenate, potassium oleate, tetra(2-ethylhexyl) titanate, stannic chloride, ferric chloride, or antimony trichloride, thereby enabling the polyurethane to be obtained in a short time.
[0046] When producing the polyurethane according to one embodiment of the present invention, the chlorine-containing polyether polyol according to one embodiment of the present invention may be mixed with other known polyols, stabilizers, antioxidants, foam stabilizers, crosslinking agents, foaming agents, interconnecting agents, and the like, as necessary.
[0047] The polyurethane according to one embodiment of the present invention can be used for urethane foam applications such as rigid or flexible foams, as coatings, adhesives, sealants, thermoplastic or thermosetting elastomers, leather, spandex, various inks, etc.
[0048] Polyurethane foams are broadly classified into flexible and rigid types. When attempting to obtain polyurethane foam using the chlorine-containing polyether polyol according to one embodiment of the present invention, conventionally known production methods can be applied to both flexible and rigid types.
[0049] For example, a method may be mentioned in which a mixture liquid that is liquid at room temperature and that is prepared by mixing the chlorine-containing polyether polyol according to one embodiment of the present invention with other known polyols, stabilizers, antioxidants, catalysts, foam stabilizers, crosslinking agents, foaming agents, connecting agents, etc., as necessary, is stirred and mixed, and then the mixture is stirred and mixed with a polyisocyanate compound, and the mixture is poured into a suitable mold and foamed and cured.
[0050] In addition, the chlorine-containing polyether polyol according to one embodiment of the present invention is mixed with another known polyol, a catalyst, a foam stabilizer, a blowing agent, and a polyisocyanate compound by a known agitator mixer to prepare a foamable mixture, which is then poured into a mold with its top open to allow free foaming and cured into a slab.
[0051] The expansion ratio of the polyurethane foam is not particularly limited, but in order to improve the handleability, it is preferably from 1.2 to 100, and particularly preferably from 10 to 80.
[0052] The polyurethane foam is not particularly limited in its application, and due to the characteristics of the polyurethane foam made of the reaction product of the composition according to one embodiment of the present invention, it can be used in applications where soft polyurethane foam is used, such as automobile and vehicle ceiling materials and seats, pillows, furniture and interiors, bedding, shoe soles, sponges, various cushions, tennis balls, landing mats, etc. Also, the polyurethane foam according to one embodiment of the present invention can be used in applications where hard polyurethane foam is used, such as heat insulation and cold insulation materials, vibration and sound absorption materials, cushioning materials, and buoyancy materials. For example, for ships as insulation material for fishing boats, large ships, refrigerated cargo ships, LNG ships, LPG ships, liquefied gas ships, and containers, and as core material for FRP boats, for use as buoyancy material for large ships, lifeboats, buoys, and floats, for use in refrigerated cars, cooler cars, railway containers, and tank trucks, for use in vehicles as insulation material for the ceilings of cars and trucks, for use in plants as insulation material for tanks and piping at chemical industry equipment, for thermal insulation materials for heavy oil tanks and piping, for insulation material for LPG and LNG low-temperature liquefied gas cooling and piping, for insulation covers and tank lids, for use as insulation material for refrigerators and freezers, for insulation components for air conditioners, for insulation material for various insulation equipment such as showcases, storage units, vending machines, water heaters, and hot water tanks, and for use in housing, Examples of applications include insulation for homes and office buildings (walls, under floors, ceilings, under roofs, etc.), insulating building materials (laminate boards, composite panels, siding materials, etc.), insulation for bathtubs (stainless steel, FRP, enamel), insulation for freezers, refrigerated warehouses, agricultural warehouses, livestock barns, etc., void filling (insulated sashes), insulation for temperature-controlled rooms and district central heating and cooling systems, construction and building materials such as insulation for road floors and vibration prevention materials for civil engineering, as well as chair core materials, door panels, decorative crafts, recreational equipment (cooler boxes, water bottles), teaching materials (3D maps, etc.), mold materials, jigs, surfing core materials, RIM products (ski core materials, racket core materials, housings, etc.), packaging materials, etc.
[0053] In addition, due to the characteristics of the polyurethane according to one embodiment of the present invention, the polyurethane can be used as an adhesive, for example, for laminating flexible packaging materials, i.e., for bonding laminated food bags for snacks, boiled foods, and retort foods, and laminated non-food bags for detergents, etc.; in the construction field, for bonding wrapping, heated floors, and flooring; and in the electronics field, for bonding back sheets for solar cells, LCD televisions, and other battery-related items.
[0054] Furthermore, due to the characteristics of the polyurethane according to one embodiment of the present invention, in the application of a sealant, it can be used for architectural exteriors, for example, sealing of ALC panels and sashes, sealing of RC wall joints, sealing of frameworks under tiles and window frames, architectural interiors, sealing of plumbing and plasterboards, and sealing of architectural materials such as waterproof bases and roofs, sealing of window frames of special vehicles such as refrigerated trucks, and electric / electronic devices, and communication devices, particularly gaskets in hard disk drives.
[0055] Furthermore, due to the characteristics of the polyurethane according to one embodiment of the present invention, the applications of the polyurethane as an elastomer include, as a thermoplastic elastomer, hoses such as high pressure hoses, fire hoses, agricultural chemical hoses, and painting hoses, tubes such as air pressure tubes, hydraulic tubes, fuel tubes, dialysis tubes, and arterial, venous, and cardiac tubes, scratch-resistant films and sheets for automobiles, instrument panel covering materials, scratch-resistant films for sofas, air mats, nursing bed sheets, diaphragms, keyboard sheets, rubber screens, conveyor belts, gaskets, synthetic leather, stretch sheets, flexible filters, etc. films and sheets such as rubber, tarpaulins, clothing, life jackets, wet suits, hot melts, diapers, cushioning film for packaging, medical surgical film, various gears, various grips, solid tires, casters, rollers, vibration and soundproofing parts, pickers, bushes, bearings, slip prevention parts, building materials, packing, caps, watch straps, connectors, rubber screens, printing drums, grease covers, hammers, dust covers, sieve parts, industrial parts such as ball joints, instrument panel skins, gear knob skins, console box skins, leather seats It can be used for automobile parts such as car seats, bumpers and side moldings, tail lamp seals, snow chains, bushes, dust covers, gears, bearings, caps, ball joints, pedal stoppers, door lock strikers, spring covers, vibration-proof parts, belts such as conveyor belts, timing belts, round belts, V-belts, flat belts, power and communication cables, automotive ABS sensor cables, robot cables, industrial cables, computer wiring, and other electrical wires. It can also be used for sports shoes, hiking boots, ski boots, skis, snowboards, motocross, etc. Cross boots, safety shoes, high heels, snorkels, fins, golf ball covers, slip-proof staircases, road pole cones, roller skate wheels, various tags, sailboard equipment, ski parts, various ropes, binders, medical dressings, catheters, medical ropes, bandages, etc. Thermosetting elastomers are used in a wide range of applications, including papermaking, steel plate rolling rolls, printing, small rolls for office equipment, platen rolls, skate rollers, and other rolls, solid tires, casters, battery forklifts, work transport vehicles (pallet lifts, etc.),It can be used for a wide range of applications, including industrial truck wheels and other wheels, conveyor belt idlers, cable and belt guide rolls, prairie springs, belt buffers, belts such as oil seals, electronics equipment parts, cleaning grade for copiers, and other office automation equipment, as well as secondary processing materials such as round bars, pipes, square columns, plates, and sheets. It can also be used for a wide range of applications, including various gears, connection rings and liners, pump linings, impeller cyclone cones, cyclone liners, and polishing pads. EXAMPLES
[0056] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. First, the details of the raw materials used in the production of the chlorine-containing polyether polyol, the analysis method and the production method of the chlorine-containing polyether polyol will be described.
[0057] (Method of analysis of chlorine-containing polyether polyol) (1) Molecular weight of chlorine-containing polyether polyol (unit: g / mol) The hydroxyl value d (unit: mgKOH / g) of the chlorine-containing polyether polyol was measured by the method described in JIS K-1557. The number of functional groups of the obtained chlorine-containing polyether polyol was defined as e, and the molecular weight of the chlorine-containing polyether polyol was calculated by the following formula. Molecular weight=(56100 / d)×e
[0058] (2) Molecular weight distribution of chlorine-containing polyether polyol (unit: none) Measurements were performed at 40°C using a gel permeation chromatograph (GPC) (Tosoh Corporation, HLC8020) with tetrahydrofuran as a solvent, and polystyrene was used as the standard substance to determine the number average molecular weight (Mn) and weight average molecular weight (Mw) of the chlorine-containing polyether polyol. From the Mn and Mw calculated by the above method, the molecular weight distribution (Mw / Mn) of the chlorine-containing polyether polyol was calculated.
[0059] (3) Degree of unsaturation of chlorine-containing polyether polyol (unit: meq / g) The degree of unsaturation of chlorine-containing polyether polyol was measured by the method described in JIS K-1557. was calculated.
[0060] (4) Aluminum concentration in the chlorine-containing polyether polyol composition (unit: ppm) The chlorine-containing polyether polyol composition was incinerated and then dissolved in acid to obtain a solution, which was then measured using an ICP-AES Optima 8300 (manufactured by PerkinElmer Co., Ltd.).
[0061] (5) Thermal stability: Increase in acid value (unit: ΔmgKOH / g) A thermal stability test was carried out by holding the chlorine-containing polyether polyol composition in a Geer oven heated to 150° C. for 30 hours, and the acid values before and after the test were calculated according to the method described in JIS K-1557. The oxidation increase was calculated by subtracting the acid value before the thermal stability test from the acid value after the thermal stability test calculated by the above method. A (pass): less than 0.1 mgKOH / g B (Pass): 0.1mgKOH / g or more, less than 0.5mgKOH / g C (fail): 0.5mgKOH / g or more
[0062] (6) Thermal stability: Viscosity retention rate (unit: %) A thermal stability test was carried out by holding the chlorine-containing polyether polyol composition in a Geer oven heated to 150° C. for 30 hours, and the viscosity before and after the test was measured using a B-type viscometer. Using the viscosity values measured by the above method, the viscosity retention was calculated according to the following formula. Viscosity after thermal stability test / Viscosity before thermal stability test x 100 A (pass): 95% or higher B (Pass): 90% or more, less than 95% C (Fail): Less than 90%
[0063] (7) Thermal stability: Appearance (unit: none) A thermal stability test was carried out by holding the chlorine-containing polyether polyol composition in a Geer oven heated to 150° C. for 30 hours, and the color after the test was visually observed. A (pass): light yellow B (Pass): Dark yellow C (Fail): Brown to black
[0064] Example 1. In a 2-liter four-neck flask equipped with a stirring blade, 283.2 g of polypropylene glycol having a molecular weight of 400 (manufactured by Sanyo Chemical Industries, Ltd., product name: Sannix PP-400) and 3.42 g of tetrabutylammonium bromide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added. After the flask was filled with nitrogen, the inside temperature was set to 100°C, and dehydration treatment was performed for 2 hours under reduced pressure of 0.5 kPa. Thereafter, 6.51 g of triisopropoxyaluminum (manufactured by Kawaken Fine Chemicals Co., Ltd., PADM) was added, the inside temperature was set to 100°C, and decompression treatment was performed for 2 hours under reduced pressure of 0.5 kPa to obtain an initiator composition. The obtained initiator composition was heated to 98°C, and 960 mL of epichlorohydrin (ECH, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was continuously supplied over 4 hours. After feeding epichlorohydrin, the mixture was aged for 2 hours at an internal temperature of 90 to 100°C, and then the remaining epichlorohydrin was removed at 100°C under reduced pressure of 0.5 kPa to obtain 1415 g of crude chlorine-containing polyol. The temperature was then lowered to 80°C, and 42.5 g of Epomic R-140 (Mitsui Chemicals, liquid epoxy compound, epoxy equivalent 188 g / eq) was added as bisphenol A diglycidyl ether to obtain a pale yellow crude chlorine-containing polyether polyol composition [A-1]. The molecular weight of the obtained crude chlorine-containing polyether polyol [A-1] was 2010 g / mol, the degree of unsaturation was 0.0045 meq / g, Mw / Mn was 1.55, and the primary content rate was 4%. Aluminum alcoholate bound to the crude chlorine-containing polyether polyol composition [A-1] remained, and the aluminum concentration was 602 ppm. Furthermore, when evaluated according to the above-mentioned thermal stability test method, the chlorine-containing polyether polyol composition had a deep yellow appearance, little increase in acid value or decrease in viscosity, and excellent thermal stability.
[0065] Example 2. 100 parts by weight of the crude chlorine-containing polyether polyol composition [A-1] obtained in Example 1 was mixed with 1 part by weight of diatomaceous earth (Radiolite #3000, manufactured by Showa Chemical Industry Co., Ltd.) and 5 parts by weight of water (ion-exchanged water) and stirred at 80°C for 2 hours.
[0066] Thereafter, dehydration was started while increasing the temperature and reducing the pressure, and finally, dehydration was performed under reduced pressure at 100°C and 0.2kPa for 3 hours. Then, pressure filtration was performed at 90°C and 0.3MPa using a stainless steel holder KST-142 with a tank manufactured by Advantec Toyo Co., Ltd. (filter material: stainless steel mesh, 120 mesh) to obtain a pale yellow chlorine-containing polyether polyol composition [A-2]. The obtained chlorine-containing polyether polyol composition [A-2] contained aluminum hydroxide, and the aluminum concentration was 6ppm. In addition, when evaluated according to the above-mentioned thermal stability test method, the appearance was pale yellow, there was little increase in acid value or decrease in viscosity, and it was a chlorine-containing polyether polyol composition with excellent thermal stability.
[0067] Example 3. To 100 parts by weight of the crude chlorine-containing polyether polyol composition [A-1] obtained in Example 1, 1 part by weight of diatomaceous earth (Radiolite #3000, manufactured by Showa Chemical Industry Co., Ltd.) and 5 parts by weight of water (ion-exchanged water) were added, and the mixture was stirred at 80°C for 2 hours.
[0068] Thereafter, dehydration was started while increasing the temperature and reducing the pressure, and finally, dehydration was performed under reduced pressure at 100°C and 0.2kPa for 3 hours. Then, pressure filtration was performed twice at 90°C and 0.3MPa using a stainless steel holder KST-142 with a tank manufactured by Advantech Toyo Co., Ltd. (filter material: quantitative filter paper No. 5A manufactured by Advantech Toyo Co., Ltd.) to obtain a pale yellow chlorine-containing polyether polyol composition [A-3]. The aluminum concentration in the obtained chlorine-containing polyether polyol composition [A-3] was less than 1ppm. In addition, when evaluated according to the above-mentioned thermal stability test method, the composition had a pale yellow appearance, little increase in acid value and little decrease in viscosity, and was a chlorine-containing polyether polyol composition with excellent thermal stability.
[0069] Example 4. In a 2-liter four-neck flask equipped with a stirring blade, 283.2 g of polypropylene glycol having a molecular weight of 400 (manufactured by Sanyo Chemical Industries, Ltd., product name: Sannix PP-400) and 3.42 g of tetrabutylammonium bromide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added. After the flask was filled with nitrogen, the inside temperature was set to 100°C, and dehydration treatment was performed for 2 hours under reduced pressure of 0.5 kPa. Thereafter, 6.51 g of triisopropoxyaluminum (manufactured by Kawaken Fine Chemicals Co., Ltd., PADM) was added, the inside temperature was set to 100°C, and decompression treatment was performed for 2 hours under reduced pressure of 0.5 kPa to obtain an initiator composition. The obtained initiator composition was heated to 98°C, and 960 mL of epichlorohydrin (ECH, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was continuously supplied over 4 hours. After feeding epichlorohydrin, the mixture was aged for 2 hours at an internal temperature of 90-100°C, and then the residual epichlorohydrin was removed at 100°C and a reduced pressure of 0.5kPa to obtain 1415g of crude chlorine-containing polyol. The temperature was then lowered to 80°C, and 42.5g of Epiclon 4050 (DIC, solid epoxy compound, epoxy equivalent 920g / eq) was added to obtain a pale yellow crude chlorine-containing polyether polyol composition. The molecular weight of the obtained crude chlorine-containing polyether polyol was 1980g / mol, the degree of unsaturation was 0.0044meq / g, Mw / Mn was 1.62, and the primary content was 3%.
[0070] To 100 parts by weight of the obtained crude chlorine-containing polyether polyol composition, 1 part by weight of diatomaceous earth (Radiolite #3000, manufactured by Showa Chemical Industry Co., Ltd.) and 5 parts by weight of water (ion-exchanged water) were added, and the mixture was stirred at 80°C for 2 hours.
[0071] Thereafter, dehydration was started while increasing the temperature and reducing the pressure, and finally, dehydration was performed under reduced pressure at 100°C and 0.2kPa for 3 hours. Then, pressure filtration was performed at 90°C and 0.3MPa using a stainless steel holder KST-142 with a tank manufactured by Advantec Toyo Co., Ltd. (filter material: stainless steel mesh, 120 mesh) to obtain a pale yellow chlorine-containing polyether polyol composition [A-4]. The obtained chlorine-containing polyether polyol composition [A-4] contained aluminum hydroxide, and the aluminum concentration was 7ppm. In addition, when evaluated according to the above-mentioned thermal stability test method, the appearance was deep yellow, there was little increase in acid value and decrease in viscosity, and it was a chlorine-containing polyether polyol composition with excellent thermal stability.
[0072] Example 5. In a 2-liter four-neck flask equipped with a stirring blade, 849.6 g of polycarbonate diol having a molecular weight of 1000 (manufactured by Tosoh Corporation, trade name: Nipolan-965) and 6.85 g of tetrabutylammonium bromide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added. After the flask was filled with nitrogen, the inside temperature was set to 100°C, and dehydration treatment was performed for 2 hours under reduced pressure of 0.5 kPa. Thereafter, 13.02 g of triisopropoxyaluminum (manufactured by Kawaken Fine Chemicals Co., Ltd., PADM) was added, the inside temperature was set to 100°C, and decompression treatment was performed for 2 hours under reduced pressure of 0.5 kPa to obtain an initiator composition. The obtained initiator composition was heated to 98°C, and 720 mL of epichlorohydrin (ECH, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was continuously supplied over 4 hours. After feeding epichlorohydrin, the mixture was aged for 2 hours at an internal temperature of 90 to 100°C, and then the residual epichlorohydrin was removed at 100°C and a reduced pressure of 0.5 kPa to obtain 1700 g of crude chlorine-containing polyol. The temperature was then lowered to 80°C, and 51.2 g of Epomic R-140 (Mitsui Chemicals, liquid epoxy compound, epoxy equivalent 188 g / eq) was added to obtain a pale yellow crude chlorine-containing polyether polyol composition. The molecular weight of the obtained crude chlorine-containing polyether polyol was 2000 g / mol, the degree of unsaturation was 0.0052 meq / g, Mw / Mn was 1.88, and the primary content rate was 6%.
[0073] To 100 parts by weight of the obtained crude chlorine-containing polyether polyol composition, 1 part by weight of diatomaceous earth (Radiolite #3000, manufactured by Showa Chemical Industry Co., Ltd.) and 5 parts by weight of water (ion-exchanged water) were added, and the mixture was stirred at 80°C for 2 hours.
[0074] Thereafter, dehydration was started while increasing the temperature and reducing the pressure, and finally, dehydration was performed under reduced pressure at 100°C and 0.2kPa for 3 hours. Then, pressure filtration was performed at 90°C and 0.3MPa using a stainless steel holder KST-142 with a tank manufactured by Advantec Toyo Co., Ltd. (filter material: stainless steel mesh, 120 mesh) to obtain a pale yellow chlorine-containing polyether polyol composition [A-5]. The obtained chlorine-containing polyether polyol composition [A-5] contained aluminum hydroxide, and the aluminum concentration was 8ppm. In addition, when evaluated according to the above-mentioned thermal stability test method, the appearance was pale yellow, there was little increase in acid value and decrease in viscosity, and it was a chlorine-containing polyether polyol composition with excellent thermal stability.
[0075] Example 6. In a 2-liter four-neck flask equipped with a stirring blade, 849.6 g of polycarbonate diol having a molecular weight of 1000 (manufactured by Tosoh Corporation, trade name: Nipolan-965) and 6.85 g of tetrabutylammonium bromide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added. After the flask was filled with nitrogen, the inside temperature was set to 100°C, and dehydration treatment was performed for 2 hours under reduced pressure of 0.5 kPa. Thereafter, 13.02 g of triisopropoxyaluminum (manufactured by Kawaken Fine Chemicals Co., Ltd., PADM) was added, the inside temperature was set to 100°C, and decompression treatment was performed for 2 hours under reduced pressure of 0.5 kPa to obtain an initiator composition. The obtained initiator composition was heated to 98°C, and 720 mL of epichlorohydrin (ECH, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was continuously supplied over 4 hours. After feeding epichlorohydrin, the mixture was aged for 2 hours at an internal temperature of 90 to 100°C, and then the remaining epichlorohydrin was removed at 100°C and a reduced pressure of 0.5 kPa to obtain 1698 g of crude chlorine-containing polyol. The temperature was then lowered to 80°C, and 271.9 g of Epomic R-140 (Mitsui Chemicals, liquid epoxy compound, epoxy equivalent 188 g / eq) was added to obtain a pale yellow crude chlorine-containing polyether polyol composition. The molecular weight of the obtained crude chlorine-containing polyether polyol was 2000 g / mol, the degree of unsaturation was 0.0052 meq / g, Mw / Mn was 1.88, and the primary content rate was 6%.
[0076] To 100 parts by weight of the obtained crude chlorine-containing polyether polyol composition, 0.4 parts by weight of diatomaceous earth (Radiolite #3000, manufactured by Showa Chemical Industry Co., Ltd.) and 5 parts by weight of water (ion-exchanged water) were added, and the mixture was stirred at 80°C for 2 hours.
[0077] Thereafter, dehydration was started while increasing the temperature and reducing the pressure, and finally, dehydration was performed under reduced pressure at 100°C and 0.2kPa for 3 hours. Then, pressure filtration was performed at 90°C and 0.3MPa using a stainless steel holder KST-142 with a tank manufactured by Advantec Toyo Co., Ltd. (filter material: stainless steel mesh, 120 mesh) to obtain a pale yellow chlorine-containing polyether polyol composition [A-6]. The obtained chlorine-containing polyether polyol composition [A-6] contained aluminum hydroxide, and the aluminum concentration was 83ppm. In addition, when evaluated according to the above-mentioned thermal stability test method, the appearance was pale yellow, there was little increase in acid value and decrease in viscosity, and it was a chlorine-containing polyether polyol composition with excellent thermal stability.
[0078] Example 7. In a 2-liter four-neck flask equipped with a stirring blade, 590 g of polyester polyol having a molecular weight of 1000 (manufactured by Kuraray Co., Ltd., product name: Kuraray Polyol P-1010) and 8.07 g of tetrabutylammonium bromide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added. After the flask was filled with nitrogen, the inside temperature was set to 100°C, and dehydration treatment was performed for 2 hours under reduced pressure of 0.5 kPa. Thereafter, 9.04 g of triisopropoxyaluminum (manufactured by Kawaken Fine Chemical Co., Ltd., PADM) was added, the inside temperature was set to 100°C, and decompression treatment was performed for 2 hours under reduced pressure of 0.5 kPa to obtain an initiator composition. The obtained initiator composition was heated to 98°C, and 500 mL of epichlorohydrin (ECH, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was continuously supplied over 4 hours. After feeding epichlorohydrin, the mixture was aged for 2 hours at an internal temperature of 90 to 100°C, and then the residual epichlorohydrin was removed at 100°C and a reduced pressure of 0.5 kPa to obtain 1698 g of crude chlorine-containing polyol. The temperature was then lowered to 80°C, and 62.11 g of Adeka Cizer O-130P (manufactured by ADEKA Corporation, liquid epoxy compound, epoxy equivalent 184 g / eq) was added as an epoxidized vegetable oil to obtain a pale yellow crude chlorine-containing polyether polyol composition. The molecular weight of the obtained crude chlorine-containing polyether polyol was 2000 g / mol, the degree of unsaturation was 0.0420 meq / g, Mw / Mn was 1.79, and the primary content rate was 4%.
[0079] To 100 parts by weight of the obtained crude chlorine-containing polyether polyol composition, 0.4 parts by weight of diatomaceous earth (Radiolite #3000, manufactured by Showa Chemical Industry Co., Ltd.) and 5 parts by weight of water (ion-exchanged water) were added, and the mixture was stirred at 80°C for 2 hours.
[0080] Thereafter, dehydration was started while increasing the temperature and reducing the pressure, and finally, dehydration was performed under reduced pressure at 100°C and 0.2kPa for 3 hours. Then, pressure filtration was performed at 90°C and 0.3MPa using a stainless steel holder KST-142 with a tank manufactured by Advantec Toyo Co., Ltd. (filter material: stainless steel mesh, 120 mesh) to obtain a pale yellow chlorine-containing polyether polyol composition [A-7]. The obtained chlorine-containing polyether polyol composition [A-7] contained aluminum hydroxide, and the aluminum concentration was 7ppm. In addition, when evaluated according to the above-mentioned thermal stability test method, the appearance was pale yellow, there was little increase in acid value and decrease in viscosity, and it was a chlorine-containing polyether polyol composition with excellent thermal stability.
[0081] Comparative Example 1 A crude chlorine-containing polyol composition was obtained in the same manner as in Example 1, except that 424.8 g of Epomic R-140 (liquid epoxy compound) was used.
[0082] To 100 parts by weight of the obtained crude chlorine-containing polyether polyol, 1 part by weight of diatomaceous earth (Radiolite #3000, manufactured by Showa Chemical Industry Co., Ltd.) and 5 parts by weight of water (ion-exchanged water) were added, and the mixture was stirred at 80°C for 2 hours.
[0083] Thereafter, dehydration was started while increasing the temperature and reducing the pressure, and finally, dehydration was performed under reduced pressure at 100°C and 0.2kPa for 3 hours. Then, pressure filtration was performed at 90°C and 0.3MPa using a stainless steel holder KST-142 with a tank manufactured by Advantec Toyo Co., Ltd. (filter material: stainless steel mesh, 120 mesh) to obtain a pale yellow chlorine-containing polyether polyol composition [B-1]. The obtained chlorine-containing polyether polyol composition [B-1] contained aluminum hydroxide, and the aluminum concentration was 3ppm. In addition, when evaluated according to the above-mentioned thermal stability test method, the appearance was pale yellow, there was little increase in acid value or decrease in viscosity, and it was a chlorine-containing polyether polyol composition with excellent thermal stability.
[0084] Comparative Example 2 The same procedure as in Example 1 was carried out except that Epomic R-140 was not added, to obtain a crude chlorine-containing polyol composition.
[0085] To 100 parts by weight of the obtained crude chlorine-containing polyether polyol, 1 part by weight of diatomaceous earth (Radiolite #3000, manufactured by Showa Chemical Industry Co., Ltd.) and 5 parts by weight of water (ion-exchanged water) were added, and the mixture was stirred at 80°C for 2 hours.
[0086] Thereafter, dehydration was started while increasing the temperature and reducing the pressure, and finally, dehydration was performed under reduced pressure at 100°C and 0.2kPa for 3 hours. Then, pressure filtration was performed at 90°C and 0.3MPa using a stainless steel holder KST-142 with a tank manufactured by Advantec Toyo Co., Ltd. (filter material: stainless steel mesh, 120 mesh) to obtain a pale yellow chlorine-containing polyether polyol composition [B-2]. The obtained chlorine-containing polyether polyol composition [B-2] contained aluminum hydroxide, and the aluminum concentration was 12ppm. In addition, when evaluated according to the above-mentioned thermal stability test method, the appearance was brown, the acid value increased significantly, the viscosity decreased significantly, and the chlorine-containing polyether polyol composition had poor thermal stability.
[0087] The results of Examples 1 to 7 and Comparative Examples 1 and 2 are shown in Tables 1 and 2.
[0088] [Table 1]
[0089] [Table 2]
[0090] The evaluation method and preparation of polyurethane, which is the reaction product of the dye-containing polyether polyol composition of the present invention and an isocyanate compound, will be described below.
[0091] (How to make polyurethane) (1) Raw materials <<Commercially available PPG>> In all of the examples and comparative examples, Sannix GP-3000 manufactured by Sanyo Chemical Industries, Ltd. was used. <Foaming agent> In all of the Examples and Comparative Examples, ion-exchanged water was used as the foaming agent. <Foam stabilizer> In all of the Examples and Comparative Examples, SZ-1142 manufactured by Dow Toray was used as the silicone foam stabilizer. <Catalyst> In all of the Examples and Comparative Examples, a solution of triethylenediamine dissolved in dipropylene glycol at a concentration of 33% by weight (TEDA-L33, manufactured by Tosoh Corporation) and tin octoate (Nikka Octix Tin, manufactured by Nippon Kagaku Sangyo Co., Ltd.) were used as catalysts. <Isocyanate compounds> In all of the Examples and Comparative Examples, tolylene diisocyanate (Coronate T-80, manufactured by Tosoh Corporation) having a mixture ratio of 2,4 / 2,6 isomers of 80 / 20 was used.
[0092] Chlorine-containing polyether polyol and water were mixed in the compounding ratios shown in Tables 3 and 4, and the mixture was further mixed with a catalyst and a foam stabilizer. The mixture was stirred and mixed at 2000 revolutions per minute for 20 minutes using a small high-speed mixer (PRIMIX manufactured by Primix Corporation) to obtain a stirred mixture (hereinafter referred to as premix) excluding the isocyanate compound.
[0093] <Preparation of polyurethane foam> A predetermined amount of isocyanate compound was added to the premix prepared as above so that the ratio of isocyanate-reactive groups (NCO reactive groups) that can react with the NCO groups, including the total amount of isocyanate groups (NCO groups) and hydroxyl groups (OH groups) contained in water, i.e., NCO / NCO reactive groups, was 1.0. The mixture was stirred and mixed at 4,000 rpm for 8 seconds using a small high-speed mixer (PRIMIX, manufactured by Primix Corporation), and then immediately poured into an acrylic water tank measuring 250 mm x 250 mm x 250 mm to obtain a polyurethane foam.
[0094] (Method of measuring physical properties of polyurethane) (1) Formability The polyurethane foam thus produced was allowed to stand for 24 hours in a thermostatic chamber at 23°C and 50% RH, and the appearance was visually inspected to determine moldability. A (Pass): The foam surface is smooth and no shrinkage is observed. B (Pass): Some shrinkage is observed (no effect on physical properties) C (Fail): Shrinkage
[0095] (2) Tensile breaking strength: TB (unit: kPa) The polyurethane foam thus produced was allowed to stand for 24 hours in a thermostatic chamber at 23°C and 50% Rh, and then the tensile breaking strength was measured using a method in accordance with JIS K-6400. A (pass): 85kPa or more B (Pass): 70kPa or more, less than 85kPa C (Fail): Less than 70kPa
[0096] (3) Tensile elongation at break: EB (unit: %) The polyurethane foam thus produced was allowed to stand for 24 hours in a thermostatic chamber at 23°C and 50Rh%, and then the tensile elongation at break was measured by a method in accordance with JIS K-6400. A (pass): 230% or higher B (Pass): 210% or more, 230% or less C (fail): 210% or less
[0097] (4) Flame retardancy (burning distance) The polyurethane foam thus prepared was cut into a test piece measuring 200mm x 100mm x 10mm, held horizontally, and a flame was applied 38mm from the left end for 15 seconds, and the burning distance from the A mark (38mm from the left end) was measured. The test was repeated 10 times, and the maximum value was recorded as the burning distance of the test piece. A (pass): Less than 51 mm B (pass): 51mm or more, less than 127mm C (fail): 127mm or more
[0098] (5) Heat aging test: Tensile breaking strength retention rate (unit: %) The polyurethane foam thus produced was kept in a Geer oven at 150°C for 72 hours, and then the tensile breaking strength was measured using a method in accordance with JIS K-6400. Using the tensile breaking strength measured by the above method, the tensile breaking strength retention was calculated according to the following formula. Tensile breaking strength after heat resistance test / Tensile breaking strength before heat resistance test x 100 A (pass): 90% or more B (Pass): 70% or more, less than 90% C (Fail): Less than 70%
[0099] (6) Heat resistance test: Tensile elongation retention at break (unit: %) The polyurethane foam thus produced was kept in a Geer oven at 150°C for 30 hours, and then the tensile elongation at break was measured using a method in accordance with JIS K-6400. Using the tensile elongation at break measured by the above method, the retention of tensile elongation at break was calculated according to the following formula. Tensile elongation at break after heat resistance test / Tensile elongation at break before heat resistance test x 100 A (pass): 90% or more B (Pass): 70% or more, less than 90% C (Fail): Less than 70%
[0100] (7) Heat resistance test: flame retardancy (burning distance) The polyurethane foam thus produced was kept in a gear oven at 150℃ for 30 hours, and then cut into test pieces measuring 200mm x 100mm x 10mm, held horizontally, and a flame was applied 38mm from the left end for 15 seconds, and the burning distance from the A mark (38mm from the left end) was measured. The test was repeated 10 times, and the maximum value was recorded as the burning distance of the test piece. A (pass): Less than 51 mm B (pass): 51mm or more, less than 127mm C (fail): 127mm or more
[0101] Example 8. According to the above-mentioned method for preparing polyurethane foam, a polyurethane foam was prepared using the chlorine-containing polyether polyol composition [A-1] and evaluated. The polyurethane foam had excellent tensile strength at break, tensile elongation at break, flame retardancy, and heat resistance.
[0102] Example 9. According to the above-mentioned polyurethane foam preparation method, a polyurethane foam was prepared using the chlorine-containing polyether polyol composition [A-2] and evaluated. The polyurethane foam was excellent in moldability, tensile strength at break, tensile elongation at break, flame retardancy, and heat resistance.
[0103] Example 10. According to the above-mentioned polyurethane foam preparation method, a polyurethane foam was prepared using the chlorine-containing polyether polyol composition [A-3] and evaluated. The polyurethane foam was excellent in moldability, flame retardancy, and heat resistance.
[0104] Example 11. According to the above-mentioned polyurethane foam preparation method, a polyurethane foam was prepared using the chlorine-containing polyether polyol composition [A-4] and evaluated. The polyurethane foam was excellent in moldability, tensile strength at break, tensile elongation at break, and flame retardancy.
[0105] Example 12. According to the above-mentioned polyurethane foam preparation method, a polyurethane foam was prepared using the chlorine-containing polyether polyol composition [A-5] and evaluated. The polyurethane foam was excellent in moldability, flame retardancy, and heat resistance.
[0106] Example 13. According to the above-mentioned polyurethane foam preparation method, a polyurethane foam was prepared using the chlorine-containing polyether polyol composition [A-6] and evaluated. The polyurethane foam had excellent tensile elongation at break, flame retardancy, and heat resistance.
[0107] Example 14. According to the above-mentioned polyurethane foam preparation method, a polyurethane foam was prepared using the chlorine-containing polyether polyol composition [A-7] and evaluated. The polyurethane foam was excellent in moldability, flame retardancy, and heat resistance.
[0108] The results of Examples 8 to 14 are shown in Table 3.
[0109] [Table 3]
[0110] Comparative Example 3. According to the above-mentioned method for preparing a polyurethane foam, a polyurethane foam was prepared without using a chlorine-containing polyether polyol composition, and was evaluated. The polyurethane foam had excellent moldability and heat resistance, but was inferior in tensile strength at break, tensile elongation at break, and flame retardancy.
[0111] Comparative Example 4. A polyurethane foam was produced and evaluated in the same manner as in Comparative Example 3, except that 3 parts by weight of Epomic R-140 was added to 100 parts by weight of general-purpose PPG. The polyurethane foam was excellent in moldability and heat resistance, but was poor in tensile breaking strength, tensile breaking elongation, and flame retardancy.
[0112] Comparative Example 5. According to the above-mentioned polyurethane foam preparation method, an attempt was made to prepare a polyurethane foam using the chlorine-containing polyether polyol composition [B-1], but due to poor moldability, it was not possible to measure the physical properties.
[0113] Comparative Example 6. According to the above-mentioned polyurethane foam preparation method, a polyurethane foam was prepared using the chlorine-containing polyether polyol composition [B-2] and evaluated. The polyurethane foam was excellent in moldability, tensile strength at break, and tensile elongation at break, but was poor in heat resistance.
[0114] The results of Comparative Examples 3 to 6 are shown in Table 4.
[0115] [Table 4]
Claims
1. The composition contains 0.5 to 20 parts by weight of an epoxy compound relative to 100 parts by weight of a chlorine-containing polyether polyol having a molecular weight of 400 to 5000, The molecular weight (unit: g / mol) of the chlorine-containing polyether polyol is a value calculated by the following formula, where d (unit: mgKOH / g) is the hydroxyl value of the chlorine-containing polyether polyol measured by the method described in JIS K-1557, and e is the number of functional groups of the chlorine-containing polyether polyol. Molecular weight = (56100 / d) x e
2. The chlorine-containing polyether polyol composition according to claim 1, wherein the chlorine-containing polyether polyol is a compound represented by the following formula (1): 【Chemistry 1】 (In the above formula (1), R 1 represents a hydroxy compound residue having a molecular weight of 100 or more and 2500 or less, n represents an integer of 1 or more and less than 25, and m represents 2 or 3.
3. 2. The chlorine-containing polyether polyol composition according to claim 1, wherein the epoxy compound is a liquid epoxy compound having an epoxy equivalent of 100 to 1,000.
4. The chlorine-containing polyether polyol composition according to claim 1, which contains 1 to 100 ppm of an aluminum compound.
5. The chlorine-containing polyether polyol composition of claim 4, wherein the aluminum compound is aluminum hydroxide.
6. A polyurethane which is a reaction product of the chlorine-containing polyether polyol composition according to claim 1 and an isocyanate compound.
Citation Information
Patent Citations
Impact resistance-enhanced chlorinated polyether material and preparation method thereof
CN107815085A
Capsaicin antifouling paint
CN110484139A
JP1969014590B
Adhesive composition
JP1990202573A